Method for catalytically synthesizing tetracyclic[7.3.1.0<2.7>.1<7.11>]tetradecane through solid acid
A solid acid catalysis, tetradecane technology, applied in chemical instruments and methods, catalysts, carbon compound catalysts, etc., can solve problems such as difficult separation and serious environmental pollution
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2016-07-27
Abstract
Description
technical field
[0001] The invention relates to a solid acid catalyzed synthesis of tetracyclic [7.3.1.0 2,7 .1 7,11 ] The method of tetradecane belongs to the technical field of catalytic synthesis. Background technique
[0002] High-density hydrocarbon fuels are those with a density greater than 0.9 g / cm 3 A kind of synthetic fuel, which has high density and volume heat of combustion, can effectively increase the range and speed of aircraft, and it has been widely valued as a high-energy fuel with excellent performance. Four Rings [7.3.1.0 2,7 .1 7,11 ] Tetradecane is a polycyclic hydrocarbon compound with a bridged ring structure. It is a hydrocarbon fuel with excellent performance and can be used as a high-density hydrocarbon fuel or additive.
[0003] The method for preparing this compound reported in the literature is: in the presence of organic solvent and acid catalyst, tetracyclic [7.4.0.0 2,7 .1 3,6 Tetracycline [7.3.1.0] tetradecane is obtained through isom...
Examples
Embodiment 1
[0015] The reaction tube containing 5g spherical γ-alumina was heated to 500°C, and the reaction tube containing 50g powdered γ-alumina was heated to 300°C, while purging the reaction system with nitrogen. Slowly pass 10mL of carbon tetrachloride into the reaction tube filled with spherical γ-alumina through a flow pump within 2 hours, and react at 500°C to generate aluminum trichloride vapor. Nitrogen brings aluminum trichloride vapor into the reaction tube filled with powdery γ-alumina, and forms a catalyst loaded with aluminum trichloride at 300°C. After it was punched into pieces, it was fired at 500°C for 4h.
[0016] In a nickel tube fixed-bed reactor with an inner diameter of 38mm, 30mL of the above-mentioned catalyst was loaded for tetracyclic [7.4.0.0 2,7 .1 3,6 Tetracyclo[7.3.1.0 prepared by isomerization of tetradecane 2,7 .1 7,11 ] Tetradecane reaction. Pass 50% Tetracycle [7.4.0.0 2,7 .1 3,6 ] Tetradecane in 1,2-dichloroethane, the flow rate is 15mL / h. The...
Embodiment 2
[0018] The reaction tube containing 5g spherical γ-alumina was heated to 500°C, and the reaction tube containing 50g powdered γ-alumina was heated to 300°C, while purging the reaction system with nitrogen. Slowly pass 10mL of carbon tetrachloride into the reaction tube filled with spherical γ-alumina through a flow pump within 2 hours, and react at 500°C to generate aluminum trichloride vapor. Nitrogen brings aluminum trichloride vapor into the reaction tube filled with powdery γ-alumina, and forms a catalyst loaded with aluminum trichloride at 300°C. After it was punched into pieces, it was fired at 500°C for 4h.
[0019] In a nickel tube fixed-bed reactor with an inner diameter of 38mm, 30mL of the above-mentioned catalyst was loaded for tetracyclic [7.4.0.0 2,7 .1 3,6 Tetracyclo[7.3.1.0 prepared by isomerization of tetradecane 2,7 .1 7,11 ] Tetradecane reaction. Pass 50% Tetracycle [7.4.0.0 2,7 .1 3,6 ] The cyclohexane solution of tetradecane, flow rate is 15mL / h. T...
Embodiment 3
[0021] The temperature of the reaction tube containing 5g spherical γ-alumina was raised to 500°C, the temperature of the reaction tube containing 50g of silicon dioxide was raised to 300°C, and the reaction system was purged with nitrogen. Slowly pass 10mL of carbon tetrachloride into the reaction tube filled with spherical γ-alumina through a flow pump within 2 hours, and react at 500°C to generate aluminum trichloride vapor. Nitrogen brings aluminum trichloride vapor into the reaction tube filled with silica, and forms a catalyst loaded with aluminum trichloride at 300°C. After it was punched into pieces, it was fired at 500°C for 4h.
[0022] In a nickel tube fixed-bed reactor with an inner diameter of 38mm, 30mL of the above-mentioned catalyst was loaded for tetracyclic [7.4.0.0 2,7 .1 3,6 Tetracyclo[7.3.1.0 prepared by isomerization of tetradecane 2,7 .1 7,11 ] Tetradecane reaction. Pass 50% Tetracycle [7.4.0.0 2,7 .1 3,6 ] Tetradecane in 1,2-dichloroethane, the f...