Supported non-metallocene catalyst, preparation method and application thereof
By controlling the alcohol concentration and simplifying the preparation process, the problems of short activity of supported non-metallocene catalysts and insufficient molecular weight of polymers are solved, and efficient olefin polymerization is achieved, which significantly improves the catalyst activity and polymer bulk density, and is in hydrogen-free conditions. Ultra-high molecular weight polyethylene was obtained.
Patent Information
- Application Number
- CN201710814593.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-09-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2037-09-11
AI Technical Summary
The existing supported non-metallocene catalysts have problems such as short active duration, easy sticking, high methyl aluminoxane usage and insufficient polymer molecular weight in the olefin polymerization reaction, and the heterophase composition formed during the preparation process limits the catalyst performance and Particle morphology.
By controlling the concentration of alcohol in the composite support, the preparation method without proton duct and electron donor is simplified to prepare the supported non-metallocene catalyst, avoid harsh reaction conditions, and use magnesium compounds and non-metallocene ligands in Dissolve in the alcohol solution, combines thermal activation and chemical activation treatment, followed by drying and processing to obtain a modified composite carrier, and finally chemically treated with a Group IV B metal compound.
The activity of the catalyst and the polymer bulk density are significantly improved, the amount of cocatalyst is reduced, the activity life of the catalyst is extended, the particle morphology of the polymer is improved, and the polymerization of ultra-high molecular weight polyethylene is achieved under hydrogen-free conditions.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] This application is based on the ongoing project of the National 11th Five-Year Plan. This project has received great attention and strong support from the Ministry of Science and Technology. Its goal is to form a new generation of polyolefin catalyst technology with independent intellectual property rights, improve the homogeneity of related domestic products, improve the quality of my country's polyolefin varieties, and promote its development in the direction of diversification, serialization, specialization, and high performance. Technical Field
[0002] The present invention relates to a non-metallocene catalyst, and more particularly to a supported non-metallocene catalyst, a preparation method thereof and an application thereof in olefin homopolymerization / copolymerization. Background Art
[0003] The non-metallocene catalysts that appeared in the mid-to-late 1990s are also called post-metallocene catalysts. The central atom of the main catalyst includes almost all transition metal elements. It is the fourth generation of olefin polymerization catalysts after Ziegler, Ziegler-Natta and metallocene catalysts. This type of catalyst has reached or even exceeded metallocene catalysts in some performances. Non-metallocene catalysts do not contain cyclopentadiene groups, and the coordinating atoms are oxygen, nitrogen, sulfur and phosphorus. They are characterized by strong electrophilicity of the central ion and a cis-alkyl or halogen metal central structure, which is easy to insert olefins and transfer σ-bonds. The central metal is easy to alkylate, which is conducive to the formation of cationic active centers; the complex formed has a limited geometric configuration, stereoselectivity, electronegativity and chirality adjustability. In addition, the formed metal-carbon bond is easy to polarize, which is conducive to the polymerization of olefins. Therefore, even at higher polymerization reaction temperatures, olefin polymers with higher molecular weights can be obtained.
[0004] However, homogeneous olefin polymerization catalysts have been proven to have shortcomings in olefin polymerization reactions, such as short activity duration, easy kettle sticking, high methylaluminoxane dosage, and too low or too high molecular weight of the obtained polymer, which seriously limit their industrial application.
[0005] An olefin homopolymerization / copolymerization catalyst or catalytic system prepared by patents ZL01126323.7, ZL02151294.9, ZL02110844.7 and WO03 / 010207 has a wide range of olefin homopolymerization / copolymerization properties and is suitable for various forms of polymerization processes. However, the catalyst or catalytic system disclosed in the patent requires a higher amount of co-catalyst during olefin polymerization to obtain suitable olefin polymerization activity, and there is a sticking kettle phenomenon during the polymerization process.
[0006] The usual practice is to make non-metallocene catalysts into supported catalysts through certain supporting technologies, thereby improving the polymerization performance of olefins and the particle morphology of the resulting polymers. This is manifested in that the initial activity of the catalyst is appropriately reduced to a certain extent, the polymerization activity life of the catalyst is extended, the agglomeration or violent polymerization phenomenon during the polymerization process is reduced or even avoided, the morphology of the polymer is improved, and the apparent density of the polymer is increased, so that it can meet more polymerization process, such as gas phase polymerization or slurry polymerization.
[0007] Regarding the non-metallocene catalysts disclosed in patents ZL01126323.7, ZL02151294.9, ZL02110844.7 and WO03 / 010207, patents CN1539855A, CN 1539856A, CN1789291A, CN1789292A, CN1789290A, WO / 2006 / 063501, 200510119401.x, etc., various methods are used for loading to obtain loaded non-metallocene catalysts. However, these patents all involve loading non-metallocene organic compounds containing transition metals (or non-metallocene catalysts, or non-metallocene complexes) on treated carriers, and either the loading amount of the non-metallocene catalyst is low, or it is not very tightly bound to the carrier.
[0008] Most of the existing olefin polymerization catalyst patents are based on metallocene catalysts, such as US 4808561, US 5240894, CN 1049439, CN 1136239, CN 1344749, CN 1126480, CN1053673, CN 1307594, CN 1130932, CN 1103069, CN1363537, CN1060179, US574417, EP685494, US4871705 and EP0206794, but these patents also involve loading a metallocene catalyst containing a transition metal on a treated carrier.
[0009] Patent EP708116 discloses that gasified zirconium tetrachloride is first contacted with a carrier at a temperature of 160-450°C and loaded, and then the loaded zirconium tetrachloride is reacted with a lithium salt of a ligand to obtain a loaded metallocene catalyst, which is then used for olefin polymerization by combining with a co-catalyst. The problem with this catalyst is that the loading process requires high temperature and high vacuum, and is not suitable for industrial production.
[0010] There are literature reports that MgCl2(THF)2 was treated with ethylaluminum chloride and loaded with zirconocene dichloride to prepare a supported metallocene catalyst. The process is: magnesium chloride is dissolved in tetrahydrofuran, precipitated and washed with hexane, then treated with ethylaluminum chloride, and finally loaded with zirconocene dichloride (EUROPEAN POLYMER JOURNAL, 2005, 41, 941-947).
[0011] Sun Min et al. published in their paper “Preparation of CpTi(dbm)Cl2 / MgCl2 Supported Catalyst by In-situ Reaction Method and Study on Its Catalytic Ethylene Polymerization” (Acta Polymerica Sinica, 2004, (1): 138), in which they prepared the magnesium chloride support by Grignard reagent method and added CpTi(dbm)Cl2 to prepare the CpTi(dbm)Cl2 / MgCl2 supported catalyst. In this way, the alkylation and loading of the catalyst were completed in one step, greatly reducing the catalyst preparation process.
[0012] Patent CN200510080210.7 discloses an in-situ synthesized supported vanadium-based non-cyclopentadienyl polyolefin catalyst and its preparation method and application, wherein dialkyl magnesium is first reacted with acyl naphthol or β-diketone to form acyl naphthol magnesium or β-diketone magnesium compound, which is then reacted with tetravalent vanadium chloride to simultaneously form a carrier and an active catalytic component.
[0013] Patent CN200610026765.8 discloses a type of single-active-center Ziegler-Natta olefin polymerization catalyst. The catalyst uses salicylaldehyde or a substituted salicylaldehyde derivative containing a coordination group as an electron donor, and is obtained by adding a pretreated carrier (such as silica gel), a metal compound (such as titanium tetrachloride) and the electron donor to a magnesium compound (such as magnesium chloride) / tetrahydrofuran solution, and treating the mixture.
[0014] Patent CN200610026766.2 is similar thereto, disclosing a class of organic compounds containing heteroatoms and their application in Ziegler-Natta catalysts.
[0015] Patent CN200710162676.0 discloses a magnesium compound supported non-metallocene catalyst and a preparation method thereof, which is obtained by directly contacting a non-metallocene ligand with a magnesium compound containing a catalytically active metal through an in-situ loading method. However, the contact between the catalytically active metal and the magnesium compound described therein refers to adding a Group IV B metal compound to a formed magnesium compound solid (such as a magnesium compound solid or a modified magnesium compound solid). Such contact cannot achieve a full reaction between the catalytically active metal and the magnesium compound, and the obtained magnesium compound carrier containing the catalytically active metal must be heterogeneous, not a full contact and reaction between molecules, thereby limiting the full effect of the non-metallocene ligand added subsequently.
[0016] Similarly, patent CN200710162667.1 discloses a magnesium compound supported non-metallocene catalyst and its preparation method, which also has similar problems. It is obtained by directly contacting a compound of a catalytically active metal with a magnesium compound containing a non-metallocene ligand through an in-situ loading method. However, the contact described therein refers to adding a non-metallocene ligand solution to a formed magnesium compound solid (such as a magnesium compound solid or a modified magnesium compound solid). Such contact cannot achieve a full reaction between the non-metallocene ligand and the magnesium compound. The obtained magnesium compound carrier containing the non-metallocene ligand must be heterogeneous, not a full contact and reaction between molecules, thereby limiting the full play of the effect of the non-metallocene ligand.
[0017] The PCT patent PCT / CN2008 / 001739 applied for based on the above two patents still has the above problems.
[0018] Catalysts supported by anhydrous magnesium chloride show high catalytic activity in olefin polymerization, but such catalysts are very brittle and easily broken in the polymerization reactor, resulting in poor polymer morphology. Catalysts supported by silica have good fluidity and can be used for gas phase fluidized bed polymerization, but silica-supported metallocene and non-metallocene catalysts show low catalytic activity. Therefore, if magnesium chloride and silica are well organically combined, it is possible to prepare a catalyst with high catalytic activity, controllable particle size and good wear resistance.
[0019] Patent ZL01131136.3 discloses a method for synthesizing supported metallocene catalysts. In this method, silica gel and IV B group transition metal halide are mixed in a solvent under normal pressure, and then directly reacted with ligand anions, thereby achieving the synthesis and loading of metallocene catalysts in one step. However, this method requires a molar ratio of transition metal to ligand of 1:1, and requires the addition of a proton donor, such as butyl lithium, etc., and the ligand used is a bridged or non-bridged metallocene ligand containing a cyclopentadiene group.
[0020] Xiao Yizhi et al. published in their paper "Study on Preparation of Branched Polyethylene by Catalytic Ethylene Polymerization with New Ni(acac)2 / TiCl4 / L Ligand Composite Catalyst" (Journal of Sun Yat-sen University: Natural Science Edition, 2003, 42(3): 28). They dissolved anhydrous MgCl2, Ni(acac)2 and L in a tetrahydrofuran-ethanol mixed solvent, added silica gel to stir the reaction, added a certain amount of titanium tetrachloride to continue the reaction, then added a certain amount of Et2AlCl to react, and dried the catalyst to obtain a Ni(acac)2 / TiCl4 composite catalyst with magnesium chloride-silica gel as a carrier and modified with α-diimine ligand L. Branched polyethylene can be obtained by catalyzing mono-ethylene polymerization with the catalyst, wherein the ligand L2 produces branched polyethylene with a branching degree of 4-12 branches / 1000C.
[0021] Patent CN200910210991.5 discloses a method for preparing a supported non-metallocene catalyst, comprising the following steps: dissolving a magnesium compound and a non-metallocene ligand in a solvent in the presence of an alcohol to obtain a magnesium compound solution; mixing a porous carrier optionally subjected to a heat activation treatment with the magnesium compound solution to obtain a mixed slurry; adding a precipitant to the mixed slurry to obtain a composite carrier; and treating the composite carrier with a chemical treatment agent selected from Group IV B metal compounds to obtain the supported non-metallocene catalyst. According to the disclosure, the role of the introduced alcohol is only to serve as a cosolvent for the magnesium compound and the non-metallocene ligand, and is then removed during the drying process.
[0022] As can be seen from the above, a common problem of supported non-metallocene catalysts in the prior art is that the heterogeneous composition and distribution formed during the preparation of the catalysts limits the performance of the catalyst polymerization products and their particle morphology.
[0023] Therefore, the current situation is that there is still a need for a supported non-metallocene catalyst, which has a simple preparation method, is suitable for industrial production, and can overcome the problems existing in the supported non-metallocene catalysts in the prior art. Summary of the invention
[0024] The inventors have found through diligent research based on the prior art that the above-mentioned problems can be solved by using a specific preparation method to manufacture the supported non-metallocene catalyst, especially by controlling the concentration of alcohol in the composite carrier to further play its role in improving the catalyst activity and polymer particle morphology, and thus completing the present invention.
[0025] In the preparation method of the supported non-metallocene catalyst of the present invention, no proton donor (such as those conventionally used in the art) is added. In addition, in the preparation method of the supported non-metallocene catalyst of the present invention, no electron donor (such as compounds such as monoesters, diesters, diethers, diketones and diol esters conventionally used in the art for this purpose) is added. Furthermore, in the preparation method of the supported non-metallocene catalyst of the present invention, no harsh reaction requirements and reaction conditions are required. Therefore, the preparation method of the supported catalyst is simple and very suitable for industrial production.
[0026] Specifically, the present invention relates to a method for preparing a supported non-metallocene catalyst, comprising the following steps:
[0027] A step of dissolving a magnesium compound in a solvent in the presence of an alcohol to obtain a magnesium compound solution;
[0028] A step of mixing a porous carrier which has been optionally subjected to a thermal activation treatment and / or a chemical activation treatment with the magnesium compound solution to obtain a mixed slurry;
[0029] The step of drying the mixed slurry or adding a precipitant to the mixed slurry to obtain a composite carrier, wherein the content of the alcohol in the composite carrier is 0.5-2.5wt%, preferably 1.0-2.0wt%;
[0030] treating the composite support with a non-metallocene ligand to obtain a modified composite support; and
[0031] The step of treating the modified composite support with a chemical treatment agent selected from Group IV B metal compounds to obtain the supported non-metallocene catalyst.
[0032] The invention also relates to a supported non-metallocene catalyst prepared by the preparation method and application thereof in olefin homopolymerization / copolymerization.
[0033] Technical Effects
[0034] The preparation method of the supported non-metallocene catalyst of the present invention is simple and feasible.
[0035] By using the catalyst preparation method provided by the present invention, it is surprisingly found that due to the strict control and retention of a certain alcohol content during the drying process of the composite carrier, the catalytic activity and polymer bulk density are significantly improved, and the amount of co-catalyst required in the polymerization process is also low.
[0036] The supported non-metallocene catalyst prepared by the present invention has a remarkable copolymerization effect, that is, the copolymerization activity of the catalyst is higher than the homopolymerization activity, and the copolymerization reaction can increase the bulk density of the polymer, that is, improve the particle morphology of the polymer.
[0037] By using the supported non-metallocene catalyst provided by the present invention, ultra-high molecular weight polyethylene with a relatively high molecular weight can be obtained by polymerization under homopolymerization conditions without the participation of hydrogen. DETAILED DESCRIPTION
[0038] The specific embodiments of the present invention are described in detail below, but it should be pointed out that the protection scope of the present invention is not limited by these specific embodiments, but is determined by the claims in the appendix.
[0039] In the context of the present invention, unless otherwise expressly defined or the meaning is beyond the comprehension of a person skilled in the art, hydrocarbon or hydrocarbon derivative groups having more than 3 carbon atoms (such as propyl, propoxy, butyl, butane, butene, butenyl, hexane, etc.) have the same meaning when not preceded by the prefix "n". For example, propyl is generally understood to be n-propyl, and butyl is generally understood to be n-butyl.
[0040] In the context of the present invention, unless otherwise specified, the physical properties of a substance (such as boiling point) are measured at normal temperature (25° C.) and normal pressure (101325 Pa).
[0041] According to the present invention, it relates to a method for preparing a supported non-metallocene catalyst, comprising the following steps: dissolving a magnesium compound in a solvent in the presence of an alcohol to obtain a magnesium compound solution; mixing a porous carrier that has been optionally subjected to a thermal activation treatment and / or a chemical activation treatment with the magnesium compound solution to obtain a mixed slurry; drying the mixed slurry or adding a precipitant to the mixed slurry to obtain a composite carrier, wherein the content of the alcohol in the composite carrier is 0.5-2.5wt%; treating the composite carrier with a non-metallocene ligand to obtain a modified composite carrier; and treating the modified composite carrier with a chemical treatment agent selected from Group IV B metal compounds to obtain the supported non-metallocene catalyst.
[0042] The steps of obtaining the magnesium compound solution are described in detail below.
[0043] According to this step, a magnesium compound is dissolved in an appropriate solvent (ie, a solvent for dissolving the magnesium compound) in the presence of an alcohol, thereby obtaining the magnesium compound solution.
[0044] As the solvent, for example, C 6-12 Aromatic hydrocarbons, halogenated C 6-12 Aromatic hydrocarbons, esters and ethers are preferred solvents. Specific examples include toluene, xylene, trimethylbenzene, ethylbenzene, diethylbenzene, chlorotoluene, chloroethylbenzene, bromotoluene, bromoethylbenzene, ethyl acetate and tetrahydrofuran. Among them, C 6-12 Aromatic hydrocarbons and tetrahydrofuran, most preferably tetrahydrofuran.
[0045] These solvents may be used alone or in combination of two or more in any proportion.
[0046] According to the present invention, the term "alcohol" refers to a hydrocarbon chain (such as C 1-30 A compound obtained by replacing at least one hydrogen atom on a hydrocarbon with a hydroxyl group.
[0047] As the alcohol, for example, C 1-30 Fatty alcohol (preferably C 1-30 Aliphatic monohydric alcohol), C 6-30 Aromatic alcohol (preferably C 6-30 Aromatic monohydric alcohol) and C 4-30 Alicyclic alcohol (preferably C 4-30 Alicyclic monohydric alcohol), among which C 1-30 Aliphatic monohydric alcohol or C 2-8 Aliphatic monohydric alcohols, more preferably ethanol and butanol. In addition, the alcohol may be optionally selected from halogen atoms or C 1-6 The substituents of the alkoxy group are substituted.
[0048] As the C 1-30 Examples of the aliphatic alcohol include methanol, ethanol, propanol, 2-propanol, butanol, pentanol, 2-methylpentanol, 2-ethylpentanol, 2-hexylbutanol, hexanol and 2-ethylhexanol, among which ethanol, butanol and 2-ethylhexanol are preferred.
[0049] As the C 6-30 Examples of the aromatic alcohol include benzyl alcohol, phenethyl alcohol and methylbenzyl alcohol, among which phenethyl alcohol is preferred.
[0050] As the C 4-30 Examples of the alicyclic alcohol include cyclohexanol, cyclopentanol, cyclooctanol, methylcyclopentanol, ethylcyclopentanol, propylcyclopentanol, methylcyclohexanol, ethylcyclohexanol, propylcyclohexanol, methylcyclooctanol, ethylcyclooctanol and propylcyclooctanol, among which cyclohexanol and methylcyclohexanol are preferred.
[0051] Examples of the alcohol substituted with a halogen atom include trichloromethanol, trichloroethanol and trichlorohexanol, among which trichloromethanol is preferred.
[0052] Examples of the alcohol substituted with an alkoxy group include ethylene glycol monoethyl ether, ethylene glycol monon-butyl ether and 1-butoxy-2-propanol, among which ethylene glycol monoethyl ether is preferred.
[0053] These alcohols can be used alone or in combination. When used in a combination of multiple alcohols, the ratio between any two alcohols in the alcohol mixture can be arbitrarily determined and is not particularly limited.
[0054] To prepare the magnesium compound solution, the magnesium compound may be added to a mixed solvent formed of the solvent and the alcohol for dissolution, or the magnesium compound may be added to the solvent and alcohol may be added simultaneously or subsequently for dissolution, but is not limited thereto.
[0055] When preparing the magnesium compound solution, the molar ratio of the magnesium compound (solid) to the alcohol calculated as magnesium element is 1:0.02-4.00, preferably 1:0.05-3.00, more preferably 1:0.10-2.50, and the ratio of the magnesium compound (solid) to the solvent calculated as magnesium element is generally 1 mol:75-400 ml, preferably 1 mol:150-300 ml, more preferably 1 mol:200-250 ml.
[0056] The preparation time of the magnesium compound solution (i.e., the dissolution time of the magnesium compound) is not particularly limited, but is generally 0.5 to 24 hours, preferably 4 to 24 hours. During the preparation process, stirring can be used to promote the dissolution of the magnesium compound. The stirring can be in any form, such as a stirring paddle (the rotation speed is generally 10 to 1000 rpm). As needed, dissolution can sometimes be promoted by appropriate heating.
[0057] The magnesium compound is described in detail below.
[0058] According to the present invention, the term "magnesium compound" uses the common concept in the art and refers to an organic or inorganic solid anhydrous magnesium-containing compound conventionally used as a carrier for supported olefin polymerization catalysts.
[0059] According to the present invention, the magnesium compound may include, for example, magnesium halide, alkoxymagnesium halide, alkoxymagnesium, alkylmagnesium, alkylmagnesium halide and alkylalkoxymagnesium.
[0060] Specifically, examples of the magnesium halide include magnesium chloride (MgCl2), magnesium bromide (MgBr2), magnesium iodide (MgI2) and magnesium fluoride (MgF2), among which magnesium chloride is preferred.
[0061] Examples of the alkoxy magnesium halide include methoxymagnesium chloride (Mg(OCH3)Cl), ethoxymagnesium chloride (Mg(OC2H5)Cl), propoxymagnesium chloride (Mg(OC3H7)Cl), n-butoxymagnesium chloride (Mg(OC4H9)Cl), isobutoxymagnesium chloride (Mg(i-OC4H9)Cl), methoxymagnesium bromide (Mg(OCH3)Br), ethoxymagnesium bromide (Mg(OC2H5)Br), propoxymagnesium bromide (Mg(OC3H7 )Br), n-butoxymagnesium bromide (Mg(OC4H9)Br), isobutoxymagnesium bromide (Mg(i-OC4H9)Br), methoxymagnesium iodide (Mg(OCH3)I), ethoxymagnesium iodide (Mg(OC2H5)I), propoxymagnesium iodide (Mg(OC3H7)I), n-butoxymagnesium iodide (Mg(OC4H9)I) and isobutoxymagnesium iodide (Mg(i-OC4H9)I), etc., among which methoxymagnesium chloride, ethoxymagnesium chloride and isobutoxymagnesium chloride are preferred.
[0062] As the alkoxymagnesium, for example, methoxymagnesium (Mg(OCH3)2), ethoxymagnesium (Mg(OC2H5)2), propoxymagnesium (Mg(OC3H7)2), butoxymagnesium (Mg(OC4H9)2), isobutoxymagnesium (Mg(i-OC4H9)2) and 2-ethylhexyloxymagnesium (Mg(OCH2CH(C2H5)C4H)2) can be mentioned, among which ethoxymagnesium and isobutoxymagnesium are preferred.
[0063] As the alkyl magnesium, for example, methyl magnesium (Mg(CH3)2), ethyl magnesium (Mg(C2H5)2), propyl magnesium (Mg(C3H7)2), n-butyl magnesium (Mg(C4H9)2) and isobutyl magnesium (Mg(i-C4H9)2) can be mentioned, among which ethyl magnesium and n-butyl magnesium are preferred.
[0064] As the alkyl magnesium halide, for example, methyl magnesium chloride (Mg(CH3)Cl), ethyl magnesium chloride (Mg(C2H5)Cl), propyl magnesium chloride (Mg(C3H7)Cl), n-butyl magnesium chloride (Mg(C4H9)Cl), isobutyl magnesium chloride (Mg(i-C4H9)Cl), methyl magnesium bromide (Mg(CH3)Br), ethyl magnesium bromide (Mg(C2H5)Br), propyl magnesium bromide (Mg(C3H7)Cl), )Br), n-butylmagnesium bromide (Mg(C4H9)Br), isobutylmagnesium bromide (Mg(i-C4H9)Br), methylmagnesium iodide (Mg(CH3)I), ethylmagnesium iodide (Mg(C2H5)I), propylmagnesium iodide (Mg(C3H7)I), n-butylmagnesium iodide (Mg(C4H9)I) and isobutylmagnesium iodide (Mg(i-C4H9)I), etc., among which methylmagnesium chloride, ethylmagnesium chloride and isobutylmagnesium chloride are preferred.
[0065] Examples of the alkyl alkoxy magnesium include methyl methoxy magnesium (Mg(OCH3)(CH3)), methyl ethoxy magnesium (Mg(OC2H5)(CH3)), methyl propoxy magnesium (Mg(OC3H7)(CH3)), methyl n-butoxy magnesium (Mg(OC4H9)(CH3)), methyl isobutoxy magnesium (Mg(i-OC4H9)(CH3)), ethyl methoxy magnesium (Mg(OCH3)(C2H5)), ethyl ethoxy magnesium (Mg(OC2H5)(C2H5)), ethyl propoxy magnesium (Mg(OC3H7)(C2H5)), ethyl n-butoxy magnesium (Mg(OC4H9)(C2H5)), ethyl isobutoxy magnesium (Mg(i-OC4H9)(C2H5)), propyl methoxy magnesium (Mg(OCH3)(C3H7)), propyl ethoxy magnesium (Mg(OC2H5)(C3H7)), propyl propoxy magnesium (Mg(OC3H7)(C3H7)), Propyl magnesium n-butoxide (Mg(OC4H9)(C3H7)), propyl magnesium isobutoxide (Mg(i-OC4H9)(C3H7)), n-butyl magnesium methoxide (Mg(OCH3)(C4H9)), n-butyl magnesium ethoxide (Mg(OC2H5)(C4H9)), n-butyl magnesium propoxide (Mg(OC3H7)(C4H9)), n-butyl magnesium n-butoxide (Mg(OC4H9)(C4H9)), n-butyl magnesium isobutoxide (Mg(i-OC4H9)(C3H7)), n-butyl magnesium methoxide (Mg(OCH3)(C4H9)), n-butyl magnesium ethoxide (Mg(OC2H5)(C4H9)), n-butyl magnesium propoxide (Mg(OC3H7)(C4H9)), n-butyl magnesium n-butoxide (Mg(OC4H9)(C4H9)), n-butyl magnesium isobutoxide (Mg(i -OC4H9)(C4H9)), isobutyl methoxymagnesium (Mg(OCH3)(i-C4H9)), isobutyl ethoxymagnesium (Mg(OC2H5)(i-C4H9)), isobutyl propoxymagnesium (Mg(OC3H7)(i-C4H9)), isobutyl n-butoxymagnesium (Mg(OC4H9)(i-C4H9)) and isobutyl isobutoxymagnesium (Mg(i-OC4H0)(i-C4H9)), etc., among which butyl ethoxymagnesium is preferred.
[0066] These magnesium compounds may be used alone or in combination of two or more, without particular limitation.
[0067] When used in a mixed form, the molar ratio between any two magnesium compounds in the magnesium compound mixture is, for example, 0.25 to 4:1, preferably 0.5 to 3:1, and more preferably 1 to 2:1.
[0068] The porous carrier is mixed with the magnesium compound solution, thereby obtaining a mixed slurry.
[0069] According to the present invention, the mixing process of the porous carrier and the magnesium compound solution can be carried out by a common method without special limitation. For example, the porous carrier is metered into the magnesium compound solution at room temperature to the preparation temperature of the magnesium compound solution, or the magnesium compound solution is metered into the porous carrier, and mixed for 0.1 to 8 hours, preferably 0.5 to 4 hours, and optimally 1 to 2 hours (with stirring if necessary).
[0070] According to the present invention, the porous carrier is used in an amount such that the mass ratio of the magnesium compound (based on the magnesium compound solid contained in the magnesium compound solution) to the porous carrier reaches 1:0.1-20, preferably 1:0.5-10, and more preferably 1:1-5.
[0071] According to the present invention, the mixed slurry is a semi-dry system without free liquid. Although not necessary, in order to ensure the uniformity of the system, the mixed slurry is preferably allowed to stand in a closed state for a certain period of time (2 to 48 hours, preferably 4 to 24 hours, and most preferably 6 to 18 hours) after preparation.
[0072] The porous carrier is described in detail below.
[0073] According to the present invention, the porous carrier may be, for example, organic or inorganic porous solids conventionally used as carriers in the preparation of supported olefin polymerization catalysts in the art.
[0074] Specifically, the organic porous solid includes, for example, olefin homopolymers or copolymers, polyvinyl alcohol or its copolymers, cyclodextrin, (co)polyester, (co)polyamide, vinyl chloride homopolymers or copolymers, acrylate homopolymers or copolymers, methacrylate homopolymers or copolymers, styrene homopolymers or copolymers, and partially cross-linked forms of these homopolymers or copolymers, among which partially cross-linked (for example, a cross-linking degree of at least 2% but less than 100%) styrene polymers are preferred.
[0075] According to a preferred embodiment of the present invention, the surface of the organic porous solid preferably carries any one or more active functional groups selected from the group consisting of hydroxyl, primary amino, secondary amino, sulfonic acid, carboxyl, amide, N-monosubstituted amide, sulfonamide, N-monosubstituted sulfonamide, thiol, imido and hydrazide, wherein at least one of carboxyl and hydroxyl is preferred.
[0076] According to one embodiment of the present invention, the organic porous solid is subjected to a thermal activation treatment and / or a chemical activation treatment before use.
[0077] According to the present invention, the organic porous solid may be subjected to only a thermal activation treatment before use, or may be subjected to only a chemical activation treatment before use, or may be subjected to the thermal activation treatment and the chemical activation treatment in sequence in any combination order before use, without any particular limitation.
[0078] The thermal activation treatment can be carried out in the usual manner. For example, the organic porous solid is subjected to a heat treatment under reduced pressure or in an inert atmosphere. The inert atmosphere mentioned here refers to a gas containing only extremely trace amounts or no components that can react with the organic porous solid. As the inert atmosphere, for example, nitrogen or a rare gas atmosphere can be cited, preferably a nitrogen atmosphere. Since organic porous solids have poor heat resistance, the thermal activation process is based on the premise of not destroying the structure and basic composition of the organic porous solid itself. Generally, the thermal activation temperature is 50 to 400°C, preferably 100 to 250°C, and the thermal activation time is 1 to 24 hours, preferably 2 to 12 hours.
[0079] After the thermal activation / chemical activation treatment, the organic porous solid needs to be stored under positive pressure in an inert atmosphere for future use.
[0080] As the inorganic porous solid, for example, refractory oxides of metals of Group II A, III A, IV A or IV B of the periodic table (such as silicon dioxide (also known as silicon oxide or silica gel), aluminum oxide, magnesium oxide, titanium oxide, zirconium oxide or thorium oxide, etc.), or any refractory composite oxides of these metals (such as silicon aluminum oxide, magnesium aluminum oxide, titanium silicon oxide, titanium magnesium oxide and titanium aluminum oxide, etc.), as well as clay, molecular sieves (such as ZSM-5 and MCM-41), mica, montmorillonite, bentonite and diatomaceous earth, etc. As the inorganic porous solid, oxides generated by high-temperature hydrolysis of gaseous metal halides or gaseous silicon compounds, such as silica gel obtained by high-temperature hydrolysis of silicon tetrachloride, or aluminum oxide obtained by high-temperature hydrolysis of aluminum trichloride, etc. can also be cited.
[0081] As the inorganic porous solid, silicon dioxide, aluminum oxide, magnesium oxide, silicon aluminum oxide, magnesium aluminum oxide, titanium silicon oxide, titanium dioxide, molecular sieves, and montmorillonite are preferred, and silicon dioxide is particularly preferred.
[0082] According to the present invention, suitable silica can be manufactured by conventional methods, or can be any commercially available product, such as Grace 955, Grace 948, Grace SP9-351, Grace SP9-485, Grace SP9-10046, Davsion Syloid 245 and Aerosil 812 from Grace Company, ES70, ES70X, ES70Y, ES70W, ES757, EP10X and EP11 from Ineos Company, and CS-2133 and MS-3040 from PQ Company.
[0083] According to a preferred embodiment of the present invention, the surface of the inorganic porous solid preferably has active functional groups such as hydroxyl groups.
[0084] According to the present invention, in one embodiment, the inorganic porous solid is subjected to a thermal activation treatment and / or a chemical activation treatment before use.
[0085] According to the present invention, the inorganic porous solid can be subjected to only thermal activation treatment before use, or can be subjected to only chemical activation treatment before use, or can be subjected to the thermal activation treatment and the chemical activation treatment in any combination order before use, without any particular limitation.
[0086] The thermal activation treatment can be carried out in the usual manner, such as heating the inorganic porous solid under reduced pressure or in an inert atmosphere. The inert atmosphere mentioned here refers to a gas containing only extremely trace amounts or no components that can react with the inorganic porous solid. As the inert atmosphere, for example, nitrogen or a rare gas atmosphere can be cited, preferably a nitrogen atmosphere. Generally, the thermal activation temperature is 200-800°C, preferably 400-700°C, most preferably 400-650°C, and the heating time is, for example, 0.5-24h, preferably 2-12h, and most preferably 4-8h.
[0087] After the thermal activation / chemical activation treatment, the inorganic porous solid needs to be stored under positive pressure in an inert atmosphere for future use.
[0088] According to the present invention, the chemical activation treatment performed on the organic porous solid or the inorganic porous solid can be performed in a common manner, for example, a method of performing chemical activation treatment on the organic porous solid or the inorganic porous solid using a chemical activating agent can be cited.
[0089] The chemical activator will first be described in detail below.
[0090] According to the present invention, a Group IV B metal compound is used as the chemical activator.
[0091] Examples of the Group IV B metal compound include at least one selected from Group IV B metal halides, Group IV B metal alkyl compounds, Group IV B metal alkoxy compounds, Group IV B metal alkyl halides and Group IV B metal alkoxy halides.
[0092] Examples of the IV B Group metal halide, the IV B Group metal alkyl compound, the IV B Group metal alkoxy compound, the IV B Group metal alkyl halide and the IV B Group metal alkoxy halide include compounds having the following general structure:
[0093] M(OR 1 ) m X n R 2 4-m-n
[0094] in:
[0095] m is 0, 1, 2, 3 or 4;
[0096] n is 0, 1, 2, 3 or 4;
[0097] M is a metal of Group IV B in the periodic table, such as titanium, zirconium and hafnium;
[0098] X is a halogen, such as F, Cl, Br, and I; and
[0099] R 1 and R 2 Each independently selected from C1- 10 Alkyl, such as methyl, ethyl, propyl, n-butyl, isobutyl, etc., R 1 and R 2 It can be the same or different.
[0100] Specifically, as the IV B group metal halide, for example, titanium tetrafluoride (TiF4), titanium tetrachloride (TiCl4), titanium tetrabromide (TiBr4), titanium tetraiodide (TiI4) can be cited;
[0101] Zirconium tetrafluoride (ZrF4), zirconium tetrachloride (ZrCl4), zirconium tetrabromide (ZrBr4), zirconium tetraiodide (ZrI4);
[0102] Hafnium tetrafluoride (HfF4), Hafnium tetrachloride (HfCl4), Hafnium tetrabromide (HfBr4), Hafnium tetraiodide (HfI4).
[0103] As the above-mentioned IV B group metal alkyl compound, for example, tetramethyl titanium (Ti(CH3)4), tetraethyl titanium (Ti(CH3CH2)4), tetraisobutyl titanium (Ti(i-C4H9)4), tetra-n-butyl titanium (Ti(C4H9)4), triethyl methyl titanium (Ti(CH3)(CH3CH2)3), diethyl dimethyl titanium (Ti(CH3)2(CH3CH2)2), trimethyl ethyl titanium (Ti(CH3)3(CH3CH2)), triisobutyl methyl titanium (Ti(CH3)(i-C4H9)3), diisobutyl dimethyl titanium (Ti(CH3)2(i-C4H9)2), trimethyl isobutyl titanium (Ti(CH3)3(i-C4H9)), triisobutyl methyl ... Butyl ethyl titanium (Ti(CH3CH2)(i-C4H9)3), diisobutyl diethyl titanium (Ti(CH3CH2)2(i-C4H9)2), triethyl isobutyl titanium (Ti(CH3CH2)3(i-C4H9)), tri-n-butyl methyl titanium (Ti(CH3)(C4H9)3), di-n-butyl dimethyl titanium (Ti(CH3)2(C4H9)2), trimethyl n-butyl titanium (Ti(CH3)3(C4H9)), tri-n-butyl methyl titanium (Ti(CH3CH2)(C4H9)3), di-n-butyl diethyl titanium (Ti(CH3CH2)2(C4H9)2), triethyl n-butyl titanium (Ti(CH3CH2)3(C4H9)), etc.;
[0104] Tetramethyl zirconium (Zr(CH3)4), tetraethyl zirconium (Zr(CH3CH2)4), tetraisobutyl zirconium (Zr(i-C4H9)4), tetra-n-butyl zirconium (Zr(C4H9)4), triethyl methyl zirconium (Zr(CH3)(CH3CH2)3), diethyl dimethyl zirconium (Zr(CH3)2(CH3CH2)2), trimethyl ethyl zirconium (Zr(CH3)3(CH3CH2)), triisobutyl methyl zirconium (Zr(CH3)(i-C4H9)3), diisobutyl dimethyl zirconium (Zr(CH3)2(i-C4H9)2), trimethyl isobutyl zirconium (Zr(CH3)3(i-C4H9)), triisobutyl ethyl zirconium (Zr (CH3CH2)(i-C4H9)3), diisobutyldiethyl zirconium (Zr(CH3CH2)2(i-C4H9)2), triethylisobutyl zirconium (Zr(CH3CH2)3(i-C4H9)), tri-n-butylmethyl zirconium (Zr(CH3)(C4H9)3), di-n-butyldimethyl zirconium (Zr(CH3)2(C4H9)2), trimethyl-n-butyl zirconium (Zr(CH3)3(C4H9)), tri-n-butylmethyl zirconium (Zr(CH3CH2)(C4H9)3), di-n-butyldiethyl zirconium (Zr(CH3CH2)2(C4H9)2), triethyl-n-butyl zirconium (Zr(CH3CH2)3(C4H9)), etc.;
[0105] Tetramethyl hafnium (Hf(CH3)4), tetraethyl hafnium (Hf(CH3CH2)4), tetraisobutyl hafnium (Hf(i-C4H9)4), tetra-n-butyl hafnium (Hf(C4H9)4), triethyl methyl hafnium (Hf(CH3)(CH3CH2)3), diethyl dimethyl hafnium (Hf(CH3)2(CH3CH2)2), trimethyl ethyl hafnium (Hf(CH3)3(CH3CH2)), triisobutyl methyl hafnium (Hf(CH3)(i-C4H9)3), diisobutyl dimethyl hafnium (Hf(CH3)2(i-C4H9)2), trimethyl isobutyl hafnium (Hf(CH3)3(i-C4H9)), triisobutyl ethyl hafnium (Hf (CH3CH2)(i-C4H9)3), diisobutyldiethylhafnium (Hf(CH3CH2)2(i-C4H9)2), triethylisobutylhafnium (Hf(CH3CH2)3(i-C4H9)), tri-n-butylmethylhafnium (Hf(CH3)(C4H9)3), di-n-butyldimethylhafnium (Hf(CH3)2(C4H9)2), trimethyl-n-butylhafnium (Hf(CH3)3(C4H9)), tri-n-butylmethylhafnium (Hf(CH3CH2)(C4H9)3), di-n-butyldiethylhafnium (Hf(CH3CH2)2(C4H9)2), triethyl-n-butylhafnium (Hf(CH3CH2)3(C4H9)), etc.
[0106] As the IV B group metal alkoxide compound, for example, tetramethoxytitanium (Ti(OCH3)4), tetraethoxytitanium (Ti(OCH3CH2)4), tetraisobutoxytitanium (Ti(i-OC4H9)4), tetra-n-butoxytitanium (Ti(OC4H9)4), triethoxymethoxytitanium (Ti(OCH3)(OCH3CH2)3), diethoxydimethoxytitanium (Ti(OCH3)2(OCH3CH2)2), trimethoxyethoxytitanium (Ti(OCH3)3(OCH3CH2)), triisobutoxymethoxytitanium (Ti(OCH3)(i-OC4H9)3), diisobutoxydimethoxytitanium (Ti(OCH3)2(i-OC4H9)2), trimethoxyisobutoxytitanium (Ti(OCH3)3(i-OC4H9)), triisobutoxy Titanium ethoxide (Ti(OCH3CH2)(i-OC4H9)3), diisobutoxydiethoxytitanium (Ti(OCH3CH2)2(i-OC4H9)2), triethoxyisobutoxytitanium (Ti(OCH3CH2)3(i-OC4H9)), tri-n-butoxymethoxytitanium (Ti(OCH3)(OC4H9)3), di-n-butoxydimethoxytitanium (Ti(OCH3)2(OC4H9)2), trimethoxy-n-butoxytitanium (Ti(OCH3)3(OC4H9)), tri-n-butoxymethoxytitanium (Ti(OCH3CH2)(OC4H9)3), di-n-butoxydiethoxytitanium (Ti(OCH3CH2)2(OC4H9)2), triethoxy-n-butoxytitanium (Ti(OCH3CH2)3(OC4H9)), etc.;
[0107] Zirconium tetramethoxide (Zr(OCH3)4), zirconium tetraethoxide (Zr(OCH3CH2)4), zirconium tetraisobutoxide (Zr(i-OC4H9)4), zirconium tetra-n-butoxide (Zr(OC4H9)4), zirconium triethoxymethoxide (Zr(OCH3)(OCH3CH2)3), zirconium diethoxydimethoxide (Zr(OCH3)2(OCH3CH2)2), zirconium trimethoxyethoxide (Zr(OCH3)3(OCH3CH2)), zirconium triisobutoxide (Zr(OCH3)(i-OC4H9)3), zirconium diisobutoxide (Zr(OCH3)2(i-OC4H9)2), zirconium trimethoxyisobutoxide (Zr(OCH3)3(i-C4H9)), zirconium triisobutoxide (Zr( OCH3CH2)(i-OC4H9)3), diisobutoxydiethoxyzirconium (Zr(OCH3CH2)2(i-OC4H9)2), triethoxyisobutoxyzirconium (Zr(OCH3CH2)3(i-OC4H9)), tri-n-butoxymethoxyzirconium (Zr(OCH3)(OC4H9)3), di-n-butoxydimethoxyzirconium (Zr(OCH3)2(OC4H9)2), trimethoxy-n-butoxyzirconium (Zr(OCH3)3(OC4H9)), tri-n-butoxymethoxyzirconium (Zr(OCH3CH2)(OC4H9)3), di-n-butoxydiethoxyzirconium (Zr(OCH3CH2)2(OC4H9)2), triethoxy-n-butoxyzirconium (Zr(OCH3CH2)3(OC4H9)), etc.;
[0108] Hafnium tetramethoxide (Hf(OCH3)4), hafnium tetraethoxide (Hf(OCH3CH2)4), hafnium tetraisobutoxide (Hf(i-OC4H9)4), hafnium tetra-n-butoxide (Hf(OC4H9)4), hafnium triethoxymethoxide (Hf(OCH3)(OCH3CH2)3), hafnium diethoxydimethoxide (Hf(OCH3)2(OCH3CH2)2), hafnium trimethoxyethoxide (Hf(OCH3)3(OCH3CH2)), hafnium triisobutoxide (Hf(OCH3)(i-OC4H9)3), hafnium diisobutoxide (Hf(OCH3)2(i-OC4H9)2), hafnium trimethoxyisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf (OCH3CH2)(i-OC4H9)3), diisobutoxydiethoxyhafnium (Hf(OCH3CH2)2(i-OC4H9)2), triethoxyisobutoxyhafnium (Hf(OCH3CH2)3(i-C4H9)), tri-n-butoxymethoxyhafnium (Hf(OCH3)(OC4H9)3), di-n-butoxydimethoxyhafnium (Hf(OCH3)2(OC4H9)2), trimethoxy-n-butoxyhafnium (Hf(OCH3)3(OC4H9)), tri-n-butoxymethoxyhafnium (Hf(OCH3CH2)(OC4H9)3), di-n-butoxydiethoxyhafnium (Hf(OCH3CH2)2(OC4H9)2), triethoxy-n-butoxyhafnium (Hf(OCH3CH2)3(OC4H9)), etc.
[0109] As the IV B group metal alkyl halide, for example, trimethyl titanium chloride (TiCl(CH3)3), triethyl titanium chloride (TiCl(CH3CH2)3), triisobutyl titanium chloride (TiCl(i-C4H9)3), tri-n-butyl titanium chloride (TiCl(C4H9)3), dimethyl titanium dichloride (TiCl2(CH3)2), diethyl titanium dichloride (TiCl2(CH3CH2)2), diisobutyl titanium dichloride (TiCl2(i-C4H9)2), tri-n-butyl titanium chloride (TiCl(C4H9)3), methyl titanium trichloride (Ti(CH3)Cl3), ethyl titanium trichloride (Ti(CH3CH2)Cl3), isobutyl titanium trichloride (Ti(i-C4H9)Cl3), and n-butyl titanium trichloride (Ti(C4H9)Cl3);
[0110] Trimethyltitanium bromide (TiBr(CH3)3), triethyltitanium bromide (TiBr(CH3CH2)3), triisobutyltitanium bromide (TiBr(i-C4H9)3), tri-n-butyltitanium bromide (TiBr(C4H9)3), dimethyltitanium dibromide (TiBr2(CH3)2), diethyltitanium dibromide (TiBr2(CH3CH2)2), diisobutyltitanium dibromide (TiBr2(i-C4H9)2), tri-n-butyltitanium bromide (TiBr(C4H9)3), methyltitanium tribromide (Ti(CH3)Br3), ethyltitanium tribromide (Ti(CH3CH2)Br3), isobutyltitanium tribromide (Ti(i-C4H9)Br3), n-butyltitanium tribromide (Ti(C4H9)Br3);
[0111] Trimethyl zirconium chloride (ZrCl(CH3)3), triethyl zirconium chloride (ZrCl(CH3CH2)3), triisobutyl zirconium chloride (ZrCl(i-C4H9)3), tri-n-butyl zirconium chloride (ZrCl(C4H9)3), dimethyl zirconium dichloride (ZrCl2(CH3)2), diethyl zirconium dichloride (ZrCl2(CH3CH2)2), diisobutyl zirconium dichloride (ZrCl2(i-C4H9)2), tri-n-butyl zirconium chloride (ZrCl(C4H9)3), methyl zirconium trichloride (Zr(CH3)Cl3), ethyl zirconium trichloride (Zr(CH3CH2)Cl3), isobutyl zirconium trichloride (Zr(i-C4H9)Cl3), n-butyl zirconium trichloride (Zr(C4H9)Cl3);
[0112] Trimethyl zirconium bromide (ZrBr(CH3)3), triethyl zirconium bromide (ZrBr(CH3CH2)3), triisobutyl zirconium bromide (ZrBr(i-C4H9)3), tri-n-butyl zirconium bromide (ZrBr(C4H9)3), dimethyl zirconium dibromide (ZrBr2(CH3)2), diethyl zirconium dibromide (ZrBr2(CH3CH2)2), diisobutyl zirconium dibromide (ZrBr2(i-C4H9)2), tri-n-butyl zirconium bromide (ZrBr(C4H9)3), methyl zirconium tribromide (Zr(CH3)Br3), ethyl zirconium tribromide (Zr(CH3CH2)Br3), isobutyl zirconium tribromide (Zr(i-C4H9)Br3), n-butyl zirconium tribromide (Zr(C4H9)Br3);
[0113] Trimethyl hafnium chloride (HfCl(CH3)3), triethyl hafnium chloride (HfCl(CH3CH2)3), triisobutyl hafnium chloride (HfCl(i-C4H9)3), tri-n-butyl hafnium chloride (HfCl(C4H9)3), dimethyl hafnium dichloride (HfCl2(CH3)2), diethyl hafnium dichloride (HfCl2(CH3CH2)2), diisobutyl hafnium dichloride (HfCl2(i-C4H9)2), tri-n-butyl hafnium chloride (HfCl(C4H9)3), methyl hafnium trichloride (Hf(CH3)Cl3), ethyl hafnium trichloride (Hf(CH3CH2)Cl3), isobutyl hafnium trichloride (Hf(i-C4H9)Cl3), n-butyl hafnium trichloride (Hf(C4H9)Cl3);
[0114] Trimethyl hafnium bromide (HfBr(CH3)3), triethyl hafnium bromide (HfBr(CH3CH2)3), triisobutyl hafnium bromide (HfBr(i-C4H9)3), tri-n-butyl hafnium bromide (HfBr(C4H9)3), dimethyl hafnium dibromide (HfBr2(CH3)2), diethyl hafnium dibromide (HfBr2(CH3CH2)2), diisobutyl hafnium dibromide (HfBr2(i-C4H9)2), tri-n-butyl hafnium bromide (HfBr(C4H9)3), methyl hafnium tribromide (Hf(CH3)Br3), ethyl hafnium tribromide (Hf(CH3CH2)Br3), isobutyl hafnium tribromide (Hf(i-C4H9)Br3), n-butyl hafnium tribromide (Hf(C4H9)Br3).
[0115] As the IV B group metal alkoxy halide, for example, trimethoxytitanium chloride (TiCl(OCH3)3), triethoxytitanium chloride (TiCl(OCH3CH2)3), triisobutoxytitanium chloride (TiCl(i-OC4H9)3), tri-n-butoxytitanium chloride (TiCl(OC4H9)3), dimethoxytitanium dichloride (TiCl2(OCH3)2), diethoxytitanium dichloride (TiCl2(OCH3CH2)2), diisobutoxytitanium dichloride (TiCl2(i-OC4H9)2), tri-n-butoxytitanium chloride (TiCl(OC4H9)3), methoxytitanium trichloride (Ti(OCH3)Cl3), ethoxytitanium trichloride (Ti(OCH3CH2)Cl3), isobutoxytitanium trichloride (Ti(i-C4H9)Cl3), and n-butoxytitanium trichloride (Ti(OC4H9)Cl3);
[0116] Trimethoxytitanium bromide (TiBr(OCH3)3), triethoxytitanium bromide (TiBr(OCH3CH2)3), triisobutoxytitanium bromide (TiBr(i-OC4H9)3), tri-n-butoxytitanium bromide (TiBr(OC4H9)3), dimethoxytitanium dibromide (TiBr2(OCH3)2), diethoxytitanium dibromide (TiBr2(OCH3CH2)2), diisobutoxytitanium dibromide (TiBr2(i-OC4H9)2), tri-n-butoxytitanium bromide (TiBr(OC4H9)3), methoxytitanium tribromide (Ti(OCH3)Br3), ethoxytitanium tribromide (Ti(OCH3CH2)Br3), isobutoxytitanium tribromide (Ti(i-C4H9)Br3), n-butoxytitanium tribromide (Ti(OC4H9)Br3);
[0117] Trimethoxy zirconium chloride (ZrCl(OCH3)3), triethoxy zirconium chloride (ZrCl(OCH3CH2)3), triisobutoxy zirconium chloride (ZrCl(i-OC4H9)3), tri-n-butoxy zirconium chloride (ZrCl(OC4H9)3), dimethoxy zirconium dichloride (ZrCl2(OCH3)2), diethoxy zirconium dichloride (ZrCi2(OCH3CH2)2), diisobutoxy zirconium dichloride (ZrCl2(i-OC4H9)2), tri-n-butoxy zirconium chloride (ZrCl(OC4H9)3), methoxy zirconium trichloride (Zr(OCH3)Cl3), ethoxy zirconium trichloride (Zr(OCH3CH2)Cl3), isobutoxy zirconium trichloride (Zr(i-C4H9)Cl3), n-butoxy zirconium trichloride (Zr(OC4H9)Cl3);
[0118] Trimethoxyzirconium bromide (ZrBr(OCH3)3), triethoxyzirconium bromide (ZrBr(OCH3CH2)3), triisobutoxyzirconium bromide (ZrBr(i-OC4H9)3), tri-n-butoxyzirconium bromide (ZrBr(OC4H9)3), dimethoxyzirconium dibromide (ZrBr2(OCH3)2), diethoxyzirconium dibromide (ZrBr2(OCH3CH2)2), diisobutoxyzirconium dibromide (ZrBr2(i-OC4H9)2), tri-n-butoxyzirconium bromide (ZrBr(OC4H9)3), methoxyzirconium tribromide (Zr(OCH3)Br3), ethoxyzirconium tribromide (Zr(OCH3CH2)Br3), isobutoxyzirconium tribromide (Zr(i-C4H9)Br3), n-butoxyzirconium tribromide (Zr(OC4H9)Br3);
[0119] Hafnium trimethoxychloride (HfCl(OCH3)3), Hafnium triethoxychloride (HfCl(OCH3CH2)3), Hafnium triisobutoxychloride (HfCl(i-OC4H9)3), Hafnium tri-n-butoxychloride (HfCl(OC4H9)3), Hafnium dimethoxychloride (HfCl2(OCH3)2), Hafnium diethoxychloride (HfCl2(OCH3CH2)2), Hafnium dichloride (HfCl2(i-OC4H9)2), tri-n-butoxy hafnium chloride (HfCl(OC4H9)3), methoxy hafnium trichloride (Hf(OCH3)Cl3), ethoxy hafnium trichloride (Hf(OCH3CH2)Cl3), isobutoxy hafnium trichloride (Hf(i-C4H9)Cl3), n-butoxy hafnium trichloride (Hf(OC4H9)Cl3);
[0120] Hafnium bromide trimethoxy (HfBr(OCH3)3), hafnium bromide triethoxy (HfBr(OCH3CH2)3), hafnium bromide triisobutoxy (HfBr(i-OC4H9)3), hafnium bromide tri-n-butoxy (HfBr(OC4H9)3), hafnium dimethoxy (HfBr2(OCH3)2), hafnium diethoxy (HfBr2(OCH3CH2)2), Hafnium dibromide (HfBr2(i-OC4H9)2), tri-n-butoxy hafnium bromide (HfBr(OC4H9)3), methoxy hafnium tribromide (Hf(OCH3)Br3), ethoxy hafnium tribromide (Hf(OCH3CH2)Br3), isobutoxy hafnium tribromide (Hf(i-C4H9)Br3), and n-butoxy hafnium tribromide (Hf(OC4H9)Br3).
[0121] As the IV B Group metal compound, the IV B Group metal halide is preferred, TiCl 4 , TiBr 4 , ZrCl 4 , ZrBr 4 , HfCl 4 and HfBr 4 are more preferred, and TiCl 4 and ZrCl 4 are most preferred.
[0122] These Group IV B metal compounds may be used alone or in combination of two or more in any ratio.
[0123] When the chemical activating agent is in liquid form at room temperature, the chemical activating agent can be used by directly dropping a predetermined amount of the chemical activating agent into an organic porous solid or an inorganic porous solid to be activated by the chemical activating agent.
[0124] When the chemical activator is solid at room temperature, it is preferably used in the form of a solution for the convenience of metering and operation. Of course, when the chemical activator is liquid at room temperature, it can also be used in the form of a solution as needed, without particular limitation.
[0125] When preparing the solution of the chemical activator, there is no particular limitation on the solvent used at this time, as long as it can dissolve the chemical activator.
[0126] Specifically, we can cite C 5-12 Alkanes, C 5-12 Cycloalkanes, halogenated C 5-12 Alkanes, halogenated C 5-12 Cycloalkanes, C 6-12 Aromatic or halogenated C 6-12 Aromatic hydrocarbons include, for example, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, toluene, ethylbenzene, xylene, chloropentane, chlorohexane, chloroheptane, chlorooctane, chlorononane, chlorodecane, chloroundecane, chlorododecane, chlorocyclohexane, chlorotoluene, chloroethylbenzene and chloroxylene, among which pentane, hexane, decane, cyclohexane and toluene are preferred, and hexane and toluene are most preferred.
[0127] These solvents may be used alone or in combination of two or more in any ratio.
[0128] In addition, there is no particular limitation on the concentration of the chemical activator in its solution, and it can be appropriately selected as needed, as long as it can achieve the chemical activation with a predetermined amount of the chemical activator. As mentioned above, if the chemical activator is liquid, the chemical activator can be used directly for the activation, but it can also be used after being prepared into a chemical activator solution.
[0129] Conveniently, the molar concentration of the chemical activator in its solution is generally set to 0.01 to 1.0 mol / L, but is not limited thereto.
[0130] As a method for carrying out the chemical activation, for example, when the chemical activator is in a solid state (such as zirconium tetrachloride), a solution of the chemical activator is first prepared, and then the solution containing a predetermined amount of the chemical activator is added (preferably dripped) to the organic porous solid or inorganic porous solid to be activated to carry out the chemical activation reaction. When the chemical activator is in a liquid state (such as titanium tetrachloride), a predetermined amount of the chemical activator can be directly added (preferably dripped) to the organic porous solid or inorganic porous solid to be activated to carry out the chemical activation reaction, or after the chemical activator is prepared into a solution, the solution containing a predetermined amount of the chemical activator is added (preferably dripped) to the organic porous solid or inorganic porous solid to be activated to carry out the chemical activation reaction.
[0131] Generally speaking, the chemical activation reaction is carried out (with stirring if necessary) at a reaction temperature of -30 to 60°C (preferably -20 to 30°C) for 0.5 to 24 hours, preferably 1 to 8 hours, more preferably 2 to 6 hours.
[0132] After the chemical activation reaction is completed, the chemically activated organic porous solid or inorganic porous solid can be obtained by filtering, washing and drying.
[0133] According to the present invention, the filtering, washing and drying can be carried out by conventional methods, wherein the washing solvent can be the same solvent used to dissolve the chemical activator. According to the needs, the washing is generally carried out 1 to 8 times, preferably 2 to 6 times, and most preferably 2 to 4 times.
[0134] The drying can be carried out by conventional methods, such as inert gas drying, vacuum drying or vacuum heating drying, preferably inert gas drying or vacuum heating drying, most preferably vacuum heating drying. The drying temperature range is generally from room temperature to 140°C, and the drying time is generally 2-20 hours, but is not limited thereto.
[0135] According to the present invention, the surface area of the porous carrier is not particularly limited, but is generally 10 to 1000 m 2 / g (measured by BET method), preferably 100 to 600 m 2 / g; the pore volume of the porous carrier (determined by nitrogen adsorption) is generally 0.1 to 4 cm 3 / g, preferably 0.2 to 2 cm 3 / g, and its average particle size (measured by laser particle size analyzer) is preferably 1 to 500 mm, more preferably 1 to 100 mm.
[0136] According to the present invention, the porous carrier may be in any form, such as fine powder, granules, spheres, aggregates or other forms.
[0137] The composite carrier is obtained by metering a precipitant into the mixed slurry to precipitate solid matter from the mixed slurry, or directly drying the mixed slurry to obtain the composite carrier.
[0138] The precipitant is described in detail below.
[0139] According to the present invention, the term "precipitant" uses the common concept in the art and refers to a chemically inert liquid that can reduce the solubility of a solute (such as the magnesium compound) in its solution and thereby precipitate it from the solution in a solid form.
[0140] According to the present invention, the precipitant may be a solvent that is a poor solvent for the magnesium compound but a good solvent for the solvent for dissolving the magnesium compound, such as alkanes, cycloalkanes, halogenated alkanes and halogenated cycloalkanes.
[0141] Examples of the alkane include pentane, hexane, heptane, octane, nonane and decane. Among them, hexane, heptane and decane are preferred, and hexane is most preferred.
[0142] Examples of the cycloalkane include cyclohexane, cyclopentane, cycloheptane, cyclodecane and cyclononane, and cyclohexane is most preferred.
[0143] Examples of the halogenated alkane include dichloromethane, dichlorohexane, dichloroheptane, chloroform, trichloroethane, trichlorobutane, dibromomethane, dibromoethane, dibromoheptane, bromoform, tribromoethane, and tribromobutane.
[0144] Examples of the halogenated cycloalkane include chlorocyclopentane, chlorocyclohexane, chlorocycloheptane, chlorocyclooctane, chlorocyclononane, chlorocyclodecane, bromocyclopentane, bromocyclohexane, bromocycloheptane, bromocyclooctane, bromocyclononane and bromocyclodecane.
[0145] These precipitants may be used alone or in combination of two or more in any proportion.
[0146] The precipitant may be added in one go or in drops, preferably in one go. During the precipitation process, stirring may be used to promote the dispersion of the precipitant in the mixed slurry and facilitate the final precipitation of the solid product. The stirring may be in any form, such as a stirring paddle (generally with a rotation speed of 10 to 1000 rpm).
[0147] There is no particular limitation on the amount of the precipitant used, but generally, by volume, the ratio of the precipitant to the solvent for dissolving the magnesium compound is 1:0.2-5, preferably 1:0.5-2, and more preferably 1:0.8-1.5.
[0148] The temperature of the precipitant is not particularly limited, but is generally preferably room temperature. Moreover, the precipitation process is generally preferably carried out at room temperature.
[0149] After complete precipitation, the obtained solid product is filtered, optionally washed and dried to obtain a composite carrier. There is no particular limitation on the filtering, washing and drying methods, and those conventionally used in the art can be used as needed.
[0150] The washing is generally performed 1 to 6 times, preferably 2 to 3 times, as required. The washing solvent is preferably the same as the precipitant, but may also be different.
[0151] According to the present invention, the alcohol content in the composite carrier is controlled to be 0.5-2.5 wt %, preferably 1.0-2.0 wt %, by drying the mixed slurry or drying the solid product (optionally after washing).
[0152] According to the present invention, the drying can be carried out by conventional methods, such as inert gas drying, vacuum drying or heating drying under vacuum, preferably inert gas drying or heating drying under vacuum, most preferably heating drying under vacuum.
[0153] According to the present invention, according to the present invention, the drying method (including drying temperature, drying vacuum degree and drying time) is limited to the alcohol content in the composite carrier meeting the aforementioned requirements of the present invention. For example, the mixed slurry is dried for 2-48 hours, preferably 4-24 hours, at a temperature 5-40°C lower than the boiling point of the solvent, preferably 10-30°C lower, under an absolute pressure of 2-100mBar vacuum, preferably 5-50mBar, and then dried for 1-24 hours, preferably 2-12 hours, at a temperature from the boiling point of the solvent to 50°C higher than the boiling point of the solvent, preferably from the boiling point of the solvent to 40°C higher than the boiling point of the solvent, under an absolute pressure of 2-100mBar vacuum, preferably 5-50mBar, to obtain the composite carrier. Alternatively, a precipitant is added to the mixed slurry, and the obtained precipitate (optionally after washing) is dried at a temperature 5-40°C lower than the boiling point of the solvent, preferably 10-30°C lower, under a vacuum of an absolute pressure of 2-100 mBar, preferably 5-50 mBar, for 2-48 h, preferably 4-24 h, and then dried at a temperature from the boiling point of the solvent to 50°C higher than the boiling point of the solvent, preferably from the boiling point of the solvent to 40°C higher than the boiling point of the solvent, under a vacuum of an absolute pressure of 2-100 mBar, preferably 5-50 mBar, for 1-24 h, preferably 2-12 h, thereby obtaining the composite carrier.
[0154] Next, the composite support is treated with a non-metallocene ligand to obtain a modified composite support.
[0155] According to the present invention, the term "non-metallocene complex" is a single-center olefin polymerization catalyst relative to a metallocene catalyst, which does not contain cyclopentadienyl groups such as cyclopentadienyl rings, fluorene rings or indenyl rings or their derivatives in the structure, and is a metal organic compound that can show olefin polymerization catalytic activity when combined with a cocatalyst (such as those described below) (therefore, the non-metallocene complex is sometimes also referred to as a non-metallocene olefin polymerizable complex). The compound comprises a central metal atom and at least one multidentate ligand (preferably a tridentate ligand or a multidentate ligand) that is bound to the central metal atom by a coordination bond, and the term "non-metallocene ligand" is the aforementioned multidentate ligand.
[0156] According to the present invention, the non-metallocene ligand is selected from compounds having the following chemical formula:
[0157]
[0158] According to the present invention, the groups A, D and E (coordinating groups) in the compound form coordination bonds through the coordinating atoms (such as heteroatoms such as N, O, S, Se and P) contained therein and the Group IV B metal atom contained in the Group IV B metal compound used as a chemical treatment agent in the present invention, thereby forming a complex with the Group IV B metal atom as the central metal atom M (i.e., the non-metallocene complex described in the present invention).
[0159] In a more specific embodiment, the non-metallocene ligand is selected from compound (A) and compound (B) having the following chemical formula:
[0160]
[0161] In a more specific embodiment, the non-metallocene ligand is selected from compounds (A-1) to (A-4) and compounds (B-1) to (B-4) having the following chemical formulas:
[0162]
[0163]
[0164]
[0165] In all the above chemical structures,
[0166] q is 0 or 1;
[0167] d is 0 or 1;
[0168] A is selected from oxygen atom, sulfur atom, selenium atom, -NR 23 R 24、-N(O)R 25 R 26 , -PR 28 R 29 、-P(O)R 30 OR 31 , sulfone, sulfoxide or -Se(O)R 39 , wherein N, O, S, Se and P are each a coordinating atom;
[0169] B is selected from nitrogen atoms, nitrogen-containing groups, phosphorus-containing groups or C1-C 30 Hydrocarbon;
[0170] D is selected from nitrogen atoms, oxygen atoms, sulfur atoms, selenium atoms, phosphorus atoms, nitrogen-containing groups, phosphorus-containing groups, C1-C 30 A hydrocarbon group, a sulfone group or a sulfoxide group, wherein N, O, S, Se and P are each a coordinating atom;
[0171] E is selected from nitrogen-containing groups, oxygen-containing groups, sulfur-containing groups, selenium-containing groups, phosphorus-containing groups or cyano groups (-CN), wherein N, O, S, Se and P are each a coordinating atom;
[0172] F is selected from a nitrogen atom, a nitrogen-containing group, an oxygen-containing group, a sulfur-containing group, a selenium-containing group or a phosphorus-containing group, wherein N, O, S, Se and P are each a coordinating atom;
[0173] G is selected from C1-C 30 Hydrocarbyl, substituted C1-C 30 Hydrocarbon groups or inert functional groups;
[0174] Y is selected from nitrogen-containing groups, oxygen-containing groups, sulfur-containing groups, selenium-containing groups or phosphorus-containing groups, wherein N, O, S, Se and P are each a coordinating atom;
[0175] Z is selected from nitrogen-containing groups, oxygen-containing groups, sulfur-containing groups, selenium-containing groups, phosphorus-containing groups or cyano groups (-CN), for example, -NR 23 R 24 、-N(O)R 25 R 26 , -PR 28 R 29 、-P(O)R 30 R 31 、-OR 34 、-SR 35 、-S(O)R 36 , -SeR 38 or-Se(O)R 39 , wherein N, O, S, Se and P are each a coordinating atom;
[0176] → represents a single bond or a double bond;
[0177] - represents a covalent bond or an ionic bond.
[0178] R 1 To R 4 , R 6 To R 21 Each independently selected from hydrogen, C1-C 30 Hydrocarbyl, substituted C1-C 30 A hydrocarbon group (preferably a halogenated hydrocarbon group, such as -CH2Cl and -CH2CH2Cl) or an inert functional group. 22 To R 36 , R 38 and R 39 Each independently selected from hydrogen, C1-C 30 Hydrocarbon or substituted C1-C 30 Hydrocarbon (preferably halogenated hydrocarbon, such as -CH2Cl and -CH2CH2Cl). The above groups may be the same or different from each other, wherein adjacent groups such as R 1 With R 2 , R 6 With R 7 , R 7 With R 8 , R 8 With R 9 , R 13 With R 14 , R 14 With R 15 , R 15 With R 16 , R 18 With R 19 , R 19 With R 20 , R 20 With R 21 , R 23 With R 24 , or R 25 With R 26 The compounds may be combined with each other to form a bond or a ring, preferably to form an aromatic ring, such as an unsubstituted benzene ring or a ring with 1-4 C1-C 30 Hydrocarbon or substituted C1-C 30 A benzene ring substituted with a hydrocarbon group (preferably a halogenated hydrocarbon group such as -CH2Cl and -CH2CH2Cl).
[0179] R 5 Selected from lone pairs of electrons on nitrogen, hydrogen, C1-C 30 Hydrocarbyl, substituted C1-C 30 A hydrocarbon group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a selenium-containing group or a phosphorus-containing group. 5When R is an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a selenium-containing group or a phosphorus-containing group, 5 The N, O, S, P and Se in the cation may serve as coordinating atoms (coordinate with the central metal atom M).
[0180] In the context of the present invention, the inert functional group can be selected from halogen, oxygen-containing group, nitrogen-containing group, silicon-containing group, germanium-containing group, sulfur-containing group, tin-containing group, C1-C 10 At least one of an ester group or a nitro group (-NO2), etc., but usually does not include C1-C 30 Hydrocarbyl and substituted C1-C 30 Hydrocarbon.
[0181] In the context of the present invention, limited by the chemical structure of the multidentate ligand of the present invention, the inert functional group has the following characteristics:
[0182] (1) does not interfere with the coordination process between the group A, D, E, F, Y or Z and the central metal atom M, and
[0183] (2) The coordination ability with the central metal atom M is lower than that of the A, D, E, F, Y and Z groups, and does not replace the existing coordination between these groups and the central metal atom M.
[0184] According to the present invention, in all the above chemical formulae, depending on the specific circumstances, any two or more adjacent groups, such as R 21 With group Z, or R 13 and group Y, can be combined with each other to form a ring, preferably forming a C6-C 30 Aromatic heterocycles, such as pyridine ring, wherein the aromatic heterocycle is optionally substituted by one or more selected from C1-C 30 Hydrocarbyl and substituted C1-C 30 The substituents of the hydrocarbon group are substituted.
[0185] In the context of the present invention,
[0186] The halogen is selected from F, Cl, Br or I. The nitrogen-containing group is selected from -NR 23 R 24 、-T-NR 23 R 24 or -N(O)R 25 R 26 The phosphorus-containing group is selected from -PR 28 R 29 、-P(O)R 30 R 31 or -P(O)R32 (OR 33 ). The oxygen-containing group is selected from hydroxyl, -OR 34 AND-T-OR 34 The sulfur-containing group is selected from -SR 35 、-T-SR 35 、-S(O)R 36 or-T-SO2R 37 The selenium-containing group is selected from -SeR 38 ,-T-SeR 38 、-Se(O)R 39 or-T-Se(O)R 39 The group T is selected from C1-C 30 Hydrocarbon or substituted C1-C 30 The R 37 Selected from hydrogen, C1-C 30 Hydrocarbon or substituted C1-C 30 Hydrocarbon.
[0187] In the context of the present invention, the C1-C 30 The hydrocarbon group is selected from C1-C 30 Alkyl (preferably C1-C6 alkyl, such as isobutyl), C7-C 30 Alkyl (such as tolyl, xylyl, diisobutylphenyl, etc.), C7-C 30 Aralkyl (such as benzyl), C3-C 30 Cyclic alkyl, C2-C 30 Alkenyl, C2-C 30 Alkynyl, C6-C 30 Aryl (such as phenyl, naphthyl, anthracenyl, etc.), C8-C 30 Condensed ring or C4-C 30 Heterocyclic group, wherein the heterocyclic group contains 1-3 heteroatoms selected from nitrogen atom, oxygen atom or sulfur atom, such as pyridyl, pyrrolyl, furyl or thienyl.
[0188] According to the present invention, in the context of the present invention, according to the specific circumstances of the relevant groups to which it is combined, the C1-C 30 Hydrocarbyl is sometimes referred to as C1-C 30 Hydrocarbon diyl (divalent group, also known as C1-C 30 Alkylene) or C1-C 30 Hydrocarbon triyl (trivalent group), which is obvious to those skilled in the art.
[0189] In the context of the present invention, the substituted C1-C 30 Hydrocarbyl refers to a C1-C2-alkyl group with one or more inert substituents. 30The so-called inert substituents refer to those substituents that are inert to the aforementioned coordinating groups (referring to the aforementioned groups A, D, E, F, Y and Z, or optionally including R 5 ) has no substantial interference with the coordination process of the central metal atom M (i.e., the aforementioned Group IV B metal atom); in other words, limited by the chemical structure of the ligand of the present invention, these substituents have no ability or opportunity (such as due to steric hindrance, etc.) to react with the Group IV B metal atom to form a coordination bond. Generally speaking, the inert substituent is selected from halogen or C1-C 30 Alkyl (preferably C1-C6 alkyl, such as isobutyl).
[0190] In the context of the present invention, the silicon-containing group is selected from -SiR 42 R 43 R 44 or-T-SiR 45 ; The germanium-containing group is selected from -GeR 46 R 47 R 48 Or-T-GeR 49 ; The tin-containing group is selected from -SnR 50 R 51 R 52 、-T-SnR 53 or-T-Sn(O)R 54 ; and said R 42 To R 54 Each independently selected from hydrogen, the aforementioned C1-C 30 Hydrocarbyl or the aforementioned substituted C1-C 30 The hydrocarbon group may be the same or different from each other, and adjacent groups may be combined to form a bond or a ring. The definition of group T is the same as above.
[0191] As the non-metallocene ligand, for example, the following compounds can be cited:
[0192]
[0193]
[0194]
[0195]
[0196] The non-metallocene ligand is preferably selected from the following compounds:
[0197]
[0198]
[0199] The non-metallocene ligand is further preferably selected from the following compounds:
[0200]
[0201] The non-metallocene ligand is more preferably selected from the following compounds:
[0202]
[0203] These non-metallocene ligands may be used alone or in combination of two or more in any ratio.
[0204] According to the present invention, the non-metallocene ligand is not a diether compound commonly used as an electron donor compound in the art.
[0205] The non-metallocene ligand can be prepared by any method known to those skilled in the art. For details of its preparation method, see WO03 / 010207 and Chinese patents ZL01126323.7 and ZL02110844.7, etc., the full texts of which are incorporated herein by reference.
[0206] According to the present invention, for the convenience of metering and operation, the non-metallocene ligand is used in the form of a solution when necessary.
[0207] When preparing the solution of the non-metallocene ligand, there is no particular limitation on the solvent used, as long as it can dissolve the non-metallocene ligand and does not destroy (e.g., dissolve) the existing support structure of the composite support. 6-12 Aromatic hydrocarbons, halogenated C 6-12 Aromatic hydrocarbons, halogenated C 1-10 One or more of alkanes, esters and ethers. Specific examples include toluene, xylene, trimethylbenzene, ethylbenzene, diethylbenzene, chlorotoluene, chloroethylbenzene, bromotoluene, bromoethylbenzene, dichloromethane, dichloroethane, ethyl acetate and tetrahydrofuran. Among them, C 6-12 Aromatic hydrocarbons, tetrahydrofuran and dichloromethane.
[0208] These solvents may be used alone or in combination of two or more in any ratio.
[0209] When dissolving the non-metallocene ligand, stirring may be used as needed (the stirring speed is generally 10 to 500 rpm).
[0210] According to the present invention, the ratio of the non-metallocene ligand to the solvent is generally 0.02 to 0.30 g / ml, preferably 0.05 to 0.15 g / ml, but sometimes it is not limited thereto.
[0211] As a method for carrying out the treatment with the non-metallocene ligand, for example, there can be mentioned that, first, a solution of the non-metallocene ligand is prepared, and then the solution (containing a predetermined amount of the non-metallocene ligand) is metered (preferably dropped) into the composite support to be treated at a temperature of -30-60°C (preferably -20-30°C), or the composite support is metered into the solution, and the treatment reaction is carried out (with stirring if necessary) at a reaction temperature of -30-60°C (preferably -20-30°C) for 0.5 to 24 hours, preferably 1 to 8 hours, more preferably 2 to 6 hours, and then filtered, optionally washed and dried.
[0212] According to the present invention, the filtering, washing and drying can be carried out by conventional methods, wherein the washing solvent can be the same solvent used to dissolve the non-metallocene ligand. The washing is generally carried out 1 to 8 times, preferably 2 to 6 times, and most preferably 2 to 4 times.
[0213] According to the present invention, the molar ratio of the magnesium compound to the non-metallocene ligand calculated as Mg element is 1:0.0001-1, preferably 1:0.0002-0.4, more preferably 1:0.0008-0.2, and further preferably 1:0.001-0.1.
[0214] Next, the modified composite support is treated with a chemical treatment agent selected from Group IV B metal compounds, thereby obtaining the supported non-metallocene catalyst of the present invention.
[0215] According to the present invention, by chemically treating the modified composite carrier with the chemical treatment agent, the chemical treatment agent can react with the non-metallocene ligand contained in the modified composite carrier, thereby generating a non-metallocene complex in situ on the carrier (in situ loading reaction), thereby obtaining the supported non-metallocene catalyst of the present invention.
[0216] The chemical treatment agent is described in detail below.
[0217] According to the present invention, a Group IV B metal compound is used as the chemical treatment agent.
[0218] Examples of the Group IVB metal compound include Group IVB metal halides, Group IVB metal alkyl compounds, Group IVB metal alkoxy compounds, Group IVB metal alkyl halides and Group IVB metal alkoxy halides.
[0219] Examples of the Group IVB metal halide, the Group IVB metal alkyl compound, the Group IVB metal alkoxy compound, the Group IVB metal alkyl halide and the Group IVB metal alkoxy halide include compounds of the following general formula (IV):
[0220] M(OR 1 ) m X n R 2 4-m-n (IV)
[0221] in:
[0222] m is 0, 1, 2, 3 or 4;
[0223] n is 0, 1, 2, 3 or 4;
[0224] M is a metal of Group IV B in the periodic table, such as titanium, zirconium and hafnium;
[0225] X is a halogen, such as F, Cl, Br, and I; and
[0226] R 1 and R 2 Each independently selected from C 1-10 Alkyl, such as methyl, ethyl, propyl, n-butyl, isobutyl, etc., R 1 and R 2 It can be the same or different.
[0227] Specifically, as the IV B group metal halide, for example, titanium tetrafluoride (TiF4), titanium tetrachloride (TiCl4), titanium tetrabromide (TiBr4), titanium tetraiodide (TiI4) can be cited;
[0228] Zirconium tetrafluoride (ZrF4), zirconium tetrachloride (ZrCl4), zirconium tetrabromide (ZrBr4), zirconium tetraiodide (ZrI4);
[0229] Hafnium tetrafluoride (HfF4), Hafnium tetrachloride (HfCl4), Hafnium tetrabromide (HfBr4), Hafnium tetraiodide (HfI4).
[0230] As the above-mentioned IV B group metal alkyl compound, for example, tetramethyl titanium (Ti(CH3)4), tetraethyl titanium (Ti(CH3CH2)4), tetraisobutyl titanium (Ti(i-C4H9)4), tetra-n-butyl titanium (Ti(C4H9)4), triethyl methyl titanium (Ti(CH3)(CH3CH2)3), diethyl dimethyl titanium (Ti(CH3)2(CH3CH2)2), trimethyl ethyl titanium (Ti(CH3)3(CH3CH2)), triisobutyl methyl titanium (Ti(CH3)(i-C4H9)3), diisobutyl dimethyl titanium (Ti(CH3)2(i-C4H9)2), trimethyl isobutyl titanium (Ti(CH3)3(i-C4H9)), triisobutyl methyl ... Butyl ethyl titanium (Ti(CH3CH2)(i-C4H9)3), diisobutyl diethyl titanium (Ti(CH3CH2)2(i-C4H9)2), triethyl isobutyl titanium (Ti(CH3CH2)3(i-C4H9)), tri-n-butyl methyl titanium (Ti(CH3)(C4H9)3), di-n-butyl dimethyl titanium (Ti(CH3)2(C4H9)2), trimethyl n-butyl titanium (Ti(CH3)3(C4H9)), tri-n-butyl methyl titanium (Ti(CH3CH2)(C4H9)3), di-n-butyl diethyl titanium (Ti(CH3CH2)2(C4H9)2), triethyl n-butyl titanium (Ti(CH3CH2)3(C4H9)), etc.;
[0231] Tetramethyl zirconium (Zr(CH3)4), tetraethyl zirconium (Zr(CH3CH2)4), tetraisobutyl zirconium (Zr(i-C4H9)4), tetra-n-butyl zirconium (Zr(C4H9)4), triethyl methyl zirconium (Zr(CH3)(CH3CH2)3), diethyl dimethyl zirconium (Zr(CH3)2(CH3CH2)2), trimethyl ethyl zirconium (Zr(CH3)3(CH3CH2)), triisobutyl methyl zirconium (Zr(CH3)(i-C4H9)3), diisobutyl dimethyl zirconium (Zr(CH3)2(i-C4H9)2), trimethyl isobutyl zirconium (Zr(CH3)3(i-C4H9)), triisobutyl ethyl zirconium (Zr (CH3CH2)(i-C4H9)3), diisobutyldiethyl zirconium (Zr(CH3CH2)2(i-C4H9)2), triethylisobutyl zirconium (Zr(CH3CH2)3(i-C4H9)), tri-n-butylmethyl zirconium (Zr(CH3)(C4H9)3), di-n-butyldimethyl zirconium (Zr(CH3)2(C4H9)2), trimethyl-n-butyl zirconium (Zr(CH3)3(C4H9)), tri-n-butylmethyl zirconium (Zr(CH3CH2)(C4H9)3), di-n-butyldiethyl zirconium (Zr(CH3CH2)2(C4H9)2), triethyl-n-butyl zirconium (Zr(CH3CH2)3(C4H9)), etc.;
[0232] Tetramethyl hafnium (Hf(CH3)4), tetraethyl hafnium (Hf(CH3CH2)4), tetraisobutyl hafnium (Hf(i-C4H9)4), tetra-n-butyl hafnium (Hf(C4H9)4), triethyl methyl hafnium (Hf(CH3)(CH3CH2)3), diethyl dimethyl hafnium (Hf(CH3)2(CH3CH2)2), trimethyl ethyl hafnium (Hf(CH3)3(CH3CH2)), triisobutyl methyl hafnium (Hf(CH3)(i-C4H9)3), diisobutyl dimethyl hafnium (Hf(CH3)2(i-C4H9)2), trimethyl isobutyl hafnium (Hf(CH3)3(i-C4H9)), triisobutyl ethyl hafnium (Hf (CH3CH2)(i-C4H9)3), diisobutyldiethylhafnium (Hf(CH3CH2)2(i-C4H9)2), triethylisobutylhafnium (Hf(CH3CH2)3(i-C4H9)), tri-n-butylmethylhafnium (Hf(CH3)(C4H9)3), di-n-butyldimethylhafnium (Hf(CH3)2(C4H9)2), trimethyl-n-butylhafnium (Hf(CH3)3(C4H9)), tri-n-butylmethylhafnium (Hf(CH3CH2)(C4H9)3), di-n-butyldiethylhafnium (Hf(CH3CH2)2(C4H9)2), triethyl-n-butylhafnium (Hf(CH3CH2)3(C4H9)), etc.
[0233] As the IV B group metal alkoxide compound, for example, tetramethoxytitanium (Ti(OCH3)4), tetraethoxytitanium (Ti(OCH3CH2)4), tetraisobutoxytitanium (Ti(i-OC4H9)4), tetra-n-butoxytitanium (Ti(OC4H9)4), triethoxymethoxytitanium (Ti(OCH3)(OCH3CH2)3), diethoxydimethoxytitanium (Ti(OCH3)2(OCH3CH2)2), trimethoxyethoxytitanium (Ti(OCH3)3(OCH3CH2)), triisobutoxymethoxytitanium (Ti(OCH3)(i-OC4H9)3), diisobutoxydimethoxytitanium (Ti(OCH3)2(i-OC4H9)2), trimethoxyisobutoxytitanium (Ti(OCH3)3(i-OC4H9)), triisobutoxy Titanium ethoxide (Ti(OCH3CH2)(i-OC4H9)3), diisobutoxydiethoxytitanium (Ti(OCH3CH2)2(i-OC4H9)2), triethoxyisobutoxytitanium (Ti(OCH3CH2)3(i-OC4H9)), tri-n-butoxymethoxytitanium (Ti(OCH3)(OC4H9)3), di-n-butoxydimethoxytitanium (Ti(OCH3)2(OC4H9)2), trimethoxy-n-butoxytitanium (Ti(OCH3)3(OC4H9)), tri-n-butoxymethoxytitanium (Ti(OCH3CH2)(OC4H9)3), di-n-butoxydiethoxytitanium (Ti(OCH3CH2)2(OC4H9)2), triethoxy-n-butoxytitanium (Ti(OCH3CH2)3(OC4H9)), etc.;
[0234] Zirconium tetramethoxide (Zr(OCH3)4), zirconium tetraethoxide (Zr(OCH3CH2)4), zirconium tetraisobutoxide (Zr(i-OC4H9)4), zirconium tetra-n-butoxide (Zr(OC4H9)4), zirconium triethoxymethoxide (Zr(OCH3)(OCH3CH2)3), zirconium diethoxydimethoxide (Zr(OCH3)2(OCH3CH2)2), zirconium trimethoxyethoxide (Zr(OCH3)3(OCH3CH2)), zirconium triisobutoxide (Zr(OCH3)(i-OC4H9)3), zirconium diisobutoxide (Zr(OCH3)2(i-OC4H9)2), zirconium trimethoxyisobutoxide (Zr(OCH3)3(i-C4H9)), zirconium triisobutoxide (Zr( OCH3CH2)(i-OC4H9)3), diisobutoxydiethoxyzirconium (Zr(OCH3CH2)2(i-OC4H9)2), triethoxyisobutoxyzirconium (Zr(OCH3CH2)3(i-OC4H9)), tri-n-butoxymethoxyzirconium (Zr(OCH3)(OC4H9)3), di-n-butoxydimethoxyzirconium (Zr(OCH3)2(OC4H9)2), trimethoxy-n-butoxyzirconium (Zr(OCH3)3(OC4H9)), tri-n-butoxymethoxyzirconium (Zr(OCH3CH2)(OC4H9)3), di-n-butoxydiethoxyzirconium (Zr(OCH3CH2)2(OC4H9)2), triethoxy-n-butoxyzirconium (Zr(OCH3CH2)3(OC4H9)), etc.;
[0235] Hafnium tetramethoxide (Hf(OCH3)4), hafnium tetraethoxide (Hf(OCH3CH2)4), hafnium tetraisobutoxide (Hf(i-OC4H9)4), hafnium tetra-n-butoxide (Hf(OC4H9)4), hafnium triethoxymethoxide (Hf(OCH3)(OCH3CH2)3), hafnium diethoxydimethoxide (Hf(OCH3)2(OCH3CH2)2), hafnium trimethoxyethoxide (Hf(OCH3)3(OCH3CH2)), hafnium triisobutoxide (Hf(OCH3)(i-OC4H9)3), hafnium diisobutoxide (Hf(OCH3)2(i-OC4H9)2), hafnium trimethoxyisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf(OCH3)3(i-OC4H9)), hafnium triisobutoxide (Hf (OCH3CH2)(i-OC4H9)3), diisobutoxydiethoxyhafnium (Hf(OCH3CH2)2(i-OC4H9)2), triethoxyisobutoxyhafnium (Hf(OCH3CH2)3(i-C4H9)), tri-n-butoxymethoxyhafnium (Hf(OCH3)(OC4H9)3), di-n-butoxydimethoxyhafnium (Hf(OCH3)2(OC4H9)2), trimethoxy-n-butoxyhafnium (Hf(OCH3)3(OC4H9)), tri-n-butoxymethoxyhafnium (Hf(OCH3CH2)(OC4H9)3), di-n-butoxydiethoxyhafnium (Hf(OCH3CH2)2(OC4H9)2), triethoxy-n-butoxyhafnium (Hf(OCH3CH2)3(OC4H9)), etc.
[0236] As the IV B group metal alkyl halide, for example, trimethyl titanium chloride (TiCl(CH3)3), triethyl titanium chloride (TiCl(CH3CH2)3), triisobutyl titanium chloride (TiCl(i-C4H9)3), tri-n-butyl titanium chloride (TiCl(C4H9)3), dimethyl titanium dichloride (TiCl2(CH3)2), diethyl titanium dichloride (TiCl2(CH3CH2)2), diisobutyl titanium dichloride (TiCl2(i-C4H9)2), tri-n-butyl titanium chloride (TiCl(C4H9)3), methyl titanium trichloride (Ti(CH3)Cl3), ethyl titanium trichloride (Ti(CH3CH2)Cl3), isobutyl titanium trichloride (Ti(i-C4H9)Cl3), and n-butyl titanium trichloride (Ti(C4H9)Cl3);
[0237] Trimethyltitanium bromide (TiBr(CH3)3), triethyltitanium bromide (TiBr(CH3CH2)3), triisobutyltitanium bromide (TiBr(i-C4H9)3), tri-n-butyltitanium bromide (TiBr(C4H9)3), dimethyltitanium dibromide (TiBr2(CH3)2), diethyltitanium dibromide (TiBr2(CH3CH2)2), diisobutyltitanium dibromide (TiBr2(i-C4H9)2), tri-n-butyltitanium bromide (TiBr(C4H9)3), methyltitanium tribromide (Ti(CH3)Br3), ethyltitanium tribromide (Ti(CH3CH2)Br3), isobutyltitanium tribromide (Ti(i-C4H9)Br3), n-butyltitanium tribromide (Ti(C4H9)Br3);
[0238] Trimethyl zirconium chloride (ZrCl(CH3)3), triethyl zirconium chloride (ZrCl(CH3CH2)3), triisobutyl zirconium chloride (ZrCl(i-C4H9)3), tri-n-butyl zirconium chloride (ZrCl(C4H9)3), dimethyl zirconium dichloride (ZrCl2(CH3)2), diethyl zirconium dichloride (ZrCl2(CH3CH2)2), diisobutyl zirconium dichloride (ZrCl2(i-C4H9)2), tri-n-butyl zirconium chloride (ZrCl(C4H9)3), methyl zirconium trichloride (Zr(CH3)Cl3), ethyl zirconium trichloride (Zr(CH3CH2)Cl3), isobutyl zirconium trichloride (Zr(i-C4H9)Cl3), n-butyl zirconium trichloride (Zr(C4H9)Cl3);
[0239] Trimethyl zirconium bromide (ZrBr(CH3)3), triethyl zirconium bromide (ZrBr(CH3CH2)3), triisobutyl zirconium bromide (ZrBr(i-C4H9)3), tri-n-butyl zirconium bromide (ZrBr(C4H9)3), dimethyl zirconium dibromide (ZrBr2(CH3)2), diethyl zirconium dibromide (ZrBr2(CH3CH2)2), diisobutyl zirconium dibromide (ZrBr2(i-C4H9)2), tri-n-butyl zirconium bromide (ZrBr(C4H9)3), methyl zirconium tribromide (Zr(CH3)Br3), ethyl zirconium tribromide (Zr(CH3CH2)Br3), isobutyl zirconium tribromide (Zr(i-C4H9)Br3), n-butyl zirconium tribromide (Zr(C4H9)Br3);
[0240] Trimethyl hafnium chloride (HfCl(CH3)3), triethyl hafnium chloride (HfCl(CH3CH2)3), triisobutyl hafnium chloride (HfCl(i-C4H9)3), tri-n-butyl hafnium chloride (HfCl(C4H9)3), dimethyl hafnium dichloride (HfCl2(CH3)2), diethyl hafnium dichloride (HfCl2(CH3CH2)2), diisobutyl hafnium dichloride (HfCl2(i-C4H9)2), tri-n-butyl hafnium chloride (HfCl(C4H9)3), methyl hafnium trichloride (Hf(CH3)Cl3), ethyl hafnium trichloride (Hf(CH3CH2)Cl3), isobutyl hafnium trichloride (Hf(i-C4H9)Cl3), n-butyl hafnium trichloride (Hf(C4H9)Cl3);
[0241] Trimethyl hafnium bromide (HfBr(CH3)3), triethyl hafnium bromide (HfBr(CH3CH2)3), triisobutyl hafnium bromide (HfBr(i-C4H9)3), tri-n-butyl hafnium bromide (HfBr(C4H9)3), dimethyl hafnium dibromide (HfBr2(CH3)2), diethyl hafnium dibromide (HfBr2(CH3CH2)2), diisobutyl hafnium dibromide (HfBr2(i-C4H9)2), tri-n-butyl hafnium bromide (HfBr(C4H9)3), methyl hafnium tribromide (Hf(CH3)Br3), ethyl hafnium tribromide (Hf(CH3CH2)Br3), isobutyl hafnium tribromide (Hf(i-C4H9)Br3), n-butyl hafnium tribromide (Hf(C4H9)Br3).
[0242] As the IV B group metal alkoxy halide, for example, trimethoxytitanium chloride (TiCl(OCH3)3), triethoxytitanium chloride (TiCl(OCH3CH2)3), triisobutoxytitanium chloride (TiCl(i-OC4H9)3), tri-n-butoxytitanium chloride (TiCl(OC4H9)3), dimethoxytitanium dichloride (TiCl2(OCH3)2), diethoxytitanium dichloride (TiCl2(OCH3CH2)2), diisobutoxytitanium dichloride (TiCl2(i-OC4H9)2), tri-n-butoxytitanium chloride (TiCl(OC4H9)3), methoxytitanium trichloride (Ti(OCH3)Cl3), ethoxytitanium trichloride (Ti(OCH3CH2)Cl3), isobutoxytitanium trichloride (Ti(i-C4H9)Cl3), and n-butoxytitanium trichloride (Ti(OC4H9)Cl3);
[0243] Trimethoxytitanium bromide (TiBr(OCH3)3), triethoxytitanium bromide (TiBr(OCH3CH2)3), triisobutoxytitanium bromide (TiBr(i-OC4H9)3), tri-n-butoxytitanium bromide (TiBr(OC4H9)3), dimethoxytitanium dibromide (TiBr2(OCH3)2), diethoxytitanium dibromide (TiBr2(OCH3CH2)2), diisobutoxytitanium dibromide (TiBr2(i-OC4H9)2), tri-n-butoxytitanium bromide (TiBr(OC4H9)3), methoxytitanium tribromide (Ti(OCH3)Br3), ethoxytitanium tribromide (Ti(OCH3CH2)Br3), isobutoxytitanium tribromide (Ti(i-C4H9)Br3), n-butoxytitanium tribromide (Ti(OC4H9)Br3);
[0244] Trimethoxy zirconium chloride (ZrCl(OCH3)3), triethoxy zirconium chloride (ZrCl(OCH3CH2)3), triisobutoxy zirconium chloride (ZrCl(i-OC4H9)3), tri-n-butoxy zirconium chloride (ZrCl(OC4H9)3), dimethoxy zirconium dichloride (ZrCl2(OCH3)2), diethoxy zirconium dichloride (ZrCl2(OCH3CH2)2), diisobutoxy zirconium dichloride (ZrCl2(i-OC4H9)2), tri-n-butoxy zirconium chloride (ZrCl(OC4H9)3), methoxy zirconium trichloride (Zr(OCH3)Cl3), ethoxy zirconium trichloride (Zr(OCH3CH2)Cl3), isobutoxy zirconium trichloride (Zr(i-C4H9)Cl3), n-butoxy zirconium trichloride (Zr(OC4H9)Cl3);
[0245] Trimethoxyzirconium bromide (ZrBr(OCH3)3), triethoxyzirconium bromide (ZrBr(OCH3CH2)3), triisobutoxyzirconium bromide (ZrBr(i-OC4H9)3), tri-n-butoxyzirconium bromide (ZrBr(OC4H9)3), dimethoxyzirconium dibromide (ZrBr2(OCH3)2), diethoxyzirconium dibromide (ZrBr2(OCH3CH2)2), diisobutoxyzirconium dibromide (ZrBr2(i-OC4H9)2), tri-n-butoxyzirconium bromide (ZrBr(OC4H9)3), methoxyzirconium tribromide (Zr(OCH3)Br3), ethoxyzirconium tribromide (Zr(OCH3CH2)Br3), isobutoxyzirconium tribromide (Zr(i-C4H9)Br3), n-butoxyzirconium tribromide (Zr(OC4H9)Br3);
[0246] Hafnium trimethoxychloride (HfCl(OCH3)3), Hafnium triethoxychloride (HfCl(OCH3CH2)3), Hafnium triisobutoxychloride (HfCl(i-OC4H9)3), Hafnium tri-n-butoxychloride (HfCl(OC4H9)3), Hafnium dimethoxychloride (HfCl2(OCH3)2), Hafnium diethoxychloride (HfCl2(OCH3CH2)2), Hafnium dichloride (HfCl2(i-OC4H9)2), tri-n-butoxy hafnium chloride (HfCl(OC4H9)3), methoxy hafnium trichloride (Hf(OCH3)Cl3), ethoxy hafnium trichloride (Hf(OCH3CH2)Cl3), isobutoxy hafnium trichloride (Hf(i-C4H9)Cl3), n-butoxy hafnium trichloride (Hf(OC4H9)Cl3);
[0247] Hafnium bromide trimethoxy (HfBr(OCH3)3), hafnium bromide triethoxy (HfBr(OCH3CH2)3), hafnium bromide triisobutoxy (HfBr(i-OC4H9)3), hafnium bromide tri-n-butoxy (HfBr(OC4H9)3), hafnium dimethoxy (HfBr2(OCH3)2), hafnium diethoxy (HfBr2(OCH3CH2)2), Hafnium dibromide (HfBr2(i-OC4H9)2), tri-n-butoxy hafnium bromide (HfBr(OC4H9)3), methoxy hafnium tribromide (Hf(OCH3)Br3), ethoxy hafnium tribromide (Hf(OCH3CH2)Br3), isobutoxy hafnium tribromide (Hf(i-C4H9)Br3), and n-butoxy hafnium tribromide (Hf(OC4H9)Br3).
[0248] As the IV B Group metal compound, the IV B Group metal halide is preferred, TiCl 4 , TiBr 4 , ZrCl 4 , ZrBr 4 , HfCl 4 and HfBr 4 are more preferred, and TiCl 4 and ZrCl 4 are most preferred.
[0249] These Group IV B metal compounds may be used alone or in combination of two or more in any ratio.
[0250] When the chemical treatment agent is in liquid state at room temperature, the chemical treatment agent can be directly used to carry out the chemical treatment reaction. When the chemical treatment agent is in solid state at room temperature, for the sake of convenient measurement and operation, the chemical treatment agent is preferably used in the form of a solution. Of course, when the chemical treatment agent is in liquid state at room temperature, the chemical treatment agent can sometimes be used in the form of a solution as needed, without particular limitation.
[0251] When preparing the solution of the chemical treatment agent, there is no particular limitation on the solvent used at this time, as long as it can dissolve the chemical treatment agent and does not destroy (eg, dissolve) the existing carrier structure of the carrier.
[0252] Specifically, we can cite C 5-12 Alkanes, C 5-12 Cycloalkanes, halogenated C 5-12 Alkanes and halogenated C 5-12 Cycloalkanes include, for example, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, chloropentane, chlorohexane, chloroheptane, chlorooctane, chlorononane, chlorodecane, chloroundecane, chlorododecane and chlorocyclohexane, among which pentane, hexane, decane and cyclohexane are preferred, and hexane is most preferred.
[0253] These solvents may be used alone or in combination of two or more in any ratio.
[0254] In addition, there is no particular limitation on the concentration of the chemical treatment agent in its solution, and it can be appropriately selected as needed, as long as it can achieve the chemical treatment reaction with a predetermined amount of the chemical treatment agent. As mentioned above, if the chemical treatment agent is liquid, the chemical treatment agent can be used directly for the treatment, but it can also be used after being prepared into a solution of the chemical treatment agent.
[0255] Generally speaking, the molar concentration of the chemical treatment agent in its solution is generally set to 0.01-1.0 mol / L, but is not limited thereto.
[0256] As a method for carrying out the chemical treatment, for example, when a solid chemical treatment agent (such as zirconium tetrachloride) is used, a solution of the chemical treatment agent is first prepared, and then a predetermined amount of the chemical treatment agent is added (preferably dropped) to the carrier to be treated; when a liquid chemical treatment agent (such as titanium tetrachloride) is used, a predetermined amount of the chemical treatment agent can be directly added (preferably dropped) to the carrier to be treated (but it can also be added after preparing a solution), and the chemical treatment reaction is carried out at a reaction temperature of -30-60°C (preferably -20-30°C) (with stirring if necessary) for 0.5 to 24 hours, preferably 1 to 8 hours, more preferably 2 to 6 hours, and then filtered, washed and dried.
[0257] According to the present invention, the filtering, washing and drying can be carried out by conventional methods, wherein the washing solvent can be the same solvent used to dissolve the chemical treatment agent. The washing is generally carried out 1 to 8 times, preferably 2 to 6 times, and most preferably 2 to 4 times.
[0258] According to the present invention, the amount of the chemical treatment agent used is such that the molar ratio of the magnesium compound (solid) calculated as Mg element to the chemical treatment agent calculated as Group IV B metal (such as Ti) element reaches 1:0.01-1, preferably 1:0.01-0.50, and more preferably 1:0.10-0.30.
[0259] According to a particular embodiment of the present invention, the method for preparing a supported non-metallocene catalyst of the present invention further comprises a step of pre-treating the modified composite support with an auxiliary chemical treatment agent selected from aluminoxane, alkyl aluminum or any combination thereof before treating the modified composite support with the chemical treatment agent (pre-treatment step). Then, the chemical treatment is performed with the chemical treatment agent in exactly the same manner as above, except that the modified composite support is replaced with the pre-treated modified composite support.
[0260] The auxiliary chemical treatment agent is described in detail below.
[0261] According to the present invention, the auxiliary chemical treatment agent may include, for example, aluminoxane and alkylaluminum.
[0262] As the aluminoxane, for example, linear aluminoxane represented by the following general formula (I) can be cited: (R)(R)Al-(Al(R)-O) n -O-Al(R)(R), and a cyclic aluminoxane represented by the following general formula (II): -(Al(R)-O-) n+2 -.
[0263]
[0264] In the aforementioned general formula, the groups R are the same or different (preferably the same) and are independently selected from C1-C8 alkyl, preferably methyl, ethyl and isobutyl, most preferably methyl; n is any integer in the range of 1-50, preferably any integer in the range of 10 to 30.
[0265] As the aluminoxane, methylaluminoxane, ethylaluminoxane, isobutylaluminoxane and n-butylaluminoxane are preferred, and methylaluminoxane and isobutylaluminoxane are more preferred.
[0266] These aluminoxanes may be used alone or in combination of two or more in any ratio.
[0267] As the alkyl aluminum, for example, there can be mentioned the compound represented by the following general formula (III):
[0268] Al(R)3 (III)
[0269] The groups R are identical or different (preferably identical) to each other, and are each independently selected from C1-C8 alkyl, preferably methyl, ethyl and isobutyl, most preferably methyl.
[0270] Specifically, examples of the alkyl aluminum include trimethyl aluminum (Al(CH3)3), triethyl aluminum (Al(CH3CH2)3), tripropyl aluminum (Al(C3H7)3), triisobutyl aluminum (Al(i-C4H9)3), tri-n-butyl aluminum (Al(C4H9)3), triisopentyl aluminum (Al(i-C5H 11 )3), tri-n-pentyl aluminum (Al(C5H 11 )3) Trihexylaluminum (Al(C6H 13 )3) Triisohexyl aluminum (Al(i-C6H 13 )3), diethylmethylaluminum (Al(CH3)(CH3CH2)2) and dimethylethylaluminum (Al(CH3CH2)(CH3)2), etc., among which trimethylaluminum, triethylaluminum, tripropylaluminum and triisobutylaluminum are preferred, and triethylaluminum and triisobutylaluminum are most preferred.
[0271] These aluminum alkyls may be used alone or in combination of two or more in any ratio.
[0272] According to the present invention, as the auxiliary chemical treatment agent, only the aluminoxane or only the alkylaluminum can be used, or any mixture of the aluminoxane and the alkylaluminum can be used. Moreover, there is no particular limitation on the proportion of each component in the mixture, and it can be arbitrarily selected as needed.
[0273] According to the present invention, the auxiliary chemical treatment agent is generally used in the form of a solution. When preparing the solution of the auxiliary chemical treatment agent, there is no particular limitation on the solvent used at this time, as long as it can dissolve the auxiliary chemical treatment agent and does not destroy (such as dissolve) the existing carrier structure of the carrier.
[0274] Specifically, as the solvent, for example, C 5-12 Alkanes and halogenated C 5-12 Alkanes and the like include, for example, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, cyclohexane, chloropentane, chlorohexane, chloroheptane, chlorooctane, chlorononane, chlorodecane, chloroundecane, chlorododecane and chlorocyclohexane, among which pentane, hexane, decane and cyclohexane are preferred, and hexane is most preferred.
[0275] These solvents may be used alone or in combination of two or more in any ratio.
[0276] In addition, there is no particular limitation on the concentration of the auxiliary chemical treatment agent in the solution thereof, and it can be appropriately selected as required, as long as it can achieve the pretreatment with a predetermined amount of the auxiliary chemical treatment agent.
[0277] As a method for carrying out the pretreatment, for example, a solution of the auxiliary chemical treatment agent is first prepared, and then the auxiliary chemical treatment agent solution (containing a predetermined amount of the auxiliary chemical treatment agent) is metered (preferably dripped) into the carrier to be pretreated with the auxiliary chemical treatment agent at a temperature of -30-60°C (preferably -20-30°C), or the carrier is metered into the auxiliary chemical treatment agent solution to form a reaction mixture, which is reacted for 1-8 hours, preferably 2-6 hours, and most preferably 3-4 hours (with stirring if necessary). Then, the obtained pretreatment product is separated from the reaction mixture by filtering, washing (1 to 6 times, preferably 1 to 3 times) and optionally drying, or it can be directly used in the subsequent reaction step (i.e., the aforementioned chemical treatment step) in the form of a mixed solution without separation. At this time, since the mixed solution already contains a certain amount of solvent, the amount of solvent involved in the subsequent reaction step can be reduced accordingly.
[0278] According to the present invention, the amount of the auxiliary chemical treatment agent used is such that the molar ratio of the magnesium compound (solid) calculated as Mg element to the auxiliary chemical treatment agent calculated as Al element reaches 1:0-1.0, preferably 1:0-0.5, and more preferably 1:0.1-0.5.
[0279] It is known to those skilled in the art that all the aforementioned method steps are preferably carried out under substantially anhydrous and oxygen-free conditions. Here, substantially anhydrous and oxygen-free means that the water and oxygen content in the system is continuously less than 10 ppm. Moreover, after preparation, the supported non-metallocene catalyst of the present invention usually needs to be stored under a slightly positive pressure under closed conditions for standby use.
[0280] According to the present invention, the molar ratio of the magnesium compound calculated as Mg element to the non-metallocene ligand is 1:0.0001-1, preferably 1:0.0002-0.4, more preferably 1:0.0008-0.2, further preferably 1:0.001-0.1, the ratio of the magnesium compound to the solvent is 1 mol:75-400 ml, preferably 1 mol:150-300 ml, more preferably 1 mol:200-250 ml, the ... to the solvent is 1 mol:75-400 ml, preferably 1 mol:150-300 ml, more preferably 1 mol:200-250 ml, the ratio of the magnesium compound to the non-metallocene ligand is 1:0.0001-1 The molar ratio of the alcohol is 1:0.02-4.00, preferably 1:0.05-3.00, more preferably 1:0.10-2.50, the mass ratio of the magnesium compound calculated as magnesium compound solid to the porous carrier is 1:0.1-20, preferably 1:0.5-10, more preferably 1:1-5, the volume ratio of the precipitant to the solvent is 1:0.2-5, preferably 1:0.5-2, more preferably 1:0.8-1.5, and the molar ratio of the magnesium compound calculated as Mg element to the chemical treatment agent calculated as Group IV B metal element is 1:0.01-1, preferably 1:0.01-0.50, more preferably 1:0.10-0.30.
[0281] In one embodiment, the present invention also relates to a supported non-metallocene catalyst (sometimes also referred to as a supported non-metallocene olefin polymerization catalyst) produced by the aforementioned method for preparing a supported non-metallocene catalyst.
[0282] In a further embodiment, the present invention relates to an olefin homopolymerization / copolymerization process, wherein the supported non-metallocene catalyst of the present invention is used as a catalyst for olefin polymerization to homopolymerize or copolymerize olefins.
[0283] As for the olefin homopolymerization / copolymerization method involved in the present invention, except for the contents specifically mentioned below, other unspecified contents (such as polymerization reactor, olefin dosage, catalyst and olefin addition method, etc.) can be directly applied to those conventionally known in the art without any special limitation, and their description is omitted here.
[0284] According to the homopolymerization / copolymerization method of the present invention, the supported non-metallocene catalyst of the present invention is used as a main catalyst, and one or more selected from aluminoxane, alkyl aluminum, halogenated alkyl aluminum, borofluorane, alkyl boron and alkyl boron ammonium salt are used as co-catalysts to homopolymerize or copolymerize olefins.
[0285] The main catalyst and the co-catalyst can be added to the polymerization reaction system by first adding the main catalyst and then adding the co-catalyst, or by first adding the co-catalyst and then adding the main catalyst, or by first contacting and mixing the two and then adding them together, or by adding them separately at the same time. When the main catalyst and the co-catalyst are added separately, they can be added sequentially in the same feeding line or in multiple feeding lines, and when the two are added separately at the same time, multiple feeding lines should be selected. For continuous polymerization, it is preferred to add them continuously in multiple feeding lines at the same time, and for intermittent polymerization, it is preferred to mix the two first and then add them together in the same feeding line, or to first add the co-catalyst and then the main catalyst in the same feeding line.
[0286] According to the present invention, there is no particular limitation on the reaction mode of the olefin homopolymerization / copolymerization method, and those known in the art can be adopted, such as a slurry method, an emulsion method, a solution method, a bulk method and a gas phase method, among which a slurry method and a gas phase method are preferred.
[0287] According to the present invention, the olefins include, for example, C2 to C 10 Mono-olefins, di-olefins, cyclic olefins and other ethylenically unsaturated compounds.
[0288] Specifically, as the C2 to C 10 As monoolefins, for example, ethylene, propylene, 1-butene, 1-hexene, 1-heptene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-undecene, 1-dodecene and styrene can be cited; as the cyclic olefins, for example, 1-cyclopentene and norbornene can be cited; as the diolefins, for example, 1,4-butadiene, 2,5-pentadiene, 1,6-hexadiene, norbornadiene and 1,7-octadiene can be cited; and as the other ethylenically unsaturated compounds, for example, vinyl acetate and (meth)acrylate can be cited. Among them, homopolymerization of ethylene or copolymerization of ethylene with propylene, 1-butene or 1-hexene is preferred.
[0289] According to the present invention, homopolymerization refers to the polymerization of only one of the olefins, while copolymerization refers to the polymerization between two or more of the olefins.
[0290] According to the present invention, the cocatalyst is selected from aluminoxane, alkylaluminum, halogenated alkylaluminum, borofluorane, alkylboron and alkylboron ammonium salt, among which aluminoxane and alkylaluminum are preferred.
[0291] As the aluminoxane, for example, there can be mentioned the linear aluminoxane represented by the following general formula (I-1): (R)(R)Al-(Al(R)-O) n -O-Al(R)(R), and a cyclic aluminoxane represented by the following general formula (II-1): -(Al(R)-O-)n+2 -.
[0292]
[0293] In the aforementioned general formula, the groups R are the same or different (preferably the same) and are independently selected from C1-C8 alkyl, preferably methyl, ethyl and isobutyl, most preferably methyl; n is any integer in the range of 1-50, preferably any integer in the range of 10 to 30.
[0294] As the aluminoxane, methylaluminoxane, ethylaluminoxane, isobutylaluminoxane and n-butylaluminoxane are preferred, methylaluminoxane and isobutylaluminoxane are further preferred, and methylaluminoxane is most preferred.
[0295] These aluminoxanes may be used alone or in combination of two or more in any ratio.
[0296] As the alkyl aluminum, for example, there can be mentioned the compound represented by the following general formula (III-1):
[0297] Al(R)3 (III-1)
[0298] The groups R are identical or different (preferably identical) to each other, and are each independently selected from C1-C8 alkyl, preferably methyl, ethyl and isobutyl, most preferably methyl.
[0299] Specifically, examples of the alkyl aluminum include trimethyl aluminum (Al(CH3)3), triethyl aluminum (Al(CH3CH2)3), tripropyl aluminum (Al(C3H7)3), triisobutyl aluminum (Al(i-C4H9)3), tri-n-butyl aluminum (Al(C4H9)3), triisopentyl aluminum (Al(i-C5H 11 )3), tri-n-pentyl aluminum (Al(C5H 11 )3) Trihexylaluminum (Al(C6H 13 )3) Triisohexyl aluminum (Al(i-C6H 13 )3), diethylmethylaluminum (Al(CH3)(CH3CH2)2) and dimethylethylaluminum (Al(CH3CH2)(CH3)2), etc., among which trimethylaluminum, triethylaluminum, tripropylaluminum and triisobutylaluminum are preferred, triethylaluminum and triisobutylaluminum are further preferred, and triethylaluminum is most preferred.
[0300] These aluminum alkyls may be used alone or in combination of two or more in any ratio.
[0301] As the alkylaluminum halide, the borane, the alkyl boron and the alkyl boron ammonium salt, those commonly used in the art may be used directly without particular limitation.
[0302] In addition, according to the present invention, the co-catalyst may be used alone or in combination of a plurality of the co-catalysts in any ratio as required, without any particular limitation.
[0303] According to the present invention, depending on the reaction mode of the olefin homopolymerization / copolymerization method, it is sometimes necessary to use a polymerization solvent.
[0304] As the polymerization solvent, those conventionally used in the art for olefin homopolymerization / copolymerization may be used without particular limitation.
[0305] Examples of the polymerization solvent include C 4-10 Alkanes (such as butane, pentane, hexane, heptane, octane, nonane or decane, etc.), halogenated C 1-10 Alkanes (such as dichloromethane), aromatic hydrocarbon solvents (such as toluene and xylene), ether solvents (such as diethyl ether or tetrahydrofuran), ester solvents (such as ethyl acetate) and ketone solvents (such as acetone), etc. Among them, hexane is preferably used as the polymerization solvent.
[0306] These polymerization solvents may be used alone or in combination of two or more in any ratio.
[0307] According to the present invention, the polymerization reaction pressure of the olefin homopolymerization / copolymerization method is generally 0.1 to 10 MPa, preferably 0.1 to 4 MPa, more preferably 1 to 3 MPa, but sometimes not limited thereto. According to the present invention, the polymerization reaction temperature is generally -40°C to 200°C, preferably 10°C to 100°C, more preferably 40°C to 90°C, but sometimes not limited thereto.
[0308] In addition, according to the present invention, the olefin homopolymerization / copolymerization method can be carried out in the presence of hydrogen or in the absence of hydrogen. In the presence of hydrogen, the partial pressure of hydrogen can be 0.01% to 99%, preferably 0.01% to 50% of the polymerization pressure, but sometimes it is not limited thereto.
[0309] According to the present invention, when carrying out the olefin homopolymerization / copolymerization method, the molar ratio of the cocatalyst calculated as aluminum or boron to the supported non-metallocene catalyst calculated as Group IV B metal is generally 1:1-1000, preferably 1:1-500, more preferably 1:10-500, but sometimes not limited thereto.
[0310] Example
[0311] The present invention is further described in detail below using examples, but the present invention is not limited to these examples.
[0312] Bulk density of polymer (in g / cm3 ) is determined in accordance with Chinese national standard GB1636-79.
[0313] The contents of Group IV B metals (such as Ti) and Mg in the supported non-metallocene catalyst are determined by ICP-AES, and the content of the non-metallocene ligand is determined by elemental analysis.
[0314] The polymerization activity of the catalyst is calculated according to the following method: after the polymerization reaction is completed, the polymerization product in the reactor is filtered and dried, and then the mass of the polymerization product is weighed. The polymerization activity of the catalyst is expressed as the ratio of the mass of the polymerization product divided by the mass of the supported non-metallocene catalyst used (the unit is kg polymer / g catalyst or kg polymer / gCat).
[0315] The viscosity-average molecular weight of the polymer is calculated according to the following method: According to standard ASTM D4020-00, the intrinsic viscosity of the polymer is measured by a high-temperature dilution Ubbelohde viscometer method (the inner diameter of the capillary is 0.44 mm, the constant temperature bath medium is No. 300 silicone oil, the dilution solvent is decahydronaphthalene, and the measurement temperature is 135°C), and then the viscosity-average molecular weight Mv of the polymer is calculated according to the following formula.
[0316] Mv=5.37×10 4 ×[η] 1.37
[0317] Here, η is the intrinsic viscosity.
[0318] The alcohol content in the carrier is determined according to the following method: quantitative analysis is performed using capillary gas chromatography, the instrument is Agilent 6890N gas chromatograph, equipped with an automatic sample injector and a hydrogen flame ionization detector (FID); the chromatographic column is DB-1 (30m×0.32mm×0.25μm), and the gas chromatography operating conditions are: temperature: vaporization chamber 250°C, column temperature 60°C, detector 250°C; carrier gas is high-purity nitrogen; carrier gas flow rate is 1.4ml / min; split ratio is 70:1; injection volume is 0.2ml; the test reagent is chromatographically pure ethanol or n-butanol, wherein n-butanol is used to determine the ethanol content, ethanol is used to determine the n-butanol content, and ethanol or n-butanol can be used to determine the content of other alcohols. The relative retention time is determined to be 2.426min for ethanol and 3.151min for n-butanol. Accurately prepare ten different concentrations of the alcohol to be tested in the reagent alcohol solution as standard samples. Under gas chromatography conditions, use the area normalization method to calculate the correction factor of each component and make a relationship diagram between the alcohol concentration index and the actual concentration. Accurately weigh 1.00g of the carrier, add 10ml of alcohol reagent, stir and dissolve at room temperature for 20 minutes, then filter and take the filtrate for use. Under gas chromatography conditions, take a quantitative filtrate and add it to the automatic sampler for automatic program injection and determination. Calculate the filtrate alcohol concentration index by dividing the peak area of the alcohol to be tested by the normalized total area, substitute it into the relationship diagram to obtain the actual alcohol concentration, and finally obtain the alcohol content in the carrier after conversion.
[0319] Example 1
[0320] The magnesium compound is anhydrous magnesium chloride, and the porous carrier is silicon dioxide, that is, silica gel, model ES757 of Ineos. First, the silica gel is continuously calcined at 600°C in a nitrogen atmosphere for 4 hours for thermal activation. The alcohol is butanol, the solvent for dissolving the magnesium compound is tetrahydrofuran, and the non-metallocene ligand is a structural formula The compound, the precipitant is hexane, and the chemical treatment agent is titanium tetrachloride.
[0321] Weigh 2.5g of the magnesium compound anhydrous magnesium chloride (MgCl2), add a certain amount of butanol and tetrahydrofuran, heat to 60°C to dissolve, continue stirring at 60°C to completely dissolve, add silica gel to form a mixed slurry, stir for 2h, add precipitant hexane to precipitate, filter, and wash twice, the amount of precipitant used each time is the same as the previous amount added.
[0322] The obtained precipitate was dried at a temperature of 50°C (15.4°C lower than the boiling point of the solvent) under a vacuum of 5 mBar absolute pressure for 12 h, and then dried at a temperature of 90°C (24.6°C higher than the boiling point) under a vacuum of 5 mBar absolute pressure for 8 h to obtain a composite carrier in which the alcohol content was 1.6 wt%.
[0323] Measure 25 ml of hexane solvent and add it to the composite carrier. Add non-metallocene ligand under stirring conditions, react at 30°C for 4 hours, filter, wash with hexane 3 times, 25 ml each time, and vacuum dry to obtain the modified composite carrier.
[0324] Measure 25 ml of hexane solvent and add it to the modified composite support. Add titanium tetrachloride (TiCl4) chemical treatment agent dropwise under stirring for 15 minutes. After reacting at 30°C for 4 hours, filter, wash with hexane 3 times, 25 ml each time, and finally vacuum dry to obtain a supported non-metallocene catalyst.
[0325] The ratios are as follows: the molar ratio of the magnesium compound to butanol is 1:0.5; the molar ratio of the magnesium compound to the tetrahydrofuran solvent for dissolving the magnesium compound is 1 mol:200 ml; the molar ratio of the magnesium compound to the non-metallocene ligand is 1:0.004; the mass ratio of the magnesium compound to the porous carrier silica gel is 1:2; the volume ratio of the precipitant hexane to the tetrahydrofuran solvent for dissolving the magnesium compound is 1:1; the molar ratio of the magnesium compound to the chemical treatment agent titanium tetrachloride is 1:0.20.
[0326] This catalyst was designated as CAT-1.
[0327] Example 2
[0328] It is basically the same as Example 1, but with the following changes:
[0329] The mixed slurry was dried at a temperature 25.4°C lower than the boiling point of the solvent under a vacuum of an absolute pressure of 5 mBar for 16 h, and then dried at a temperature 34.6°C higher than the boiling point of the solvent under a vacuum of an absolute pressure of 5 mBar for 10 h to obtain a composite carrier in which the alcohol content was 1.4 wt%.
[0330] This catalyst was designated as CAT-2.
[0331] Example 3
[0332] It is basically the same as Example 1, but with the following changes:
[0333] Prior to treating the modified composite support with the chemical treatment agent, the modified composite support is pretreated with a co-chemical treatment agent of triethylaluminum (Al(C2H5)3).
[0334] Measure 25 ml of hexane solvent and add it to the modified composite carrier obtained in Example 1. Under stirring conditions, first add the auxiliary chemical treatment agent triethylaluminum (Al(C2H5)3) dropwise within 15 minutes. After stirring for 1 hour, filter and wash with hexane twice, 25 ml each time. Filter, wash, and vacuum dry to obtain the pretreated modified composite carrier.
[0335] The molar ratio of the magnesium compound to the auxiliary chemical treatment agent is 1:0.35.
[0336] This catalyst was designated as CAT-3.
[0337] Example 4
[0338] It is basically the same as Example 3, but with the following changes:
[0339] The auxiliary chemical treatment agent was changed to methylaluminoxane (MAO).
[0340] Wherein: the molar ratio of the magnesium compound to the auxiliary chemical treatment agent is 1:0.5.
[0341] This catalyst was designated as CAT-4.
[0342] Comparative Example A
[0343] It is basically the same as Example 1, but with the following changes:
[0344] The mixed slurry was added with precipitant hexane to precipitate, filtered and washed twice, with the amount of precipitant used each time being the same as the previous amount. The obtained precipitate was uniformly heated to 120°C (higher than the boiling point of the solvent 54.6°C), and dried for 24 hours under a vacuum with an absolute pressure of 5 mBar to obtain a composite carrier, in which the alcohol content was 0.02 wt%.
[0345] The catalyst was designated as CAT-A.
[0346] Comparative Example B
[0347] It is basically the same as Example 1, but with the following changes:
[0348] The obtained precipitate was dried at a temperature of 20° C. (lower than the boiling point of the solvent, 45.4° C.) under a vacuum of an absolute pressure of 5 mBar for 12 h to obtain a composite carrier, wherein the alcohol content was 3.5 wt %.
[0349] The catalyst was designated as CAT-B.
[0350] Example 3 (Application Example)
[0351] The supported non-metallocene catalysts CAT-1 to 4 and CAT-A to B were weighed respectively, and homopolymerized and copolymerized ethylene and prepared ultra-high molecular weight polyethylene with a co-catalyst (methylaluminoxane or triethylaluminum) under the following conditions and according to the following method.
[0352] Homopolymerization is: 5 liters of polymerization autoclave, slurry polymerization process, 2.5 liters of hexane solvent, total polymerization pressure of 0.8MPa, polymerization temperature of 85°C, hydrogen partial pressure of 0.2MPa, reaction time of 2h. First, 2.5 liters of hexane are added to the polymerization autoclave, stirring is turned on, then 20 mg of supported non-metallocene catalyst and co-catalyst mixture are added, hydrogen is added to 0.2MPa, and finally ethylene is continuously introduced to make the total polymerization pressure constant at 0.8MPa. After the reaction is completed, the gas in the autoclave is vented, the polymer in the autoclave is released, and the mass is weighed after drying. The specific conditions of the polymerization reaction and the polymerization evaluation results are shown in Table 1.
[0353] The copolymerization is as follows: 5 liters of polymerization autoclave, slurry polymerization process, 2.5 liters of hexane solvent, total polymerization pressure of 0.8 MPa, polymerization temperature of 85°C, hydrogen partial pressure of 0.2 MPa, and reaction time of 2 hours. First, 2.5 liters of hexane are added to the polymerization autoclave, stirring is started, then 20 mg of supported non-metallocene catalyst and co-catalyst mixture are added, 50 g of hexene-1 comonomer is added at one time, and hydrogen is added to 0.2 MPa, and finally ethylene is continuously introduced to make the total polymerization pressure constant at 0.8 MPa. After the reaction is completed, the gas in the autoclave is vented, the polymer in the autoclave is released, and the mass is weighed after drying. The specific conditions of the polymerization reaction and the polymerization evaluation results are shown in Table 1.
[0354] The preparation of ultra-high molecular weight polyethylene polymerization is as follows: 5 liters of polymerization autoclave, slurry polymerization process, 2.5 liters of hexane solvent, total polymerization pressure of 0.5 MPa, polymerization temperature of 70°C, and reaction time of 6 hours. First, 2.5 liters of hexane are added to the polymerization autoclave, stirring is turned on, and then 20 mg of a supported non-metallocene catalyst and a co-catalyst mixture are added, the molar ratio of the co-catalyst to the catalyst active metal is 100, and finally ethylene is continuously introduced to keep the total polymerization pressure constant at 0.5 MPa. After the reaction is completed, the gas in the autoclave is vented, the polymer in the autoclave is released, and the mass is weighed after drying. The specific conditions of the polymerization reaction and the polymerization evaluation results are shown in Table 2.
[0355] Table 1. Summary of the effects of supported non-metallocene catalysts on olefin polymerization
[0356]
[0357] Table 2. Summary of the effects of supported non-metallocene catalysts on the preparation of ultra-high molecular weight polyethylene polymerization
[0358]
[0359] From the comparison of the effects obtained by No. 1 and 3 in Table 1, it can be seen that the copolymerization effect of the catalyst is significant, that is, the copolymerization activity of the catalyst is higher than the homopolymerization activity, and the copolymerization reaction can increase the bulk density of the polymer, that is, improve the particle morphology of the polymer.
[0360] From the comparison of the effects obtained by No. 1 and No. 2 in Table 1, it can be seen that the polymerization performance obtained under the conditions of the co-catalyst required for the polymerization process and the catalyst active metal molar ratio of 50 and 100 is equivalent, which shows that the amount of co-catalyst required for olefin polymerization provided by the catalyst of the present invention is relatively small.
[0361] From the comparison between sequence numbers 1, 2 and 7, 8 in Table 1, and sequence numbers 1, 2 and 3, 4 in Table 2, it can be seen that the catalyst obtained by controlling the alcohol content in the composite carrier during the catalyst preparation process of the present invention has better catalytic activity, polymer bulk density, ultra-high molecular weight polyethylene viscosity-average molecular weight and other properties than the catalyst performance obtained when the composite carrier is completely dried or has a higher alcohol content.
[0362] Although the specific implementations of the present invention have been described in detail above in conjunction with the embodiments, it should be pointed out that the protection scope of the present invention is not limited by these specific implementations, but is determined by the appended claims. Those skilled in the art may make appropriate changes to these implementations without departing from the technical ideas and purposes of the present invention, and these changed implementations are obviously also included in the protection scope of the present invention.
Claims
1. A method for preparing a supported non-metallocene catalyst, comprising the following steps: A step of dissolving a magnesium compound in a solvent in the presence of an alcohol to obtain a magnesium compound solution; A step of mixing a porous carrier which has been optionally subjected to a thermal activation treatment and / or a chemical activation treatment with the magnesium compound solution to obtain a mixed slurry; The step of drying the mixed slurry or adding a precipitant to the mixed slurry to obtain a composite carrier, wherein the content of the alcohol in the composite carrier is 1.0-2.0 wt %; treating the composite support with a non-metallocene ligand to obtain a modified composite support; and a step of treating the modified composite support with a chemical treatment agent selected from Group IVB metal compounds to obtain the supported non-metallocene catalyst, The step of obtaining the composite carrier is carried out in the following manner: The mixed slurry is dried for 2-48 hours at a temperature 5-40°C lower than the boiling point of the solvent and under a vacuum of an absolute pressure of 2-100 mBar, and then dried for 1-24 hours at a temperature from the boiling point of the solvent to 50°C higher than the boiling point of the solvent and under a vacuum of an absolute pressure of 2-100 mBar to obtain the composite carrier. Alternatively, a precipitant is added to the mixed slurry, and the obtained precipitate is optionally washed, dried for 2-48 hours at a temperature 5-40° C. lower than the boiling point of the solvent and under a vacuum of an absolute pressure of 2-100 mBar, and then dried for 1-24 hours at a temperature from the boiling point of the solvent to 50° C. higher than the boiling point of the solvent and under a vacuum of an absolute pressure of 2-100 mBar, to obtain the composite carrier. The non-metallocene ligand is selected from one or more of the compounds (A) and (B) having the following chemical formula: In the chemical structure, q is 0 or 1; d is 0 or 1; A is selected from oxygen atom, sulfur atom, selenium atom, -NR 23 R 24 、-N(O)R 25 R 26 , -PR 28 R 29 、-P(O)R 30 OR 31 , sulfone, sulfoxide or -Se(O)R 39 , wherein N, O, S, Se and P are each a coordinating atom; B is selected from nitrogen atoms, nitrogen-containing groups, phosphorus-containing groups or C1-C 30 Hydrocarbon; E is selected from a nitrogen-containing group, an oxygen-containing group, a sulfur-containing group, a selenium-containing group, a phosphorus-containing group or a cyano group, wherein N, O, S, Se and P are each a coordinating atom; F is selected from a nitrogen atom, a nitrogen-containing group, an oxygen-containing group, a sulfur-containing group, a selenium-containing group or a phosphorus-containing group, wherein N, O, S, Se and P are each a coordinating atom; G is selected from C1-C 30 Hydrocarbon, substituted C1-C 30 Hydrocarbon groups or inert functional groups; — represents a covalent bond or an ionic bond; R 1 To R 3 are independently selected from hydrogen, C1-C 30 Hydrocarbon, substituted C1-C 30 Hydrocarbon or inert functional group, R 22 To R 31 , R 39 are independently selected from hydrogen, C1-C 30 Hydrocarbon or substituted C1-C 30 Hydrocarbyl groups, the above groups may be the same or different from each other, wherein adjacent groups may be combined with each other to form a bond or a ring; The inert functional group is selected from halogen, oxygen-containing group, nitrogen-containing group, silicon-containing group, germanium-containing group, sulfur-containing group, tin-containing group, C1-C 10 Ester and nitro groups; The substituted C1-C 30 The hydrocarbon group is selected from the group consisting of one or more halogen or C1-C 30 C1-C 30 Hydrocarbon.
2. The preparation method according to claim 1 further comprises the step of pre-treating the modified composite support with an auxiliary chemical treatment agent selected from aluminoxane, alkyl aluminum or any combination thereof before treating the modified composite support with the chemical treatment agent.
3. The preparation method according to claim 1, characterized in that: The porous carrier is selected from one or more of olefin homopolymers or copolymers, polyvinyl alcohol or its copolymers, cyclodextrin, polyester or copolyester, polyamide or copolyamide, vinyl chloride homopolymer or copolymer, acrylate homopolymer or copolymer, methacrylate homopolymer or copolymer, styrene homopolymer or copolymer, partially cross-linked forms of these homopolymers or copolymers, refractory oxides or refractory composite oxides of metals of Groups IIA, IIIA, IVA or IVB of the Periodic Table, clay, molecular sieve, mica, montmorillonite, bentonite and diatomaceous earth.
4. The preparation method according to claim 1, characterized in that: The magnesium compound is selected from one or more of magnesium halide, alkoxymagnesium halide, alkoxymagnesium, alkylmagnesium, alkylmagnesium halide and alkylalkoxymagnesium.
5. The preparation method according to claim 1, characterized in that: The solvent is selected from C 6-12 Aromatic hydrocarbons, halogenated C 6-12 One or more of aromatic hydrocarbons, esters and ethers, the alcohol is selected from one or more of aliphatic alcohols, aromatic alcohols and alicyclic alcohols, wherein the alcohol is optionally selected from halogen atoms or C 1-6 The substituents of the alkoxy group are substituted.
6. The preparation method according to claim 1, characterized in that: The non-metallocene ligand is selected from one or more of compounds (A-1) to (A-4) and compounds (B-1) to (B-4) having the following chemical structural formulas: In all the above chemical structures, q is 0 or 1; d is 0 or 1; A is selected from oxygen atom, sulfur atom, selenium atom, -NR 23 R 24 、-N(O)R 25 R 26 , -PR 28 R 29 、-P(O)R 30 OR 31 , sulfone, sulfoxide or -Se(O)R 39 , wherein N, O, S, Se and P are each a coordinating atom; E is selected from a nitrogen-containing group, an oxygen-containing group, a sulfur-containing group, a selenium-containing group, a phosphorus-containing group or a cyano group, wherein N, O, S, Se and P are each a coordinating atom; F is selected from a nitrogen atom, a nitrogen-containing group, an oxygen-containing group, a sulfur-containing group, a selenium-containing group or a phosphorus-containing group, wherein N, O, S, Se and P are each a coordinating atom; G is selected from C1-C 30 Hydrocarbon, substituted C1-C 30 Hydrocarbon groups or inert functional groups; Y is selected from nitrogen-containing groups, oxygen-containing groups, sulfur-containing groups, selenium-containing groups or phosphorus-containing groups, wherein N, O, S, Se and P are each a coordinating atom; Z is selected from a nitrogen-containing group, an oxygen-containing group, a sulfur-containing group, a selenium-containing group, a phosphorus-containing group or a cyano group, wherein N, O, S, Se and P are each a coordinating atom; — represents a covalent bond or an ionic bond; R 1 To R 4 , R 6 To R 21 are independently selected from hydrogen, C1-C 30 Hydrocarbon, substituted C1-C 30 Hydrocarbon or inert functional group, R 22 To R 31 , R 39 are independently selected from hydrogen, C1-C 30 Hydrocarbon or substituted C1-C 30 Hydrocarbyl groups, the above groups may be the same or different from each other, wherein adjacent groups may be combined with each other to form a bond or a ring; The inert functional group is selected from halogen, oxygen-containing group, nitrogen-containing group, silicon-containing group, germanium-containing group, sulfur-containing group, tin-containing group, C1-C 10 Ester and nitro groups; R 5 Selected from lone pairs of electrons on nitrogen, hydrogen, C1-C 30 Hydrocarbon, substituted C1-C 30 a hydrocarbon group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a selenium-containing group or a phosphorus-containing group; when R 5 When R is an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a selenium-containing group or a phosphorus-containing group, 5 N, O, S, P and Se in can be used as coordination atoms; The substituted C1-C 30 The hydrocarbon group is selected from the group consisting of one or more halogen or C1-C 30 C1-C 30 Hydrocarbon.
7. The preparation method according to claim 1 or 6, characterized in that: The halogen is selected from F, Cl, Br or I; The nitrogen-containing group is selected from -NR 23 R 24 、-T-NR 23 R 24 or -N(O)R 25 R 26 ; The phosphorus-containing group is selected from -PR 28 R 29 、-P(O)R 30 R 31 or -P(O)R 32 (OR 33 ); The oxygen-containing group is selected from hydroxyl, -OR 34 AND-T-OR 34 ; The sulfur-containing group is selected from -SR 35 、-T-SR 35 、-S(O)R 36 or-T-SO2R 37 ; The selenium-containing group is selected from -SeR 38 ,-T-SeR 38 、-Se(O)R 39 or-T-Se(O)R 39 ; The group T is selected from C1-C 30 Hydrocarbon or substituted C1-C 30 Hydrocarbon; R 32 To R 36 , R 38 are independently selected from hydrogen, C1-C 30 Hydrocarbon or substituted C1-C 30 Hydrocarbyl groups, the above groups may be the same or different from each other, wherein adjacent groups may be combined with each other to form a bond or a ring; The R 37 Selected from hydrogen, C1-C 30 Hydrocarbon or substituted C1-C 30 Hydrocarbon; The C1-C 30 The hydrocarbon group is selected from C1-C 30 Alkyl, C7-C 30 Alkyl, C7-C 30 Aralkyl, C3-C 30 Cyclic alkyl, C2-C 30 Alkenyl, C2-C 30 Alkynyl, C6-C 30 Aryl, C8-C 30 Condensed ring or C4-C 30 A heterocyclic group, wherein the heterocyclic group contains 1 to 3 heteroatoms selected from nitrogen atoms, oxygen atoms or sulfur atoms; The silicon-containing group is selected from -SiR 42 R 43 R 44 or-T-SiR 45 ; The germanium-containing group is selected from -GeR 46 R 47 R 48 Or-T-GeR 49 ; The tin-containing group is selected from -SnR 50 R 51 R 52 、-T-SnR 53 or -T-Sn(O)R 54 ; The R 42 To R 54 are independently selected from hydrogen, the aforementioned C1-C 30 Hydrocarbyl or the aforementioned substituted C1-C 30 The above groups may be the same or different from each other, wherein adjacent groups may be combined with each other to form a bond or a ring, and The group T is as defined above.
8. The preparation method according to claim 1, characterized in that: The molar ratio of the magnesium compound calculated as Mg element to the non-metallocene ligand is 1:0.0001-1, the ratio of the magnesium compound to the solvent is 1 mol:75-400 ml, the molar ratio of the magnesium compound calculated as Mg element to the alcohol is 1:0.02-4.00, the mass ratio of the magnesium compound calculated as magnesium compound solid to the porous carrier is 1:0.1-20, the volume ratio of the precipitant to the solvent is 1:0.2-5, and the molar ratio of the magnesium compound calculated as Mg element to the chemical treatment agent calculated as Group IVB metal element is 1:0.01-1.
9. The preparation method according to claim 1, characterized in that: The Group IVB metal compound is selected from one or more of Group IVB metal halides, Group IVB metal alkyl compounds, Group IVB metal alkoxy compounds, Group IVB metal alkyl halides and Group IVB metal alkoxy halides.
10. The preparation method according to claim 2, characterized in that: The aluminoxane is selected from one or more of methylaluminoxane, ethylaluminoxane, isobutylaluminoxane and n-butylaluminoxane, and the alkylaluminum is selected from one or more of trimethylaluminum, triethylaluminum, tripropylaluminum, triisobutylaluminum, tri-n-butylaluminum, triisopentylaluminum, tri-n-pentylaluminum, trihexylaluminum, triisohexylaluminum, diethylmethylaluminum and dimethylethylaluminum.
11. The preparation method according to claim 2, characterized in that: The molar ratio of the magnesium compound calculated as Mg element to the auxiliary chemical treatment agent calculated as Al element is 1:0-1.
0.
12. The preparation method according to claim 1, characterized in that: The precipitant is selected from one or more of alkanes, cycloalkanes, halogenated alkanes and halogenated cycloalkanes.
13. The preparation method according to claim 1, characterized in that: At least one of the following conditions is met: The porous carrier is selected from one or more of partially cross-linked styrene polymers, silicon dioxide, aluminum oxide, magnesium oxide, silicon aluminum oxide, magnesium aluminum oxide, titanium dioxide, molecular sieves and montmorillonite; The solvent is selected from C 6-12 One or more of aromatic hydrocarbons and tetrahydrofuran, wherein the alcohol is selected from one or more of ethanol and butanol; The molar ratio of the magnesium compound calculated as Mg element to the non-metallocene ligand is 1:0.001-0.1, the ratio of the magnesium compound to the solvent is 1 mol:200-250 ml, the molar ratio of the magnesium compound calculated as Mg element to the alcohol is 1:0.10-2.50, the mass ratio of the magnesium compound calculated as magnesium compound solid to the porous carrier is 1:1-5, the volume ratio of the precipitant to the solvent is 1:0.8-1.5, and the molar ratio of the magnesium compound calculated as Mg element to the chemical treatment agent calculated as Group IVB metal element is 1:0.10-0.30; The Group IVB metal compound is selected from one or more of TiCl4, TiBr4, ZrCl4, ZrBr4, HfCl4 and HfBr4; The precipitating agent is selected from one or more of pentane, hexane, heptane, octane, nonane, decane, cyclohexane, cyclopentane, cycloheptane, cyclodecane, cyclononane, dichloromethane, dichlorohexane, dichloroheptane, chloroform, trichloroethane, trichlorobutane, dibromomethane, dibromoethane, dibromoheptane, bromoform, tribromoethane, tribromobutane, chlorocyclopentane, chlorocyclohexane, chlorocycloheptane, chlorocyclooctane, chlorocyclononane, chlorocyclodecane, bromocyclopentane, bromocyclohexane, bromocycloheptane, bromocyclooctane, bromocyclononane and bromocyclodecane.
14. The preparation method according to claim 1, characterized in that: The non-metallocene ligand is selected from one or more compounds having the following chemical formula:
15. A supported non-metallocene catalyst produced by the preparation method according to any one of claims 1 to 14.
16. An olefin polymerization method, characterized in that: The method comprises the steps of using the supported non-metallocene catalyst according to claim 14 as the main catalyst and one or more selected from aluminoxane, alkyl aluminum, halogenated alkyl aluminum, borofluorane, alkyl boron and alkyl boron ammonium salt as the co-catalyst to homopolymerize or copolymerize olefins.
Citation Information
Cited By
Ethylene polymer and preparation method thereof
CN114524893B
Method for continuously producing ultra-high molecular weight polyethylene through slurry polymerization
CN114634587A
Method for continuous production of ultra-high molecular weight polyethylene by slurry polymerization
CN114634587B
Broad-peak distribution polyethylene, and preparation method and application thereof
CN119529152A
Easily-processable ultra-high molecular weight polyethylene and preparation method thereof
CN120157971A