Wiring film and method for forming wiring film
By forming an initial layer and a second layer of multi-layer structure wiring films on the substrate, and using sputtering technology in a vacuum atmosphere, the problem of poor crystal orientation on large substrates is solved, and efficient metal atom arrangement and film quality improvement are achieved.
Patent Information
- Application Number
- CN201910291541.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-04-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-12-02
AI Technical Summary
It is difficult to effectively control temperature and vacuum conditions on large substrates with existing technology, resulting in poor crystal orientation of the Al wiring film, and the method of removing moisture from the substrate surface is not clear enough, limiting the stable arrangement of metal atoms and excellent film formation of crystals.
By forming an initial layer with a thickness of 3nm to 200nm on the substrate, and forming a second layer on the initial layer, a wiring film with a multilayer structure is formed. Using sputtering technology in a vacuum atmosphere, the orientation of the crystal is significantly improved and simplified. The process of removing moisture from the surface of a substrate.
It significantly improves the crystal orientation of the wiring film, and easily and effectively forms an excellent multi-layer structure wiring film without relying on temperature control and long-term pressure reduction, improving the stable arrangement of metal atoms and film quality.
Smart Images

Figure CN110364538B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a wiring film and a method for forming the wiring film. Background Art
[0002] In recent years, as the substrates used in display manufacturing have become larger, it has become difficult to maintain the quality of the Al wiring film of displays including TFT (Thin Film Transistor) elements. Indicators of the quality of metal wiring include its crystallinity and orientation to the Al (111) crystal plane in the case of Al wiring (Non-Patent Documents 1, 2).
[0003] When a large substrate is used, uniform and rapid temperature control and vacuuming of the substrate become difficult, and the residual gas partial pressure of moisture, oxygen, nitrogen, etc. becomes high, so the orientation of the crystal becomes poor. When the residual gas partial pressure is high, stacking faults are generated during the growth of the crystal, so that growth nuclei facing different directions are generated. For example, in the case of Al, it is believed that the Al (111) orientation becomes weaker. As a method for improving orientation, it is particularly important to remove the moisture present on the surface of the substrate (Non-patent Document 1, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 3938437
[0007] Non-patent literature
[0008] Non-patent literature 1: Takashi Ito, Thin Film Technology for VLSI, 1986
[0009] Non-patent document 2: S. Vaidya, AK Sinha, Thin Solid Films, Vol. 75, No. 3, January 16, 1981, pp. 253-259 Summary of the invention
[0010] Problems to be solved by the invention
[0011] As a method for removing moisture from the surface of a substrate, it is generally known to set the temperature of the substrate and the pressure in the vacuum tank to appropriate conditions. For example, when the temperature of the substrate is increased, degassing is promoted and the moisture near the surface of the substrate is reduced. In addition, when the pressure in the vacuum tank is reduced, the gas such as moisture in the atmosphere and adsorbed on the substrate is reduced. As a result, the factors that hinder the migration of metal atoms are reduced, and as a result, the metal atoms can be arranged most stably, so the orientation of the crystal is improved.
[0012] However, the relationship between these factors and orientation is not fully understood, and the optimal conditions need to be determined through experiments, and the selection is not easy. In addition, even if the optimal conditions are determined, these factors need to be set within a certain range due to the limitations of device structure and production cycle, and there are limits on improvement.
[0013] In view of the above problems, the present invention provides a wiring film having excellent crystal orientation and a method for forming the wiring film simply and efficiently.
[0014] Means used to solve problems
[0015] The inventors of the present invention discovered that by forming an initial layer with a thickness of 3nm to 200nm on a substrate by sputtering in a vacuum atmosphere, and forming a second layer and subsequent layers on the initial layer, it is possible to obtain a wiring film with a multilayer structure containing metal elements and having excellent crystal orientation, and the present invention was completed based on the above findings.
[0016] That is, the present invention is as follows.
[0017] 1. A wiring film having a multilayer structure provided on a substrate, characterized in that:
[0018] The wiring film comprises:
[0019] an initial layer, which is formed on the substrate, has a thickness of 3 nm to 200 nm, and contains a metal or alloy composed of a metal element, or a compound of the metal or alloy; and
[0020] The second layer and the layers after the second layer are formed on the initial layer and contain a metal or an alloy composed of a metal element, or a compound of a metal or an alloy, and
[0021] The wiring film has an interface between the initial layer and the second layer.
[0022] 2. The wiring film according to item 1 above, wherein main components of the initial layer and the second layer and subsequent layers are the same metal or alloy, or a compound of the metal or alloy.
[0023] 3. The wiring film according to 1 or 2 above, wherein the initial layer is a layer containing oxygen atoms.
[0024] 4. The wiring film according to item 3 above, wherein the interlayer oxygen atom content ratio of the wiring film is 2 or more.
[0025] 5. The wiring film according to item 4 above, wherein the initial layer of the wiring film has an oxygen atom content ratio of 0.02 to 1.5.
[0026] 6. The wiring film according to any one of 1 to 5 above, wherein
[0027] The metal element is at least one selected from the group consisting of Al, Cu, Ti, Mo, C, Si, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, As, Se, Zr, Nb, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, Ta, W, Ir, Pt, Au, Pb, Ru and Bi.
[0028] 7. A wiring film having a multilayer structure including a metal element and provided on a substrate by sputtering in a vacuum atmosphere, wherein:
[0029] The wiring film comprises:
[0030] An initial layer, which is formed on the substrate and has a thickness of 3 nm to 200 nm; and
[0031] The second layer and the layers after the second layer are layers formed on the initial layer after vacuum is evacuated after the initial layer is formed.
[0032] 8. The wiring film according to item 7, wherein:
[0033] The pressure of the initial layer after vacuuming after film formation is 1.0×10 -3 Below Pa.
[0034] 9. A wiring film as described in 7 or 8, wherein the wiring film is composed of a metal or alloy of at least one metal element selected from the group consisting of Al, Cu, Ti, Mo, C, Si, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, As, Se, Zr, Nb, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, Ta, W, Ir, Pt, Au, Pb, Ru and Bi, or a compound of the metal or the alloy.
[0035] 10. The wiring film according to any one of 1 to 9 above, wherein
[0036] The wiring film has a ratio of a largest first diffraction peak to a second largest second diffraction peak among diffraction peaks due to specific crystal planes obtained by X-ray diffraction, that is, first diffraction peak / second diffraction peak, of 5.0 or more.
[0037] 11. A wiring film as described in any one of 1 to 9, wherein the thickness of the wiring film is less than 200 nm, and the ratio of the largest first diffraction peak to the second largest second diffraction peak among the diffraction peaks caused by specific crystal planes obtained by X-ray diffraction of the wiring film, i.e., the first diffraction peak / the second diffraction peak, is greater than 2.3.
[0038] 12. The wiring film according to any one of 1 to 11 above, wherein
[0039] The ratio of the largest first diffraction peak to the second largest second diffraction peak among the diffraction peaks caused by specific crystal planes obtained by X-ray diffraction of the wiring film, i.e., the first diffraction peak / second diffraction peak, is more than 5% larger than the first diffraction peak / second diffraction peak of a wiring film composed of a single layer with the same film thickness and the same composition as the initial layer formed on the substrate by sputtering.
[0040] 13. The wiring film according to any one of 1 to 12 above, wherein the wiring film contains Al or Cu as a main component.
[0041] 14. A wiring film as described in 13, wherein the wiring film is a wiring film with Al as the main component, and the ratio of the diffraction peak caused by the Al(111) crystal plane and the diffraction peak caused by the Al(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Al(111) / Al(200), is greater than 5.0.
[0042] 15. A wiring film as described in 13, wherein the wiring film is a wiring film with Al as the main component, the film thickness of the wiring film is less than 200nm, and the ratio of the diffraction peak caused by the Al(111) crystal plane and the diffraction peak caused by the Al(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Al(111) / Al(200) is greater than 2.3.
[0043] 16. The wiring film according to 13, wherein the wiring film is a wiring film containing Al as a main component, and the half-peak width (2θ) of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction of the wiring film measured under the following conditions is 0.38° or less,
[0044] Installation: Ultima III by Rigaku Corporation, Japan
[0045] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0046] X-ray source: Cu-Kα ray (without using Kβ filter)
[0047] Tube voltage: 40kV
[0048] Tube current: 40mA
[0049] Sampling step: 0.02° / step
[0050] Scanning speed: 1° / min.
[0051] 17. The wiring film according to 13 above, wherein the wiring film is a wiring film containing Al as a main component, and a peak-to-peak distance when a rocking curve of the wiring film is measured at a position of a diffraction peak caused by an Al (111) crystal plane is 15° or less.
[0052] 18. The wiring film according to item 13, wherein the wiring film is a double-layered wiring film having Al as a main component, and the ratio of the intensity of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction measured under the following conditions to the film thickness of the double layer of the wiring film is 5.0 [counts / nm] or more,
[0053] Installation: Ultima III by Rigaku Corporation, Japan
[0054] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0055] X-ray source: Cu-Kα ray (without using Kβ filter)
[0056] Tube voltage: 40kV
[0057] Tube current: 40mA
[0058] Sampling step: 0.02° / step
[0059] Scanning speed: 1° / min.
[0060] 19. A wiring film as described in 13, wherein the wiring film is a wiring film with Al as the main component, and the half-width (2θ) of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction of the wiring film is more than 5% smaller than the half-width (2θ) of the wiring film composed of a single layer with the same film thickness formed on the substrate by sputtering and the same composition as the initial layer.
[0061] 20. A wiring film as described in 13, wherein the wiring film is a wiring film with Cu as the main component, and the ratio of the diffraction peak caused by the Cu (111) crystal plane and the diffraction peak caused by the Cu (200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Cu (111) / Cu (200) is greater than 5.0.
[0062] 21. The wiring film according to item 13, wherein the wiring film is a wiring film containing Cu as a main component, and the half-peak width (2θ) of the diffraction peak caused by the Cu (111) crystal plane obtained by X-ray diffraction of the wiring film measured under the following conditions is 0.38° or less,
[0063] Installation: Ultima III by Rigaku Corporation, Japan
[0064] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0065] X-ray source: Cu-Kα ray (without using Kβ filter)
[0066] Tube voltage: 40kV
[0067] Tube current: 40mA
[0068] Sampling step: 0.02° / step
[0069] Scanning speed: 1° / min.
[0070] 22. A wiring film as described in item 13, wherein the wiring film is a wiring film having Cu as a main component, and the half-width (2θ) of the diffraction peak caused by the Cu (111) crystal plane obtained by X-ray diffraction of the wiring film is more than 5% smaller than the half-width (2θ) of the wiring film composed of a single layer of the same film thickness formed on the substrate by sputtering and having the same composition as the initial layer.
[0071] 23. The wiring film according to any one of 1 to 22, wherein
[0072] The substrate is a glass substrate, a silicon substrate, a quartz substrate, a resin substrate, a ceramic substrate or a metal substrate.
[0073] 24. A method for forming a wiring film having a multilayer structure including a metal element by sputtering in a vacuum atmosphere, wherein the method comprises the following steps:
[0074] A process of forming an initial layer with a thickness of 3 nm to 200 nm on the substrate and then performing vacuuming; and
[0075] A step of forming a second layer and subsequent layers on the initial layer.
[0076] 25. The method according to 24, wherein:
[0077] The pressure of the initial layer after vacuuming after film formation is 1.0×10 -3 Below Pa.
[0078] 26. The method according to 24 or 25, wherein:
[0079] The wiring film includes a metal or alloy of at least one metal element selected from the group consisting of Al, Cu, Ti, Mo, C, Si, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, As, Se, Zr, Nb, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, Ta, W, Ir, Pt, Au, Pb, Ru and Bi, or a compound of the metal or alloy.
[0080] 27. The method according to any one of 24 to 26, wherein:
[0081] The wiring film has a ratio of a largest first diffraction peak to a second largest second diffraction peak among diffraction peaks due to specific crystal planes obtained by X-ray diffraction, that is, first diffraction peak / second diffraction peak, of 5.0 or more.
[0082] 28. The method according to any one of 24 to 26, wherein:
[0083] The wiring film has a thickness of less than 200 nm, and the ratio of the largest first diffraction peak to the second largest second diffraction peak among the diffraction peaks caused by specific crystal planes obtained by X-ray diffraction of the wiring film, i.e., the first diffraction peak / the second diffraction peak is greater than 2.3.
[0084] 29. The method according to any one of 24 to 28, wherein:
[0085] The ratio of the largest first diffraction peak to the second largest second diffraction peak among the diffraction peaks caused by specific crystal planes obtained by X-ray diffraction of the wiring film, i.e., the first diffraction peak / second diffraction peak, is more than 5% larger than the first diffraction peak / second diffraction peak of a wiring film composed of a single layer with the same film thickness and the same composition as the initial layer formed on the substrate by sputtering.
[0086] 30. The method according to any one of 24 to 29, wherein:
[0087] The wiring film contains Al or Cu as a main component.
[0088] 31. The method according to 30, wherein:
[0089] The wiring film is a wiring film with Al as its main component, and the ratio of the diffraction peak caused by the Al(111) crystal plane and the diffraction peak caused by the Al(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Al(111) / Al(200), is greater than 5.0.
[0090] 32. The method according to claim 30, wherein:
[0091] The wiring film is a wiring film with Al as the main component, the film thickness of the wiring film is less than 200nm, and the ratio of the diffraction peak caused by the Al(111) crystal plane and the diffraction peak caused by the Al(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Al(111) / Al(200) is greater than 2.3.
[0092] 33. The method according to claim 30, wherein:
[0093] The wiring film is a wiring film containing Al as a main component, and the half-value width (2θ) of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction of the wiring film measured under the following conditions is 0.38° or less,
[0094] Installation: Ultima III by Rigaku Corporation, Japan
[0095] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0096] X-ray source: Cu-Kα ray (without using Kβ filter)
[0097] Tube voltage: 40kV
[0098] Tube current: 40mA
[0099] Sampling step: 0.02° / step
[0100] Scanning speed: 1° / min.
[0101] 34. The method according to claim 30, wherein:
[0102] The wiring film is a wiring film containing Al as a main component, and a peak-to-peak distance of the wiring film when a rocking curve is measured at a position of a diffraction peak caused by an Al (111) crystal plane is 15° or less.
[0103] 35. The method according to claim 30, wherein:
[0104] The wiring film is a wiring film of a double-layer structure with Al as a main component, and the ratio of the intensity of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction measured under the following conditions to the film thickness of the double layer of the wiring film is 5.0 [counts / nm] or more,
[0105] Installation: Ultima III by Rigaku Corporation, Japan
[0106] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0107] X-ray source: Cu-Kα ray (without using Kβ filter)
[0108] Tube voltage: 40kV
[0109] Tube current: 40mA
[0110] Sampling step: 0.02° / step
[0111] Scanning speed: 1° / min.
[0112] 36. The method according to claim 30, wherein:
[0113] The wiring film is a wiring film with Al as its main component, and the half-width (2θ) of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction of the wiring film is more than 5% smaller than the half-width (2θ) of the wiring film composed of a single layer of the same film thickness formed on the substrate by sputtering and with the same composition as the initial layer.
[0114] 37. The method according to claim 30, wherein:
[0115] The wiring film is a wiring film with Cu as its main component, and the ratio of the diffraction peak caused by the Cu(111) crystal plane and the diffraction peak caused by the Cu(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Cu(111) / Cu(200), is greater than 5.0.
[0116] 38. The method according to claim 30, wherein:
[0117] The wiring film is a wiring film containing Cu as a main component, and the half-peak width (2θ) of the diffraction peak caused by the Cu (111) crystal plane obtained by X-ray diffraction of the wiring film measured under the following conditions is 0.38° or less,
[0118] Installation: Ultima III by Rigaku Corporation, Japan
[0119] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0120] X-ray source: Cu-Kα ray (without using Kβ filter)
[0121] Tube voltage: 40kV
[0122] Tube current: 40mA
[0123] Sampling step: 0.02° / step
[0124] Scanning speed: 1° / min.
[0125] 39. The method according to claim 30, wherein:
[0126] The wiring film is a wiring film with Cu as its main component, and the half-width (2θ) of the diffraction peak caused by the Cu (111) crystal plane obtained by X-ray diffraction of the wiring film is more than 5% smaller than the half-width (2θ) of the wiring film composed of a single layer of the same film thickness formed on the substrate by sputtering and with the same composition as the initial layer.
[0127] 40. The method according to any one of 24 to 39, wherein:
[0128] The substrate is a glass substrate, a silicon substrate, a quartz substrate, a resin substrate, a ceramic substrate or a metal substrate.
[0129] Effects of the Invention
[0130] The crystal orientation of the wiring film of the present invention is significantly improved. In addition, according to the method of the present invention, by forming an initial layer with a film thickness within a specific range on a substrate, and then forming a second layer and subsequent layers on the initial layer, a wiring film including a multilayer structure film is formed, thereby significantly removing water molecules on the substrate during sputtering to form the initial layer, and easily and effectively forming a wiring film with significantly improved crystal orientation without relying on methods such as temperature control of the substrate and reducing pressure for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0131] Figure 1 This is a cross-sectional view for explaining a first example of a sputtering device used in a method according to one embodiment of the present invention.
[0132] Figure 2 (a) to (e) are cross-sectional views for explaining an example of a process for forming a wiring film according to one embodiment of the present invention.
[0133] Figure 3 This is a cross-sectional view for explaining an example of a liquid crystal display device including a wiring film according to one embodiment of the present invention.
[0134] Figure 4 It is a cross-sectional view for explaining a second example of the sputtering device used in the method according to one embodiment of the present invention.
[0135] Figure 5 It is a cross-sectional view for explaining a third example of the sputtering device used in the method according to one embodiment of the present invention.
[0136] Figure 6 (a) to (c) are schematic diagrams showing the process of forming a wiring film by conventional single-layer film formation. Figure 6(d) to (g) are schematic views showing the process of forming a wiring film with a bilayer structure by the method of one embodiment of the present invention.
[0137] Figure 7(a) is a diagram showing a cross-section of the films obtained in Comparative Example 1-1 and Example 1-1 observed by SEM, and Figure 7(b) is an enlarged view of the cross-section of the film obtained in Example 1-1 in Figure 7(a).
[0138] Figure 8 (a) is a diagram showing the surface of the film obtained in Comparative Example 1-1 observed by SEM, Figure 8 (b) is a diagram showing the surface of the film obtained in Example 1-1 observed by SEM.
[0139] Fig. 9 is a diagram showing the results obtained by performing depth-direction analysis from the surface of the Al film toward the glass side on the films obtained in Comparative Example 1-5 and Example 1-7 using XPS.
[0140] Fig.10 is a diagram showing the relationship between the film thickness of the initial layer, the intensity of the diffraction peak caused by the Al(111) crystal plane [hereinafter, also referred to as the Al(111) peak intensity] obtained by X-ray diffraction of the obtained film, and the pressure after evacuation in a film formed into a bilayer so that the total film thickness is 600 nm. Here, the point (プ口ツト) with a film thickness of 600 nm is represented as a single layer.
[0141] Fig.11 is a diagram showing the relationship between the pressure after evacuation and the Al(111) peak intensity obtained by X-ray diffraction of the obtained film in a film formed into a bilayer so that the total film thickness is 600 nm.
[0142] Fig.12 is a diagram showing the relationship between the film thickness of the initial layer, the intensity of the Al(111) peak obtained by X-ray diffraction of the obtained film, and the pressure after evacuation in a film formed into a bilayer so that the total film thickness is 100 nm. Here, the point (プ口ツト) with a film thickness of 100 nm is represented as a single layer.
[0143] Fig.13 is a diagram showing the results obtained by measuring the rocking curve of the Al(111) crystal plane for the films obtained in Comparative Example 1-1 and Example 1-1. Detailed Embodiments
[0144] Hereinafter, a wiring film of one embodiment of the present invention will be described in detail. In this specification, "~" indicating a numerical range is used to mean including the numerical values described before and after it as the lower limit value and the upper limit value, and unless otherwise specified, "~" hereinafter is used with the same meaning.
[0145] [Wiring film]
[0146] A wiring film according to a first aspect of the present invention is a metal film, which is a wiring film of a multilayer structure provided on a substrate, characterized in that the wiring film includes:
[0147] an initial layer, which is formed on the substrate, has a thickness of 3 nm to 200 nm, and contains a metal or alloy composed of a metal element, or a compound of the metal or alloy; and
[0148] The second layer and the layers after the second layer are formed on the initial layer and contain a metal or alloy composed of a metal element, or a compound of a metal or an alloy, and the wiring film has an interface between the initial layer and the second layer. Here, the interface refers to a boundary between the initial layer and the second layer where light and dark in the image become discontinuous when the cross section is observed by reflection electron image observation using a SEM (Scanning Electron Microscopy). The difference in light and dark in the reflection electron image generally means a difference in composition, and these differences mean that there is a difference in the crystal state, that is, a grain boundary where crystal growth becomes discontinuous, and it is inferred that the second layer did not undergo epitaxial growth, but it is not limited to this.
[0149] In addition, an interface is formed between the initial layer and the second layer, and an interface may or may not exist between other layers.
[0150] The wiring film of the first aspect is characterized in that the initial layer is a layer containing oxygen atoms, and the interlayer oxygen atom content ratio of the wiring film is 2 or more.
[0151] Here, the interlayer oxygen atom content ratio refers to a value obtained by measuring the depth distribution using XPS (X-ray Photoelectron Spectroscopy), which is a value obtained by dividing the oxygen atom percentage value of the initial layer by the oxygen atom percentage value in the area after removing the surface air oxidation layer of the second layer and the layers after the second layer.
[0152] The wiring film of the first aspect is characterized in that the oxygen atom content ratio of the initial layer of the wiring film is 0.02 to 1.5.
[0153] Here, the initial layer oxygen atom content ratio is a value obtained by dividing the oxygen atom percentage value in the initial layer by the metal atom percentage value in the initial layer, which is obtained by measuring the depth direction distribution using XPS.
[0154] It is considered that hydrogen atoms accompanying water retention still exist in the initial layer, but hydrogen atoms cannot be captured in XPS, so the oxygen atom detection amount is determined as a value representing the water retention component.
[0155] It is speculated that the interlayer oxygen atom content ratio and the initial layer oxygen atom ratio in the wiring film of the first mode are high because the initial layer is formed while reacting with the moisture attached to the substrate and / or while the moisture is ejected by sputtering, so the water-retaining component of the initial layer is more than that of the second layer formed after the moisture on the glass surface is ejected. Alternatively, it is believed that there is also the following possibility: after the initial layer is formed, the sputtering is stopped and the vacuum is evacuated, so at this time, the surface is oxidized by the trace amount of moisture remaining in the space, so that the oxygen atom content becomes high. Although the film is formed while reacting with the moisture attached to the substrate and / or while the moisture is ejected by sputtering in the case of continuous film formation, in this case, the moisture diffuses into the film, so it is believed that it becomes uniform.
[0156] It should be noted that the possibility of the presence of oxygen not bonded to hydrogen cannot be denied in the above discussion, but the present invention is not affected by this possibility.
[0157] It should be noted that XPS is suitable for measuring the interlayer oxygen atom content ratio and the initial layer oxygen atom ratio, but there is no particular limitation as long as it is a method that can measure the atomic ratio of oxygen to metal in the film. As other methods, for example, cross-sectional SEM-EDX (Scanning Electron Microscopy-Energy Dispersive X-ray Spectroscopy), cross-sectional TEM-EDX (Transmission Electron Microscope-Energy Dispersive X-ray Spectroscopy), Auger electron spectroscopy, RBS (Rutherford Backscattering Spectrometry), D-SIMS (Dynamic-Secondary Ion Mass Spectrometry), etc. can be considered.
[0158] It should be noted that when performing cross-sectional analysis, there is a concern that the cross-sectional layer may be oxidized by air or the like when the cross section is produced. Therefore, it goes without saying that a method for producing a cross section that is not oxidized or a method for obtaining analysis values that eliminates the influence of oxidation when producing the cross section is required.
[0159] The initial layer of the wiring film of the first embodiment contains a metal or alloy composed of a metal element, or a compound of a metal or alloy, preferably a metal or alloy composed of a metal element. In addition, the second layer and subsequent layers of the wiring film of the first embodiment of the present invention contain a metal or alloy composed of a metal element, or a compound of a metal or alloy, preferably a metal or alloy composed of a metal element. Examples of the compound of the metal or alloy include oxides and nitrides of the metal or alloy.
[0160] The metal element is preferably at least one selected from the group consisting of Al, Cu, Ti, Mo, C, Si, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, As, Se, Zr, Nb, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, Ta, W, Ir, Pt, Au, Pb, Ru and Bi, more preferably Al, Cu, Ti, Mo, and further preferably Al or Cu.
[0161] A wiring film according to a second aspect of the present invention is a wiring film having a multilayer structure including metal elements and provided on a substrate by sputtering in a vacuum atmosphere, wherein:
[0162] The wiring film comprises:
[0163] An initial layer, wherein the initial layer is formed on the substrate and has a thickness of 3 nm to 200 nm; and
[0164] The second layer and the layers after the second layer are layers formed on the initial layer after vacuum is evacuated after the initial layer is formed.
[0165] The pressure after vacuuming after the initial layer of the wiring film of the second embodiment is preferably 1.0×10 -3 Pa or less, more preferably 5.0×10 -4 Pa or less, more preferably 3.0×10 -4 The pressure was adjusted to 1.0×10 -3 Pa or less, and then forming the second layer and subsequent layers on the initial layer, thereby improving the crystal orientation of the wiring film.
[0166] The wiring film of the second embodiment is preferably composed of a metal or alloy of at least one metal element selected from the group consisting of Al, Cu, Ti, Mo, C, Si, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, As, Se, Zr, Nb, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, Ta, W, Ir, Pt, Au, Pb, Ru and Bi, or a compound of a metal or an alloy, more preferably composed of a metal or alloy of a metal element of Al, Cu, Ti, Mo, or a compound of a metal or an alloy, further preferably composed of a metal or alloy of a metal element of Al or Cu, or a compound of a metal or an alloy.
[0167] The initial layer of the wiring film of the second embodiment preferably contains a metal or alloy composed of a metal element, or a compound of a metal or alloy, and more preferably contains a metal or alloy composed of a metal element. In addition, the second layer and subsequent layers of the wiring film of the second embodiment of the present invention preferably contain a metal or alloy composed of a metal element, or a compound of a metal or alloy, and more preferably contain a metal or alloy.
[0168] The initial layer and the second layer and subsequent layers of the wiring film of the first embodiment and the second embodiment may have the same composition or different compositions. In addition, the main components of the initial layer and the second layer and subsequent layers may be the same or different, but based on the fact that double-layer processing can be performed using the same target and that etching performed after film formation does not require multiple solutions, it is preferred that the main components are the same from the perspective of improving productivity.
[0169] The wiring films of the first and second embodiments preferably contain Al or Cu as a main component. In the present invention, the main component means an element containing 50 atomic % or more as a main component. Therefore, "containing Al as a main component" means "containing 50 atomic % or more of Al atoms". The wiring films of the first and second embodiments more preferably contain 75 atomic % or more of Al or Cu, further preferably contain 90 atomic % or more of Al or Cu, and particularly preferably consist of Al or Cu.
[0170] The thickness of the initial layer in the wiring film of the first and second embodiments is 3 nm to 200 nm, preferably 4 nm to 100 nm, more preferably 5 nm to 50 nm, and further preferably 10 nm to 30 nm. By setting the thickness of the initial layer to 3 nm to 200 nm, a wiring film having excellent crystal orientation is obtained.
[0171] The film thickness of the initial layer is preferably adjusted according to the film thickness of the wiring film. Specifically, when the film thickness of the wiring film is 200 nm or less, the film thickness of the initial layer is preferably 3 nm or more, more preferably 5 nm or more, and further preferably 10 nm or more. In addition, the film thickness of the initial layer is preferably 50% or less of the film thickness of the wiring film, more preferably 30% or less, and further preferably 10% or less. By setting the film thickness of the initial layer to 3 nm or more and 50% or less of the film thickness of the wiring film, a wiring film having excellent crystal orientation is obtained.
[0172] The thickness of the wiring film in the first and second embodiments is preferably 30 nm to 1000 nm, more preferably 50 nm to 700 nm, and further preferably 100 nm to 400 nm. When the wiring film thickness is 30 nm or more, it is possible to prevent the resistance from increasing due to the influence of surface scattering of electrons, and the film quality can be further improved because the film thickness of the high-quality second layer and the layers after the second layer becomes thicker. In addition, when the film thickness is 1000 nm or less, it is possible to prevent the film from being easily peeled off from the substrate due to film stress, and it is possible to improve production efficiency.
[0173] The total number of layers of the multilayer structure of the wiring film of the first and second aspects is preferably 2 to 10, more preferably 2 to 5, and even more preferably 2 to 4. By setting the total number of layers of the multilayer structure to 2 to 10, it is possible to achieve both improved film quality and reduced tact time in the film forming process.
[0174] The interconnect film of the first aspect preferably has an interlayer oxygen atom content ratio of 2 or more, more preferably 4 or more. When the second layer and subsequent layers contain no oxygen at all, the interlayer oxygen atom content ratio becomes infinite.
[0175] The initial layer oxygen atom content ratio of the wiring film of the first embodiment is preferably 0.02 to 1.5, more preferably 0.02 to 0.5, further preferably 0.02 to 0.3, and particularly preferably 0.03 to 0.15. This can provide a suitable initial layer capable of improving the crystal orientation of the second layer and subsequent layers.
[0176] The ratio of the largest first diffraction peak to the second largest second diffraction peak among the diffraction peaks caused by specific crystal planes obtained by X-ray diffraction of the wiring films of the first and second modes, that is, the first diffraction peak / second diffraction peak is preferably greater than 5.0, more preferably greater than 8.0, further preferably greater than 12.0, and particularly preferably greater than 15.0.
[0177] The thickness of the wiring film of the first and second modes is less than 200 nm, and the ratio of the largest first diffraction peak to the second largest second diffraction peak among the diffraction peaks caused by specific crystal planes obtained by X-ray diffraction of the wiring film, that is, the first diffraction peak / second diffraction peak is preferably greater than 2.3, more preferably greater than 3.5, and further preferably greater than 5.0.
[0178] The ratio of the largest first diffraction peak to the second largest second diffraction peak among the diffraction peaks caused by specific crystal planes obtained by X-ray diffraction of the wiring films of the first and second modes, i.e., the first diffraction peak / the second diffraction peak, is preferably 5% or more larger than the first diffraction peak / the second diffraction peak of a wiring film composed of a single layer of the same film thickness and the same composition as the initial layer formed on the substrate by sputtering, more preferably 10% or more larger, further preferably 20% or more larger, and particularly preferably 40% or more larger.
[0179] The wiring film of the first embodiment and the second embodiment is a wiring film having Al as a main component, and the ratio of the diffraction peak caused by the Al(111) crystal plane to the diffraction peak caused by the Al(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Al(111) / Al(200), is preferably 5.0 or more, more preferably 10.0 or more, and further preferably 15.0 or more. When Al(111) / Al(200) is 5.0 or more, a wiring film with improved orientation can be obtained. The upper limit of Al(111) / Al(200) is not particularly limited, and is typically 50.0 or less.
[0180] The wiring film of the first embodiment and the second embodiment is a wiring film having Al as a main component, the film thickness of the wiring film is 200 nm or less, and the ratio of the diffraction peak caused by the Al(111) crystal plane to the diffraction peak caused by the Al(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Al(111) / Al(200), is preferably 2.3 or more, more preferably 3.5 or more, and further preferably 5.0 or more. When Al(111) / Al(200) is 2.3 or more, a wiring film with improved orientation can be obtained. The upper limit of Al(111) / Al(200) is not particularly limited, and is typically 50.0 or less.
[0181] The wiring film of the first embodiment and the second embodiment is a wiring film having Al as a main component, and when the crystallite size is limited by the half-peak width of the peak caused by the Al (111) crystal plane obtained by X-ray diffraction measured under the following conditions, the half-peak width (2θ) of the diffraction peak is preferably 0.38° or less, more preferably 0.36° or less, and further preferably 0.34° or less. By making the half-peak width (2θ) of the diffraction peak 0.38° or less, a wiring film with improved orientation can be obtained. The lower limit of the half-peak width (2θ) of the diffraction peak is not particularly limited, and is typically 0.30° or more.
[0182] Installation: Ultima III by Rigaku Corporation, Japan
[0183] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0184] X-ray source: Cu-Kα ray (without using Kβ filter)
[0185] Tube voltage: 40kV
[0186] Tube current: 40mA
[0187] Sampling step: 0.02° / step
[0188] Scanning speed: 1° / min
[0189] The wiring film of the first embodiment and the second embodiment is a wiring film with Al as the main component, and the peak distance of the rocking curve (ω scan) about the Al (111) crystal plane is preferably 15 [°] or less, more preferably 12 [°] or less, and further preferably 9 [°] or less. When the peak distance is 15 [°] or less, an oriented film with excellent crystal orientation and reduced dispersion (fluctuation, variation) of the crystal axis is obtained. The lower limit of the peak distance is not particularly limited, and is typically 2 [°] or more.
[0190] Generally, the strength of orientation is often represented by the half-peak width of the rocking curve. In the wiring film of the first mode and the second mode, the rocking curve has two maximum points. Therefore, in the present invention, the peak distance between the two peaks is used instead of the half-peak width to discuss the strength of orientation. For example, the peak distance of the rocking curve is measured as shown below. X-ray diffraction measurement is performed, 2θ is fixed at the position of the diffraction peak caused by the Al (111) crystal plane (the position where the angle 2θ between the X-ray incident direction and the X-ray diffraction direction is 38.5°), and the X-ray diffraction measurement is performed by only changing the angle ω between the incident X-ray and the crystal surface. In the obtained diffraction intensity distribution (rocking curve), the peak distance between each peak when the peak fitting is performed by the pseudo-Voight function so that the waveform becomes a synthetic waveform of the two peaks is used instead of the half-peak width. The peak distance between each peak is preferably less than 15 [°], more preferably less than 12 [°], and further preferably less than 9 [°]. The lower limit of the peak distance is not particularly limited, and is typically greater than 2 [°].
[0191] The wiring film of the first embodiment and the second embodiment is a wiring film of a double-layer structure with Al as a main component, and the ratio of the intensity of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction measured under the following conditions to the film thickness of the double layer of the wiring film is preferably 5.0 [counts / nm] or more, more preferably 7.0 [counts / nm] or more, and further preferably 10.0 [counts / nm] or more. The upper limit of the ratio is not particularly limited, and is typically 30.0 [counts / nm] or less.
[0192] Installation: Ultima III by Rigaku Corporation, Japan
[0193] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0194] X-ray source: Cu-Kα ray (without using Kβ filter)
[0195] Tube voltage: 40kV
[0196] Tube current: 40mA
[0197] Sampling step: 0.02° / step
[0198] Scanning speed: 1° / min
[0199] The wiring film of the first embodiment and the second embodiment is a wiring film containing Al as a main component, and the half-peak width (2θ) of the diffraction peak caused by the Al (111) crystal plane obtained by X-ray diffraction of the wiring film is preferably 5% or more smaller than the half-peak width (2θ) of the wiring film composed of a single layer of the same film thickness and the same composition as the initial layer formed on the substrate by sputtering, more preferably 10% or more smaller, and further preferably 15% or more smaller. By being within the above range, a wiring film with improved crystal orientation can be obtained.
[0200] The wiring film of the first embodiment and the second embodiment is a wiring film having Cu as a main component, and the ratio of the diffraction peak caused by the Cu(111) crystal plane to the diffraction peak caused by the Cu(200) crystal plane obtained by X-ray diffraction of the wiring film, i.e., Cu(111) / Cu(200), is preferably 5.0 or more, more preferably 5.5 or more, and further preferably 6.0 or more. When Cu(111) / Cu(200) is 5.0 or more, a wiring film with improved orientation can be obtained. The upper limit of Cu(111) / Cu(200) is not particularly limited, and is typically 10.0 or less.
[0201] The wiring film of the first embodiment and the second embodiment is a wiring film containing Cu as a main component, and the half-peak width (2θ) of the diffraction peak caused by the Cu (111) crystal plane obtained by X-ray diffraction measured under the following conditions of the wiring film is preferably 0.38° or less, more preferably 0.36° or less, and further preferably 0.34° or less. The lower limit of the half-peak width (2θ) of the diffraction peak is not particularly limited, and is typically 0.30° or more.
[0202] Installation: Ultima III by Rigaku Corporation, Japan
[0203] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0204] X-ray source: Cu-Kα ray (without using Kβ filter)
[0205] Tube voltage: 40kV
[0206] Tube current: 40mA
[0207] Sampling step: 0.02° / step
[0208] Scanning speed: 1° / min
[0209] The wiring film of the first mode and the second mode is a wiring film having Cu as a main component, and the half-peak width (2θ) of the diffraction peak caused by the Cu (111) crystal plane obtained by X-ray diffraction of the wiring film is preferably 5% or more smaller than the half-peak width (2θ) of the wiring film composed of a single layer of the same film thickness and the same composition as the initial layer formed on the substrate by sputtering, more preferably 10% or more smaller, and further preferably 15% or more smaller. By being within the above range, a wiring film with improved crystal orientation can be obtained.
[0210] The wiring film of the first aspect and the second aspect preferably has a substrate that is a glass substrate, a silicon substrate, a quartz substrate, a resin substrate, a ceramic substrate, or a metal substrate.
[0211] [Method for forming wiring film]
[0212] A method in one embodiment of the present invention is a method for forming a wiring film of a multilayer structure containing metal elements by sputtering in a vacuum atmosphere, wherein the method includes the following steps: forming an initial layer with a film thickness of 3nm to 200nm on the substrate and then evacuating the substrate; and forming a second layer and subsequent layers on the initial layer.
[0213] Figure 1 Reference numeral 1 denotes a first example of a sputtering device used in the method according to one embodiment of the present invention. The sputtering device 1 includes a vacuum chamber 2 , and a sputtering target 11 containing a metal element is disposed in the vacuum chamber 2 .
[0214] A vacuum system 9 and a gas introduction system 8 are connected to the vacuum chamber 2. The substrate 21 is held on the substrate holder 7 and then transported to the vacuum chamber 2. The vacuum system 9 is used to evacuate the vacuum chamber 2 to form a vacuum atmosphere.
[0215] The sputtering target 11 is connected to a power source 5 disposed outside the vacuum chamber 2. When the sputtering gas is introduced from the gas introduction system 8, the power source 5 applies a voltage to the sputtering target 11, and plasma is formed near the surface of the sputtering target 11. When the sputtering target 11 is sputtered, particles of the material constituting the sputtering target 11 are released and reach the surface of the substrate 21, as shown in FIG. Figure 2 (b) shows the formation of the initial layer 22.
[0216] The pressure in the vacuum chamber 2 when forming the initial layer 22 is usually 1.0×10 -3 Pa~1.0×10 -7 Pa, preferably 5.0×10 -4 Pa~1.0×10 -6 Pa, more preferably 3.0×10 -4 Pa~1.0×10 -5Pa. The temperature in the vacuum chamber 2 during formation of the initial layer 22 is usually 25°C to 250°C, preferably 75°C to 200°C, and more preferably 100°C to 150°C.
[0217] When the film thickness of the initial layer 22 is formed to be 3nm to 200nm, the voltage application and the introduction of the sputtering gas are stopped. After the initial layer 23 is formed, the vacuum is evacuated, and then the sputtering target 11 is sputtered in the vacuum chamber 2, and the second layer and the subsequent layer 23 are formed on the surface of the initial layer 22. Figure 2 (c)].
[0218] The pressure after vacuuming after forming the initial layer 22 is preferably 1.0×10 -3 Pa or less, more preferably 5.0×10 - 4 Pa or less, more preferably 3.0×10 -4 Pa or less. In this specification, "the pressure after vacuuming after the formation of the initial layer" refers to the pressure after vacuuming after the formation of the initial layer and before the sputtering gas is introduced, that is, just before the second layer is formed. In addition, the temperature in the vacuum chamber 2 when the second layer and the layer 23 after the second layer are formed is usually 25°C to 250°C, preferably 75°C to 200°C, and more preferably 100°C to 150°C.
[0219] When the second layer and the subsequent layers 23 are formed to a predetermined film thickness, the substrate 21 is removed from the sputtering device 1. Figure 2 As shown in (c), a wiring film 24 including an initial layer 22, a second layer, and a layer 23 subsequent to the second layer is formed.
[0220] Then, if Figure 2 As shown in (d), a patterned resist film 26 is disposed on the surface of the wiring film 24, and the wiring film 24 exposed on the bottom surface of the resist film 26 is exposed to an etching liquid such as a weak acid or an etching gas. Figure 2 As shown in (e), a patterned wiring film 25 is formed.
[0221] When the initial layer 22 and the second and subsequent layers 23 have the same main component, etching can be performed using an etching solution (or etching gas) of the same composition, and there is no need to reconfigure the resist film when etching the initial layer 22 .
[0222] In the above example, the initial layer 22, the second layer, and the layer 23 after the second layer are formed in the vacuum chamber 2 of the same sputtering device 1, but the present invention is not limited to this. Figure 4 , 5 As shown, different targets may be sputtered in different vacuum chambers to form the initial layer 22, the second layer, and the layer 23 subsequent to the second layer.
[0223] The substrate 21 is a substrate used in a TFT substrate or a semiconductor device described later, and examples thereof include a glass substrate, a silicon substrate, a quartz substrate, a resin substrate, a ceramic substrate, and a metal substrate.
[0224] If the initial layer 22 and the second and subsequent layers 23 are continuously formed in the same sputtering device 1 , there is no concern that the initial layer 22 and the second and subsequent layers 23 are exposed to the atmosphere, so that the film quality can be improved.
[0225] Figure 4 Reference numeral 80 denotes a sputtering device of the second example, Figure 5 The reference numeral 90 indicates a sputtering device of the third example. The sputtering devices 80 and 90 of the second and third examples include: a first vacuum chamber 2a, a second vacuum chamber 2b connected to the first vacuum chamber 2a, a first sputtering target 11a disposed in the first vacuum chamber 2a, and a second sputtering target 11b disposed in the second vacuum chamber 2b.
[0226] The process of forming a multilayer structure film for a wiring film using the sputtering apparatuses 80 and 90 of the second and third examples will be described.
[0227] First, a vacuum atmosphere is formed in the first and second vacuum chambers 2a and 2b by the vacuum system 9. While maintaining the vacuum atmosphere, the substrate 21 is transported into the first vacuum chamber 2a and held on the substrate holder 7a.
[0228] While the vacuum is being continuously evacuated, sputtering gas is introduced into the first vacuum chamber 2a from the gas introduction system 8, and voltage is applied to the first sputtering target 11a by the power supply 5 to sputter the first sputtering target 11a in a vacuum atmosphere to form an initial layer 22, and then the introduction of the sputtering gas is stopped and the vacuum is evacuated.
[0229] In the sputtering apparatuses 80 and 90 of the second and third examples, different vacuum atmospheres are formed in different vacuum tanks 2a to 2c. Therefore, compared with the case where different vacuum atmospheres are alternately formed in the same vacuum tank 2 as in the sputtering apparatus 1 of the first example, it is not necessary to vacuumize for a long time from the end of forming one film to the formation of the next film. In addition, since the initial layer and the second layer and the layers after the second layer can be formed in each vacuum tank at the same time, the productivity can be improved.
[0230] Furthermore, if the number of vacuum chambers 2a to 2c is equal to the number of layers constituting the multilayer structure of the wiring films 24 and 25 as in the sputtering apparatus 90 of the third example, and each film is formed in a dedicated vacuum chamber 2a to 2c, productivity can be improved.
[0231] The sputtering device 80 of the second example can be as follows Figure 4 As shown, the first and second vacuum chambers 2a and 2b are directly connected, or the first and second vacuum chambers 2a and 2b may be connected to the same transport chamber, and the substrate 21 may be transported in and out between the first and second vacuum chambers 2a and 2b via the transport chamber.
[0232] In addition, the sputtering device 90 of the third example can also be Figure 5 As shown, the first to third vacuum tanks 2a to 2c are connected in series, and the substrate 21 is transported from the first vacuum tank 2a to the third vacuum tank 2c via the second vacuum tank 2b. In addition, the first to third vacuum tanks 2a to 2c can be connected to the same transport chamber, and the substrate 21 can be transported in and out between the first to third vacuum tanks 2a to 2c via the transport chamber.
[0233] In either case, since the substrate 21 is moved between the vacuum chambers without coming into contact with the atmosphere, it is possible to obtain wiring films 24 and 25 having good film quality.
[0234] The substrate 21 with the initial layer 22 formed thereon is carried from the first vacuum chamber 2a to the second vacuum chamber 2b and held on the substrate holder 7b. While the second vacuum chamber 2a is being evacuated, a sputtering gas is introduced to sputter the second sputtering target 11b in a vacuum atmosphere to form the second layer and the subsequent layer 23.
[0235] Figure 6 (a) to (c) are schematic diagrams showing the process of forming a wiring film by conventional single-layer film formation. Figure 6 (d) to (g) are schematic diagrams showing a process of forming a wiring film having a two-layer structure by a method according to one embodiment of the present invention.
[0236] like Figure 6 As shown in (a) and (d), Si-OH groups and water molecules 17 exist near the surface of the substrate 21 before the treatment. Figure 6 As shown in (b) to (c), in conventional single-layer film formation, when a target containing a metal element is sputtered to form a single layer 18 on a substrate 21, due to the interaction between the sputtered metal atoms and the Si-OH groups and adsorbed water molecules, and the influence of the water molecules 17 near the substrate 21 knocked out during sputtering, a wiring film with reduced crystal orientation is obtained.
[0237] In one embodiment of the method of the present invention, an initial layer 22 having a film thickness of 3 nm to 200 nm is formed on a substrate 16 by sputtering in a vacuum atmosphere. Figure 6 (e) to (f)], the film formation is stopped and vacuum is performed, and then the second layer and the subsequent layer 23 are formed on the initial layer 22, thereby forming a wiring film 24 [ Figure 6 (g)].
[0238] It is considered that in the present invention, the water content near the substrate surface is removed to the maximum extent by sputtering the film-forming initial layer 23. Figure 6 (f)] The second layer and subsequent layers are formed on the initial layer 23, thereby improving the crystal orientation and obtaining a high-quality wiring film 24. This assumption can be considered as the reason why the method of one embodiment of the present invention exerts an effect, but the present invention is not limited to this.
[0239] [Electronic devices]
[0240] Next, refer to Figure 3 , a liquid crystal display device is described as an example of an electronic device having the wiring film of the present invention. Figure 3 In FIG. 8 , the liquid crystal display device 3 includes a TFT substrate 75 and a color filter substrate 95 .
[0241] The liquid crystal display device 3 is of an active matrix type, and a TFT substrate 75 includes display pixels 80 , storage capacitors 84 , and TFTs (thin film transistors) 85 on a glass substrate 76 .
[0242] The storage capacitor 84 has a storage electrode 83, the display pixel 80 has a pixel electrode 81, and the TFT 85 has a gate electrode 86, a source electrode 87, and a drain electrode 88. The storage electrode 83, the gate electrode 86, the source electrode 87, and the drain electrode 88 are formed by the wiring films 24 and 25 described above.
[0243] In addition, the TFT 85 includes a gate insulating film 89 , a channel semiconductor layer 91 , a source semiconductor layer 92 , and a drain semiconductor layer 93 .
[0244] A portion of the surface of the drain electrode 88 is exposed and contacts the pixel electrode 81 extending from the display pixel 80. The pixel electrode 81 extends to the portion where the storage capacitor 84 is located, and is arranged opposite to the storage electrode 83 arranged on the glass substrate 76 via an insulating film (gate insulating film 89), and a storage capacitor is formed by the opposing portions.
[0245] The gate electrode 86 and the gate insulating film 89 are disposed on one surface of the channel semiconductor layer 91 between the source semiconductor layer 92 and the drain semiconductor layer 93. The source semiconductor layer 92 and the drain semiconductor layer 93 are in contact with the opposite surface of the channel semiconductor layer 91 with a gap therebetween.
[0246] The source electrode 87 and the drain electrode 88 are in contact with the surfaces of the source semiconductor layer 92 and the drain semiconductor layer 93, respectively. The gate electrode 86 and the source electrode 87 are led out of the TFT 85 so as to be able to apply a voltage from an external power source.
[0247] The TFT 85 and the color filter substrate 95 are arranged at a certain distance, and the liquid crystal 49 is sealed therebetween. The black matrix 97 of the color filter substrate 95 is arranged at a position opposite to the TFT 85, and the color filter 98 is arranged at a position opposite to the display pixel 80. A common electrode 100 is arranged at least at a portion of the color filter substrate 95 opposite to the display pixel 80. The pixel electrode 81 and the common electrode 100 may be, for example, a transparent conductive film such as ITO.
[0248] The TFT substrate 75 has a polarizing plate 94, and the color filter substrate 95 has a polarizing plate 104. When a voltage is applied between the pixel electrode 81 and the common electrode 100 by turning the TFT 85 on and off, the orientation of the liquid crystal 49 on the display pixel 80 changes, thereby changing the polarization direction of light passing through the liquid crystal 49, and controlling the blocking and transmission of light directed to the outside of the liquid crystal display device 3 and irradiated onto the display pixel 80.
[0249] The storage electrode 83 , the gate electrode 86 , the source electrode 87 , and the drain electrode 88 are composed of the wiring films 24 and 25 formed by the present invention, and the initial layer 22 is in contact with the glass substrate 76 or the semiconductor layers 92 and 93 .
[0250] The storage electrode 83 and the gate electrode 86 are in contact with the glass substrate 76 , and the source electrode 87 and the drain electrode 88 are in contact with the semiconductor layer (the source semiconductor layer 92 , the drain semiconductor layer 93 ).
[0251] It should be noted that the electronic device having the wiring film of the present invention is not limited to a liquid crystal display device, and the substrate is not limited to a glass substrate. As long as there is moisture in the surface layer and the crystal growth of the film is hindered, the same effect can be exerted. For example, a semiconductor substrate (silicon substrate), a quartz substrate, a resin substrate, a ceramic substrate, or a metal substrate can also be used as a substrate.
[0252] Example
[0253] Hereinafter, the present invention will be described by way of examples, but the present invention is not limited to these examples. It should be noted that, regarding the measurement results of physical properties in the table, blank columns indicate that the results were not measured.
[0254] [Evaluation method]
[0255] (X-ray diffraction measurement)
[0256] X-ray diffraction was measured using the following apparatus and conditions.
[0257] Installation: Ultima III by Rigaku Corporation, Japan
[0258] Optical system: Parallel beam optical system (PB) [Thin film (normal)]
[0259] X-ray source: Cu-Kα ray (without using Kβ filter)
[0260] Detector: Scintillation counter
[0261] Incident side Sola slit (vertical) opening angle: 5°
[0262] Light receiving side solar slit (horizontal) opening angle: 0.5°
[0263] Tube voltage: 40kV
[0264] Tube current: 40mA
[0265] Attenuator (ATT): Open
[0266] Divergence slit (DS): 1.00mm
[0267] Scattering slit (SS): Open
[0268] Receiving slit (RS): Open
[0269] Scan mode: 2θ / ω scan
[0270] 2θ scanning range: varies depending on the metal constituting the film. In the case of Al film, 37.5° to 39.5° and 44.0° to 45.5°
[0271] Sampling step: 0.02° / step
[0272] Scanning speed: 1° / min
[0273] It should be noted that the values in the tables and graphs are values obtained from the original waveforms without performing various processing (smoothing, BG removal, Kα removal, etc.) on the obtained waveforms.
[0274] (Peak-to-peak distance of the rocking curve)
[0275] X-ray diffraction measurement was performed on the X-ray diffraction pattern. 2θ was fixed at the position of the diffraction peak caused by the Al (111) crystal plane (the position where the angle 2θ formed by the X-ray incident direction and the X-ray diffraction direction was 38.5°), and X-ray diffraction measurement was performed while only the angle ω formed by the incident X-ray and the crystal surface was changed. In the obtained diffraction intensity distribution (rocking curve), the peak distance between the two peaks when the pseudo-Voight function was used to perform peak fitting to make this waveform a synthetic waveform of the two peaks was measured instead of the half-peak width.
[0276] When measuring the rocking curve, the following conditions were changed from those of the above-mentioned 2θ / ω measurement.
[0277] Scan mode: ω scan
[0278] ω range: 3°~33°
[0279] Sampling step: 0.1° / step
[0280] Scanning speed: 3° / min
[0281] It should be noted that the values in the tables and graphs are values obtained from the original waveforms without performing various processing (smoothing, BG removal, Kα removal, etc.) on the obtained waveforms.
[0282] (Dektak film thickness)
[0283] The Dektak film thickness was measured using Dektak150 manufactured by ULVAC under the following conditions.
[0284] Scan type: Standard scan
[0285] Stylus radius: 12.5μmR
[0286] Scan length: 2000 μm
[0287] Time: 13 seconds
[0288] Horizontal resolution: 0.513μm / data point
[0289] Load: 3.00mg
[0290] Vertical measurement range: 6.5μm
[0291] Contour: Hills & Valleys
[0292] (SEM)
[0293] Observation was performed using SU8230 manufactured by Hitachi High-Technologies Corporation at an accelerating voltage of 2.0 kV or 5.0 kV and at magnifications of 22,000 and 100,000.
[0294] (Cross-section SEM film thickness)
[0295] For cross-sectional SEM film thickness, the film thickness is calculated based on the image obtained in the cross-sectional observation of the SEM by comparing it with the scale bar. It should be noted that regarding the method of calculating the film thickness, other methods such as cross-sectional observation of TEM can be used if the film thickness can be calculated with an appropriate resolution.
[0296] (XPS)
[0297] XPS was measured by Quantera-SXM manufactured by ULVAC-PHI under the following conditions.
[0298] X-ray source: monochromatized AlKα rays
[0299] Photoelectron detection angle: 45° to the sample surface
[0300] Pass energy: 140eV
[0301] Step energy: 0.5eV / step
[0302] Sputtering ions: Ar +
[0303] Acceleration voltage of sputtering ions: 1kV
[0304] Grating size of sputtered ions: 2×2mm 2
[0305] For the depth distribution, the sputtering rate of the thermal oxide film (SiO2 film) on the silicon wafer with a known film thickness is calculated in advance, and the converted depth of the thermal oxide film (SiO2 film) on the silicon wafer calculated using this value is used as the horizontal axis of the depth distribution. The measurement interval of the depth distribution is set to be less than 3.0nm in terms of the converted depth of the thermal oxide film (SiO2 film) on the silicon wafer. The sputtering rate of the thermal oxide film (SiO2 film) on the silicon wafer in the embodiment is 2.5nm / minute, and the measurement interval is 2.5nm.
[0306] [Test Example 1] Analysis by X-ray Diffraction
[0307] Example 1-1
[0308] In Example 1-1, as a first example of the sputtering device 1, a vertical in-line sputtering device with a vacuum chamber (manufactured by Shimadzu Corporation) was used to produce a wiring film. The structure of the wiring film 24 of Example 1-1 is as follows: Figure 2 As shown in the cross-sectional view shown in (c), a glass substrate having a size of 40 mm×40 mm×0.5 mm in thickness was used as the substrate 21 .
[0309] (Film formation of initial layer)
[0310] The substrate 21 is held on the substrate holder 7 and then transported into the vacuum chamber 2. The vacuum chamber 2 is evacuated by the vacuum system 9 to a pressure of 5.5×10 -4 Pa, a vacuum atmosphere was formed. A sputtering target made of aluminum (purity: 4N, width in the transport direction: 127 mm, width in the transport orthogonal direction: 559 mm) was used as the sputtering target 11. Ar gas was introduced from the gas introduction system 8 as the sputtering gas while the temperature of the substrate 21 was maintained at 110°C. The pressure was adjusted to 4.0×10 -1When the temperature reaches Pa and becomes stable, the power supply is started, and 2.0 kW of electric power is supplied to the sputtering target 11. The substrate 21 is pre-sputtered for 2 minutes while being placed outside the surface of the sputtering target 11. Then, the substrate 21 is conveyed at a speed of 1347 mm / min through the front of the target, and an initial layer 22 is formed on the substrate 21 by a DC magnetron sputtering method. By forming the film at this conveying speed, the film thickness of the initial layer 22 containing aluminum becomes 20 nm.
[0311] (Film formation of the second layer)
[0312] When the substrate 21 has passed the target, the voltage application and the introduction of the sputtering gas are stopped, and the vacuum is evacuated until the pressure reaches 3.4×10 -4 Pa, and then Ar gas is introduced again from the gas introduction system 8 as a sputtering gas, and the pressure is adjusted to 4.0×10 -1 Pa, then the power supply is started to supply 2.0 kW of electric power to the sputtering target 11 containing aluminum, and the substrate is pre-sputtered for 2 minutes while being placed outside the surface of the sputtering target 11. Then, the substrate passes in front of the target at a conveying speed of 47 mm / min so that the film thickness of the second layer 23 containing aluminum becomes 580 nm, and the second layer 23 is formed on the initial layer 22 by a DC magnetron sputtering method. The introduction of the sputtering gas is stopped at the moment when the substrate 21 has passed in front of the target, and the substrate 21 is transported out of the sputtering device 1 to obtain a wiring film 24 containing the initial layer 22 and the second layer 23. The film forming conditions of Example 1-1 are shown in Table 1.
[0313] Example 1-2
[0314] Under the conditions shown in Table 1, the power supply under the film forming conditions of the initial layer 22 was set to an electric power of 1.0 kW, the conveying speed was set to 1347 mm / min, and the initial layer 22 with a film thickness of 10 nm was formed on the substrate 21. Then, the conveying speed under the film forming conditions of the second layer 23 was set to 46 mm / min, and the second layer 23 with a film thickness of 590 nm was formed on the initial layer 22. Except for this, the same procedure as in Example 1-1 was carried out to obtain a wiring film 24.
[0315] Examples 1-3
[0316] Under the conditions shown in Table 1, the conveying speed under the film forming conditions of the initial layer 22 was set to 540 mm / min, and the initial layer 22 with a film thickness of 50 nm was formed on the substrate 21. Then, the conveying speed under the film forming conditions of the second layer 23 was set to 49 mm / min, and the second layer 23 with a film thickness of 550 nm was formed on the initial layer 22. Except for this, the same procedure as Example 1-1 was carried out to obtain a wiring film 24.
[0317] Examples 1-4
[0318] Under the conditions shown in Table 1, the conveying speed under the film formation conditions of the initial layer 22 was set to 270 mm / min, and the initial layer 22 with a film thickness of 100 nm was formed on the substrate 21. Then, the conveying speed under the film formation conditions of the second layer 23 was set to 54 mm / min, and the second layer 23 with a film thickness of 500 nm was formed on the initial layer 22. Except for this, the same procedure as Example 1-1 was carried out to obtain a wiring film 24.
[0319] Examples 1-5
[0320] Under the conditions shown in Table 1, the power supply under the film forming conditions of the initial layer 22 was set to an electric power of 1.0 kW, the conveying speed was set to 1346 mm / min, and the initial layer 22 with a thickness of 10 nm was formed on the substrate 21. Then, the conveying speed under the film forming conditions of the second layer 23 was set to 302 mm / min, and the second layer 23 with a thickness of 90 nm was formed on the initial layer 22. Except for this, the same procedure as in Example 1-1 was carried out to obtain a wiring film 24.
[0321] Examples 1-6
[0322] Under the conditions shown in Table 1, the conveying speed under the film forming conditions of the initial layer 22 was set to 1345 mm / min, and the initial layer 22 with a film thickness of 20 nm was formed on the substrate 21. Then, the conveying speed under the film forming conditions of the second layer 23 was set to 338 mm / min, and the second layer 23 with a film thickness of 80 nm was formed on the initial layer 22. Except for this, the same procedure as Example 1-1 was carried out to obtain a wiring film 24.
[0323] Examples 1-7
[0324] Under the conditions shown in Table 1, the conveying speed under the film forming conditions of the initial layer 22 was set to 1345 mm / min, and the initial layer 22 with a film thickness of 20 nm was formed on the substrate 21. Then, the conveying speed under the film forming conditions of the second layer 23 was set to 540 mm / min, and the second layer 23 with a film thickness of 50 nm was formed on the initial layer 22. Except for this, the same procedure as Example 1-1 was carried out to obtain a wiring film 24.
[0325] Comparative Example 1-1
[0326] Under the conditions shown in Table 1, a single-layer film was obtained in the same manner as in Example 1-1 except that the conveying speed was set to 45 mm / min and the film was formed to a thickness of 600 nm by one sputtering.
[0327] Comparative Example 1-2
[0328] Under the conditions shown in Table 1, a two-layer film was obtained in the same manner as in Example 1-1 except that the conveying speed during the formation of the initial layer 22 and the second layer 23 was set to 90 mm / min and the films were each formed to a thickness of 300 nm.
[0329] Comparative Examples 1-3
[0330] Under the conditions shown in Table 1, a single-layer film was obtained in the same manner as in Example 1-1 except that the conveying speed was set to 45 mm / min and the film was formed to a thickness of 600 nm by one sputtering.
[0331] Comparative Examples 1-4
[0332] Under the conditions shown in Table 1, a single-layer film was obtained in the same manner as in Example 1-1 except that the conveying speed was set to 271 mm / min and the film was formed to a thickness of 100 nm by one sputtering.
[0333] Comparative Examples 1-5
[0334] Under the conditions shown in Table 1, a single-layer film was obtained in the same manner as in Example 1-1 except that the conveying speed was set to 386 mm / min and the film was formed to a thickness of 70 nm by one sputtering.
[0335] The results of evaluating the test samples obtained in Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-5 by X-ray diffraction are shown in Tables 1, Figures 10 to 13 In Table 1, “-” means not evaluated.
[0336]
[0337] As shown in Table 1, the Al(111) peak intensity of Examples 1-1 to 1-4, which are wiring films of the present invention, is higher than that of Comparative Examples 1-1, 1-3, and 1-4, which are conventional single-layer films. In addition, in Table 1, the Al(111) peak intensity of Comparative Example 1-2, in which the film thickness of the initial layer is greater than 200 nm, is lower than that of Examples 1-1 to 1-4.
[0338] The Al(111) peak intensity indicates the amount (volume) of crystallites oriented to the Al(111) plane. The larger the value of the Al(111) peak intensity, the more the crystal grows, the larger the amount of crystallites, and the more consistent the orientation. Therefore, it can be seen that the crystal orientation of the wiring film of the present invention is superior to that of the comparative example.
[0339] In addition, as shown in Table 1, it can be seen that the Al(111) / Al(200) of Examples 1-1 to 1-5 as the wiring film of the present invention is 5.0 or more, and is composed of high-quality crystals highly oriented to the Al(111) plane. In addition, the ratio of the Al(111) peak intensity to the film thickness of the double layer of Examples 1-1 to 1-5 as the wiring film of the present invention is 5.0 [counts / nm] or more, and the orientation to the Al(111) plane is excellent.
[0340] Fig.10 and Fig.12 This is a graph showing the relationship between the thickness of the initial layer, the Al(111) peak intensity of the obtained film obtained by X-ray diffraction, and the pressure after evacuation. Fig.10 As shown in Tables 1 and 2, although the pressure after vacuuming after the initial layer formation (Example 1-1, Comparative Example 1-2) is the same as the pressure after vacuuming before the single layer formation (Comparative Example 1-1), the Al (111) peak intensity of Example 1-1 is significantly higher than that of Comparative Example 1-1 and Comparative Example 1-2. Fig.12 As shown in the figure, by setting the film thickness of the initial layer to 3 nm to 200 nm or less, it is possible to form a wiring film having excellent crystal orientation without taking a long time to reduce the pressure in the vacuum chamber.
[0341] Fig.11 : is a graph showing the relationship between the pressure after vacuuming and the intensity of the Al(111) peak obtained by X-ray diffraction of the obtained film. Fig.11 As shown, the Al(111) peak intensity of Example 1-1 is significantly higher than that of Comparative Examples 1-1 and 1-3.
[0342] Fig.13 This is a graph showing the results of measuring the rocking curve of the Al(111) crystal plane for the films obtained in Comparative Example 1-1 and Example 1-1. Fig.13 As shown, compared with Comparative Examples 1-1 to 1-5, Examples 1-1 to 1-4 and Example 1-7, which are wiring films of the present invention, have small peak distances of rocking curves, excellent crystal orientation, and reduced dispersion of crystal axes.
[0343] From these results, it is understood that according to the method of the present invention, a wiring film having excellent crystal orientation can be formed without taking a long time to reduce the pressure in the vacuum chamber.
[0344] [Test Example 2] Observation using SEM
[0345] Figure 7(a) and (b), Figure 8(a) and (b) are SEM images of the films obtained in Comparative Example 1-1 and Example 1-1. Figures 7(a) and (b) are cross-sectional views (SEM conditions: 2.0 kV, 22,000 times), and Figure 7(b) is an enlarged view of Example 1-1 in Figure 7(a) (SEM conditions: 2.0 kV, 100,000 times). In addition, Figure 8 (a) and Figure 8 (b) is a diagram obtained by observing the surface of the film obtained in Comparative Example 1-1 and Example 1-1 using SEM (observation conditions: 5.0 kV, 100,000 times). As shown in Figures 7 (a) and (b), the film of Comparative Example 1-1 grows continuously, while on the other hand, the boundary between the initial layer and the second layer of Example 1-1 is clearly present and is discontinuous. By observing the film cross section using SEM in this way, it can be proved that it is the wiring film of the first embodiment and the second embodiment of the present invention. As a proof of the wiring film of the first embodiment and the second embodiment, SEM observation is exemplified, but the proof is not limited to this.
[0346] As shown in Figure 7(a) and (b), Figure 8 As shown in (a) and (b), Example 1-1 shows a tendency that the proportion of large-diameter crystals increases as a whole and the variation of the particle size decreases compared to Comparative Example 1-1. In addition, the surface roughness is reduced.
[0347] [Test Example 3] Analysis using XPS
[0348] Fig. 9 (a) and (b) are graphs showing the results of XPS analysis of the films obtained in Comparative Example 1-5 and Example 1-7 in the depth direction from the Al film surface to the glass side. In addition, Table 2 shows the composition of O and Al at the depth from the surface read from the data.
[0349] In Comparative Example 1-5, the depth of about 0nm to about 10nm is the area where the air oxidation layer of the surface exists, the depth of about 10nm to about 60nm is the area where the single-layer Al film exists, and the depth of about 60nm to about 80nm is the area where the single-layer Al film and glass exist. In the area of about 60nm to about 80nm, the oxygen atomic weight increases. Near the depth of about 50nm, the oxygen atomic weight becomes 0 atomic%. In Example 1-7, the depth of about 0nm to about 10nm is also the area where the air oxidation layer of the surface exists, the depth of about 10nm to about 40nm is the area where the second layer Al film exists, the depth of about 40nm to about 60nm is the area where the second layer Al film and the initial layer exist, and the depth of about 60nm to about 80nm is the area where the initial layer and glass exist. It can be seen that in Example 1-7, the oxygen atomic weight at a depth of about 40nm to about 60nm increases, and near the depth of about 50nm, the oxygen atomic weight shows a maximum value, reaching 5 atomic%. At this time, the interlayer oxygen atom content ratio was 12.5, and the initial layer oxygen atom content ratio was 0.053.
[0350] Thus, it can be seen that the oxygen atomic weight of the initial layer of Example 1-7 is greater than that of the initial layer of Comparative Example 1-5. Such a result is presumed to be because, in Example 1-7, the initial layer is formed while reacting with moisture attached to the substrate and / or while water is ejected by sputtering, and therefore has more water-retaining components than the second layer formed after water is ejected from the glass surface.
[0351] Table 2
[0352]
[0353] [Test Example 4] Analysis by X-ray Diffraction
[0354] Example 2-1
[0355] In Example 2-1, a wiring film was produced using a vertical in-line sputtering apparatus with a vacuum chamber (manufactured by Shimadzu Corporation) as the first example of the sputtering apparatus 1. Under the conditions shown in Table 3, a sputtering target containing molybdenum (purity: 4N, width in the transport direction: 127 mm, width in the direction perpendicular to the transport direction: 559 mm) was used as the sputtering target 11, and a wiring film 24 was obtained in the same manner as in Example 1-1 except that the sputtering target 11 was made.
[0356] Comparative Example 2-1
[0357] Under the conditions shown in Table 3, a single-layer film was obtained in the same manner as in Example 2-1 except that the conveying speed was set to 101 mm / min and the film was formed to a thickness of 300 nm by one sputtering.
[0358] The results of evaluating the obtained test samples by X-ray diffraction are shown in Table 3. The 2θ scanning range of the Mo film was measured in a range covering the positions of diffraction lines from each (hkl) plane of the crystal as shown below.
[0359] Mo(110): 39.0°~41.0°, Mo(211): 73.0°~75.0°
[0360] Table 3
[0361]
[0362] As shown in Table 3, although the pressure after vacuuming after the initial layer formation (Example 2-1) and the pressure after vacuuming before the single layer formation (Comparative Example 2-1) are of the same level, the Mo(110) peak intensity and Mo(110) / Mo(211) of Example 2-1 are significantly higher than those of Comparative Example 2-1. Therefore, it can be seen that according to the method of the present invention, a wiring film with excellent crystal orientation can be formed without taking a long time to reduce the pressure in the vacuum tank.
[0363] [Test Example 5] Analysis by X-ray Diffraction
[0364] Example 3-1
[0365] In Example 3-1, a wiring film was produced using a vertical in-line sputtering apparatus with a vacuum chamber (manufactured by Shimadzu Corporation) as a first example of sputtering apparatus 1. Under the conditions shown in Table 4, a sputtering target made of titanium (purity: 4N, width in the transport direction: 127 mm, width in the direction perpendicular to the transport direction: 559 mm) was used as the sputtering target 11, and a wiring film 24 was obtained in the same manner as in Example 1-1.
[0366] Comparative Example 3-1
[0367] Under the conditions shown in Table 4, a single-layer film was obtained in the same manner as in Example 3-1 except that the conveying speed was set to 73 mm / min and the film was formed to a thickness of 300 nm by one sputtering.
[0368] The results of evaluating the obtained test samples by X-ray diffraction are shown in Table 4. The 2θ scanning range of the Ti film was measured in the range covering the positions of diffraction lines from each (hkl) plane of the crystal as shown below.
[0369] Ti(002): 37.0°~39.0°, Ti(004): 81.5°~83.5°
[0370] Table 4
[0371]
[0372] As shown in Table 4, although the pressure after vacuuming after the initial layer formation (Example 3-1) is about the same as the pressure after vacuuming before the single layer formation (Comparative Example 3-1), the peak intensity of Ti (002) and Ti (002) / Ti (004) of Example 3-1 are significantly higher than those of Comparative Example 3-1. Therefore, it can be seen that according to the method of the present invention, a wiring film with excellent crystal orientation can be formed without taking a long time to reduce the pressure in the vacuum tank.
[0373] [Test Example 6] Analysis by X-ray Diffraction
[0374] Example 4-1
[0375] In Example 4-1, under the conditions shown in Table 5, an in-line sputtering device (manufactured by Nissin Seiki Co., Ltd.) was used, and a sputtering target containing copper (purity: 4N, width in the transport direction: 70 mm, width in the transport direction orthogonal to the transport direction: 200 mm) was used as the sputtering target 11 to obtain a wiring film 24 in the same manner as in Example 1-1.
[0376] Comparative Example 4-1
[0377] Under the conditions shown in Table 5, the conveying speed was set to 66 mm / min, and the film was formed to a thickness of 300 nm by one sputtering. A single-layer film was obtained in the same manner as in Example 4-1.
[0378] Table 5 shows the results of evaluation of the obtained test samples by X-ray diffraction.
[0379] Table 5
[0380]
[0381] As shown in Table 5, it can be seen that the value of Cu(111) / Cu(200) of Example 4-1, which is the wiring film of the present invention, is higher than that of Comparative Example 4-1, and the crystal orientation is excellent.
[0382] While the present invention has been described in detail and with reference to specific embodiments thereof, it will be apparent to one skilled in the art that various changes and modifications can be made therein without departing from the spirit and scope of the present invention.
[0383] This application is based on Japanese Patent Application No. 2018-076267 filed on April 11, 2018 and Japanese Patent Application No. 2019-073658 filed on April 8, 2019, the contents of which are incorporated herein by reference.
Claims
1. A wiring film having a multilayer structure provided on a substrate, characterized in that: The wiring film comprises: an initial layer, which is formed on the substrate, has a thickness of 3 nm to 200 nm, and contains a metal or alloy composed of a metal element, or a compound of the metal or alloy; and The second layer and subsequent layers are formed on the initial layer and contain a metal or alloy composed of a metal element, or a compound of a metal or an alloy, The wiring film has an interface between the initial layer and the second layer, The main components of the initial layer and the second layer and the layers after the second layer are composed of the same metal or alloy, or a compound of the metal or alloy. The initial layer is a layer containing oxygen atoms, the interlayer oxygen atom content ratio is 2 or more, and the initial layer oxygen atom content ratio is 0.03 to 0.15, The wiring film has a ratio of a largest first diffraction peak to a second largest second diffraction peak among diffraction peaks due to specific crystal planes obtained by X-ray diffraction, that is, first diffraction peak / second diffraction peak, of 5.0 or more. 2 . The wiring film according to claim 1 , which is a wiring film of a multilayer structure including a metal element and is provided on a substrate by sputtering in a vacuum atmosphere.
3. The wiring film according to claim 1 or 2, wherein: The wiring film is composed of a metal or alloy of at least one metal element selected from the group consisting of Al, Cu, Ti, Mo, C, Si, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, As, Se, Zr, Nb, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, Ta, W, Ir, Pt, Au, Pb and Bi, or a compound of the metal or alloy.
4. A method for forming a wiring film having a multilayer structure including a metal element by sputtering in a vacuum atmosphere, wherein: The method comprises the following steps: In a vacuum atmosphere, an initial layer with a film thickness of 3 nm to 200 nm is formed on the substrate, and then vacuuming is directly performed; and a step of forming a second layer and subsequent layers on the initial layer, There is an interface between the initial layer and the second layer, The main components of the initial layer and the second layer and the layers after the second layer are composed of the same metal or alloy, or a compound of the metal or alloy. The initial layer is a layer containing oxygen atoms, the interlayer oxygen atom content ratio is 2 or more, and the initial layer oxygen atom content ratio is 0.03 to 0.15, The wiring film has a ratio of a largest first diffraction peak to a second largest second diffraction peak among diffraction peaks due to specific crystal planes obtained by X-ray diffraction, that is, first diffraction peak / second diffraction peak, of 5.0 or more.
5. The method of claim 4, wherein: The pressure of the initial layer after vacuuming after film formation is 1.0×10 -3 Below Pa.
6. The method according to claim 4 or 5, wherein: The wiring film contains a metal or alloy of at least one metal element selected from the group consisting of Al, Cu, Ti, Mo, C, Si, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, As, Se, Zr, Nb, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, Ta, W, Ir, Pt, Au, Pb and Bi, or a compound of the metal or alloy.
Citation Information
Patent Citations
Method for forming a film and method for manufacturing a laminate substrate using the same
CN107130218A
Laminated coating member containing crystal orientated hard coating
JP1998330914A
Low resistivity metallic thin film and liquid crystal display device using the same, and method for manufacturing low resistivity metallic thin film and method for manufacturing liquid crystal display device using the same
JP2002020855A
Sputtering target consisting of high purity aluminum or its alloy
JP2004300565A
Thin film wiring layer
JP2006279022A