A sandwich insulation operating rod and a preparation method thereof
Through the sandwich structure and molding process, combined with the expansion characteristics of the plastic thermosetting polymer foam core material, the problem of insufficient mechanical strength and excessive weight of the insulated operating rod is solved, and lightweight, high-strength insulation performance and safety are achieved.
Patent Information
- Application Number
- CN201910612921.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2039-07-09
AI Technical Summary
Existing insulated operating rods have problems such as insufficient mechanical strength, excessive weight, and poor insulation performance during high-voltage operations, resulting in potential safety hazards and risks of equipment damage.
The insulated operating rod adopts a sandwich structure. The inner layer is fiberglass prepreg, the interlayer is foam core material, and the outer layer is fiberglass prepreg. The molding process improves the design freedom and mechanics of the fiber cloth laminate structure. performance, combined with the expansion characteristics of the plastic thermosetting polymer foam core material, to achieve lightweight and high-strength insulation performance.
The weight of the operating rod is significantly reduced, the mechanical performance and insulation performance are improved, ensuring safety during operation and long life of the equipment.
Smart Images

Figure CN110254000B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fiber composite molding, and in particular to a sandwich insulating operating rod and a preparation method thereof. Background Art
[0002] During high-voltage operations, it is often necessary to open and close live switches in the lines or handle other matters. Since there is a large voltage difference between the live lines and the operating rods, the operating rods need to have high insulation performance to prevent damage during operation, which would pose a safety hazard to live equipment, power grids and personnel.
[0003] Insulated operating rods (also known as high-voltage pull-off rods, insulating rods, high-voltage operating rods, and commonly known as multi-purpose link rods) can be divided into 10KV, 35KV, 110KV, 220KV, 330KV, and 500KV according to voltage levels. They are applicable products developed according to the production, operation, and maintenance needs of power systems. Insulated operating rods are insulating tools used to operate live equipment in a short period of time, such as connecting or disconnecting high-voltage disconnectors, drop fuses, etc. The insulating operating rod is required to have the advantages of easy operation, flexible structure, good insulation performance, light weight, high mechanical strength, wide application range, easy to carry, and strong moisture resistance.
[0004] At present, the insulating operating rods are generally made of glass fiber epoxy resin rods, which are hand-rolled rods and mechanically pultruded rods.
[0005] One advantage of hand-rolled rods is their high tensile strength, but their longitudinal strength is relatively small compared to pultruded rods. This type of process has a low strength yield, as tiny bubbles between layers during the molding process are difficult to completely eliminate, resulting in incomplete tight bonding between the layers of glass fiber epoxy resin, which can lead to a loss in mechanical strength.
[0006] Secondly, the advantages of mechanical pultruded rods are high strength and high continuous production capacity, but the lateral tension is smaller than that of hand-rolled rods. Due to the pultrusion process, the design freedom of the interlayer laying is insufficient, resulting in a relatively single direction of the internal fiber cloth, which leads to serious various irregularities in the mechanical properties of the rod body and low overall comprehensive strength. Summary of the invention
[0007] In order to overcome the above industry difficulties, the purpose of the present invention is to provide a light and high-strength sandwich insulation operating rod, which can effectively reduce the weight of the operating rod, improve the mechanical properties, and obtain high-quality operating performance.
[0008] To achieve the above purpose, the present invention provides a sandwich insulating operating rod, which is a hollow sandwich structure, from the inside to the outside, the inner layer is glass fiber prepreg cloth, the interlayer is foamed core material, and the outer layer is glass fiber prepreg cloth.
[0009] Furthermore, the volume ratio of the inner layer: the interlayer: the outer layer is (0.1-10): (0.1-5): (1-10). The sandwich insulation operating rod made with this volume ratio has good strength.
[0010] Furthermore, the weight ratio of the glass fiber prepreg is 85-98%, and the weight ratio of the foam core is 2-15%. If the content of the foam core is too little, the weight reduction is not obvious, and if it is too much, the strength decreases significantly. The applicant found that when the weight ratio of the glass fiber prepreg is 85-98% and the weight ratio of the foam core is 2-15%, it can achieve the advantage of obvious weight reduction and meet the strength requirements.
[0011] Furthermore, the outer diameter of the sandwich insulation operating rod is 20-50 mm, and the density is 1.1-2.6 g / cm 3 .
[0012] Further, the glass fiber prepreg is an untwisted E-grade electrical insulation (alkali-free) continuous glass fiber or an untwisted S-grade high mechanical strength (high strength) continuous glass fiber, and the glass fiber prepreg is a unidirectional cloth or a woven cloth, wherein the FAW is 100-400g / m 2 , the RC value of epoxy resin is 32-42%.
[0013] Furthermore, the foam core material refers to a plastic thermosetting polymer composition that can start to expand within a certain temperature range, the starting expansion temperature is 50-200°C, the volume ratio before and after expansion is 1-50 times, and the pressure generated during the expansion process is in the range of 1-20kgf / cm 2 Preferably, the starting expansion temperature of the foam core material is 50-180°C, the volume ratio before and after expansion is 5-20 times, and the pressure generated during the expansion process is in the range of 2-12kgf / cm 2 .
[0014] Further, the preparation method is as follows:
[0015] Cutting: Cut the glass fiber prepreg and foam core material according to the structural dimensions of the sandwich insulation operating rod;
[0016] Rolling: Using the iron core brushed with release agent and iron core glue, rolling glass fiber prepreg cloth according to the mechanical structure design of the sandwich insulation operating rod body, and then rolling the foam core material outside it, and finally rolling the glass fiber prepreg cloth outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg cloth;
[0017] Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down;
[0018] Heating: The mold is placed in a hot environment. During the heating process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg on its periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg is cured and formed during the heating process.
[0019] Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment;
[0020] Obtaining the rough embryo: Cooling to the mold opening temperature, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo;
[0021] Appearance treatment: The rough body is subjected to surface painting to obtain a sandwich structure operating rod body.
[0022] Furthermore, in the heating step, the temperature is 120°C-200°C, and the mold heating time is 10-120 minutes;
[0023] Optionally, in the curing step, the maximum internal expansion force ranges from 0.1 to 100 kgf / cm 2 ;
[0024] Optionally, in the step of obtaining the rough embryo body, the mold opening temperature is 10-80° C. and the cooling time is 10-120 min.
[0025] The present invention also provides a method for preparing the sandwich insulating operating rod, characterized in that:
[0026] Cutting: Cut the glass fiber prepreg and foam core material according to the structural dimensions of the sandwich insulation operating rod;
[0027] Rolling: Using the iron core brushed with release agent and iron core glue, rolling glass fiber prepreg cloth according to the mechanical structure design of the sandwich insulation operating rod body, and then rolling the foam core material outside it, and finally rolling the glass fiber prepreg cloth outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg cloth;
[0028] Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down;
[0029] Heating: The mold is placed in a hot environment. During the heating process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg on its periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg is cured and formed during the heating process.
[0030] Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment;
[0031] Obtaining the rough embryo: Cooling to the mold opening temperature, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo;
[0032] Appearance treatment: The rough body is subjected to surface painting to obtain a sandwich structure operating rod body.
[0033] Furthermore, in the heating step, the temperature is 120°C-200°C, and the mold heating time is 10-120 minutes;
[0034] Optionally, in the curing step, the maximum internal expansion force ranges from 0.1 to 100 kgf / cm 2 ;
[0035] Optionally, in the step of obtaining the rough embryo body, the mold opening temperature is 10-80° C. and the cooling time is 10-120 min.
[0036] The glass fiber material of the outer layer requires absolute insulation and can withstand voltage shock of more than 10KV. The S-grade long fiber has better strength and impact resistance and good insulation. Other materials have not yet achieved this performance and cannot replace the sandwich insulated operating rod involved in the present invention. It has excellent insulation performance and service life and can fully ensure the safety of equipment and personnel during operation.
[0037] Compared with the traditional existing solutions, it has the following significant advantages of light weight and high strength:
[0038] 1. Compared with the traditional solid insulating operating rod, the sandwich structure of the present invention has a lower design density, which can significantly reduce the weight of the product under the same appearance size;
[0039] 2. Compared with the pultrusion process of the traditional solid insulating operating rod, the internal fiber cloth arrangement direction is relatively single, resulting in large differences in the mechanical properties in all directions. The present invention adopts a compression molding process, which can freely design the layer structure of the fiber cloth, effectively compensate for the differences in the mechanical properties in all directions, and thus improve the comprehensive performance of the product.
[0040] 3. When rolling, the foam core material is directly wrapped inside, and no secondary heating is required, so it is formed in one step. It has the effect of saving costs and simplifying the operation procedures. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a cross-sectional view during the preparation process of the sandwich insulation operating rod body of the present invention.
[0042] Figure 2 It is a schematic cross-sectional view of the sandwich insulation operating rod body of the present invention. DETAILED DESCRIPTION
[0043] Embodiments of the present invention are described in detail below, and the examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements with the same or similar functions from beginning to end. The embodiments described below by reference to the accompanying drawings are exemplary, are intended to be used to explain the present invention, and are not to be construed as limitations of the present invention. Those who do not indicate specific techniques or conditions in the embodiments are carried out according to the techniques or conditions described in the documents in this area or according to the product specification. Those who do not indicate the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially.
[0044] A sandwich insulating operating rod, which is a hollow sandwich structure, wherein from inside to outside, the inner layer is glass fiber prepreg cloth, the interlayer is foamed core material, and the outer layer is glass fiber prepreg cloth.
[0045] Furthermore, the volume ratio of the inner layer: the interlayer: the outer layer is (0.1-10): (0.1-5): (1-10).
[0046] Furthermore, the weight ratio of the glass fiber prepreg is 85-98%, and the weight ratio of the foamed core material is 2-15%.
[0047] Furthermore, the outer diameter of the sandwich insulation operating rod is 20-50 mm, and the density is 1.1-2.6 g / cm 3 .
[0048] Further, the glass fiber prepreg is an untwisted E-grade electrical insulation (alkali-free) continuous glass fiber or an untwisted S-grade high mechanical strength (high strength) continuous glass fiber, and the glass fiber prepreg is a unidirectional cloth or a woven cloth, wherein the FAW is 100-400g / m 2 , the RC value of epoxy resin is 32-42%.
[0049] Furthermore, the foam core material refers to a plastic thermosetting polymer composition that can start to expand within a certain temperature range, the starting expansion temperature is 50-200°C, the volume ratio before and after expansion is 1-50 times, and the pressure generated during the expansion process is in the range of 1-20kgf / cm 2 Preferably, the starting expansion temperature of the foam core material is 50-180°C, the volume ratio before and after expansion is 5-20 times, and the pressure generated during the expansion process is in the range of 2-12kgf / cm 2 .
[0050] Further, the preparation method is as follows:
[0051] Cutting: Cut the glass fiber prepreg and foam core material according to the structural dimensions of the sandwich insulation operating rod;
[0052] Rolling: Using the iron core brushed with release agent and iron core glue, rolling glass fiber prepreg cloth according to the mechanical structure design of the sandwich insulation operating rod body, and then rolling the foam core material outside it, and finally rolling the glass fiber prepreg cloth outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg cloth;
[0053] Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down;
[0054] Heating: The mold is placed in a hot environment. During the heating process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg on its periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg is cured and formed during the heating process.
[0055] Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment;
[0056] Obtaining the rough embryo: Cooling to the mold opening temperature, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo;
[0057] Appearance treatment: The rough body is subjected to surface painting to obtain a sandwich structure operating rod body.
[0058] Furthermore, in the heating step, the temperature is 120°C-200°C, and the mold heating time is 10-120 minutes;
[0059] Optionally, in the curing step, the maximum internal expansion force ranges from 0.1 to 100 kgf / cm 2 ;
[0060] Optionally, in the step of obtaining the rough embryo body, the mold opening temperature is 10-80° C. and the cooling time is 10-120 min.
[0061] The foam core material in the following embodiments is produced by Xiamen Haoer New Materials Co., Ltd., and the specific models are HR-312-W, HR-313, HR-313-1, HR-316, HR-318, HR-330 or other core materials that can expand when heated are also applicable.
[0062] The following embodiments are combined with the attached Figure 1 and Figure 2 Here is a schematic diagram to illustrate. 1 is the upper mold, 2 is the glass fiber prepreg cloth, 3 is the foam core material, 4 is the iron core, and 5 is the lower mold.
[0063] Example 1 Preparation of Sandwich Insulated Operating Rod
[0064] Cutting: Cut glass fiber prepreg and foam core material according to the structural size of sandwich insulation operating rod, among which untwisted E-class electrical insulation (alkali-free) continuous glass fiber with FAW of 200g / m 2 ,RC is 35%, foam core material is HR-313, FAW is 200g / m 2 ;
[0065] Rolling: using an iron core (with a diameter of 25 mm and a length of 1.5 m) brushed with a mold release agent and iron core glue, rolling glass fiber prepreg (specifically 5 layers) according to the mechanical structure design of the operating rod body, and then rolling a layer of foam core material outside it, and finally rolling glass fiber prepreg (5 layers) outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg;
[0066] Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down;
[0067] Heating: The mold is placed in a hot environment with an ambient temperature of 150°C and a molding time of 30 minutes. During the heating process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg on the periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg is cured and formed during the heating process.
[0068] Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment;
[0069] Obtaining the rough embryo: Cooling to the mold opening temperature, which is 40°C, the cooling time is 30 minutes, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo;
[0070] Appearance treatment: the appearance of the rough body is treated and painted to obtain a sandwich structure operating rod body.
[0071] The volume ratio of the inner layer: the interlayer: the outer layer in this embodiment is 5:1:5; the total wall thickness is 2.5 mm.
[0072] The weight ratio of the glass fiber prepreg is 95%, and the weight ratio of the foamed core material is 5%.
[0073] The density of the sandwich structure operating rod is 2.0 g / cm 3, with an outer diameter of 30mm, three-point bending is performed in accordance with GB 13398-2008 "Hollow insulating tubes, foam-filled insulating tubes and solid insulating rods for live working", with a width of 1.1m, a breaking load of 2100±15N, and a deflection value of 13.2±0.5mm. Compared with the non-sandwich structure, the operating rod made of pure glass fiber prepreg cloth of the same size is made in a similar way to the sandwich operating rod, except that there is no rolled sandwich material in the middle, and all are rolled with glass fiber prepreg cloth. The weight of the sandwich structure operating rod body obtained in this embodiment is reduced by 23%, and the strength is slightly higher by 3.4%.
[0074] Example 2 Preparation of Sandwich Insulated Operating Rod
[0075] Cutting: Cut glass fiber prepreg and foam core material according to the structural size of the insulating operating rod, among which untwisted S-grade high mechanical strength (high strength) continuous glass fiber FAW is 150g / m 2 ,RC is 35%, foam core material is HR-312, FAW is 250g / m2;
[0076] Rolling: using an iron core (with a diameter of 31 mm and a length of 2.5 m) brushed with a mold release agent and iron core glue, rolling glass fiber prepreg (specifically 3 layers) according to the mechanical structure design of the operating rod body, and then rolling a layer of foam core material outside it, and finally rolling glass fiber prepreg (10 layers) outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg;
[0077] Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down;
[0078] Heating: The mold is placed in a hot environment with an ambient temperature of 135°C and a molding time of 120 minutes. During the heating conduction process, the foamed core material of the sandwich layer is heated and expanded, causing the glass fiber prepreg cloth on the periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg cloth is cured and formed during the heating process.
[0079] Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment;
[0080] Obtaining the rough embryo: Cooling to the mold opening temperature, which is 20°C, the cooling time is 60 minutes, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo;
[0081] Appearance treatment: the appearance of the rough body is treated and painted to obtain a sandwich structure operating rod body.
[0082] The density of the sandwich structure operating rod is 1.85 g / cm 3, with an outer diameter of 36mm, three-point bending is performed in accordance with GB 13398-2008 "Hollow insulating tubes, foam-filled insulating tubes and solid insulating rods for live working", with a width of 1.5m, and a breaking load of 2700±24N, with a deflection value of 22.5±0.7mm. Compared with the non-sandwich structure, the operating rod made of pure glass fiber prepreg of the same size is 16% lighter and 5% stronger.
[0083] Example 3 Preparation of Sandwich Insulated Operating Rod
[0084] Cutting: Cut glass fiber prepreg and foam core material according to the structural size of the insulating operating rod, among which untwisted S-grade high mechanical strength (high strength) continuous glass fiber FAW is 100g / m 2 ,RC32 is %, foam core is HR-318, FAW is 250g / m 2 ;
[0085] Rolling: using an iron core (with a diameter of 31 mm and a length of 2.5 m) brushed with a mold release agent and iron core glue, rolling glass fiber prepreg (specifically 3 layers) according to the mechanical structure design of the operating rod body, and then rolling a layer of foam core material outside it, and finally rolling glass fiber prepreg (10 layers) outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg;
[0086] Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down;
[0087] Heating: The mold is placed in a hot environment with an ambient temperature of 120°C and a molding time of 80 minutes. During the heating process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg on the periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg is cured and formed during the heating process.
[0088] Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment;
[0089] Obtaining the rough embryo: Cooling to the mold opening temperature, which is 20°C, the cooling time is 120 minutes, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo;
[0090] Appearance treatment: the appearance of the rough body is treated and painted to obtain a sandwich structure operating rod body.
[0091] The density of the sandwich structure operating rod is 1.91 g / cm 3, with an outer diameter of 37mm, three-point bending is performed in accordance with GB 13398-2008 "Hollow insulating tubes, foam-filled insulating tubes and solid insulating rods for live working", with a width of 1.5m, and a breaking load of 2750±18N, with a deflection value of 22.1±0.7mm. Compared with the non-sandwich structure, the operating rod made of pure glass fiber prepreg of the same size is 15% lighter and 6% stronger.
[0092] Example 4: Preparation of sandwich insulation operating rod
[0093] Cutting: Cut glass fiber prepreg and foam core material according to the structural size of the insulating operating rod, among which untwisted S-grade high mechanical strength (high strength) continuous glass fiber FAW is 400g / m 2 ,RC42 is %, foam core material is HR-316, FAW is 250g / m 2 ;
[0094] Rolling: using an iron core (with a diameter of 31 mm and a length of 2.5 m) brushed with a mold release agent and iron core glue, rolling a glass fiber prepreg (specifically 1 layer) according to the mechanical structure design of the operating rod body, and then rolling a layer of foam core material outside it, and finally rolling a glass fiber prepreg (10 layers) outside it, to obtain a sandwich structure preform of foam core material and glass fiber prepreg;
[0095] Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down;
[0096] Heating: The mold is placed in a hot environment with an ambient temperature of 200°C and a molding time of 10 minutes. During the heating conduction process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg cloth on the periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg cloth is cured and formed during the heating process.
[0097] Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment;
[0098] Obtaining the rough embryo: Cooling to the mold opening temperature, which is 80°C, the cooling time is 10 minutes, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo;
[0099] Appearance treatment: the appearance of the rough body is treated and painted to obtain a sandwich structure operating rod body.
[0100] The density of the sandwich structure operating rod is 1.75 g / cm 3, with an outer diameter of 35mm, three-point bending is performed in accordance with GB 13398-2008 "Hollow insulating tubes, foam-filled insulating tubes and solid insulating rods for live working", with a width of 1.5m, and a breaking load of 2600±20N, with a deflection value of 21.6±0.7mm. Compared with the non-sandwich structure, the operating rod made of pure glass fiber prepreg of the same size is 18% lighter and 6% stronger.
[0101] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A sandwich insulated operating rod, characterized in that: The sandwich insulated operating rod is a hollow sandwich structure, which is composed of, from inside to outside, an inner layer of glass fiber prepreg cloth, an interlayer of foamed core material, and an outer layer of glass fiber prepreg cloth; the volume ratio of the inner layer: interlayer: outer layer is (0.1-10): (0.1-5): (1-10); the weight ratio of the glass fiber prepreg cloth is 85-98%, and the weight ratio of the foamed core material is 2-15%; the foamed core material refers to a plastic thermosetting polymer composition that can start to expand within a certain temperature range, and its starting expansion temperature is 50-200°C, the volume ratio before and after expansion is 1-50 times, and the pressure range generated during the expansion process is 1-20kgf / cm 2 ; The glass fiber prepreg is an untwisted E-grade electrical insulation (alkali-free) continuous glass fiber or an untwisted S-grade high mechanical strength (high strength) continuous glass fiber, and the glass fiber prepreg is a unidirectional cloth or a woven cloth, wherein the FAW is 100-400g / m 2 , the RC value of epoxy resin is 32-42%; The preparation method is as follows: Cutting: Cut the glass fiber prepreg and foam core material according to the structural dimensions of the sandwich insulation operating rod; Rolling: Using the iron core brushed with release agent and iron core glue, rolling glass fiber prepreg cloth according to the mechanical structure design of the sandwich insulation operating rod body, and then rolling the foam core material outside it, and finally rolling the glass fiber prepreg cloth outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg cloth; Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down; Heating: The mold is placed in a hot environment. During the heating process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg on its periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg is cured and formed during the heating process. Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment; Obtaining the rough embryo: Cooling to the mold opening temperature, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo; Appearance treatment: The rough body is subjected to surface painting to obtain a sandwich structure operating rod body.
2. The sandwich insulated operating rod according to claim 1, characterized in that: The outer diameter of the sandwich insulation operating rod is 20-50 mm; the density is 1.1-2.6 g / cm 3 .
3. The sandwich insulated operating rod according to claim 1, characterized in that: The starting expansion temperature of the foam core material is 50-180°C, the volume ratio before and after expansion is 5-20 times, and the pressure range generated during the expansion process is 2-12kgf / cm 2 .
4. The sandwich insulated operating rod according to claim 1, characterized in that: In the heating step, the temperature is 120°C-200°C, and the mold heating time is 10-120 minutes; Optionally, in the curing step, the maximum internal expansion force ranges from 0.1 to 100 kgf / cm 2 ; Optionally, in the step of obtaining the rough embryo body, the mold opening temperature is 10-80° C. and the cooling time is 10-120 min.
5. A method for preparing the sandwich insulating operating rod according to any one of claims 1 to 4, characterized in that: Cutting: Cut the glass fiber prepreg and foam core material according to the structural dimensions of the sandwich insulation operating rod; Rolling: Using the iron core brushed with release agent and iron core glue, rolling glass fiber prepreg cloth according to the mechanical structure design of the sandwich insulation operating rod body, and then rolling the foam core material outside it, and finally rolling the glass fiber prepreg cloth outside it to obtain a sandwich structure preform of foam core material and glass fiber prepreg cloth; Transferring into the mold: Transfer the preform into the operating rod mold brushed with a release agent, and close the mold up and down; Heating: The mold is placed in a hot environment. During the heating process, the foamed core material of the sandwich layer expands due to the heat, causing the glass fiber prepreg on its periphery to be squeezed and fill the mold cavity. At the same time, the epoxy resin in the glass fiber prepreg is cured and formed during the heating process. Curing and cooling: After the curing and molding is completed, the mold is transferred to a cooling environment; Obtaining the rough embryo: Cooling to the mold opening temperature, opening the mold to take out the product, and pulling out the iron core to obtain the rough embryo; Appearance treatment: The rough body is subjected to surface painting to obtain a sandwich structure operating rod body.
6. The sandwich insulated operating rod according to claim 5, characterized in that: In the heating step, the temperature is 120°C-200°C, and the mold heating time is 10-120 minutes; Optionally, in the curing step, the maximum internal expansion force ranges from 0.1 to 100 kgf / cm 2 ; Optionally, in the step of obtaining the rough embryo body, the mold opening temperature is 10-80° C. and the cooling time is 10-120 min.
Citation Information
Patent Citations
Wind power tower cylinder made of composite materials
CN102705180A
Vacuum thermal expansion molding process for composite
CN105690803A
Composite tubular product for insulation operating lever, and preparation method thereof
CN109427451A
Portable unequal-diameter insulation operating rod
CN202736775U
Sandwich insulation operating rod
CN211000307U