Bio-based hot melt adhesive composition as well as preparation method and application thereof

By using a combination of tackifying resin, antioxidant, wax and hydrophobic nanocellulose in bio-based hot melt adhesive, the poor toughness, non-surface viscosity and thermal instability of bio-based hot melt adhesive are solved, and high Hot melt adhesive with bio-based content, low melt viscosity and excellent tensile strength is suitable for disposable sanitary products and other fields.

CN119242240APending Publication Date: 2025-01-03TEX YEAR FINE CHEM GUANGZHOU CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411543993.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2025-01-03

AI Technical Summary

Technical Problem

The existing bio-based hot melt adhesives have problems such as poor toughness, non-adhesive surface, poor spraying effect, degraded peeling performance after aging, thermal instability and high energy consumption, and bio-based hot melt adhesives may become brittle over time, resulting in adhesion. decline.

Method used

Using a composition of bio-based polymer, tackifying resin, antioxidant, wax and hydrophobic nanocellulose, a bio-based hot melt adhesive is prepared by stirring and mixing. The nano-cellulose modification improves rheology and mechanical properties and increases viscosity. Resin improves peeling power, antioxidants prevent oxidation, and wax reduces melt viscosity.

Benefits of technology

It has obtained an environmentally friendly hot melt adhesive with excellent tensile strength, low melt viscosity and high biobase content. It is suitable for disposable sanitary products and other fields. It is a simple preparation method suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a bio-based hot-melt adhesive composition as well as a preparation method and application thereof. The bio-based hot-melt adhesive composition comprises the following raw materials in parts by weight: 20-80 parts of a bio-based polymer, 5-70 parts of tackifying resin, 0.5-2 parts of an antioxidant, 4-6 parts of wax and 10-15 parts of nano cellulose. Performance tests show that the bio-based hot-melt adhesive composition has excellent tensile strength, high bio-based content, low viscosity in the melting process, environmental protection and reliability, and can be applied to the fields of preparation of disposable sanitary products and the like. In addition, the preparation method of the bio-based hot melt adhesive composition is simple and convenient, and can be suitable for industrial production amplification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of adhesives, and in particular to a bio-based hot melt adhesive composition and a preparation method and application thereof. Background Art

[0002] Hot melt adhesive is an important category of adhesives. It usually refers to an adhesive that is solid at room temperature and melts into a viscous liquid when heated to a certain temperature. After being applied and moistened on the adherend, it is pressed and cooled to room temperature to complete the bonding within a few seconds. Hot melt adhesives are widely used. This adhesive product is often used to manufacture hygiene, furniture and packaging products. It is also suitable for applications in the medical, electronic and automotive industries. It is particularly suitable for applications that require streamlined processing, efficient manufacturing and final product protection. Hot melt adhesive compositions are usually based on petroleum-derived polymers. Since petroleum-based is non-renewable and has high carbon dioxide emissions, it causes damage to the ecological environment. In addition, these components will be toxic when decomposed. Therefore, environmentally friendly and degradable materials are needed to replace them.

[0003] In recent years, in order to solve this problem, various biodegradable hot melt adhesives have been developed at home and abroad. They mainly use polyester polymers such as polylactic acid (PLA), polyhydroxyalkanoate (PHA), polypropylene carbonate (PPC), polybutylene succinate (PBS), polybutylene adipate terephthalate (PBAT) or biodegradable materials such as natural polymer compounds as the matrix resin, supplemented with appropriate tackifiers, viscosity regulators, plasticizers, antioxidants, fillers and other components. Among them, polylactic acid hot melt adhesives have been the most studied, but they have the following defects: (1) The PLA molecular chain has poor flexibility, the material is hard and brittle, and has poor impact resistance. The hot melt adhesive prepared with PLA has poor toughness, which limits its application range. (2) Hot melt adhesives made from polylactic acid polymers alone are relatively hard and have no stickiness on the surface. Excessive use of polylactic acid polymers will result in poor spraying effect of the hot melt adhesive and decreased peeling performance before and after aging. During use as a hot melt adhesive, it has a high melt viscosity and is prone to clogging during extrusion, requiring higher processing temperatures and increasing energy consumption. Adhesives made from all or high content of renewable resources face challenges such as phase separation, embrittlement and thermal instability. (3) Some bio-based hot melt adhesives may become brittle over time, resulting in decreased adhesion, or exhibit poor adhesion performance within certain temperature ranges. In addition, the viscosity of bio-based hot melt adhesives may be unsatisfactory for some applications. Summary of the invention

[0004] Based on this, it is necessary to provide a bio-based hot melt adhesive composition, which has excellent tensile strength, high bio-based content, low viscosity during the melting process, and is environmentally friendly and reliable.

[0005] The technical solution of this application is as follows:

[0006] In a first aspect of the present invention, a bio-based hot melt adhesive composition is provided, wherein the raw materials thereof include the following components by weight: 20-80 parts of a bio-based polymer, 5-70 parts of a tackifying resin, 0.5-2 parts of an antioxidant, 4-6 parts of a wax and 10-15 parts of nanocellulose.

[0007] In one embodiment, the bio-based polymer is one or more of polylactic acid polyhydroxyalkanoate, polylactic acid, polybutylene succinate or starch-based plastic; and / or

[0008] The weight average molecular weight of the bio-based polymer is 500 g / mol-50000 g / mol.

[0009] In one embodiment, the nanocellulose is hydrophobized nanocellulose.

[0010] In one embodiment, the tackifying resin is one or more of terpene phenol resin, rosin resin or bio-based tackifying resin.

[0011] In one embodiment, the antioxidant is one or more of 2,6-di-tert-butylcresol, 4,4'-bis(6-tert-butyl-m-cresol) sulfide, butylated hydroxyanisole, dibutylhydroxytoluene or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0012] In one embodiment, the wax is one or more of beeswax, shellac wax, paraffin wax, microcrystalline wax, polyethylene wax, hydroxy wax, amide wax or hydrogenated vegetable oil.

[0013] A second aspect of the present invention provides a method for preparing the bio-based hot melt adhesive composition as described above, comprising the following steps:

[0014] The bio-based polymer, tackifying resin, antioxidant, plasticizer, wax and nanocellulose are mixed and stirred.

[0015] In one embodiment, the stirring temperature is 160°C-200°C.

[0016] In one embodiment, the stirring time is 40 min-180 min.

[0017] The third aspect of the present invention provides use of the bio-based hot melt adhesive composition as described above in bonding materials.

[0018] Compared with the prior art, this application has the following beneficial effects:

[0019] The present application rationally designs the formulation of the adhesive according to the raw material properties, and obtains a bio-based hot melt adhesive composition including components such as bio-based polymers, tackifying resins, antioxidants, waxes and nanocellulose. Experimental verification shows that the bio-based hot melt adhesive composition has excellent tensile strength, high bio-based content, low viscosity during the melting process, and is environmentally friendly and reliable, and can be used in the preparation of disposable sanitary products and other fields.

[0020] In addition, the preparation method of the bio-based hot melt adhesive composition is simple and convenient, and can be suitable for industrial production and scale-up. DETAILED DESCRIPTION

[0021] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0023] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0024] As used herein, "one or more" refers to any one, any two, or any two or more of the listed items.

[0025] Herein, the optional scope of "and / or", "or / and", and "and / or" includes any one of two or more relevant listed items, and also includes any and all combinations of the relevant listed items, wherein said any and all combinations include any two relevant listed items, any more relevant listed items, or a combination of all relevant listed items. (It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in the present application, the technical solution undoubtedly includes technical solutions that are all connected by "logical AND", and also undoubtedly includes technical solutions that are all connected by "logical OR". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For another example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, technical solutions that are all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, a combination of any two or any three of A, B, C, and D, and also includes a combination of four items of A, B, C, and D (that is, a technical solution that is all connected by "logical AND").)

[0026] Herein, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0027] Herein, "first aspect", "second aspect", "third aspect", "fourth aspect", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. In addition, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0028] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0029] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value itself can be combined with any other point or single value as a lower limit or upper limit or with other lower limits or upper limits to form an undefined range. The use of numerical ranges represented by endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0030] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.

[0031] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.

[0032] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±2°C, ±1°C, ±0.5°C, ±0.4°C, ±0.3°C, ±0.2°C, and ±0.1°C are allowed. Normal temperature or room temperature in this application refers to no temperature control operation, generally 4°C~35°C, preferably 20±5°C.

[0033] In a first aspect of the present invention, a bio-based hot melt adhesive composition is provided, wherein the raw materials thereof include the following components by weight: 20-80 parts of a bio-based polymer, 5-70 parts of a tackifying resin, 0.5-2 parts of an antioxidant, 4-6 parts of a wax and 10-15 parts of nanocellulose.

[0034] Specifically, in the bio-based hot melt adhesive composition, each component works synergistically: nanocellulose is hydrophobically modified, and hydrophobic nanocellulose can be evenly mixed with hydrophobic PLA. The uniformly dispersed nanocellulose is conducive to improving rheological and mechanical properties, and can improve the fluidity and dispersibility under low stress without reducing the bonding strength. Nanocellulose also plays the role of a nucleating agent. When incorporated into a bio-based polymer, it forms a nucleus for crystal growth in the bio-based polymer melt. Therefore, it is possible to accelerate the crystallization rate, increase the crystal density, and promote the miniaturization of the grain size, shortening the molding cycle. The tackifying resin can increase the peeling force of the hot melt adhesive and also give the hot melt adhesive a certain initial adhesion. The antioxidant can prevent the polymer from oxidizing, resulting in the breakage and cross-linking of the macromolecular chain, and the deterioration of the performance, which can further enhance the performance of the hot melt adhesive.

[0035] In some of these examples, the bio-based polymer is one or more of polylactic acid polyhydroxyalkanoate, polylactic acid, polybutylene succinate, or starch-based plastic.

[0036] In some examples, the bio-based polymer has a weight average molecular weight (Mw) ranging from 500 g / mol to 50,000 g / mol.

[0037] In some of the examples, the nanocellulose is hydrophobic nanocellulose. The present application uses nanocellulose to enhance the rheological and mechanical properties of hot melt adhesives, which is reflected in the following aspects: (1) After the hydrophobic modification of nanocellulose, its compatibility with bio-based polymers is improved, and nanocellulose is biodegradable and environmentally friendly. (2) Nanocellulose acts as a thixotropic agent. The application of nanocellulose reduces the viscosity when subjected to shear stress, and increases the tensile strength under external stress relaxation conditions by maintaining a stable nanostructure, which can enhance the fluidity and penetration ability of the hot melt adhesive during use. (3) Hydrophobic nanocellulose can be mixed evenly with hydrophobic PLA, and the uniformly dispersed nanocellulose is conducive to improving the rheological and mechanical properties, and can improve the fluidity and dispersibility under low stress without reducing the bonding strength. (4) In addition, the nanonetwork prevents stress concentration in the composite material by acting as a load transfer, and improves the tensile strength under external stress relaxation conditions while maintaining a stable nanostructure. (5) Nanocellulose can also be used as a plasticizer and nucleating agent.

[0038] In some examples, the tackifying resin is one or more of a terpene phenol resin, a rosin resin, or a bio-based tackifying resin.

[0039] In some examples, the antioxidant is one or more of 2,6-di-tert-butylcresol, 4,4'-bis(6-tert-butyl-m-cresol) sulfide, butylated hydroxyanisole, dibutylhydroxytoluene or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0040] In some examples, the wax is one or more of beeswax, shellac wax, paraffin wax, microcrystalline wax, polyethylene wax, hydroxy wax, amide wax or hydrogenated vegetable oil.

[0041] A second aspect of the present invention provides a method for preparing the bio-based hot melt adhesive composition as described above, comprising the following steps:

[0042] The bio-based polymer, tackifying resin, antioxidant, plasticizer, wax and nanocellulose are mixed and stirred.

[0043] In some examples, the stirring temperature is 160° C.-200° C. It can be understood that the stirring temperature includes but is not limited to 160° C., 165° C., 170° C., 175° C., 180° C., 185° C., 190° C., 195° C., and 200° C.

[0044] In some of these examples, the stirring time is 40 min-180 min. It is understandable that the stirring time includes but is not limited to 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min.

[0045] In some examples, the stirring speed is 60r / min-100r / min. It can be understood that the stirring speed includes but is not limited to 60r / min, 65r / min, 70r / min, 75r / min, 80r / min, 85r / min, 90r / min, 95r / min, 100r / min.

[0046] The third aspect of the present invention provides use of the bio-based hot melt adhesive composition as described above in bonding materials.

[0047] The present application is further described in detail below in conjunction with specific examples. For experimental parameters not specified in the following specific examples, reference is made to the instructions given in the present application document, and reference may also be made to the experimental manual of the art or other experimental methods known in the art, or to the experimental conditions recommended by the manufacturer. It is understood that the instruments and raw materials used in the following examples are relatively specific, and may not be limited thereto in other specific examples.

[0048] Some of the raw materials used in the embodiment are as follows:

[0049] Nanocellulose suspension can be purchased from Shansi Technology or prepared by yourself.

[0050] The preparation method of 1wt% nanocellulose suspension can be: soaking bleached hardwood pulp in water for 1 hour, then dispersing it with a deflaker for 10 minutes, adding 8U / g cellulase, phosphate buffer solution and deionized water, washing the pulp for multiple times, filtering and separating, collecting the pulp and filtrate, and storing them in a refrigerator at 4°C. The pulp after enzymatic refining is diluted to a concentration of 5.0% using a PFI refiner, 10g of wet pulp is weighed and stirred in a mixer for 3 minutes, and then the pulp is diluted to a 1% nanocellulose suspension, and then placed in a micro-jet high-pressure homogenizer at a pressure of 138MPa for circulation treatment to obtain a nanocellulose suspension.

[0051] Preparation of hydrophobic nanocellulose: A nanocellulose (CNF) suspension (10 mL, 1 wt%) was mixed with 40 mL of 82% isopropanol, and the CNF solution was homogenized at 6000 rpm for 2 minutes using a homogenizer. The alkaline conditions were then adjusted with 1 mL of aqueous ammonia. 1 mL of tetraethoxysilane TEOS was added dropwise, and the mixture was stirred at 500 rpm for 1-6 h. Methyltrimethoxysilane MTMS (5 mL) was then added dropwise to the suspension and stirred at 500 rpm for 2-8 h. After the completed reaction solution was centrifuged at 1000 relative centrifugal force (RCF) for 5 minutes, the supernatant was discarded, the residue was washed three times with ethanol to eliminate the reaction residues, freeze-dried and spun in a vacuum oven at 150 ◦ C to obtain hydrophobic nanocellulose.

[0052] The following are specific embodiments.

[0053] Example 1

[0054] Polylactic acid, hydrophobic nanocellulose, tackifying resin (rosin resin), antioxidant (2,6-di-tert-butylcresol), and wax (paraffin) are mixed in a mass ratio of 60:12:40:1:5, stirred at 180°C at a speed of 100 r / min for 120 min, and extruded and granulated using a twin-screw extruder to obtain polylactic acid hot-melt rubber particles.

[0055] Example 2

[0056] Polylactic acid, hydrophobic nanocellulose, tackifying resin (rosin resin), antioxidant (2,6-di-tert-butylcresol), and wax (paraffin) are mixed in a mass ratio of 20:10:5:0.5:4, stirred at 180°C at a speed of 100 r / min for 120 min, and extruded and granulated using a twin-screw extruder to obtain polylactic acid hot-melt rubber particles.

[0057] Example 3

[0058] Polylactic acid, hydrophobic nanocellulose, tackifying resin (rosin resin), antioxidant (2,6-di-tert-butylcresol), and wax (paraffin) are mixed in a mass ratio of 80:15:70:2:6, stirred at 180°C at a speed of 100 r / min for 120 min, and extruded and granulated using a twin-screw extruder to obtain polylactic acid hot-melt rubber particles.

[0059] Comparative Example 1

[0060] Polylactic acid, tackifying resin (rosin resin), antioxidant (2,6-di-tert-butylcresol), and wax (paraffin) are mixed in a mass ratio of 60:40:1:5, stirred at 180°C with a rotation speed of 100 r / min for 120 min, and extruded and granulated using a twin-screw extruder to obtain polylactic acid hot-melt rubber particles.

[0061] Comparative Example 2

[0062] Polylactic acid, non-hydrophobicized nanocellulose, tackifying resin (rosin resin), antioxidant (2,6-di-tert-butylcresol), and wax (paraffin) are mixed in a mass ratio of 60:12:40:1:5, stirred at 180°C at a speed of 100 r / min for 120 min, and extruded and granulated using a twin-screw extruder to obtain polylactic acid hot-melt rubber particles.

[0063] Comparative Example 3

[0064] Polylactic acid, tackifying resin (rosin resin), antioxidant (2,6-di-tert-butyl cresol), wax (paraffin), and plasticizer (citrate ester) are mixed in a mass ratio of 60:40:1:5:12, stirred at 180°C with a speed of 100 r / min for 120 min, and extruded and granulated using a twin-screw extruder to obtain polylactic acid hot-melt rubber particles.

[0065] The specific raw material parameters of the polylactic acid hot melt adhesive particles of Examples 1 to 3 and Comparative Examples 1 to 3 are listed in Table 1 below:

[0066] Table 1

[0067]

[0068] The polylactic acid hot melt adhesive particles prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested for properties such as viscosity, softening point, bio-based content and tensile strength. The test results are shown in Table 2 below.

[0069] Among them, the test methods or test standards for each performance test item are:

[0070] 1. Viscosity test method: According to GB / T 2794, use Brookfield viscometer (model RVDV) and rotor No. 27 to measure viscosity. The results are recorded in centipoise (cps).

[0071] 2. Softening point test method: According to GB / T 15332, use SD-0606T automatic softening point tester of Shanghai Institute of Geoscience Instruments to test the softening point. The results are recorded in degrees Celsius (℃).

[0072] 3. Bio-based content test method: Test the bio-based content of hot melt adhesive in accordance with GB / T 39715.3.

[0073] 4. Tensile strength test method: According to GB / T 528. Use a universal testing machine to perform tensile strength analysis.

[0074] Table 2

[0075]

[0076] As can be seen from Table 2 above, the hot melt adhesive prepared by the present invention has excellent tensile strength, high bio-based content, low viscosity during the melting process, is an environmentally friendly material, and can be used in the fields of disposable sanitary products.

[0077] Compared with Comparative Example 1, the addition of hydrophobic nanocellulose (CNF) can comprehensively improve the mechanical properties of the bio-based hot melt adhesive. With the increase of CNF content, the tensile strength of the adhesive increases, and the highest tensile strength (0.983 MPa) is obtained when the mass fraction of CNF is 15.

[0078] Compared with Comparative Example 2, the hot melt adhesive mechanical properties of CNF that has not been hydrophobized are poor, and the untreated CNF cannot be well dispersed in the bio-based polymer, resulting in obstruction of mechanical path conduction and a decrease in mechanical properties.

[0079] Example 1 Compared with Comparative Example 3, it is confirmed that CNF can act as a plasticizer and nucleating agent; therefore, it can be used to overcome the poor mechanical properties of bio-based polymers due to low crystallinity, slow crystallization and wide spherulite size distribution. CNF helps to achieve mechanical reinforcement through the growth of small crystals and the increase in the number of small spherulites during crystallization.

[0080] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0081] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.

Claims

1. A bio-based hot melt adhesive composition, characterized in that: The raw materials include the following components by weight: 20-80 parts of bio-based polymer, 5-70 parts of tackifying resin, 0.5-2 parts of antioxidant, 4-6 parts of wax and 10-15 parts of nano cellulose.

2. The bio-based hot melt adhesive composition according to claim 1, characterized in that The bio-based polymer is one or more of polylactic acid polyhydroxyalkanoate, polylactic acid, polybutylene succinate or starch-based plastic; and / or The weight average molecular weight of the bio-based polymer is 500 g / mol-50000 g / mol.

3. The bio-based hot melt adhesive composition according to claim 1, characterized in that: The nanocellulose is hydrophobized nanocellulose.

4. The bio-based hot melt adhesive composition according to any one of claims 1 to 3, characterized in that: The tackifying resin is one or more of terpene phenol resin, rosin resin or bio-based tackifying resin.

5. The bio-based hot melt adhesive composition according to any one of claims 1 to 3, characterized in that: The antioxidant is one or more of 2,6-di-tert-butylcresol, 4,4'-bis(6-tert-butyl-m-cresol)sulfide, butylated hydroxyanisole, dibutylhydroxytoluene or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

6. The bio-based hot melt adhesive composition according to any one of claims 1 to 3, characterized in that: The wax is one or more of beeswax, shellac wax, paraffin wax, microcrystalline wax, polyethylene wax, hydroxy wax, amide wax or hydrogenated vegetable oil.

7. A method for preparing a bio-based hot melt adhesive composition according to any one of claims 1 to 6, characterized in that: The following steps are involved: The bio-based polymer, tackifying resin, antioxidant, plasticizer, wax and nanocellulose are mixed and stirred.

8. The method for preparing the bio-based hot melt adhesive composition according to claim 7, characterized in that: The stirring temperature is 160°C-200°C.

9. The method for preparing the bio-based hot melt adhesive composition according to claim 7, characterized in that: The stirring time is 40min-180min.

10. Use of the bio-based hot melt adhesive composition according to any one of claims 1 to 6 in bonding materials.

Citation Information

Cited By

  • Pure bio-based polyhydroxyalkanoate adhesive as well as preparation and application thereof

    CN120944505A