A passivation method for martensitic stainless steel products and a passivation workshop
By using citric acid solution and combining cleaning, leaching, and neutralization processes, the problems of environmental pollution and unstable anti-rust performance of strong acids in the existing technology are solved, and low-cost, safe and reliable martensitic stainless steel passivation is achieved. chemical process to improve anti-rust performance and environmental friendliness.
Patent Information
- Application Number
- CN201910589845.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2039-07-02
AI Technical Summary
The existing passivation process of martensitic stainless steel uses highly corrosive acid, which causes environmental pollution and human hazards, and the anti-rust performance is unstable.
Citric acid solution is used as the passivation liquid, and the passivation film is formed by soaking the stainless steel products. The cleaning, leaching and neutralization processes are combined to ensure the stability and safety of the passivation film.
A low-cost, safe and reliable passivation process is achieved, which improves the anti-rust performance and environmental friendliness of stainless steel products.
Smart Images

Figure CN110257812B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a passivation method for a martensitic stainless steel product and a passivation workshop, belonging to the technical field of stainless steel surface passivation treatment. Background Art
[0002] Passivation is a method of transforming the metal surface into a state that is not easily oxidized, thereby slowing down the corrosion rate of the metal. The passivation of stainless steel materials is to form a very thin, dense, good-covering, and firmly attached passivation film (oxide film) on the metal surface; this film exists as an independent phase, usually a compound of oxygen and metal.
[0003] Martensitic stainless steel products usually have to go through a reasonable passivation process to ensure good rust resistance. A good passivation process can greatly improve the rust resistance of the product. On the contrary, if the passivation treatment is not good, it will cause corrosion and rust in the passivation process, not to mention rust resistance during use.
[0004] The Chinese invention patent, application number 02122917.1, proposes a chemical passivation process for martensitic stainless steel, which mainly uses sulfuric acid (H2SO4), hydrofluoric acid (HF) or nitric acid (HNO3) as the main raw materials, and a certain proportion of sodium dichromate (Na2Cr2O7·2H2O) to make a solution, and then immerses the product in the heated solution. Under the action of strong acid, a passivation film is formed on the surface of the product to achieve the purpose of rust prevention in the later stage.
[0005] The disadvantage of this process is that raw materials such as sulfuric acid and nitric acid are highly corrosive and dangerous to operate. In addition, the acid contains trivalent chromium due to the addition of sodium dichromate. Trivalent chromium and strong acids have a great impact on the environment, and strong acids can easily cause harm to the human body. The martensitic stainless steel products passivated by this process are not stable enough, and the anti-rust performance is average during later use. Summary of the invention
[0006] The object of the present invention is to provide a passivation method and a passivation workshop for a martensitic stainless steel product in view of the above-mentioned problems.
[0007] The technical solution adopted by the present invention is as follows:
[0008] A passivation method for a martensitic stainless steel product, using only a citric acid solution as a passivation solution, includes a passivation process: soaking the stainless steel product in a citric acid solution to form a passivation film on the surface of the stainless steel product. Citric acid is also called citric acid, and its chemical name is 2-hydroxypropane-1,2,3-tricarboxylic acid. Citric acid has two sources, natural and artificial. Citric acid extracted from plants has long been used as a food additive. Citric acid is a common industrial raw material, easy to obtain, and cheap. The present invention only uses a citric acid solution as a passivation solution for stainless steel products, and does not need to add other raw materials such as sodium dichromate, and the impact on the environment is also minimal compared to sulfuric acid, hydrofluoric acid or nitric acid. The passivation method for stainless steel products of the present invention is low in cost, simple and easy to operate, easy to operate, safe and reliable, has little harm to operators, and has little harm to the environment. The passivation film effect of the stainless steel product after passivation treatment is stable, and the anti-rust performance is good during the later use process.
[0009] Optionally, in the passivation process: the soaking temperature is 10°C-75°C, the soaking time is 30min-60min, and the mass fraction of citric acid is 5%-15%.
[0010] Optionally, a cleaning process is also included: using a cleaning agent to clean the stainless steel product to remove impurities on the surface of the stainless steel product. The cleaning agent can be washing powder, detergent and / or degreasing agent.
[0011] Optionally, before the passivation process, a leaching process is also included: the stainless steel product is immersed in an alkaline solution to remove impurities on the surface of the stainless steel product. When combined with the cleaning process, the cleaning process is performed first, followed by the leaching process; the cleaning process can clean most of the oil and other impurities on the surface of the product, and the leaching process can remove the remaining oil and other impurities on the surface of the product. After the cleaning process and the leaching process, the surface of the product is basically free of oil stains or other dirt, which is conducive to ensuring the passivation quality of the product in the passivation process and extending the service life of the passivation solution.
[0012] Preferably, the alkaline solution is a sodium hydroxide solution. Of course, the alkaline solution can also be an alkaline solution such as a calcium hydroxide solution or a potassium hydroxide solution.
[0013] Furthermore, in the leaching process: the immersion temperature is 10°C-75°C, the immersion time is 10min-40min, and the mass fraction of sodium hydroxide is 5%-10%.
[0014] Optionally, after the passivation process, a neutralization process is also included: the stainless steel product is immersed in an alkaline solution to neutralize the residual citric acid on the surface of the stainless steel product. After the passivation process is completed, after the stainless steel product is taken out, some citric acid will inevitably remain on the surface of the stainless steel product. Therefore, as a preferred method, the neutralization process is performed after the passivation process to further ensure the stability of the passivation film.
[0015] Preferably, the alkaline solution is a sodium hydroxide solution. Of course, the alkaline solution can also be an alkaline solution such as a potassium hydroxide solution or a calcium hydroxide solution.
[0016] Furthermore, in the neutralization process: the soaking temperature is 10°C-75°C, the soaking time is 10min-40min, and the mass fraction of sodium hydroxide is 5%-10%.
[0017] Optionally, the stainless steel is austenitic stainless steel, ferritic stainless steel, martensitic stainless steel, duplex stainless steel or precipitation hardening stainless steel. The present invention has strong versatility and can be applied to the passivation of various types of stainless steel, and is particularly suitable for the passivation of martensitic stainless steel products.
[0018] Optionally, the stainless steel product is a martensitic stainless steel product, which has been hardened and heat treated. Citric acid solution, as a passivation solution for martensitic stainless steel products, can also detect the quality of products that have been hardened and heat treated. If the product that has been hardened and heat treated has too much carburization, the product will turn black in the citric acid solution, which can screen out products that do not meet the heat treatment standards, ensure the quality of the products sold, and improve the quality of the products sold by the company.
[0019] A passivation workshop for martensitic stainless steel products, comprising:
[0020] A cleaning tank for holding cleaning agents to clean impurities on the surface of stainless steel products;
[0021] Used in leaching tanks containing alkaline solutions to remove residual impurities on the surface of stainless steel products;
[0022] A passivation tank containing citric acid solution to form a passivation film on the surface of stainless steel products;
[0023] A neutralization tank containing alkaline solution to neutralize the residual citric acid on the surface of stainless steel products; and,
[0024] A plurality of clean water tanks are used to hold clean water, or are provided with water pipes for spraying clean water, so as to clean off the attachments on the surface of the stainless steel products.
[0025] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0026] The passivation method for stainless steel products of the present invention is low in cost, simple and easy to operate, convenient to operate, safe and reliable, has little harm to operators and the environment, and the passivation film effect of the stainless steel products after passivation treatment is stable and has good anti-rust performance during later use. The passivation method of the present invention can be used in the passivation workshop of the present invention to carry out the passivation operation of stainless steel products. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The present invention will now be described by way of example with reference to the accompanying drawings, in which:
[0028] Figure 1 is a flow chart of a method for passivation of a martensitic stainless steel product;
[0029] Figure 2 It is a schematic diagram of the layout of a passivation workshop for martensitic stainless steel products;
[0030] Figure 3 This is a schematic diagram of the layout of another passivation workshop for martensitic stainless steel products;
[0031] Figure 4 It is a schematic diagram of the structure of a leaching tank, a passivation tank or a neutralization tank;
[0032] Figure 5 It is a schematic diagram of the connection relationship among the leaching tank, passivation tank, neutralization tank and waste liquid tank.
[0033] Markings in the figure: 1-cleaning tank, 2-leaching tank, 3-passivation tank, 4-neutralization tank, 5, 5a, 5b, 5c, 5d-clear water tank, 51-water pipe, 6-tank body, 61-heating element, 62-temperature sensor, 7-controller, 8-net bag, 9-waste liquid tank, 91-drain pipe, 10-drying box. DETAILED DESCRIPTION
[0034] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0035] Any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0036] Embodiment 1
[0037] like Figure 1As shown, a passivation method for a martensitic stainless steel product in Example 1 uses only citric acid solution as a passivation solution, including a passivation process: immersing the stainless steel product in a citric acid solution to form a passivation film on the surface of the stainless steel product. Citric acid is also known as citric acid, and its chemical name is 2-hydroxypropane-1,2,3-tricarboxylic acid. Citric acid has two sources, natural and artificial. Citric acid extracted from plants has long been used as a food additive. Citric acid is a common industrial raw material, easy to obtain and cheap. The present invention only uses citric acid solution as a passivation solution for stainless steel products, and does not need to add other raw materials such as sodium dichromate. The impact on the environment is also minimal compared to sulfuric acid, hydrofluoric acid or nitric acid. The passivation method for stainless steel products of the present invention is low in cost, simple and easy to operate, easy to operate, safe and reliable, has little harm to operators, little harm to the environment, and the passivation film effect of the passivated stainless steel product is stable, and the anti-rust performance is good during the later use process.
[0038] In the passivation process: the immersion temperature is 10°C-75°C, the immersion time is 30min-60min, and the mass fraction of citric acid is 5%-15%. The citric acid solution is composed of citric acid and water. In the passivation process, the specific immersion temperature, immersion time and mass fraction of citric acid can be selected according to the actual situation of the stainless steel product. In one embodiment, in the passivation process: the immersion temperature is 10°C, the immersion time is 60min, and the mass fraction of citric acid is 5%. In another embodiment, in the passivation process: the immersion temperature is 45°C, the immersion time is 45min, and the mass fraction of citric acid is 10%. In another embodiment, in the passivation process: the immersion temperature is 75°C, the immersion time is 30min, and the mass fraction of citric acid is 15%.
[0039] Optionally, in one embodiment, a cleaning step is further included: cleaning the stainless steel product with a cleaning agent to remove impurities on the surface of the stainless steel product. The cleaning agent may be washing powder, detergent, or / and degreasing agent.
[0040] Alternatively, in another embodiment, before the passivation process, a leaching process is also included: the stainless steel product is immersed in an alkaline solution to remove impurities on the surface of the stainless steel product. When combined with the cleaning process, the cleaning process is performed first, and then the leaching process is performed; the cleaning process can clean most of the oil and other impurities on the surface of the product, and the leaching process can remove the remaining oil and other impurities on the surface of the product. After the cleaning process and the leaching process, the surface of the product is basically free of oil stains or other dirt, which is conducive to ensuring the passivation quality of the product in the passivation process and extending the service life of the passivation solution.
[0041] Preferably, the alkaline solution is a sodium hydroxide solution. Of course, the alkaline solution can also be an alkaline solution such as a potassium hydroxide solution or a calcium hydroxide solution.
[0042] In the leaching process: the immersion temperature is 10°C-75°C, the immersion time is 10min-40min, and the mass fraction of sodium hydroxide is 5%-10%. The sodium hydroxide solution is composed of sodium hydroxide and water. In the leaching process, the specific immersion temperature, immersion time and mass fraction of sodium hydroxide can be selected according to the actual situation of the stainless steel product. In one embodiment, in the leaching process: the immersion temperature is 10°C, the immersion time is 40min, and the mass fraction of sodium hydroxide is 5%. In another embodiment, in the leaching process: the immersion temperature is 45°C, the immersion time is 25min, and the mass fraction of sodium hydroxide is 7.5%. In another embodiment, in the leaching process: the immersion temperature is 75°C, the immersion time is 10min, and the mass fraction of sodium hydroxide is 10%.
[0043] Alternatively, in another embodiment, after the passivation process, a neutralization process is further included: immersing the stainless steel product in an alkaline solution to neutralize the residual citric acid on the surface of the stainless steel product. After the passivation process is completed, after the stainless steel product is taken out, some citric acid will inevitably remain on the surface of the stainless steel product. Therefore, as a preferred embodiment, the neutralization process is performed after the passivation process to further ensure the stability of the passivation film.
[0044] Preferably, the alkaline solution is a sodium hydroxide solution. Of course, the alkaline solution can also be an alkaline solution such as a calcium hydroxide solution or a potassium hydroxide solution.
[0045] In the neutralization process: the soaking temperature is 10°C-75°C, the soaking time is 10min-40min, and the mass fraction of sodium hydroxide is 5%-10%. The sodium hydroxide solution is composed of sodium hydroxide and water. In the neutralization process, the specific soaking temperature, soaking time and mass fraction of sodium hydroxide can be selected according to the actual situation of the stainless steel product. In one embodiment, in the neutralization process: the soaking temperature is 10°C, the soaking time is 40min, and the mass fraction of sodium hydroxide is 5%. In another embodiment, in the neutralization process: the soaking temperature is 45°C, the soaking time is 25min, and the mass fraction of sodium hydroxide is 7.5%. In another embodiment, in the neutralization process: the soaking temperature is 75°C, the soaking time is 10min, and the mass fraction of sodium hydroxide is 10%.
[0046] Preferably, between each of the above steps, clean water is used to clean off the attachments on the surface of the stainless steel product.
[0047] Optionally, the stainless steel is austenitic stainless steel, ferritic stainless steel, martensitic stainless steel, duplex stainless steel or precipitation hardening stainless steel. The present invention has strong versatility and can be applied to the passivation of various types of stainless steel, and is particularly suitable for the passivation of martensitic stainless steel products.
[0048] Optionally, in one embodiment, the stainless steel product is a martensitic stainless steel product, which has been hardened and heat treated. Citric acid solution, as a passivation solution for martensitic stainless steel products, can also detect the quality of products that have been hardened and heat treated. If the hardened and heat treated product has excessive carburization, the product will turn black in the citric acid solution, which can screen out products that have failed the heat treatment, ensure the quality of the products sold, and improve the quality of the products sold by the enterprise.
[0049] Embodiment 2
[0050] The second embodiment discloses a passivation workshop for martensitic stainless steel products. The passivation method of the first embodiment can be used to perform the passivation operation of the stainless steel products in the second embodiment. The specific solutions contained in the various pools are shown in the first embodiment.
[0051] like Figure 2 , Figure 3 As shown, a passivation workshop for a martensitic stainless steel product in the second embodiment includes:
[0052] A cleaning tank 1 for containing cleaning agents to clean impurities on the surface of the stainless steel product;
[0053] A leaching tank 2 containing an alkaline solution to remove residual impurities on the surface of the stainless steel product;
[0054] A passivation tank 3 containing a citric acid solution to form a passivation film on the surface of the stainless steel product;
[0055] A neutralization tank 4 containing an alkaline solution for neutralizing the residual citric acid on the surface of the stainless steel product; and
[0056] A plurality of clean water tanks 5 are used to hold clean water, or a water pipe 51 is provided on the clean water tank to spray clean water, so as to clean the attached materials on the surface of the stainless steel product. Figure 2 As shown. Alternatively, there may be multiple clean water tanks 5, on which water pipes 51 for spraying clean water are installed. Alternatively, there may be multiple clean water tanks 5, some of which contain clean water, and the remaining clean water tanks are equipped with water pipes 51 for spraying clean water. Alternatively, there may be only one clean water tank 5, on which a water pipe 51 for spraying clean water is installed. Figure 3 shown.
[0057] like Figures 2 to 5 As shown, specifically, in one embodiment, the passivation workshop of the present invention includes:
[0058] A cleaning tank 1 for containing cleaning agent; a leaching tank 2 for containing alkaline solution; a passivation tank 3 for containing citric acid solution; a neutralization tank 4 for containing alkaline solution; and a plurality of clean water tanks 5 for containing clean water, or a plurality of clean water tanks 5 provided with water pipes 51 for spraying clean water; and a drying box 10 for drying stainless steel products.
[0059] The leaching tank 2, the passivation tank 3, and the neutralization tank 4 each include a tank body 6. The tank body 6 of the leaching tank 2 is equipped with a heating element 61 and a temperature sensor 62, and the heating element 61 and the temperature sensor 62 of the leaching tank 2 are connected to a controller 7; the tank body 6 of the passivation tank 3 is equipped with a heating element 61 and a temperature sensor 62, and the heating element 61 and the temperature sensor 62 of the passivation tank 3 are connected to a controller 7; the tank body 6 of the neutralization tank 4 is equipped with a heating element 61 and a temperature sensor 62, and the heating element 61 and the temperature sensor 62 of the neutralization tank 4 are connected to a controller 7; and also includes a plurality of net bags 8 adapted to the tank body 6, and the net bags 8 can be inserted into the tank body 6. Also included is a waste liquid tank 9 for storing old media, and the leaching tank 2, the passivation tank 3, and the neutralization tank 4 are connected to the waste liquid tank 9 through a drain pipe 91, respectively, and a drain valve is installed on the drain pipe 91. The drain valve can be manual or electric. The controller 7, the heating element 61, and the temperature sensor 62 are designed. The heating temperature of the heating element 61 is set by the controller 7 according to actual needs. The temperature sensor 62 can detect the medium temperature in real time and display it through the controller 7. The controller 7 controls the heating temperature of the heating element 61 through the detection signal from the temperature sensor 62, so that the medium temperature in the tank body can be maintained within the required range. The design of the net bag 8 is to place the stainless steel product to be soaked in the net bag 8 and then immerse it in the tank body 6, which is convenient for the stainless steel product to be soaked in the medium and also convenient for the stainless steel product to be taken out from the medium. The design of the waste liquid tank 9 is that when the medium in the leaching tank 2, the passivation tank 3 or the neutralization tank 4 needs to be replaced, the corresponding drain valve on the drain pipe 91 is opened at this time to discharge the old medium (old citric acid solution, old alkaline solution) into the waste liquid tank 9; the acidic and alkaline old medium is accumulated in the waste liquid tank 9 to undergo neutralization reaction. When the waste liquid in the waste liquid tank 9 accumulates to a certain amount, it is transferred to environmental protection treatment.
[0060] When performing passivation operations on stainless steel products:
[0061] The cleaning pool 1 contains a cleaning agent, which may be washing powder, dishwashing liquid and / or degreasing agent, etc.;
[0062] The leaching tank 2 and the neutralization tank 4 are respectively filled with alkaline solutions, wherein the alkaline solution is a sodium hydroxide solution, which is composed of sodium hydroxide and water, and the mass fraction of sodium hydroxide is 5%-10%. The alkaline solution can also be an alkaline solution such as a calcium hydroxide solution or a potassium hydroxide solution.
[0063] The passivation tank 3 is filled with a citric acid solution, which consists of citric acid and water, and the mass fraction of the citric acid is 5%-15%.
[0064] Embodiment 3
[0065] like Figure 1 , Figure 2 , Figure 3 As shown, in the passivation workshop of the second embodiment, the third embodiment adopts the passivation method of the first embodiment to perform the passivation operation on the stainless steel product. The stainless steel product is a martensitic stainless steel ball, which has been hardened and heat treated.
[0066] The steps of passivation operation are as follows:
[0067] Step 1, perform a cleaning process in a cleaning tank 1: use a cleaning agent to clean the stainless steel product to clean off impurities on the surface of the stainless steel product; most of the oil and other impurities on the surface of the product can be cleaned off.
[0068] Step 2: In the clean water tank 5a, use clean water to clean off the cleaning agent attached to the surface of the stainless steel product.
[0069] Step 3, performing a leaching process in the leaching tank 2: immersing the stainless steel product in an alkaline solution to remove impurities on the surface of the stainless steel product; impurities such as residual oil stains on the surface of the product can be removed.
[0070] Step 4: In the clean water tank 5b, clean the alkaline solution attached to the surface of the stainless steel product with clean water.
[0071] Step 5: Perform a passivation process in the passivation tank 3: immerse the stainless steel product in a citric acid solution to form a passivation film on the surface of the stainless steel product.
[0072] Step 6: In the clean water tank 5c, clean the citric acid solution attached to the surface of the stainless steel product with clean water.
[0073] Step 7, performing a neutralization process in the neutralization tank 4: immersing the stainless steel product in an alkaline solution to neutralize the residual citric acid on the surface of the stainless steel product.
[0074] Step 8: In the clean water tank for 5 days, use clean water to clean off the alkaline solution attached to the surface of the stainless steel product.
[0075] Step 9: Dry the stainless steel product using a drying box 10, or wipe the stainless steel product dry using a non-woven fabric.
[0076] After the passivation operation, a stable passivation film is formed on the surface of the martensitic stainless steel ball, which meets the requirements of the salt spray test or copper sulfate test.
[0077] Two sizes of martensitic stainless steel balls after the above passivation operation were subjected to salt spray test.
[0078] The first size of steel ball: 1 / 8 inch diameter, 2 pieces, material 440C, salt spray test standard: ASTM B117-2011, test conclusion is passed, part of the original test report is as follows:
[0079] Test Item Test Method Requirement Result Conclusion Neutral salt spray test / 2H ASTM B117-2011 No red rustappearance after 2 hours No red rustappearance after 2 hours Pass
[0080] The translation of the test report is as follows:
[0081] Test Project Test Standards Require result in conclusion Neutral salt spray test / 2H ASTM B117-2011 After 2 hours, there is no red rust on the surface After 2 hours, there is no red rust on the surface pass
[0082] The second size of steel ball: 1 inch in diameter, 2 in number, made of 440C, salt spray test standard: ASTM B117-2011, test conclusion: passed, part of the original test report is as follows:
[0083] Test Item Test Method Requirement Result Conclusion Neutral salt spray test / 2H ASTM B117-2011 No red rustappearance after 2 hours No red rustappearance after 2 hours Pass
[0084] The translation of the test report is as follows:
[0085] Test Project Test Standards Require result in conclusion Neutral salt spray test / 2H ASTM B117-2011 After 2 hours, there is no red rust on the surface After 2 hours, there is no red rust on the surface pass
[0086] In summary, the passivation method of a martensitic stainless steel product of the present invention is low in cost, simple and easy to operate, convenient to operate, safe and reliable, has little harm to operators and the environment, and the passivation film effect of the stainless steel product after passivation treatment is stable, and the rust-proof performance is good during the later use. The passivation method of the present invention can be used in the passivation workshop of the present invention to carry out the passivation operation of stainless steel products.
[0087] The present invention is not limited to the above-mentioned specific embodiments, but extends to any new features or any new combination disclosed in this specification, as well as any new method or process steps or any new combination disclosed.
Claims
1. A passivation method for a martensitic stainless steel product, characterized in that: For martensitic stainless steel products that have undergone carburizing and hardening heat treatment, the following process is used, including a passivation process: the stainless steel product is immersed in a citric acid solution to form a passivation film on the surface of the stainless steel product, and the product will turn black in the citric acid solution due to excessive carburization of the product that has undergone hardening heat treatment, so as to detect the quality of the product that has undergone hardening heat treatment.
2. A passivation method for a martensitic stainless steel product as claimed in claim 1, characterized in that : In the passivation process: the immersion temperature is 10℃-75℃, the immersion time is 30min-60min, and the mass fraction of citric acid is 5%-15%.
3. A passivation method for a martensitic stainless steel product as claimed in claim 1, characterized in that :Before the passivation process, a cleaning process is also included: the stainless steel product is cleaned with a cleaning agent to remove impurities on the surface of the stainless steel product.
4. A passivation method for a martensitic stainless steel product as claimed in claim 1, characterized in that :Before the passivation process, there is also a leaching process: the stainless steel product is immersed in an alkaline solution to remove impurities on the surface of the stainless steel product.
5. A passivation method for a martensitic stainless steel product as claimed in claim 1, characterized in that : After the passivation process, a neutralization process is also included: the stainless steel product is immersed in an alkaline solution to neutralize the residual citric acid on the surface of the stainless steel product.
6. A passivation method for a martensitic stainless steel product as claimed in claim 4 or 5, characterized in that :The alkaline solution is a sodium hydroxide solution.
7. A passivation method for a martensitic stainless steel product as claimed in claim 6, characterized in that : In the leaching process or in the neutralization process: the immersion temperature is 10°C-75°C, the immersion time is 10min-40min, and the mass fraction of sodium hydroxide is 5%-10%.