Photosensitive resin composition
By using compositions such as polyimide precursor and acrylic adhesive in AMOLED equipment, the problem of poor adhesion between the insulating film and the substrate is solved, the heat resistance is maintained, and the adhesion is improved, and the components are reduced. Undesirable phenomenon.
Patent Information
- Application Number
- CN201810392104.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-04-28
- Filing Date
- 2018-04-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2038-04-27
AI Technical Summary
In AMOLED equipment, the insulating film made of a photosensitive polyimide precursor has a poor adhesive force with the substrate, resulting in poor component, and the prior art reduces heat resistance when improving the adhesive force.
The compositions of polyimide precursors, acrylic adhesives, multifunctional monomers, photoinitiators and crosslinking agents are used to maintain the heat resistance of the polyimide precursors through specific chemical structures and proportions. At the same time, the adhesive force to the substrate is improved.
The adhesive force between the insulating film and the substrate is significantly improved while maintaining heat resistance, and the occurrence of component defects is reduced.
Smart Images

Figure CN108803240B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a photosensitive resin composition. Background Art
[0002] Recently, AMOLED devices, which are superior to TFT-LCD in image quality and flexibility, are expanding their market dominance. AMOLED is an EL (organic light-emitting material) that directly emits light after receiving an electrical signal. EL will also be affected by a trace amount of gas (GAS) and oxidize, eventually losing its component characteristics. Therefore, polyimide-based photosensitive resin compositions with excellent heat resistance and little outgassing are used in OLED devices to form an insulating film.
[0003] In particular, photosensitive polyimide precursors have the advantage of being easy to pattern and having excellent heat resistance to obtain insulating films by thermal imidization treatment based on coating, exposure, development and curing. However, the insulating films thus prepared have a problem of poor adhesion to the substrate, resulting in device failure.
[0004] In order to solve such problems, attempts have been made to change the chemical structure of the photosensitive polyimide precursor. For example, Korean Patent Publication No. 10-2009-0096365 discloses a polyimide composition comprising a polyimide of a specific structure and a polyamic acid. However, in most cases, the problem of improved adhesion and decreased heat resistance occurs.
[0005] Therefore, the present inventors made arduous efforts to solve the above-mentioned adhesion problem and found that when an acrylic adhesive is used together with a polyimide precursor as described below, the inherent heat resistance of the polyimide precursor can be maintained and the adhesion to the substrate can be improved, thereby completing the present invention. Summary of the invention
[0006] Technical issues
[0007] The present invention aims to provide a photosensitive resin composition.
[0008] Technical Solution
[0009] In order to solve the above problems, the present invention provides a photosensitive resin composition comprising: a polyimide precursor, an acrylic adhesive, a multifunctional monomer, a photoinitiator and a crosslinking agent, wherein the acrylic adhesive comprises 5 to 30 parts by weight based on 100 parts by weight of the polyimide precursor.
[0010] In addition, the present invention provides a photosensitive resin composition comprising: a polyimide precursor represented by the following Chemical Formula 1, an acrylic adhesive, a multifunctional monomer, a photoinitiator, and a crosslinking agent.
[0011] [Chemical formula 1]
[0012]
[0013] In the chemical formula 1,
[0014] X is a tetravalent organic group,
[0015] Y is a divalent organic group,
[0016] R is independently epoxy cyclohexyl methylmethacrylate (ECMMA) or methylglycidyl methacrylate (MGMA),
[0017] n is an integer from 3 to 100,000.
[0018] The present invention is described in detail below according to each component.
[0019] Polyimide Precursor
[0020] The polyimide precursor used in the present invention is represented by the chemical formula 1, which undergoes a cyclization reaction when heated to convert into polyimide.
[0021] The polyimide precursor can be prepared, for example, by the process of the following reaction formula 1. Preferably, X is a tetravalent organic group derived from 2,2-bis(3,4-anhydrodicarboxyphenyl)hexafluoropropane (6FDA, Chemical Formula 2), 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride (DOCDA, Chemical Formula 3) or 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA, Chemical Formula 4). In addition, preferably, Y is a divalent organic group derived from 4,4'-diamino-3,3'-dimethyl-diphenylmethane (DADM, Chemical Formula 5), 2,2-Bis(3-amino-4-hydroxyphenyl)-hexafluoropropane (Bis-APAF, Chemical Formula 6) or 1,3-Bis(3-aminopropyl)tetramethyldisiloxane (SiDA(PAM-E), Chemical Formula 7). In addition, preferably, R is epoxycyclohexyl methyl methacrylate (ECMMA).
[0022] [Reaction formula 1]
[0023]
[0024] [Chemical formula 2]
[0025]
[0026] [Chemical formula 3]
[0027]
[0028] [Chemical formula 4]
[0029]
[0030] [Chemical formula 5]
[0031]
[0032] [Chemical formula 6]
[0033]
[0034] [Chemical formula 7]
[0035]
[0036] The polyimide precursor converts the protection part from the existing GMA to epoxy cyclohexyl methyl methacrylate (ECMMA) or methylglycidyl methacrylate (MGMA) to facilitate the control of molecular weight and solubility, reduce the yield reduction caused by gelation from the root, and improve the sensitivity of the polyimide photosensitive resin composition.
[0037] Preferably, the weight average molecular weight of the polyimide precursor is 3000 to 10000, more preferably 3500 to 7000. When falling within the above range, solubility control, yield and sensitivity can be further improved.
[0038] Acrylic adhesive
[0039] The present invention uses an acrylic adhesive to improve the adhesive force of the insulating film formed from the photosensitive resin composition according to the present invention. As for the polyimide precursor as described above, since the adhesive force is weak, after the insulating film is formed, the adhesive force between the insulating film and the substrate is weak, resulting in a part of defect. Therefore, the present invention uses an acrylic adhesive to play a role in compensating for the adhesive force of the polyimide precursor.
[0040] Preferably, the acrylic adhesive is a copolymer of (i) a first ethylenically unsaturated monomer having one or more carboxyl groups and (ii) a second ethylenically unsaturated monomer having one or more epoxy groups. In addition, the acrylic adhesive can be copolymerized with (iii) a third ethylenically unsaturated monomer copolymerizable with the first ethylenically unsaturated monomer and the second unsaturated monomer as required.
[0041] Preferably, as the (i) first ethylenically unsaturated monomer having one or more carboxyl groups, at least one selected from acrylic acid, methacrylic acid, maleic acid, itaconic acid, and fumaric acid can be used.
[0042] Preferably, as the copolymer of the (ii) second ethylenically unsaturated monomer having one or more epoxy groups, at least one selected from glycidyl methacrylate and methyl glycidyl methacrylate may be used.
[0043] Preferably, as (iii) the third ethylenically unsaturated monomer copolymerizable with the first ethylenically unsaturated monomer and the second unsaturated monomer, at least one selected from styrene, α-methylstyrene, vinyltoluene and vinylbenzyl methyl ether can be used.
[0044] Based on 100 parts by weight of the first ethylenically unsaturated monomer, the second ethylenically unsaturated monomer is preferably used in an amount of 10 to 50 parts by weight. In addition, based on 100 parts by weight of the first ethylenically unsaturated monomer, the third ethylenically unsaturated monomer is preferably used in an amount of 20 to 70 parts by weight.
[0045] Most preferably, the acrylic adhesive preferably uses a copolymer of glycidyl methacrylate or methacrylic acid and styrene.
[0046] Preferably, the weight average molecular weight of the acrylic adhesive is from 1,000 to 100,000, more preferably from 1,500 to 15,000, and most preferably from 3,000 to 10,000.
[0047] In addition, in the photosensitive resin composition according to the present invention, the acrylic adhesive is preferably included in an amount of 5 to 30 parts by weight based on 100 parts by weight of the polyimide precursor. If the content of the acrylic adhesive is less than 5 parts by weight, the effect of improving the adhesion of the insulating film is minimal, and if the content of the acrylic adhesive is more than 30 parts by weight, the heat resistance of the insulating film is reduced.
[0048] Multifunctional monomers
[0049] The multifunctional monomer used in the present invention forms a crosslinked structure when the photosensitive resin composition according to the present invention is exposed to light.
[0050] The multifunctional monomer refers to a compound having 2 to 10 unsaturated functional groups per molecule that can form a crosslinked structure by exposure. Specifically, for example, at least one selected from the group consisting of 1,4-butanediol diacrylate, 1,3-butanediol diacrylate, ethylene glycol diacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, dipentaerythritol hexaacrylate, dipentaerythritol triacrylate, dipentaerythritol diacrylate, sorbitol diacrylate, bisphenol A diacrylate derivatives, dipentaerythritol polyacrylate, and methacrylates thereof can be used.
[0051] In addition, in the photosensitive resin composition according to the present invention, the multifunctional monomer preferably contains 50 to 200 parts by weight based on 100 parts by weight of the polyimide precursor. If the content of the multifunctional monomer is less than 50 parts by weight, the residual film rate is reduced, and if it is more than 200 parts by weight, the resolution is reduced.
[0052] Photoinitiators and crosslinkers
[0053] The photoinitiator used in the present invention is not particularly limited, and any photoinitiator used in a photosensitive resin composition may be used.
[0054] As such a photoinitiator, for example, benzophenone derivatives such as benzophenone, methyl o-benzoylbenzoate, 4-benzoyl-4'-methylbenzophenone, dibenzyl ketone, and fluorenone; acetophenone derivatives such as 2,2-diethoxyacetophenone, 2-hydroxy-2-methylpropiophenone, and 1-hydroxycyclohexylphenyl ketone; thioxanthone derivatives such as thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, and diethylthioxanthone; benzyl derivatives such as benzyl, benzyl dimethyl ketal, and benzyl-β-methoxyethyl acetal; benzyl derivatives such as phenyl benzoin derivatives such as benzoin, benzoin methyl ether; 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl) oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl) oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl) oxime, 1-phenyl-1,2-propanedione-2-(o-benzoyl) oxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl) oxime, 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl) oxime and the like, but not limited thereto. In addition, the photoinitiator can be used alone or in combination of two or more.
[0055] In addition, the crosslinking agent used in the present invention is not particularly limited, and any crosslinking agent used in the photosensitive resin composition may be used. For example, a melamine-based crosslinking agent or a silane coupling agent may be used as the crosslinking agent in the present invention.
[0056] As the melamine-based crosslinking agent, a condensation product of urea and formaldehyde, a condensation product of melamine and formaldehyde, or methylol urea alkyl ethers or methylol melamine alkyl ethers obtained from alcohols can be used.
[0057] Specifically, as the condensation product of urea and formaldehyde, monomethylol urea, dimethylol urea, etc. can be used. As the condensation product of melamine and formaldehyde, hexamethylol melamine can be used. In addition, partial condensation products of melamine and formaldehyde can also be used. In addition, the methylol urea alkyl ethers are obtained by reacting part or all of the methylol groups in the condensation product of urea and formaldehyde with alcohols, and specifically, for example, monomethylol urea methyl ether, dimethylol urea methyl ether, etc. can be used. The methylol melamine alkyl ethers are obtained by reacting part or all of the methylol groups in the condensation product of melamine and formaldehyde with alcohols, and specifically, for example, hexamethylol melamine hexamethyl ether, hexamethylol melamine hexabutyl ether, etc. can be used, but not limited to this. In addition, compounds having a structure in which the hydrogen atoms of the amino group of melamine are replaced by methylol and methoxymethyl, compounds having a structure in which the hydrogen atoms of the amino group of melamine are replaced by butoxymethyl and methoxymethyl, etc. can also be used, for example, methylol melamine alkyl ethers are preferably used, but not limited to this.
[0058] In addition, as the silane coupling agent, γ-aminopropyl dimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-glycidyloxypropyl methyl dimethoxysilane, γ-mercaptopropyl methyl dimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, dimethoxymethyl-3-piperidylpropyl silane, 3-glycidyloxypropyl methyl diethoxysilane, N -(3-diethoxymethylsilylpropyl)succinimide, N-[3-(triethoxysilyl)propyl]phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propionamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propionamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propylsuccinic anhydride, N-phenylaminopropyltrimethoxysilane, etc., but are not limited thereto.
[0059] In addition, in the photosensitive resin composition according to the present invention, based on 100 parts by weight of the polyimide precursor, the photoinitiator preferably comprises 1 to 20 parts by weight. In addition, in the photosensitive resin composition according to the present invention, based on 100 parts by weight of the polyimide precursor, the crosslinking agent preferably comprises 0.1 to 10 parts by weight.
[0060] If the content of the photoinitiator is less than 1 part by weight, the sensitivity may be reduced, and if it is more than 20 parts by weight, the resolution may be reduced. In addition, if the content of the cross-linking agent is less than 0.1 parts by weight, the adhesion may be reduced, and if it is more than 10 parts by weight, residue may be generated.
[0061] Solvents
[0062] Furthermore, the photosensitive resin composition containing the above-mentioned components may contain a solvent in order to form it on a substrate.
[0063] There is no particular limitation on the solvent, and any solvent used for the photosensitive resin composition can be used. For example, alcohols such as methanol, ethanol, benzyl alcohol, and hexanol; ethylene glycol alkyl ether acetates such as ethylene glycol methyl ether acetate and ethylene glycol ethyl ether acetate; ethylene glycol alkyl ether propionates such as ethylene glycol methyl ether propionate and ethylene glycol ethyl ether propionate; ethylene glycol monoalkyl ethers such as ethylene glycol methyl ether and ethylene glycol ethyl ether; diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether and other diethylene glycol alkyl ethers; propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether Propylene glycol alkyl ether acetates such as acetate; propylene glycol methyl ether propionate, propylene glycol ethyl ether propionate, propylene glycol propyl ether propionate and other propylene glycol alkyl ether propionates; propylene glycol monoalkyl ethers such as propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether; dipropylene glycol alkyl ethers such as dipropylene glycol dimethyl ether and dipropylene glycol diethyl ether; butanediol alkyl ethers such as butanediol monomethyl ether and butanediol monoethyl ether; or dibutylene glycol alkyl ethers such as dibutylene glycol dimethyl ether and dibutylene glycol diethyl ether; γ-butyrolactone, etc. Preferably, the solvent preferably uses a solvent in which γ-butyrolactone and propylene glycol methyl ether acetate (PGMEA) are mixed at a weight ratio of 10-90:10-90, respectively, but is not limited thereto.
[0064] The photosensitive resin composition of the present invention may contain a solvent so that the solid content of the entire photosensitive resin composition is 10 wt % to 50 wt %. If the excessive amount of solvent is included to cause the solid content to be less than 10 wt %, there is a problem in residual film formation, and if the solvent content is too little to cause the solid content to be more than 50 wt %, there is a problem in storage stability.
[0065] additive
[0066] The photosensitive resin composition of the present invention may further contain an additive, for example, a neutralizer, as required. Since the neutralizer is further contained, the photosensitive resin composition of the present invention has an effect of alleviating the white turbidity phenomenon.
[0067] As the neutralizing agent, triethanolamine, triethylamine, methylamine, etc. can be used, and triethanolamine is preferably used, but it is not limited thereto.
[0068] The neutralizer may be included in an amount of 1 to 10 parts by weight relative to 100 parts by weight of the polyimide precursor. If the neutralizer content is less than 1 part by weight, the turbidity improvement effect is minimal. If the neutralizer content is greater than 10 parts by weight, the solution may gel.
[0069] Preparation of insulating film
[0070] The photosensitive resin composition can be used to prepare an insulating film, and in particular, can be used to form a pattern of an AMOLED substrate.
[0071] As a specific example, a method of forming an insulating film using the photosensitive resin composition according to the present invention is as follows.
[0072] First, the photosensitive resin composition according to the present invention is applied on the surface of the substrate by spraying, rolling, spin coating, etc., and then the solvent is removed by pre-baking to form a coating film. At this time, the pre-baking is preferably carried out at a temperature of 80° C. to 120° C. for 1 minute to 15 minutes.
[0073] Next, according to the pre-prepared pattern, visible light, ultraviolet light, extreme ultraviolet light, electron beam, X-ray, etc. are irradiated onto the formed coating film, and then post-exposure baking (PEB) and flood exposure (Flood Exposure) are performed as needed, and then unnecessary parts are removed with a developer to form a predetermined pattern.
[0074] The developer preferably uses an alkaline aqueous solution, specifically, inorganic bases such as sodium hydroxide, potassium hydroxide, sodium carbonate, etc.; primary amines such as ethylamine, n-propylamine, etc.; secondary amines such as diethylamine, n-propylamine, etc.; tertiary amines such as trimethylamine, methyldiethylamine, dimethylethylamine, triethylamine, etc.; alcohol amines such as dimethylethanolamine, dimethyldiethanolamine, triethanolamine, etc.; or aqueous solutions of quaternary ammonium salts such as tetramethylammonium hydroxide and tetraethylammonium hydroxide, etc. At this time, after dissolving the alkaline compound to a concentration of 0.1% by weight to 10% by weight, it is used as the developer, and a water-soluble organic solvent such as methanol, ethanol, etc. and a surfactant can be appropriately added.
[0075] In addition, after development using the developer as described above, the film is washed with ultrapure water for 30 seconds to 90 seconds to remove unnecessary parts, and then dried to form a pattern. The pattern is heated at 130°C to 250°C for 30 minutes to 90 minutes by a heating device such as an oven to obtain the final pattern.
[0076] In addition, according to the following examples and comparative examples of the present invention, the adhesive force between the prepared insulating film and the substrate varies depending on whether the acrylic adhesive is used or not. The examples of the present invention have no defects due to their excellent adhesive force, while the comparative examples without the acrylic adhesive have some defects. It can be confirmed that the photosensitive resin composition according to the present invention can significantly reduce defects by improving the adhesive force with the substrate.
[0077] Effects of the Invention
[0078] As described above, according to the photosensitive resin composition of the present invention, by using an acrylic adhesive together with a polyimide precursor, the inherent heat resistance of the polyimide precursor can be maintained and the adhesiveness with the substrate can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0079] Figure 1 The results of evaluating the adhesiveness of the insulating film according to one example of the present invention are shown in SEM images.
[0080] Figure 2 The results of evaluating the adhesiveness of the insulating films of the comparative examples according to the present invention are shown in SEM images. DETAILED DESCRIPTION
[0081] Preferred embodiments are described below to help understand the present invention, but the following embodiments are merely examples of the present invention, and the scope of the present invention is not limited to the following embodiments.
[0082] Preparation Example 1: Preparation of acrylic copolymer (Mw: 6000)
[0083] A mixed solution of 400 parts by weight of tetrahydrofuran, 30 parts by weight of methacrylic acid, 30 parts by weight of styrene, and 40 parts by weight of glycidyl methacrylate was added to a flask with a condenser and an agitator. After the liquid composition was fully mixed in a mixing container at 600 rpm, 15 parts by weight of 2,2'-azobis(2,4-dimethylvaleronitrile) was added. The polymerized mixed solution was slowly heated to 55°C, maintained at this temperature for 24 hours, then cooled to room temperature, and 500 ppm of hydrobenzophenone was added as an inhibitor to obtain a polymer solution with a solid concentration of 30% by weight.
[0084] In order to remove the unreacted monomers of the polymer solution, 100 parts by weight of the polymer solution was precipitated relative to 1000 parts by weight of n-hexane. After precipitation, the poor solvent in which the unreacted products were dissolved was removed by filtering using a mesh. Then, in order to remove the solvent containing the unreacted monomers remaining after the filtering process, it was completely removed by vacuum drying at a temperature below 30° C., thereby preparing an acrylic copolymer.
[0085] The weight average molecular weight of the acrylic copolymer was 6,000. Here, the weight average molecular weight is an average molecular weight measured by GPC in terms of polystyrene.
[0086] Preparation Example 2: Preparation of acrylic copolymer (Mw: 1500)
[0087] An acrylic copolymer having a weight average molecular weight of 1500 was prepared by the same method as in Preparation Example 1 except that 28 parts by weight of 2,2′-azobis(2,4-dimethylvaleronitrile) was used.
[0088] Preparation Example 3: Preparation of acrylic copolymer (Mw: 3000)
[0089] An acrylic copolymer having a weight average molecular weight of 3000 was prepared by the same method as in Preparation Example 1 except that 21 parts by weight of 2,2′-azobis(2,4-dimethylvaleronitrile) was used.
[0090] Preparation Example 4: Preparation of acrylic copolymer (Mw: 8000)
[0091] An acrylic copolymer having a weight average molecular weight of 8,000 was prepared by the same method as in Preparation Example 1 except that 12 parts by weight of 2,2′-azobis(2,4-dimethylvaleronitrile) was used.
[0092] Preparation Example 5: Preparation of acrylic copolymer (Mw: 10000)
[0093] An acrylic copolymer having a weight average molecular weight of 10,000 was prepared by the same method as in Preparation Example 1 except that 10 parts by weight of 2,2′-azobis(2,4-dimethylvaleronitrile) was used.
[0094] Preparation Example 6: Preparation of acrylic copolymer (Mw: 15000)
[0095] An acrylic copolymer having a weight average molecular weight of 15,000 was prepared by the same method as in Preparation Example 1 except that 7 parts by weight of 2,2′-azobis(2,4-dimethylvaleronitrile) was used.
[0096] Example
[0097] (Preparation of polyimide precursor)
[0098] In a 300ml four-necked reaction container, 4g of DADM (chemical formula 5), 7g of Bis-APAF (chemical formula 6), and 1g of SiDA (chemical formula 7) as diamines were dissolved with 70g of γ-butyrolactone. In addition, 5g of 6-FDA (chemical formula 2), 3g of DOCDA (chemical formula 3), and 3g of a-BPDA (chemical formula 4) as dianhydrides were added to the reaction container and stirred for 1 hour. In order to terminate the reaction at the end, 2g of PA was added and further reacted at 20°C for 1 hour to prepare a polyimide precursor with a solid content of 30%, wherein 5g of ECMMA and MGMA as protecting substances were added, totaling 10g, and then the temperature was raised to 70°C, and TEA was added as a catalyst to react for 24 hours, thereby preparing a polyimide precursor.
[0099] (Preparation of Photosensitive Resin Composition)
[0100] 100 parts by weight of the prepared polyimide precursor, 20 parts by weight of the acrylic adhesive prepared in Preparation Example 1, 5 parts by weight of a photoinitiator (1-(o-acetoxime)-1-(9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-ethanone), 100 parts by weight of a multifunctional monomer (dipentaerythritol hexaacrylate), and 3 parts by weight of a crosslinking agent (hexahydroxymethylmelamine hexamethylenetetramine) were dissolved in a solvent of γ-butyrolactone to a solid concentration of 30% by weight, thereby preparing a photosensitive resin composition. The content of each component was changed as shown in Table 1 below to prepare a photosensitive resin composition.
[0101] (Preparation of insulating film)
[0102] The prepared photosensitive resin composition was coated on a 10 mm × 10 mm glass substrate with ITO vapor deposited thereon by a spin coater, and then pre-baked on a hot plate at 110°C for 2 minutes to form a film with a thickness of 3.0 μm. Using a predetermined pattern mask, the intensity at 365 nm was set to 10 mW / cm 2 The film was irradiated with ultraviolet light at a CD reference dose of 20 μm in an isolate pattern, and then developed with a 2.38 wt% aqueous solution of tetramethylammonium hydroxide at 23° C. for 100 seconds, and then washed with ultrapure water for 1 minute. The pattern thus developed was heated in an oven at 230° C. for 60 minutes to cure it, thereby obtaining a pattern film with a thickness of 2.5 μm.
[0103] Comparative Example
[0104] When preparing the photosensitive resin composition, an insulating film was prepared by the same method as in the above-described embodiment, except that the photosensitive resin composition was prepared according to the contents of the components listed in Table 1 below.
[0105]
Table 1
[0106]
[0107] Experimental example
[0108] The surfaces of the insulating films prepared in the examples and comparative examples were evaluated for adhesion, heat resistance, and degree of improvement of white turbidity. The results are shown in Table 2. Figure 1 (Example 2) and Figure 2 (Comparative Example 1). At this time, the adhesive force was evaluated by an optical microscope, and the heat resistance was evaluated by TGA. In addition, the improvement of the white turbidity phenomenon was evaluated by a turbidity meter. The negative photosensitive resin composition coating solution prepared in Examples 1 to 5 and Comparative Examples 1 to 3 was evaluated for performance by the following method, and the results are shown in Table 2 below.
[0109] a) Adhesion: When the pattern film with a thickness of 10 μm or more formed during the sensitivity measurement does not peel off, a value of ○ is given; when the pattern film with a thickness of 15 μm or more and less than 20 μm does not peel off, a value of △ is given; and when the pattern film with a thickness of 20 μm or less peels off, a value of X is given.
[0110] c) Heat resistance: The pattern film formed during the sensitivity measurement was measured using a thermogravimetric analysis (TGA) device. At this time, the case where the 5 wt% weight change temperature was below 260°C was represented by X, and the case where it was above 260°C was represented by ○.
[0111] d) Haze: The pattern film formed in the sensitivity measurement was measured using a haze meter, where 5 or less was indicated as ○, and 5 or more was indicated as X.
[0112]
Table 2
[0113] Adhesion Heat resistance Turbidity Example 1 ○ ○ X Example 2 ○ ○ X Example 3 ○ ○ X Example 4 Δ X ○ Example 5 ○ ○ X Example 6 ○ ○ X Example 7 ○ ○ X Example 8 Δ ○ X Example 9 ○ ○ ○ Example 10 ○ ○ ○ Comparative Example 1 X ○ X Comparative Example 2 ○ X X Comparative Example 3 ○ X X
[0114] Figure 1 No defective parts were observed, so the adhesive strength was excellent. Figure 2In addition, as shown in Table 2, the photosensitive resin composition of the present invention contains triethanolamine as a neutralizing agent as an additive at an appropriate content, so that the white turbidity phenomenon is further improved.
Claims
1. A negative photosensitive resin composition comprising: a polyimide precursor, an acrylic adhesive, a multifunctional monomer, a photoinitiator, and a crosslinking agent, Based on 100 parts by weight of the polyimide precursor, the acrylic adhesive is 5 to 30 parts by weight, the multifunctional monomer is 50 to 200 parts by weight, the photoinitiator is 1 to 20 parts by weight, and the crosslinking agent is 0.1 to 10 parts by weight. The acrylic adhesive is a copolymer of (i) a first ethylenically unsaturated monomer having one or more carboxyl groups, (ii) a second ethylenically unsaturated monomer having one or more epoxy groups, and (iii) a third ethylenically unsaturated monomer copolymerizable with the first ethylenically unsaturated monomer and the second ethylenically unsaturated monomer. The polyimide precursor is represented by the following chemical formula 1: [Chemical formula 1] In the chemical formula 1, X is a tetravalent organic group, Y is a divalent organic group, R is independently epoxycyclohexylmethyl methacrylate or methylglycidyl methacrylate, n is an integer from 3 to 100,000. 2 . The negative photosensitive resin composition according to claim 1 , comprising a solvent so that the solid content of the entire negative photosensitive resin composition is 10 wt % to 50 wt %.
3. The negative photosensitive resin composition according to claim 1, wherein X is a tetravalent organic group derived from 2,2-bis(3,4-anhydrodicarboxyphenyl)hexafluoropropane; 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride; or 2,3,3',4'-biphenyltetracarboxylic anhydride.
4. The negative photosensitive resin composition according to claim 1, wherein Y is a divalent organic group derived from 4,4′-diamino-3,3′-dimethyl-biphenylmethane; 2,2-bis(3-amino-4-hydroxyphenyl)-hexafluoropropane; or 1,3-bis(3-aminopropyl)tetramethyldisiloxane.
5. The negative photosensitive resin composition according to claim 1, wherein The weight average molecular weight of the polyimide precursor is 3,000 to 10,000.
6. The negative photosensitive resin composition according to claim 1, wherein The acrylic adhesive is a copolymer of glycidyl methacrylate, methacrylic acid and styrene.
7. The negative photosensitive resin composition according to claim 1, wherein The acrylic adhesive has a weight average molecular weight of 1,000 to 100,000.
8. The negative photosensitive resin composition according to claim 1, wherein The invention further comprises 1 to 10 parts by weight of one or more neutralizing agents selected from triethanolamine, triethylamine and methylamine, based on 100 parts by weight of the polyimide precursor.