Method for detecting infiltration effect of lithium ion battery pole piece

By testing the voltage and AC resistance of lithium-ion batteries, we can determine the infiltration effect of the pole sheet, which solves the accidental and safety hazards of the existing detection methods, achieves more accurate infiltration evaluation and improves battery consistency, and avoids the entry of defective products into the chemical equipment , ensuring safety and production efficiency.

CN119086354APending Publication Date: 2024-12-06天能新能源(湖州)有限公司
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411128470.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing lithium-ion battery pole infiltration effect detection methods have accidental, destructive and safety hazards, and cannot fully reflect the batch conditions, resulting in unqualified products flowing into subsequent processes or into users, and improper operation may cause safety problems.

Method used

By testing the voltage and AC resistance of the lithium-ion battery, it is determined that the battery pole plate is infiltrated. When the voltage is greater than 0.121V and the AC internal resistance is less than 0.606mΩ, it is determined that the infiltration is completed. Avoid disassembly of the battery for detection and a non-destructive test method is used.

Benefits of technology

It achieves a more accurate evaluation of the pole sheet wetting effect before the chemical formation, improves battery consistency and reliability, reduces the entry of defective products into the chemical formation equipment, avoids safety risks, and improves process parameter verification efficiency and accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086354A_ABST
    Figure CN119086354A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and particularly relates to a method for detecting the infiltration effect of a lithium ion battery pole piece. According to the method, whether the battery cell is fully infiltrated or not is judged in a mode of testing the voltage and the alternating-current internal resistance, and non-destructive testing is adopted, so that scrapping caused by disassembling the battery cell is avoided, and potential safety hazards existing in the disassembling process are eliminated; the standard of sufficient cell infiltration is formulated according to the lower limit of voltage and the upper limit of internal resistance, the setting method is simple, complicated calculation is not needed, full inspection can be performed on the cells in the production process, and contingency caused by disassembling individual cells to confirm the infiltration effect is completely eradicated; the wettability of the pole piece is detected by adopting test voltage and alternating-current internal resistance before the battery cell is formed, so that defects such as pseudo soldering, internal short circuit, positive and negative electrode reverse welding or reverse entering of a roll core into a shell, no liquid injection and the like generated in the previous process can be recognized in advance, defective products entering formation equipment for charging are reduced, safety risks can be avoided, and the formation productivity can be ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lithium-ion batteries, and specifically relates to a method for detecting the wetting effect of a lithium-ion battery electrode. Background Art

[0002] With the shortage of oil resources and the improvement of consumers' environmental awareness, lithium-ion batteries, as the representative of new energy, have received unprecedented attention and development. In recent years, the research and development and manufacturing levels of lithium-ion batteries have achieved a qualitative leap, and consumers' demand and quality requirements for lithium-ion battery products are also increasing. This requires battery cell manufacturers to improve product yield and performance while increasing production capacity.

[0003] In the process of preparing the battery cell, after the injection step is completed, a high-temperature standing method is usually used to promote the absorption of the electrolyte by the electrode. The quality of this absorption process is directly related to the effect of the subsequent battery formation, which in turn affects the overall performance of the battery cell. In practice, the detection of the wetting effect of the lithium-ion battery electrode mostly adopts the method of post-sampling inspection. Specifically, by disassembling the batteries sampled from the same batch and observing the black spots on the surface of the electrode, it is judged and controlled whether the high-temperature standing time is appropriate. Furthermore, according to the inspection results, the high-temperature standing time can be adjusted in the opposite direction to improve the electrolyte infiltration effect of the battery electrode thereafter, thereby improving the performance of the battery cell.

[0004] However, the above-mentioned detection method of the wetting effect of lithium-ion battery pole pieces has the following problems. Since the random inspection only tests a part of the samples, it may not be able to fully reflect the actual conditions of all battery cells. Therefore, the test results are accidental and cannot fully represent the quality status of the entire batch. Unqualified products are easy to flow into subsequent processes or the hands of end users. Random inspection is a destructive testing method, which means that the disassembled battery cells can no longer be used, which leads to a waste of cost. More importantly, if the battery cells are disassembled improperly, it may cause safety problems such as battery short circuit, thermal runaway or even explosion, posing a safety hazard. Summary of the invention

[0005] In order to solve the above technical problems, the application provides a method for detecting the wetting effect of a lithium-ion battery electrode, which is specifically achieved through the following technical solutions: A method for detecting the wetting effect of a lithium-ion battery pole piece comprises the following steps: during the process of lithium-ion battery pole piece wetting, testing the voltage and AC resistance of the lithium-ion battery; when the voltage test value is greater than 0.121V and the AC internal resistance is less than 0.606mΩ, determining that the battery pole piece wetting is completed.

[0006] In the preparation process of lithium-ion batteries, the performance measurement of the voltage and AC resistance after the battery is formed is an important indicator for evaluating the overall performance of lithium-ion batteries. However, the factors that affect the performance of lithium-ion batteries are numerous and complex, including the properties of active materials, the composition of the electrolyte, the characteristics of the diaphragm, and the specific manufacturing process. There is currently no more scientific standard for judging whether the electrode is sufficiently wetted by testing the charge and discharge performance of the battery cell. In view of this, the present application proposes a method for detecting the wetting effect of lithium-ion battery electrode pieces on the basis of clarifying the relationship between key parameters such as AC internal resistance and voltage and the wetting effect of battery electrode pieces; this method helps to more accurately evaluate the wetting effect of lithium-ion battery electrode pieces before formation, and can instantly obtain the electrolyte wetting effect of real-time electrode pieces without disassembly, which can improve the consistency and reliability of lithium-ion batteries to a certain extent and improve the efficiency of lithium-ion battery preparation.

[0007] Preferably, the raw materials for preparing the positive electrode plate of the lithium-ion battery include, by weight, 92-96 parts of lithium iron phosphate, 1-3 parts of conductive carbon black, 0.5-2 parts of carbon nanotubes and 1-3 parts of polyvinylidene fluoride binder.

[0008] As a further preference, the raw materials for preparing the positive electrode plate of the lithium-ion battery include, by weight, 95 parts of lithium iron phosphate, 2 parts of conductive carbon black, 1 part of carbon nanotubes and 2 parts of polyvinylidene fluoride binder.

[0009] Preferably, the positive electrode sheet coating surface density is 380-385 g / m 2 , compacted density is 2.1~2.4g / cm 3 .

[0010] As a further preferred embodiment, the positive electrode sheet coating surface density is 382 g / m 2 , compacted density is 2.27g / cm 3 .

[0011] Preferably, the raw materials for preparing the negative electrode plate of the lithium ion battery include, by weight, 94-97 parts of graphite, 1-2 parts of conductive carbon black, 1-2 parts of carboxymethyl cellulose, and 1-3 parts of styrene-butadiene rubber.

[0012] As a further preference, the raw materials for preparing the negative electrode plate of the lithium ion battery include, by weight, 95 parts of graphite, 1.5 parts of conductive carbon black, 1.5 parts of carboxymethyl cellulose, and 2 parts of styrene-butadiene rubber.

[0013] Preferably, the negative electrode sheet coating surface density is 172-176 g / m 2 , compacted density is 1.3~1.7g / cm 3 .

[0014] As a further preferred embodiment, the negative electrode sheet coating surface density is 174 g / m 2 , compacted density is 1.5g / cm 3 .

[0015] Preferably, the soaking temperature is 45-55°C.

[0016] As further preferred, the soaking temperature is 45°C.

[0017] Preferably, the method is characterized in that the voltage and AC resistance of the lithium-ion battery are intermittently tested.

[0018] Preferably, the initial test is started when the lithium-ion battery electrode has been soaked for 8 hours, and then the voltage and AC resistance of the lithium-ion battery are intermittently tested at integer multiples of 4 hours until the lithium-ion battery electrode has been soaked for 48 hours.

[0019] A method for preparing a lithium-ion battery comprises: during the lithium-ion battery infiltration process, using any of the above-mentioned methods to detect the infiltration effect of the lithium-ion battery pole piece.

[0020] Preferably, after the wetting effect of the lithium-ion battery pole piece is detected, the lithium-ion batteries that meet the conditions are screened out for formation treatment.

[0021] Compared with the prior art, this application has the following beneficial effects: The present application adopts the method of testing voltage and AC internal resistance to determine whether the battery cell is sufficiently wetted. It is a non-destructive test, which avoids the scrapping caused by disassembling the battery cell and eliminates the safety hazards in the disassembly process. The standard for sufficient battery cell wettability is formulated according to the voltage lower limit and internal resistance upper limit standards. The setting method is simple and does not require complicated calculations. The battery cells in the production process can be fully inspected, eliminating the randomness caused by disassembling individual battery cells to confirm the wetting effect. Before the battery cell is formed, the test voltage and AC internal resistance are used to detect the wettability of the electrode. The defects such as cold soldering, internal short circuit, reverse welding of positive and negative electrodes or reverse winding of the core into the shell, and no liquid injection generated in the previous process can be identified in advance, reducing the number of defective products entering the formation equipment for charging, avoiding safety risks and ensuring the formation capacity. This method is applicable to soft-pack, aluminum shell, and cylindrical battery cells. Regardless of whether the battery cells are made by the winding process or the stacking process, once the wetting time is verified using this method for the first batch, the parameters can be solidified for mass production, which can improve the efficiency and accuracy of process parameter verification. Similarly, if a certain material is changed during the product design process, the coating surface density, electrode compaction density, etc. are changed, this method can be used to evaluate the electrode wetting effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to clearly illustrate the embodiments, the drawings of the accompanying drawings are briefly introduced below: Figure 1This is a graph showing the surface of the electrode sheet when the lithium-ion battery electrolyte is immersed for 16 hours in performance test 1 of this application; Figure 2 This is a graph showing the surface of the electrode sheet when the lithium-ion battery electrolyte is immersed for 36 hours in performance test 1 of this application; Figure 3 This is a diagram of the surface of the electrode sheet when the lithium-ion battery is immersed in the electrolyte for 20 hours in performance test 2 of this application; Figure 4 This is a diagram of the electrode surface condition when the lithium-ion battery was immersed in the electrolyte for 40 hours in performance test 2 of this application. DETAILED DESCRIPTION

[0023] The present application will be further described below in the form of specific embodiments. Those of ordinary skill in the art will be able to implement the present application based on these descriptions. In addition, the embodiments of the present application involved in the following description are generally only embodiments of a part of the present application, rather than all embodiments. Therefore, based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present application.

[0024] Example 1 This embodiment discloses a method for detecting the wetting effect of a lithium-ion battery electrode. Specifically, the raw materials for preparing the positive electrode of the lithium-ion battery in this embodiment and their weight parts are 95 parts of lithium iron phosphate, 2 parts of conductive carbon black, 1 part of carbon nanotubes and 2 parts of polyvinylidene fluoride binder. The coating surface density of the positive electrode is 382g / m 2 , compacted density is 2.27g / cm 3 The raw materials for preparing the negative electrode of lithium-ion batteries include 95 parts of graphite, 1.5 parts of conductive carbon black, 1.5 parts of carboxymethyl cellulose, and 2 parts of styrene-butadiene rubber. The coating surface density of the negative electrode is 174g / m 2 , compacted density is 1.5g / cm 3 After the battery is filled with liquid, it is placed at 45°C. After 8 hours of placement, the AC internal resistance and voltage of the battery are tested. Thereafter, the test is performed every 4 hours until 48 hours. The specific test methods for AC internal resistance and voltage are conventional technical means and will not be described in detail here.

[0025] Example 2 This embodiment discloses a method for detecting the wetting effect of a lithium-ion battery electrode. Specifically, the raw materials for preparing the positive electrode of the lithium-ion battery in this embodiment and their weight parts are 95 parts of lithium iron phosphate, 2 parts of conductive carbon black, 1 part of carbon nanotubes and 2 parts of polyvinylidene fluoride binder. The coating surface density of the positive electrode is 382g / m 2 , compacted density is 2.4g / cm 3The raw materials for preparing the negative electrode of lithium-ion batteries include 95 parts of graphite, 1.5 parts of conductive carbon black, 1.5 parts of carboxymethyl cellulose, and 2 parts of styrene-butadiene rubber. The coating surface density of the negative electrode is 174g / m 2 , compacted density is 1.5g / cm 3 After the battery is filled with liquid, it is placed at 45°C. After 8 hours of placement, the AC internal resistance and voltage of the battery are tested. Thereafter, the test is performed every 4 hours until 48 hours. The specific test methods for AC internal resistance and voltage are conventional technical means and will not be described in detail here.

[0026] Example 3 This embodiment discloses a method for detecting the wetting effect of a lithium-ion battery electrode. Specifically, the raw materials for preparing the positive electrode of the lithium-ion battery in this embodiment are 92 parts of lithium iron phosphate, 3 parts of conductive carbon black, 2 parts of carbon nanotubes and 3 parts of polyvinylidene fluoride binder. The coating surface density of the positive electrode is 380g / m 2 , compacted density is 2.1g / cm 3 The raw materials for preparing the negative electrode of lithium-ion batteries include 94 parts of graphite, 1 part of conductive carbon black, 2 parts of carboxymethyl cellulose, and 3 parts of styrene-butadiene rubber. The coating surface density of the negative electrode is 172g / m 2 , compacted density is 1.3g / cm 3 After the battery is filled with liquid, it is placed at a high temperature of 50°C. After 8 hours of placement, the AC internal resistance and voltage of the battery are tested. Thereafter, the test is performed every 4 hours until 48 hours. The specific test methods for AC internal resistance and voltage are conventional technical means and will not be described in detail here.

[0027] Example 4 This embodiment discloses a method for detecting the wetting effect of a lithium-ion battery electrode. Specifically, the raw materials and weight percentages of the preparation of the positive electrode of the lithium-ion battery in this embodiment are 96 parts of lithium iron phosphate, 1 part of conductive carbon black, 2 parts of carbon nanotubes and 1 part of polyvinylidene fluoride binder. The coating surface density of the positive electrode is 385g / m 2 , compacted density is 2.2g / cm 3 The raw materials for preparing the negative electrode of lithium-ion batteries include 97 parts of graphite, 1 part of conductive carbon black, 1 part of carboxymethyl cellulose, and 1 part of styrene-butadiene rubber. The coating surface density of the negative electrode is 176g / m 2 , compacted density is 1.7g / cm 3 After the battery is filled with liquid, it is placed at 55°C. After 8 hours of placement, the AC internal resistance and voltage of the battery are tested. Thereafter, the test is performed every 4 hours until 48 hours. The specific test methods for AC internal resistance and voltage are conventional technical means and will not be described in detail here.

[0028] Example 5 This embodiment discloses a method for preparing a lithium-ion battery, including a method for detecting the wetting effect of a battery pole piece and a battery formation step. In this embodiment, the raw materials for preparing the positive pole piece of the lithium-ion battery are 96 parts of lithium iron phosphate, 1 part of conductive carbon black, 2 parts of carbon nanotubes and 1 part of polyvinylidene fluoride binder. The coating surface density of the positive pole piece is 385g / m 2 , compacted density is 2.2g / cm 3 The raw materials for preparing the negative electrode of lithium-ion batteries include 97 parts of graphite, 1 part of conductive carbon black, 1 part of carboxymethyl cellulose, and 1 part of styrene-butadiene rubber. The coating surface density of the negative electrode is 176g / m 2 , compacted density is 1.7g / cm 3 In this embodiment, the method for detecting the wetting effect of the battery pole piece is as follows: after the battery cell is filled with liquid, it is placed at a high temperature of 55°C, and the AC internal resistance and voltage of the battery cell are tested after 8 hours of placement, and then the test is performed every 4 hours until the test is completed at 48 hours. The specific test method of the AC internal resistance and voltage is a conventional technical means and will not be described in detail here.

[0029] Performance Test 1 This performance test is intended to verify the effectiveness of the lithium-ion battery electrode plate wetting effect detection method disclosed in Example 1. The test results of the AC internal resistance and voltage during the interval time of Example 1 are summarized as follows: Table 1. AC internal resistance and voltage of Example 1 Standing time 8H 12H 16H 20H 24H 28H 32H 36H 40H 44H 48H AC internal resistance (mΩ) 0.910 0.873 0.742 0.673 0.636 0.631 0.624 0.606 0.605 0.606 0.604 Measured voltage (V) 0.078 0.081 0.093 0.097 0.104 0.112 0.116 0.121 0.122 0.124 0.124 By observing the above table, we can find that as the standing time continues to increase, the AC internal resistance of the lithium-ion battery continues to decrease, while the open circuit voltage continues to rise. This trend shows that inside the battery, the electrochemical reaction gradually tends to a stable state. It is particularly noteworthy that after standing for 36 hours, the changes in the open circuit voltage and AC internal resistance of the battery become very small and can almost be considered stable. This means that after 36 hours of high-temperature standing, the battery's pole piece has been fully infiltrated in the electrolyte and has reached a relatively stable state. This discovery is of great significance for understanding the trend of battery performance changes over time and optimizing battery manufacturing processes.

[0030] Furthermore, this performance test screened out cells with a voltage greater than 0.121V and an internal resistance less than 0.606mΩ for formation charging and activation. The cells that had been kept at high temperature for 16h and 36h were fully charged with a current of 0.5C and then disassembled. The appearance of the pole pieces after disassembly is as follows: Figure 1 and Figure 2As shown. From the appearance, it can be seen that the battery cells that have been kept at high temperature for 16 hours have black spots on the surface of the negative electrode due to insufficient infiltration; in contrast, the battery cells that have been kept at high temperature for 36 hours have lithium embedded evenly on the surface of the pole piece, with consistent color, indicating sufficient infiltration. It can be seen that there is an obvious corresponding relationship between the voltage and AC internal resistance test in this application and the infiltration effect. By detecting the voltage and AC internal resistance, the infiltration effect can be effectively evaluated.

[0031] Performance Test 2 This performance test is intended to verify the effectiveness of the lithium-ion battery electrode plate wetting effect detection method disclosed in Example 2. The test results of the AC internal resistance and voltage during the interval time of Example 2 are summarized as follows: Table 2. AC internal resistance and voltage of Example 2 Standing time 8H 12H 16H 20H 24H 28H 32H 36H 40H 44H 48H AC internal resistance (mΩ) 0.879 0.862 0.814 0.775 0.703 0.688 0.618 0.610 0.599 0.596 0.597 Measured voltage (V) 0.085 0.088 0.092 0.099 0.102 0.109 0.113 0.122 0.124 0.125 0.125 By observing the above table, we can find that as the standing time continues to increase, the AC internal resistance of the lithium-ion battery continues to decrease, while the open circuit voltage continues to rise. This trend shows that inside the battery, the electrochemical reaction gradually tends to a stable state. It is particularly noteworthy that after standing for 40 hours (the voltage is greater than 0.121V and the AC internal resistance is less than 0.606mΩ), the changes in the open circuit voltage and AC internal resistance of the battery become very small, and can almost be considered stable. This means that after 40 hours of high-temperature standing, the battery's pole piece has been fully infiltrated in the electrolyte and has reached a relatively stable state. This discovery is of great significance for understanding the trend of battery performance over time and optimizing battery manufacturing processes.

[0032] Furthermore, this performance test screened out cells with a voltage greater than 0.121V and an internal resistance less than 0.606mΩ for formation charging and activation. The cells that had been kept at high temperature for 20h and 40h were fully charged with a 0.5C current and then disassembled. The appearance of the pole pieces after disassembly is as follows: Figure 3 and Figure 4 As shown. From the appearance, it can be seen that the battery cells that have been kept at high temperature for 20 hours have black spots on the surface of the negative electrode due to insufficient infiltration; in contrast, the battery cells that have been kept at high temperature for 40 hours have lithium embedded evenly on the surface of the pole piece, with consistent color, indicating sufficient infiltration. It can be seen that there is an obvious correspondence between the voltage and AC internal resistance test in this application and the infiltration effect. By detecting the voltage and AC internal resistance, the infiltration effect can be effectively evaluated.

Claims

1. A method for detecting the wetting effect of a lithium-ion battery pole piece, characterized in that: The method comprises the following steps: during the process of lithium-ion battery pole piece infiltration, testing the voltage and AC resistance of the lithium-ion battery; when the voltage test value is greater than 0.121V and the AC internal resistance is less than 0.606mΩ, determining that the battery pole piece infiltration is completed.

2. A method for detecting the wetting effect of a lithium-ion battery pole piece according to claim 1, characterized in that: In terms of mass, the raw materials for preparing the positive electrode plate of the lithium-ion battery include 92 to 96 parts of lithium iron phosphate, 1 to 3 parts of conductive carbon black, 0.5 to 2 parts of carbon nanotubes and 1 to 3 parts of polyvinylidene fluoride binder.

3. A method for detecting the wetting effect of a lithium-ion battery pole piece according to claim 2, characterized in that: The positive electrode sheet coating surface density is 380-385 g / m 2 , compacted density is 2.1~2.4g / cm 3 .

4. A method for detecting the wetting effect of a lithium-ion battery pole piece according to claim 1, characterized in that: Calculated by weight, the raw materials for preparing the negative electrode plate of the lithium ion battery include 94 to 97 parts of graphite, 1 to 2 parts of conductive carbon black, 1 to 2 parts of carboxymethyl cellulose, and 1 to 3 parts of styrene-butadiene rubber.

5. A method for detecting the wetting effect of a lithium-ion battery pole piece according to claim 4, characterized in that: The negative electrode sheet coating surface density is 172-176 g / m 2 , compacted density is 1.3~1.7g / cm 3 .

6. A method for detecting the wetting effect of a lithium-ion battery pole piece according to claim 1, characterized in that: The soaking temperature is 45-55°C.

7. A method for detecting the wetting effect of a lithium-ion battery pole piece according to any one of claims 1 to 6, characterized in that: Intermittently test the voltage and AC resistance of lithium-ion batteries.

8. A method for detecting the wetting effect of a lithium-ion battery pole piece according to claim 7, characterized in that: The initial test begins when the lithium-ion battery electrode is immersed for 8 hours, and then the voltage and AC resistance of the lithium-ion battery are intermittently tested at integer multiples of 4 hours until the lithium-ion battery electrode is immersed for 48 hours.

9. A method for preparing a lithium ion battery, characterized in that: During the lithium-ion battery infiltration process, the method described in any one of claims 1 to 7 is used to detect the infiltration effect of the lithium-ion battery pole piece.

10. The method for preparing a lithium ion battery according to claim 9, characterized in that: After the lithium-ion battery electrode wetting effect test is completed, the lithium-ion batteries that meet the conditions will be screened out for formation treatment.

Citation Information

Cited By

  • Method for nondestructive analysis of overall wettability of battery

    CN119556161A

  • Battery screening method

    CN121656870A