Chelate modified polyolefin diaphragm as well as preparation method and application thereof
By using chelates formed by self-polymerization of polydopamine and metal ions on the lithium-ion battery separator, the problems of insufficient thermal deformation, wetting and mechanical strength of the separator are solved, the chemical stability and safety of the battery are improved, and the Fast conduction of lithium ions and high-efficiency electrolyte wetting.
Patent Information
- Application Number
- CN202411145326.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The thermal deformation temperature of lithium-ion battery separators is low, the electrolyte wettability and insufficient mechanical strength, resulting in safety and performance problems. The existing modification methods hinder lithium ion conduction while improving the performance of the separator, affecting the high polarization of the battery and Low power output.
Polydopamine chelates and metal ions are self-polymerized under weak alkaline conditions to form polydopamine chelates. By growing in situ on the surface of polyolefin separators, the chemical stability, electrolyte wetting and thermal stability of the separators are improved. sex.
It significantly improves the chemical stability and thermal stability of the diaphragm, improves the wetting properties of the electrolyte and lithium ion conduction, enhances the safety and performance of the battery, and reduces resource consumption and environmental pollution.
Smart Images

Figure CN119092934A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a chelate-modified polyolefin diaphragm and a preparation method and application thereof. Background Art
[0002] Thanks to its advantages such as high energy, high cost-effectiveness, long life and low pollution, lithium-ion batteries have become the backbone of the new energy battery industry and are widely used in new energy vehicles, energy storage power stations, consumer electronics and other fields.
[0003] Lithium-ion batteries are mainly composed of positive electrodes, negative electrodes, separators, electrolytes, current collectors and packaging materials. As one of the important components of lithium-ion batteries, the separator is closely related to the safety performance, life span and sustainable energy storage of the battery. A separator with excellent performance is required to have excellent insulation, excellent electrochemical stability, high thermal stability, suitable pore size and porosity, good mechanical strength and electrolyte wettability, etc.
[0004] At present, the production materials of lithium-ion battery separators for large-scale commercialization are mainly polyolefins, including polypropylene (PP), polyethylene (PE), and polypropylene (PP) and polyethylene (PE) composite materials. As a commonly used separator material in lithium-ion batteries, although polyolefin battery separators have many advantages, they also have some disadvantages:
[0005] (1) The heat deformation temperature of polyolefin separators is relatively low. For example, the heat deformation temperature of polypropylene is about 100°C, while that of polyethylene is less than 80°C. At relatively low temperatures, polyolefins will melt and flow, causing the pores of the microporous membrane to change, or even causing the separator to rupture, making it impossible to isolate the positive and negative electrodes, resulting in a short circuit inside the battery and leading to safety accidents.
[0006] (2) The wettability of polyolefin separators to polar electrolytes is poor. Since polyolefin separators do not contain polar groups in their molecular chain structure, they have poor affinity with commonly used ester and ether electrolytes, resulting in low liquid absorption rate of micropores and affecting ion transmission efficiency.
[0007] (3) The mechanical strength of polyolefin separator is poor. During the charge and discharge cycle of lithium battery, due to excessive charging rate, over-discharge, temperature change, Li + Factors such as uneven current distribution will cause lithium dendrites to form at the negative electrode of the battery. Polyolefins have poor puncture resistance and are easily pierced by lithium dendrites, causing the battery to short-circuit.
[0008] In order to improve the comprehensive performance of polyolefin separators, the industry has adopted the surface coating modification method of inorganic or organic materials such as boehmite, alumina, polyvinylidene fluoride, and aramid on a large scale. However, these dense coatings formed on the separators can easily block the pores of the separators, hindering the effective migration of lithium ions on the composite separators, resulting in high polarization and low power output of lithium-ion batteries. In addition, these improved separators can only be used at limited current densities (<2mA / cm 2 ) to achieve stable lithium plating / stripping behavior. Moreover, under the existing coating process, the thickness of the single-side coating layer is basically above 1μm, which is not conducive to the high capacity and lightweight of the battery.
[0009] Therefore, there is an urgent need to study the high-performance modification methods of the diaphragm so that the polyolefin diaphragm has both good thermal stability and sufficient ion conduction channels, which can not only ensure the rapid transmission of lithium ions but also improve the safety of the battery.
[0010] At present, there is also an existing technology that improves the battery performance of some polyolefin separators by in situ polymerization of dopamine on the surface of polyolefin separators such as PE and PP. However, the self-assembled polymerized polydopamine has poor chemical stability in ester and ether electrolytes and is prone to depolymerization, which affects the long-term cycle performance of the battery. Summary of the invention
[0011] In view of the above-mentioned deficiencies in the prior art, the present invention provides a chelate-modified polyolefin diaphragm and a preparation method and application thereof.
[0012] The present invention first provides a method for preparing a chelate-modified polyolefin membrane, wherein the chelate is a polydopamine chelate, and the preparation method comprises the following steps:
[0013] (1) dissolving a pH buffer, a water-soluble metal salt, and a water-soluble oxidant in water, controlling the pH to be between 7.5 and 8.5, and adding dopamine hydrochloride to dissolve to obtain a modified precursor solution;
[0014] (2) taking a polyolefin membrane and adding it into the modified precursor solution obtained in step (1), and letting it stand to obtain the chelate-modified polyolefin membrane.
[0015] Dopamine starts to polymerize after being added to the solution, so it is best to fully dissolve other reagents before adding dopamine. In a weakly alkaline metal salt solution, dopamine self-polymerizes and chelates with metal ions to form polydopamine chelates. Thanks to the strong adhesion of polydopamine chelates, they can grow in situ on the surface of polyolefin membranes to obtain chelate-modified polyolefin membranes.
[0016] Preferably, the pH buffer is at least one of phosphate buffer, borax buffer, sodium barbital buffer, tris(hydroxymethylaminomethane) buffer (Tris buffer), and ammonia buffer. The pH buffer is used to maintain the pH value of the solution in the range of 7.5 to 8.5. The preferred pH is around 8.5, under which weakly alkaline conditions the polymerization rate and yield of dopamine are the best.
[0017] The water-soluble metal salt is used to provide metal ions. Preferably, the water-soluble metal salt is at least one of lithium salts, copper salts, aluminum salts, zinc salts, cobalt salts, iron salts, cerium salts, zirconium salts, and nickel salts. The anion in the water-soluble metal salt is selected from at least one of sulfates, hydrochlorides, and nitrates. More preferably, the sulfate metal salt is at least one of lithium sulfate, copper sulfate, aluminum sulfate, zinc sulfate, nickel sulfate, and their respective hydrates.
[0018] The water-soluble oxidant promotes the self-polymerization of dopamine. Preferably, the water-soluble oxidant is at least one of persulfate, potassium permanganate, potassium perchlorate, and potassium dichromate. The persulfate is at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.
[0019] Preferably, the molar ratio of metal ions to dopamine hydrochloride in the water-soluble metal salt is not less than 1:2. The chelation ratio of metal ions to dopamine hydrochloride is 1:2, generally two dopamine hydrochlorides are chelated with one metal ion, and to ensure complete chelation reaction, the water-soluble metal salt is preferably added in a slightly excessive amount.
[0020] Preferably, in step (2), the polyolefin membrane is one of a polypropylene membrane, a polyethylene membrane, and a composite membrane of polyethylene and polypropylene.
[0021] Preferably, in step (2), the temperature during standing is 20-60°C and the standing time is 2-48 hours. More preferably, the temperature during standing is 25°C and the standing time is 24 hours. Generally speaking, the longer the reaction time and the higher the temperature, the faster the in-situ growth rate and the thicker the generated film, but the thickness of the film has an upper limit and will not grow further after reaching a certain thickness.
[0022] Preferably, the chelate-modified polyolefin membrane obtained after standing in step (2) is further cleaned and dried.
[0023] The invention further provides a chelate-modified polyolefin diaphragm prepared by the preparation method.
[0024] The present invention also provides application of the chelate-modified polyolefin separator in preparing a lithium battery.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) Improving the chemical stability of the modified membrane: The present invention transforms the original weakly interacting π-π stacking structure of polydopamine into a strongly interacting coordination bonding structure by chelating polydopamine with metal ions, thereby greatly improving the chemical stability of the modified membrane in the electrolyte;
[0027] (2) Improve the wettability of polyolefin diaphragm electrolyte: Polydopamine chelate contains rich catechol and amino functional groups and has good affinity for polar electrolytes such as esters and ethers, which can improve the wettability and liquid retention rate of the diaphragm electrolyte;
[0028] (3) Improve the thermal stability of the separator: PDA chelates have high thermal stability and strength, which can enhance the separator's resistance to thermal shrinkage and improve the safety of battery use;
[0029] (4) Reduce resource consumption and environmental pollution: Through the research and application transformation of room temperature aqueous synthesis of PDA chelates, it is expected to reduce resource consumption and environmental pollution and promote the green production and sustainable development of modified diaphragms. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a scanning electron microscope image, where Figure 1 (a) is a commercial polypropylene diaphragm. Figure 1 (b) is the polydopamine modified membrane prepared in Example 3, Figure 1 (c) is the polydopamine nickel chelate modified diaphragm prepared in Example 2; Figure 1 (d) is the polydopamine copper chelate modified diaphragm prepared in Example 1.
[0031] Figure 2 Digital photo of the electrolyte wettability test.
[0032] Figure 3 Digital photo of the electrolyte resistance test of the separator modified layer.
[0033] Figure 4 Digital photos for heat shrink performance testing.
[0034] Figure 5 This is a graph of the cycle performance of button batteries. DETAILED DESCRIPTION
[0035] The present invention is described in detail below in conjunction with the accompanying drawings and examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment involved in the present invention are conventional reagents, methods and equipment in the technical field.
[0036] Example 1
[0037] Preparation of polydopamine copper chelate modified membrane (PP@PDA(Cu)):
[0038] 5.5 g of tris(hydroxymethyl)aminomethane, 4.8 g of copper sulfate pentahydrate, and 3.6 g of ammonium persulfate were added to 900 ml of deionized water, and after stirring and dissolving, the pH was adjusted to 8.5 with dilute hydrochloric acid, and 1.8 g of dopamine hydrochloride was added, and the mixture was stirred and dissolved again to obtain a modified precursor solution;
[0039] Take 0.02m 2 A polypropylene (PP) diaphragm was added to the modified precursor solution and allowed to react at 25°C for 24 hours to obtain a polyolefin diaphragm modified in situ with polydopamine copper chelate.
[0040] The polydopamine copper chelate modified membrane was washed with deionized water for 4 times, and then placed in a 50° C. vacuum oven to dry for 24 h. The dried modified membrane was cut into discs with a diameter of 19 mm.
[0041] Application of polydopamine copper chelate modified diaphragm in lithium battery:
[0042] LiFePO4 is used as the positive electrode, lithium sheet is used as the negative electrode, polydopamine copper chelate modified diaphragm is used as the battery diaphragm, electrolyte is added dropwise, and button batteries are assembled.
[0043] Example 2
[0044] Preparation of polydopamine nickel chelate modified membrane (PP@PDA(Ni)):
[0045] 5.5 g of tris(hydroxymethyl)aminomethane, 5.0 g of nickel sulfate hexahydrate, and 3.6 g of ammonium persulfate were added to 900 ml of deionized water, and after stirring and dissolving, the pH was adjusted to 7.5 with dilute hydrochloric acid, and 1.8 g of dopamine hydrochloride was added, and the mixture was stirred and dissolved again to obtain a modified precursor solution;
[0046] Take 0.02m 2 A polypropylene (PP) diaphragm was added to the modified precursor solution and allowed to react at 25°C for 24 hours to obtain a polyolefin diaphragm modified in situ with polydopamine nickel chelate;
[0047] The polydopamine nickel chelate modified membrane was washed with deionized water for 4 times, and then placed in a 50° C. vacuum oven to dry for 24 h. The dried modified membrane was cut into discs with a diameter of 19 mm.
[0048] Application of polydopamine nickel chelate modified diaphragm in lithium battery:
[0049] LiFePO4 is used as the positive electrode, lithium sheet is used as the negative electrode, polydopamine nickel chelate modified diaphragm is used as the battery diaphragm, electrolyte is added dropwise, and button batteries are assembled.
[0050] Example 3
[0051] Preparation of polydopamine modified membrane (PP@PDA):
[0052] 5.5 g of tris(hydroxymethyl)aminomethane) and 3.6 g of ammonium persulfate were added to 900 ml of deionized water, and after stirring and dissolving, the pH was adjusted to 8.5 with dilute hydrochloric acid, and 1.8 g of dopamine hydrochloride was added, and the mixture was stirred and dissolved again to obtain a modified precursor solution;
[0053] Take 0.02m 2 A polypropylene (PP) diaphragm is added to the modified precursor solution, and allowed to react at 25°C for 24 hours to obtain a polydopamine-modified polyolefin diaphragm;
[0054] The polydopamine modified membrane was washed with deionized water for 4 times, and then placed in a vacuum oven at 50° C. to dry for 24 h. The dried modified membrane was cut into discs with a diameter of 19 mm.
[0055] Application of polydopamine modified diaphragm in lithium battery:
[0056] LiFePO4 is used as the positive electrode, lithium sheet is used as the negative electrode, polydopamine modified diaphragm is used as the battery diaphragm, electrolyte is added dropwise, and button batteries are assembled.
[0057] Example 4
[0058] Preparation of polypropylene separator (PP) assembled battery:
[0059] Take LiFePO4 as the positive electrode, lithium sheet as the negative electrode, polypropylene diaphragm as the battery diaphragm, add electrolyte, and assemble into a button battery.
[0060] Test Example 1
[0061] 1. Experimental Materials
[0062] The polydopamine copper chelate modified membrane prepared under the conditions of Example 1 and the battery assembled with the polydopamine copper chelate modified membrane, the polydopamine nickel chelate modified membrane prepared under the conditions of Example 2 and the battery assembled with the polydopamine nickel chelate modified membrane, the polydopamine modified membrane prepared under the conditions of Example 3 and the battery assembled with the polydopamine modified membrane, and the polypropylene membrane of Example 4 and the battery assembled with the polypropylene membrane were used as experimental materials.
[0063] 2. Experimental methods
[0064] 1) Scanning electron microscopy:
[0065] The membranes in Examples 1-4 were respectively adhered to an electron microscope sample stage with conductive adhesive, and placed in a gold spraying device for gold spraying. The morphology of the samples was then observed using a scanning electron microscope (Scios2 Hivac) at a voltage of 10 KV and a magnification of 20,000 times.
[0066] 2) Electrolyte wettability:
[0067] 5 μL of electrolyte was dropped onto a 19 mm diaphragm disc. After 5 min, the wettability of the electrolyte on the diaphragm was observed and photographed.
[0068] 3) Electrolyte resistance:
[0069] Different modified separators were cut into discs with a diameter of 19 mm and immersed in 1 ml of electrolyte respectively. After immersion for 24 hours and 14 days, the color change of the electrolyte was observed.
[0070] 4) Heat shrinkage performance:
[0071] Place the stainless steel plate and two pieces of high temperature filter paper in the middle of the thermostat, and control the temperature so that the stainless steel plate and the high temperature filter paper reach 140±2℃ or 160±2℃. After measuring the longitudinal and transverse lengths of the diaphragm, place it flat on one of the high temperature filter papers on the stainless steel plate in the middle of the blast thermostat, and then press it with another piece of high temperature filter paper, close the thermostat door, start counting the time, and keep it at the test temperature for 30min±2min. After the heating is completed, take out the diaphragm, wait for the diaphragm to return to room temperature, measure the longitudinal and transverse lengths again, and calculate the thermal shrinkage. Repeat the test 3 times and take the average value.
[0072] 5) Cycle performance:
[0073] The button cells assembled with different separators were installed in the Xinwei battery testing system. In the rate mode, the battery was first run at 0.1C for 3 cycles to activate the battery, and then it was cycled at 0.5C.
[0074] 3. Experimental results
[0075] 1) Scanning electron microscope test: Figure 1 The figures are scanning electron microscope images, in which (a) is a commercial polypropylene membrane, (b) is a polydopamine modified membrane prepared in Example 3, (c) is a polydopamine nickel chelate modified membrane prepared in Example 2; and (d) is a polydopamine copper chelate modified membrane prepared in Example 1.
[0076] Figure 1The scanning electron microscopy results show that after modification, the pore size of the membrane decreased slightly and became more uniform due to the in-situ growth of polydopamine and polydopamine chelate on the membrane surface. Some pores of the polydopamine-modified membrane were blocked by polydopamine, while the pores of the polydopamine chelate-modified membrane were not blocked.
[0077] 2) Electrolyte wettability test: Figure 2 The following are digital photos of commercial polypropylene diaphragms and modified diaphragms after 5 μL of electrolyte was added and allowed to stand for 5 minutes. The upper left corner is a commercial polypropylene diaphragm, the upper right corner is a polydopamine modified diaphragm prepared in Example 3, the lower left corner is a polydopamine nickel chelate modified diaphragm prepared in Example 2, and the lower right corner is a polydopamine copper chelate modified diaphragm prepared in Example 1. It can be seen from the figure that compared with the unmodified commercial diaphragm, the electrolyte diffuses over a larger area on the modified diaphragm, and the electrolyte diffusion area on the polydopamine chelate modified diaphragm is larger than that on the polydopamine modified diaphragm, indicating that the polydopamine chelate modification can significantly improve the electrolyte wettability of the diaphragm.
[0078] 3) Electrolyte resistance test: Figure 3 These are digital photos of polydopamine and polydopamine chelate modified diaphragms just immersed in electrolyte, immersed for 24 hours, and immersed for 14 days. As can be seen from the figure, after the polydopamine modified diaphragm is immersed in the electrolyte for 24 hours, the electrolyte changes from colorless and transparent to brown. This is because polydopamine is unstable in the electrolyte and will depolymerize into small molecular polymers, which will dissolve in the electrolyte and change the color of the electrolyte. However, after the polydopamine chelate modified diaphragm is immersed in the electrolyte for 14 days, the electrolyte in which it is located is still transparent and clear. This is due to the chelation effect of metal ions, which transforms the original weakly interacting π-π stacking structure of polydopamine into a strongly interacting coordination bonding structure, greatly improving the chemical stability of the modified diaphragm in the electrolyte.
[0079] 4) Heat shrinkage performance test: Figure 4 This is a digital photo of the heat shrinkage performance test of commercial polypropylene diaphragms and chelate-modified diaphragms. Figure 4 As shown in Table 1, the heat shrinkage resistance of the polydopamine chelate modified diaphragm is significantly improved, which is due to the thermal stability of the polydopamine chelate itself and the support layer structure formed on the surface of the diaphragm and inside the pores.
[0080] Table 1 Thermal shrinkage of commercial diaphragms and chelate-modified diaphragms
[0081]
[0082] 5) Electrochemical performance test: Figure 5This is the cycle performance diagram of button cells assembled with commercial polypropylene diaphragms, polydopamine modified diaphragms, polydopamine nickel chelate modified diaphragms, and polydopamine copper chelate modified diaphragms. As can be seen from the figure, the rate performance and cycle performance of button cells assembled with polydopamine chelate modified diaphragms are better than those assembled with commercial diaphragms and polydopamine modified diaphragms, which is due to the excellent electrolyte wettability, chemical stability and improvement of the pore structure of the diaphragm by the polydopamine chelate modified diaphragm.
[0083] In summary, for polyolefin separators, polydopamine chelate modification can improve the electrochemical performance and safety performance of the assembled batteries, and polydopamine chelate modified polyolefin separators have great commercial potential.
[0084] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a chelate-modified polyolefin membrane, characterized in that: The chelate is a polydopamine chelate, and the preparation method comprises the following steps: (1) dissolving a pH buffer, a water-soluble metal salt, and a water-soluble oxidant in water, controlling the pH to be between 7.5 and 8.5, and adding dopamine hydrochloride to dissolve to obtain a modified precursor solution; (2) taking a polyolefin membrane and adding it into the modified precursor solution obtained in step (1), and letting it stand to obtain the chelate-modified polyolefin membrane.
2. The method for preparing the chelate-modified polyolefin membrane according to claim 1, characterized in that: The pH buffer is at least one of a phosphate buffer, a borax buffer, a sodium barbital buffer, a tris(hydroxymethyl)aminomethane buffer, and an ammonia buffer.
3. The method for preparing the chelate-modified polyolefin membrane according to claim 1, characterized in that: The water-soluble metal salt is at least one of lithium salt, copper salt, aluminum salt, zinc salt, cobalt salt, iron salt, cerium salt, zirconium salt and nickel salt.
4. The method for preparing the chelate-modified polyolefin membrane according to claim 1, characterized in that: The water-soluble oxidant is at least one of persulfate, potassium permanganate, potassium perchlorate and potassium dichromate; The persulfate is at least one of ammonium persulfate, potassium persulfate and sodium persulfate.
5. The method for preparing the chelate-modified polyolefin membrane according to claim 1, characterized in that: The molar ratio of metal ions to dopamine hydrochloride in the water-soluble metal salt is not less than 1:
2.
6. The method for preparing the chelate-modified polyolefin membrane according to claim 1, characterized in that: In step (2), the polyolefin membrane is one of a polypropylene membrane, a polyethylene membrane, and a polyethylene and polypropylene composite membrane.
7. The method for preparing the chelate-modified polyolefin membrane according to claim 1, characterized in that: In step (2), the temperature during standing is 20 to 60° C., and the standing time is 2 to 48 hours.
8. The method for preparing the chelate-modified polyolefin membrane according to claim 1, characterized in that: After standing in step (2), the chelate-modified polyolefin membrane obtained is further cleaned and dried.
9. The chelate-modified polyolefin membrane prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the chelate-modified polyolefin separator according to claim 9 in the preparation of lithium batteries.
Citation Information
Patent Citations
Lithium-sulfur battery modified diaphragm as well as preparation method and application thereof
CN114865217A
Preparation method of composite coated lithium ion battery polyethylene diaphragm
CN115224438A
Secondary battery, electronic device, electric power tool, electric vehicle, and power storage system
JP2012256505A