Delay composition with long-term healing per second and production method of delay composition
A production method and technology of delayed medicine, applied in the direction of explosives, etc., can solve the problems of complex production process and poor precision, and achieve the effect of simple production process, less waste water and easy operation
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2015-01-07
- Estimated Expiration
- Not applicable · inactive patent
Smart Images
Figure 1 Figure 2
Abstract
Description
technical field
[0001] The invention relates to a detonating device, in particular to a detonator detonating device, in particular to a long-second quantity delay drug and a production method thereof. Background technique
[0002] At present, in the blasting process of various mine projects, the long-delay detonator has become an indispensable detonating device. It plays an extremely important role in blasting shock absorption, reducing large block rate, and increasing tunneling speed in mine engineering. As the technical core of the long-delay detonator, the long-second delay drug has a decisive impact on the performance of the long-delay detonator.
[0003] At present, various types of long-duration delay drugs currently available mainly include: tungsten-based, molybdenum-based, and silicon-copper oxide-based delay drugs. The production methods mainly include mechanical wet mixing, co-precipitation, etc., but the prepared long-duration delay drugs Medicines generally ha...
Examples
Embodiment 1
[0033] The following components were weighed according to mass ratio: 35% molybdenum powder; 51.95% barium chromate; 8% potassium perchlorate; 5% calcium fluoride; 0.05% binder. The binder adopts polyvinyl alcohol aqueous solution with a mass concentration of 2.5%.
Embodiment 2
[0035] The following components were weighed according to mass ratio: molybdenum powder 36%; barium chromate 52.6%; potassium perchlorate 5%; calcium fluoride 6%; binder 0.4%. The binder is an aqueous solution of polyvinyl alcohol with a mass concentration of 1.0%.
Embodiment 3
[0037] The following components were weighed according to mass ratio: molybdenum powder 35%; barium chromate 54%; potassium perchlorate 5%; calcium fluoride 5.9%; binder 0.1%. The binder is an aqueous solution of polyvinyl alcohol with a mass concentration of 2%.