Anti-electromagnetic interference bridging cable for short-distance equipment bridging signal concentrated transmission
By setting up multi-layer shielding and double-layer plastic sealing structures on the wire harness, superconducting carbon black and nano-calcium carbonate/polystyrene composite materials, the poor anti-electromagnetic interference capability and large volume of the short-range equipment jumper cable is solved. , improves tensile strength and electromagnetic shielding performance, and improves transmission and safety performance.
Patent Information
- Application Number
- CN202411379581.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-27
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The existing jumper cables that centrally transmit cross signals to the near-range equipment have problems such as poor anti-electromagnetic interference capabilities, large coupling volume and poor mechanical properties.
Wire harnesses are used to wrap the shielding mesh and shielding layer, and multi-layer injection molding layers are provided on the outside, including surface-modified superconducting carbon black and nano-calcium carbonate/polystyrene composite materials, forming a 360° closed overlap through the injection molding process. and double-layer plastic seal structure to enhance electromagnetic shielding and mechanical properties.
It significantly improves the tensile strength and electromagnetic shielding performance of the jumper cable, reduces the connection volume, avoids the weight and installation space problems of traditional shielded cables, and improves transmission performance and safety.
Smart Images

Figure BDA0005069564360000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electric wires and cables, and in particular relates to a jumper cable for centralized transmission of jumper signals of short-distance devices and anti-electromagnetic interference. Background Art
[0002] As an important component for transmitting energy and signals, wires and cables are necessary supporting conditions for the normal operation of various industrial fields and the realization of science and technology. They are regarded as the blood vessels and nerves of modern society. With the advancement of science and technology and the needs of social development, there are often dozens or even hundreds of cables that need to be installed separately. There are many wire harnesses, which are crossed and difficult to construct. Multiple groups of signals between adjacent devices need to interact. The number of connections with traditional shielded cables is large and the volume is large, which affects the close installation. The cable connection is affected by electromagnetic interference and affects the signal exchange. And with the continuous development of weapons and equipment, shipbuilding industry, petrochemical industry, power communication, rail transportation, energy, building electrical and other fields, the laying and service environment of wires and cables is becoming more and more complex. In order to ensure the reliable transmission of energy and signals, the safety performance requirements of wires and cables are also getting higher and higher. In particular, high temperature resistance, low temperature resistance, fire resistance, impact resistance and other properties are important factors affecting the safety of wires and cables. Existing jumper cables generally have problems such as unsatisfactory electromagnetic shielding effect, large area occupied by jumper connections, and poor mechanical properties of plastic-sealed structures. Therefore, it is particularly important to improve the transmission performance and safety performance of jumper cables for the design and application of jumper cables. Summary of the invention
[0003] The purpose of the present invention is to provide a jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference, so as to solve the following technical problems:
[0004] The existing jumper cables for centralized transmission of electromagnetic interference resistance for short-distance device jumper signals have the problems of poor electromagnetic interference resistance, large connection volume and poor mechanical properties.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference, comprising at least:
[0007] Wire harness;
[0008] a shielding mesh wrapped around the wire bundle;
[0009] A shielding layer wrapped around the shielding net;
[0010] A connector, one end of which is at least electrically connected to the shielding net;
[0011] A first injection molding layer, wrapped around the shielding layer and the connector;
[0012] a second injection-molded layer, wrapped on the first injection-molded layer;
[0013] wherein the first injection-molded layer and the second injection-molded layer are formed by an injection molding process, and the first injection-molded layer comprises surface-modified superconducting carbon black;
[0014] The second injection molding layer comprises a nano calcium carbonate / polystyrene composite material.
[0015] Preferably, the first injection molding layer comprises at least the following raw materials in parts by weight: 45-50 parts of SEBS rubber particles, 8-12 parts of polypropylene, 0.2-0.5 parts of antioxidant, 10-12 parts of filler oil and 15-20 parts of surface-modified superconducting carbon black.
[0016] Preferably, the preparation method of the first injection molding layer at least includes:
[0017] Put the superconducting carbon black into a high-speed mixer, heat it to 100-110° C., add titanate couple, stir at a speed of 1000-1200 rpm for 20-25 minutes, then discharge the material for standby use to obtain surface-modified superconducting carbon black;
[0018] Put the SEBS rubber particles and the filler oil into the mixing tank of the mixer, stir and mix them evenly, and then let them stand;
[0019] Then, the polypropylene, the antioxidant and the surface-modified superconducting carbon black are added into the mixing tank of the mixer, and stirred until all the materials are evenly mixed;
[0020] A twin-screw extruder is used to perform a granulation process to obtain a first injection molding material.
[0021] Preferably, the second injection molding layer comprises at least the following raw materials in parts by weight: 50-60 parts of SEBS rubber particles, 8-12 parts of polypropylene, 10-12 parts of filler oil, 0.2-0.5 parts of antioxidant, 0.2-5 parts of lubricant and 10-20 parts of nano calcium carbonate / polystyrene composite material.
[0022] Preferably, the preparation method of the second injection molding layer at least includes:
[0023] The nano calcium carbonate particles are dispersed in an organic solvent, a surface treatment agent is added dropwise under stirring, an exchange reaction is carried out for 5-15 minutes, the organic solvent is removed by suction filtration, and the nano calcium carbonate particles are dispersed in a styrene monomer, an initiator is added, and a free radical polymerization reaction is initiated at a temperature of 60-150° C. for 0.5-24 hours to obtain a nano calcium carbonate / polystyrene composite material;
[0024] Put the SEBS rubber particles and the filler oil into the mixing tank of the mixer, stir and mix them evenly, and then let them stand;
[0025] Then, the polypropylene, the antioxidant, the lubricant and the nano calcium carbonate / polystyrene composite material are added into the mixing tank of the mixer, and stirred until all the materials are evenly mixed;
[0026] A twin-screw extruder was used to perform a granulation process to obtain a second injection-molded layer.
[0027] Preferably, the injection molding process of the first injection molding layer and the second injection molding layer at least includes:
[0028] Clamping and fixing a first injection mold on the outside of the wire harness with the connector, placing the first injection molding material in an injection molding machine for melting and processing, and injecting the first injection molding material into the first injection mold;
[0029] Cooling the first injection mold, and demoulding after the first injection material solidifies to form the first injection layer;
[0030] Fixing the second injection mold, placing the second injection molding material in an injection molding machine for melting and processing, and injecting the second injection molding material into the second injection mold;
[0031] Cooling the second injection mold, and demoulding after the second injection material solidifies outside the first injection layer to form the second injection layer;
[0032] After surface treatment is performed on the second injection molding layer, the injection molding process is completed to obtain a jumper cable that is resistant to electromagnetic interference and can transmit jumper signals of short-range devices in a centralized manner.
[0033] Preferably, the processing temperature of the injection molding machine for melting and processing the first injection molding material is 180-220°C, and the processing temperature of the injection molding machine for melting and processing the second injection molding material is 160-200°C.
[0034] Preferably, the shielding mesh is a braided copper mesh or a braided aluminum mesh.
[0035] Preferably, the shielding layer is a copper foil layer or an aluminum foil layer.
[0036] Beneficial effects of the present invention:
[0037] The present invention arranges a shielding layer and a shielding net outside the wire bundle, the connector is at least electrically connected to the shielding net, a first injection molding layer and a second injection molding layer are arranged outside the shielding layer, and the first injection molding layer and the second injection molding layer wrap and cover the wire bundle and the connector, the shielding layer, the shielding net, the first injection molding layer and the second injection molding layer form a multi-layer shielding and double-layer plastic sealing structure, and the obtained jumper cable has excellent tensile strength and electromagnetic shielding performance, and effectively avoids the problem of large number and large volume of traditional shielded cables, which affects close installation, and the cable connection is affected by electromagnetic interference and affects signal exchange. Specifically, a braided metal shielding net is arranged outside the wire bundle, because it has a lower critical resistance and can resist electromagnetic interference, a metal shielding layer is arranged outside the shielding net, which can resist radio frequency interference, and the shielding net and the shielding layer are arranged to wrap the wire bundle to effectively shield the interference field of high and low frequency mixture.
[0038] The present invention uses SEBS rubber particles and polypropylene to prepare injection molding materials. The plastic properties of polypropylene can improve the mechanical properties of SEBS rubber particles, and polypropylene has excellent processing properties. After being blended with SEBS rubber particles, the fluid viscosity of the modified material can be balanced, so that the modified material can be used for injection molding. Surface-modified conductive carbon black is added to the first injection molding layer, and the first injection molding layer covers the shielding layer and covers the connector, so that the shielding layer and the electrical connector are 360° closed overlapped, and the electromagnetic shielding performance of the jumper cable is improved. And through the injection molding process, the first injection molding layer is almost completely fitted with the cable and the connector, which can solve the problem that the traditional shielding with the help of a shielding card or a tail cover requires additional weight and installation space.
[0039] The present invention also provides a second injection molding layer, and the second injection molding layer is wrapped outside the first injection molding layer. The first plastic sealing layer and the second plastic sealing layer are made of the same material, so the two have good welding properties and are not prone to wire material separation. Nano calcium carbonate / polystyrene composite materials are added to the second injection molding layer, and the nano calcium carbonate / polystyrene composite materials are dispersed in the second injection molding material to enhance the toughness and strength of the material, so that the obtained jumper cable has excellent tensile strength and elongation at break. The present invention reduces the problem of large volume of multi-cable connection by providing a multi-layer shielding structure and a double-layer plastic sealing structure, and provides a double-layer plastic sealing structure with different functions, thereby improving the shielding performance, transmission performance and mechanical properties of the jumper cable. DETAILED DESCRIPTION
[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Example 1
[0042] The preparation method of the first injection molding material comprises the following steps:
[0043] 20 parts of conductive carbon black are placed in a high-speed mixer, heated to 100-110° C., 0.4 parts of titanate hyperdispersant are slowly added at a stirring speed of 1000-1200 rpm, and stirred for 20-25 minutes to obtain titanate-modified conductive carbon black;
[0044] Put 60 parts of SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of paraffin oil as filling oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly. Let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0045] Then, 10 parts of polypropylene, 0.4 parts of antioxidant thiobisphenol antioxidant and 20 parts of titanate-modified superconducting carbon black were added to the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all the materials were evenly mixed and then released;
[0046] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrudes the material strip, cools it with cooling circulating water in a cooling water tank, then pulls it to a blower for air drying, and pelletizes it with a pelletizer to prepare a first injection molding material;
[0047] The preparation method of the second injection molding material comprises the following steps:
[0048] 15 parts of nano calcium carbonate particles are dispersed in ethanol with a weight concentration of 30%, 0.3 parts of methacrylic acid as a surface treatment agent is added dropwise under stirring, and the exchange reaction is carried out for 5 minutes. The nano calcium carbonate / ethanol mixed system obtained above is filtered to remove the ethanol, and then dispersed in styrene monomer, stirred for 1 hour, and an initiator di-tert-butyl peroxide is added, and a bulk polymerization reaction is carried out at a constant temperature of 110° C. for 4 hours to obtain a nano calcium carbonate / polystyrene composite material;
[0049] Put 55 parts of weighed SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of filling oil paraffin oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly, and let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0050] Then, 15 parts of polypropylene, 0.4 parts of antioxidant thiobisphenol antioxidant, 3 parts of lubricant solid alkane wax mixture and 15 parts of nano calcium carbonate / polystyrene composite material were added to the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all materials were evenly mixed and then released;
[0051] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrude the material strips, cool them with cooling circulating water in the cooling water tank, then pull them to the blower for air drying, and pelletize them with a pelletizer to prepare the second injection molding material.
[0052] A method for preparing a jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference comprises the following steps:
[0053] The first injection mold is clamped and fixed on the outside of the wire harness with the connector, and the first injection material is placed in an injection molding machine at a constant temperature of 195° C. for melting and processing, and then injected into the first injection mold;
[0054] Air-cooling the first injection mold, and demoulding after the first injection material solidifies to form a first injection layer;
[0055] The second injection mold is fixed, and the second injection material is placed in an injection molding machine at a constant temperature of 180° C. for melting and processing, and then injected into the second injection mold until the second injection material fills the second injection mold;
[0056] The second injection mold is air-cooled, and the second injection mold is demoulded after the second injection molded material solidifies outside the first injection molded layer to form a second injection molded layer;
[0057] After surface treatment is performed on the second injection molding layer, the injection molding process is completed to obtain a jumper cable that is resistant to electromagnetic interference and can transmit centralized jumper signals of short-distance devices.
[0058] Example 2
[0059] The preparation method of the first injection molding material comprises the following steps:
[0060] 15 parts of conductive carbon black are placed in a high-speed mixer, heated to 100-110° C., 0.3 parts of a titanate hyperdispersant are slowly added at a stirring speed of 1000-1200 rpm, and stirred for 20-25 minutes to obtain a titanate-modified conductive carbon black;
[0061] Put 60 parts of SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of paraffin oil as filling oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly. Let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0062] Then, 10 parts of polypropylene, 0.4 parts of antioxidant thiobisphenol antioxidant and 15 parts of titanate-modified superconducting carbon black were added to the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all the materials were evenly mixed and then released;
[0063] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrudes the material strip, cools it with cooling circulating water in a cooling water tank, then pulls it to a blower for air drying, and pelletizes it with a pelletizer to prepare a first injection molding material;
[0064] The preparation method of the second injection molding material comprises the following steps:
[0065] 20 parts of nano calcium carbonate particles are dispersed in ethanol with a weight concentration of 30%, 0.5 parts of methacrylic acid as a surface treatment agent is added dropwise under stirring, and the exchange reaction is carried out for 5 minutes. The nano calcium carbonate / ethanol mixed system obtained above is filtered to remove the ethanol, and then dispersed in styrene monomer, stirred for 1 hour, and di-tert-butyl peroxide as an initiator is added. The bulk polymerization reaction is carried out at a constant temperature of 110° C. for 4 hours to obtain a nano calcium carbonate / polystyrene composite material;
[0066] Put 55 parts of weighed SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of filling oil paraffin oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly, and let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0067] Then, 10 parts of polypropylene, 0.4 parts of antioxidant thiobisphenol antioxidant, 4 parts of lubricant solid alkane wax mixture and 20 parts of nano calcium carbonate / polystyrene composite material were added to the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all materials were evenly mixed and then released;
[0068] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrude the material strips, cool them with cooling circulating water in the cooling water tank, then pull them to the blower for air drying, and pelletize them with a pelletizer to prepare the second injection molding material.
[0069] The other components and preparation methods are the same as those in Example 1.
[0070] Example 3
[0071] The preparation method of the first injection molding material comprises the following steps:
[0072] 20 parts of conductive carbon black were placed in a high-speed mixer, and 0.4 parts of titanate hyperdispersant were slowly added under high-speed stirring, and pre-stirred and mixed at a temperature of 70° C. for 10 minutes to obtain titanate-modified conductive carbon black;
[0073] Put 60 parts of weighed SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of paraffin oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly, and let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0074] Then, 8 parts of polypropylene, 0.4 parts of antioxidant thiobisphenol antioxidant, 5 parts of lubricant solid alkane wax mixture and 20 parts of titanate-modified superconducting carbon black were added to the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all the materials were evenly mixed and then released;
[0075] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrudes the material strip, cools it with cooling circulating water in a cooling water tank, then pulls it to a blower for air drying, and pelletizes it with a pelletizer to prepare a first injection molding material;
[0076] The preparation method of the second injection molding material comprises the following steps:
[0077] 15 parts of nano calcium carbonate particles are dispersed in ethanol with a weight concentration of 30%, 0.3 parts of methacrylic acid as a surface treatment agent is added dropwise under stirring, and the exchange reaction is carried out for 5 minutes. The nano calcium carbonate / ethanol mixed system obtained above is filtered to remove the ethanol, and then dispersed in styrene monomer, stirred for 1 hour, and an initiator di-tert-butyl peroxide is added, and a bulk polymerization reaction is carried out at a constant temperature of 110° C. for 4 hours to obtain a nano calcium carbonate / polystyrene composite material;
[0078] Put 60 parts of weighed SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of paraffin oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly, and let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0079] Then, 15 parts of polypropylene, 0.2 parts of antioxidant thiobisphenol antioxidant, 2 parts of lubricant solid alkane wax mixture and 15 parts of nano calcium carbonate / polystyrene composite material were added to the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all materials were evenly mixed and then released;
[0080] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrude the material strips, cool them with cooling circulating water in the cooling water tank, then pull them to the blower for air drying, and pelletize them with a pelletizer to prepare the second injection molding material.
[0081] The other components and preparation methods are the same as those in Example 1.
[0082] Comparative Example 1
[0083] The preparation method of the first injection molding material comprises the following steps:
[0084] Put 60 parts of weighed SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of paraffin oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly, and let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0085] Then, 10 parts of polypropylene and 0.4 parts of antioxidant thiobisphenol antioxidant were added into the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all materials were evenly mixed and then released;
[0086] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrudes the material strip, cools it with cooling circulating water in a cooling water tank, then pulls it to a blower for air drying, and pelletizes it with a pelletizer to prepare a first injection molding material;
[0087] The preparation method of the second injection molding material comprises the following steps:
[0088] Put 55 parts of weighed SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of paraffin oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly. Let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0089] Then, 15 parts of polypropylene, 0.4 parts of antioxidant thiobisphenol antioxidant and 3 parts of lubricant solid alkane wax mixture were added into the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all materials were evenly mixed and then released;
[0090] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrude the material strips, cool them with cooling circulating water in the cooling water tank, then pull them to the blower for air drying, and pelletize them with a pelletizer to prepare the second injection molding material.
[0091] The other components and preparation methods are the same as those in Example 1.
[0092] Comparative Example 2
[0093] 10 parts of conductive carbon black are placed in a high-speed mixer, heated to 100-110° C., 0.2 parts of titanate hyperdispersant are slowly added at a stirring speed of 1000-1200 rpm, and stirred for 20-25 minutes to obtain titanate-modified conductive carbon black;
[0094] 10 parts of nano calcium carbonate particles are dispersed in ethanol with a weight concentration of 30%, 0.2 parts of methacrylic acid are added dropwise under stirring, and the exchange reaction is carried out for 5 minutes. The nano calcium carbonate / ethanol mixed system obtained above is filtered to remove the ethanol, and then dispersed in styrene monomer, stirred for 1 hour, and an initiator di-tert-butyl peroxide is added, and a bulk polymerization reaction is carried out at a constant temperature of 110° C. for 4 hours to obtain a nano calcium carbonate / polystyrene composite material;
[0095] Put 60 parts of SEBS rubber particles into the mixing tank of a 100L high-speed mixer and then pour in 10 parts of paraffin oil as filling oil. Use low-speed stirring to mix the paraffin oil and SEBS rubber particles evenly. Let it stand for more than 4 hours to allow SEBS to fully absorb the oil until there is no obvious visible flowing liquid phase filling oil in the tank.
[0096] Then, 15 parts of polypropylene, 0.4 parts of antioxidant thiobisphenol antioxidant, 3 parts of lubricant solid alkane wax mixture, 10 parts of nano calcium carbonate / polystyrene composite material and 20 parts of titanate-modified superconducting carbon black were added to the mixing tank of the high-speed mixer, and stirred rapidly for 2 minutes until all the materials were evenly mixed before being released;
[0097] The mixed material is put into a twin-screw extruder for melt kneading and extrusion, the extrusion temperature is 180-250°C, the screw speed is 200-800rpm, the twin-screw extruder die head extrudes the material strip, cools it with cooling circulating water in a cooling water tank, then pulls it to a blower for air drying, and pelletizes it with a pelletizer to prepare an injection molding material;
[0098] The injection mold is clamped and fixed on the outside of the wire harness with the connector, and the injection material is placed in an injection molding machine at a constant temperature of 195°C for melting and processing, and then injected into the injection mold until the injection mold is filled;
[0099] The injection mold is air-cooled and demoulding is performed after the injection material solidifies to form an injection layer;
[0100] After surface treatment of the injection molding layer, the injection molding process is completed to obtain a jumper cable that is resistant to electromagnetic interference and can transmit centralized jumper signals of short-distance devices.
[0101] Performance testing:
[0102] The injection molding materials in Examples 1-3 and Comparative Examples 1-2 were first dried at 90° C. for 1-2 hours, and then the test specimens were tested using an injection molding mechanism. After being fully stabilized at room temperature, various performance tests were performed. The test results are shown in Table 1:
[0103] Table 1 Statistics of jumper cable performance test data in Examples 1-3 and Comparative Example 2
[0104]
[0105] It can be seen from the data in Table 1 that the first injection molding layer and the second injection molding layer formed by preparing the first injection molding material and the second injection molding material on the wire bundle and the connector in Examples 1-3 of the present invention make the jumper cable obtained have excellent tensile strength, elongation at break, tear strength and shielding performance. Among them, the first injection molding layer has excellent shielding performance, and the second injection molding layer has good tensile strength. In Comparative Example 1, the surface-modified conductive carbon black is not added to the first injection molding layer, and the nano calcium carbonate / polystyrene composite material is not added to the second injection molding layer. In Comparative Example 2, the surface-modified conductive carbon black and the nano calcium carbonate / polystyrene composite material are mixed to prepare a layer of injection molding, and the tensile strength, elongation at break, tear strength, and shielding performance measured are all reduced, indicating that by setting the first injection molding layer and the second injection molding layer, the performance of the two materials can be fully utilized, and the tensile strength, elongation at break, tear strength, and shielding performance of the jumper cable obtained can be effectively improved, and the shielding net and shielding layer on the jumper cable are matched to form a multi-shielding, double-layer plastic sealing effect.
[0106] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0107] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference, characterized in that: At least: Wire harness; a shielding mesh wrapped around the wire bundle; A shielding layer wrapped around the shielding net; A connector, one end of which is at least electrically connected to the shielding net; A first injection molding layer, wrapped around the shielding layer and the connector; a second injection-molded layer, wrapped on the first injection-molded layer; wherein the first injection-molded layer and the second injection-molded layer are formed by an injection molding process, and the first injection-molded layer comprises surface-modified superconducting carbon black; The second injection layer comprises a nano calcium carbonate / polystyrene composite material.
2. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 1, characterized in that: The first injection molding layer comprises at least the following raw materials in parts by weight: 45-50 parts of SEBS rubber particles, 8-12 parts of polypropylene, 0.2-0.5 parts of antioxidant, 10-12 parts of filler oil and 15-20 parts of surface-modified superconducting carbon black.
3. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 2, characterized in that: The preparation method of the first injection molding layer at least comprises: Put the superconducting carbon black into a high-speed mixer, heat it to 100-110° C., add titanate couple, stir at a speed of 1000-1200 rpm for 20-25 minutes, then discharge the material for standby use to obtain surface-modified superconducting carbon black; Put the SEBS rubber particles and the filler oil into the mixing tank of the mixer, stir and mix them evenly, and then let them stand; Then, the polypropylene, the antioxidant and the surface-modified superconducting carbon black are added into the mixing tank of the mixer, and stirred until all the materials are evenly mixed; A twin-screw extruder is used to perform a granulation process to obtain a first injection molding material.
4. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 1, characterized in that: The second injection molding layer comprises at least the following raw materials in parts by weight: 50-60 parts of SEBS rubber particles, 8-12 parts of polypropylene, 10-12 parts of filler oil, 0.2-0.5 parts of antioxidant, 0.2-5 parts of lubricant and 10-20 parts of nano calcium carbonate / polystyrene composite material.
5. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 4, characterized in that: The preparation method of the second injection molding layer at least comprises: The nano calcium carbonate particles are dispersed in an organic solvent, a surface treatment agent is added dropwise under stirring, an exchange reaction is carried out for 5-15 minutes, the organic solvent is removed by suction filtration, and the nano calcium carbonate particles are dispersed in a styrene monomer, an initiator is added, and a free radical polymerization reaction is initiated at a temperature of 60-150° C. for 0.5-24 hours to obtain a nano calcium carbonate / polystyrene composite material; Put the SEBS rubber particles and the filler oil into the mixing tank of the mixer, stir and mix them evenly, and then let them stand; Then, the polypropylene, the antioxidant, the lubricant and the nano calcium carbonate / polystyrene composite material are added into the mixing tank of the mixer, and stirred until all the materials are evenly mixed; A twin-screw extruder was used to perform a granulation process to obtain a second injection-molded layer.
6. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 1, characterized in that: The injection molding process of the first injection molding layer and the second injection molding layer at least includes: Clamping and fixing a first injection mold on the outside of the wire harness with the connector, placing the first injection molding material in an injection molding machine for melting and processing, and injecting the first injection molding material into the first injection mold; Cooling the first injection mold, and demoulding after the first injection material solidifies to form the first injection layer; Fixing the second injection mold, placing the second injection molding material in an injection molding machine for melting and processing, and injecting the second injection molding material into the second injection mold; Cooling the second injection mold, and demoulding after the second injection material solidifies outside the first injection layer to form the second injection layer; After surface treatment is performed on the second injection molding layer, the injection molding process is completed to obtain a jumper cable that is resistant to electromagnetic interference and can transmit centralized jumper signals of short-distance devices.
7. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 6, characterized in that: The processing temperature of the injection molding machine for melting and processing the first injection molding material is 180-220°C, and the processing temperature of the injection molding machine for melting and processing the second injection molding material is 160-200°C.
8. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 1, characterized in that: The shielding mesh is a braided copper mesh or a braided aluminum mesh.
9. The jumper cable for centralized transmission of short-distance device jumper signals and anti-electromagnetic interference according to claim 1, characterized in that: The shielding layer is a copper foil layer or an aluminum foil layer.
Citation Information
Patent Citations
Composite type high-conductivity polymer material and preparation method thereof
CN101891914A
Anti-interference solar frequency converter connecting wire harness
CN105790021A
Self-supporting anti-interference multi-core shielding communication cable
CN114360789A
Toughness reinforced mother material for nanometer calcium carbonate plastics
CN1285365A
Nano-calcium carbonate / polystyrene composite material and its preparation method