Liquid crystal alignment agent, liquid crystal alignment film, liquid crystal element, and methods for producing the same, and optical film
By using a combination of polycarboxylate containing inorganic ions (Mn+) and free polyamic acid, polyamic acid ester and polyimide in the liquid crystal alignment film, combined with water solvent and photo alignment method, the problem of existing liquid crystal alignment film is solved. In order to overcome the problems of insufficient transparency and solvent resistance, a high-performance liquid crystal alignment film was obtained.
Patent Information
- Application Number
- CN201910870200.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-04-14
AI Technical Summary
Conventional water-soluble liquid crystal alignment films have insufficient transparency and solvent resistance for liquid crystal display devices or optical films, making it difficult to prevent deterioration and quality deterioration during the manufacturing process.
Using polycarboxylate containing inorganic ions (Mn+) as the polymer component of the liquid crystal aligning agent, combining free polyamic acid, polyamic acid ester and polyimide, using water as the solvent, forming liquid crystal through coating and photo-alignment methods Orientation film.
A liquid crystal alignment film with excellent liquid crystal orientation, transparency and solvent resistance is realized, and the stability and application performance of the film are improved.
Smart Images

Figure CN110951494B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a liquid crystal alignment agent, a liquid crystal alignment film, an optical film, a liquid crystal element and a polymer. Background Art
[0002] In a liquid crystal display device or an optical film, the transmission of light is controlled by controlling the orientation of liquid crystal molecules. These liquid crystal display devices or optical films include a liquid crystal alignment film that has the function of orienting liquid crystal molecules in a liquid crystal layer in a certain direction. The liquid crystal alignment film is usually formed by applying a liquid crystal alignment agent prepared by dissolving a polymer component in an organic solvent on a substrate surface, preferably by heating the substrate.
[0003] It is proposed that as a solvent component, water or a water-soluble solvent is used to replace an organic solvent, or various liquid crystal alignment agents (for example, with reference to patent documentation 1 or patent documentation 2) as a solvent component together with an organic solvent. In patent documentation 1, it is disclosed that amine compounds such as 1-diethylamino-3-butanone and polyamic acid are formed into a film of a polycarboxylate aqueous solution, and a rubbing treatment is performed to make a liquid crystal alignment film. In addition, in patent documentation 2, it is disclosed that a liquid crystal alignment agent formed by dissolving onium salts such as triethylamine salts of acrylic acid copolymers in water is used, and a liquid crystal alignment film is made by a light orientation method. By using the liquid crystal alignment agent of this water-soluble solvent system, low-temperature calcination can be performed when the film is formed. Thus, there are advantages such as easing the restriction of substrate materials or being friendly to the working environment.
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 8-87017
[0007] [Patent Document 2] Japanese Patent Application Publication No. 2016-224151 Summary of the invention
[0008] [Problems to be solved by the invention]
[0009] The liquid crystal aligning film obtained by using the water-soluble liquid crystal aligning agent of Patent Document 1 or Patent Document 2 does not have sufficient transparency required for use in liquid crystal display devices, optical films, and the like.
[0010] In addition, the liquid crystal alignment film is required to have solvent resistance in order to prevent deterioration or quality degradation during the manufacturing process. Therefore, the liquid crystal alignment film needs to improve solvent resistance while ensuring liquid crystal orientation and transparency.
[0011] The present invention has been made in view of the above-mentioned problems, and a main object of the present invention is to provide a liquid crystal aligning agent capable of obtaining a liquid crystal aligning film having excellent liquid crystal alignment, transparency, and solvent resistance.
[0012] [Technical means to solve the problem]
[0013] In order to solve the above-mentioned problems of the prior art, intensive research has been conducted and it has been found that by containing inorganic ions (M n+ ) as a polymer component of a liquid crystal aligning agent, the above-mentioned problems can be solved, thereby completing the present invention. Specifically, the following means are provided according to the present invention.
[0014] [1] A liquid crystal aligning agent comprising a polymer having a partial structure represented by the following formula (1).
[0015] [Chemistry 1]
[0016]
[0017] (In formula (1), R 1 is a hydrogen atom or a monovalent organic group, X 1 is a tetravalent organic group, X 2 M is a divalent organic group. n+ is an n-valent cation having a typical metal element or a transition metal element. n is an integer greater than 1. m1 is 1 or 2, m2 is 0 or 1, and satisfies m1+m2=2).
[0018] [2] A liquid crystal alignment agent comprising: a polymer selected from at least one of the group consisting of polyamic acid, polyamic acid ester and polyimide; a base having a typical metal element or a transition metal element; and water.
[0019] [3] A liquid crystal alignment film formed using the liquid crystal alignment agent according to [1] or [2].
[0020] [4] An optical film comprising the liquid crystal alignment film according to [3].
[0021] [5] A liquid crystal element comprising the liquid crystal alignment film according to [3].
[0022] [6] A method for producing a liquid crystal alignment agent, comprising mixing at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester and polyimide, a base having a typical metal element or a transition metal element, and water.
[0023] [7] A method for manufacturing a liquid crystal alignment film, comprising: a step of applying the liquid crystal alignment agent of [1] or [2] to a pair of substrates to form a coating film on the pair of substrates; and a step of passivating the surfaces of the pair of substrates on which the coating film is formed.
[0024] [8] A method for manufacturing a liquid crystal element, comprising: a step of applying the liquid crystal alignment agent of [1] or [2] to a pair of substrates respectively and forming a liquid crystal alignment film by irradiating light; and a step of constructing a liquid crystal unit by arranging the pair of substrates on which the liquid crystal alignment film is formed in such a manner that the liquid crystal alignment film faces each other with a liquid crystal layer interposed therebetween.
[0025] [9] A polymer having a partial structure represented by the formula (1).
[0026] [Effects of the Invention]
[0027] According to the liquid crystal alignment agent of the present invention, at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester and polyimide and inorganic ions (M n+ ) can obtain a liquid crystal alignment film having excellent liquid crystal orientation, transparency and solvent resistance. DETAILED DESCRIPTION
[0028] Liquid crystal alignment agent
[0029] The liquid crystal aligning agent of the present disclosure contains a polymer component. Hereinafter, the components contained in the liquid crystal aligning agent and other components arbitrarily prepared as needed will be described.
[0030] In addition, in this specification, the so-called "hydrocarbon group" refers to a meaning including chain hydrocarbon groups, alicyclic hydrocarbon groups and aromatic hydrocarbon groups. The so-called "chain hydrocarbon group" refers to a straight-chain hydrocarbon group and a branched hydrocarbon group whose main chain does not contain a cyclic structure and is only composed of a chain structure. Among them, it can be saturated or unsaturated. The so-called "alicyclic hydrocarbon group" refers to a hydrocarbon group that only contains the structure of alicyclic hydrocarbon as a ring structure and does not contain an aromatic ring structure. Among them, it is not necessary to be composed of only the structure of alicyclic hydrocarbons, and it also includes hydrocarbon groups with a chain structure in part. The so-called "aromatic hydrocarbon group" refers to a hydrocarbon group that contains an aromatic ring structure as a ring structure. Among them, it is not necessary to be composed of only the aromatic ring structure, and it can also contain a chain structure or an alicyclic hydrocarbon structure in part.
[0031] <Polymer component>
[0032] The liquid crystal aligning agent contains a polymer (hereinafter also referred to as “polymer (P)”) having a partial structure represented by the following formula (1).
[0033] [Chemistry 2]
[0034]
[0035] (In formula (1), R 1 is a hydrogen atom or a monovalent organic group, X 1 is a tetravalent organic group, X 2M is a divalent organic group. n+ is an n-valent cation having a typical metal element or a transition metal element. n is an integer greater than 1. m1 is 1 or 2, m2 is 0 or 1, and satisfies m1+m2=2).
[0036] In the formula (1), R 1 Examples of the monovalent organic group include a monovalent hydrocarbon group having 1 to 10 carbon atoms and a monovalent group having a cinnamate structure. 1 A hydrogen atom or an alkyl group having 1 to 6 carbon atoms is preferred.
[0037] X 1 It is a tetravalent group derived from a tetracarboxylic acid derivative and is a residue obtained by removing anhydride groups, carboxyl groups, ester groups and halogenated acyl groups from the tetracarboxylic acid derivative. In addition, in this specification, the so-called "tetracarboxylic acid derivative" refers to the meaning including tetracarboxylic dianhydride, tetracarboxylic acid diester and tetracarboxylic acid diester dihalide.
[0038] X 2 It is a divalent group derived from a diamine compound and is a residue obtained by removing two primary amino groups from the diamine compound.
[0039] About M n+ Specific examples of cations having typical metal elements include: Li + 、Na + , K + , Rb + , Cs + 、Be 2+ Mg 2+ , Ca 2+ , Sr 2+ 、Al 3+ As specific examples of cations having transition metal elements, there are: Sc 3+ 、Ti 4+ 、V 2+ 、V 3+ 、V 4+ 、V 5+ Cr 3+ Cr 4+ Cr 6+ , Mn 2+ , Mn 3+ , Mn 4+ , Fe 2+ , Fe 3+ 、Co 2+ 、Co 3+ 、Ni 2+ , Cu + , Cu 2+ Zu 2+ , Pb 2+ Etc. Among these, Mn+ It is preferably a cation having a typical metal element, more preferably a cation having an alkali metal, and particularly preferably Li + 、Na + , K + , Rb + or Cs + .
[0040] n is preferably 1 to 4, more preferably 1 or 2, and particularly preferably 1.
[0041] The liquid crystal alignment agent containing polymer (P) can be obtained by mixing at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester and polyimide (hereinafter also referred to as "polymer (A)"), a base having a typical metal element or a transition metal element (hereinafter also referred to as "base (B)"), and water. In addition, polymer (A) can also be said to be a precursor of polymer (P).
[0042] (Polyamic acid)
[0043] The polyamic acid can be obtained by reacting tetracarboxylic dianhydride with a diamine compound.
[0044] •Tetracarboxylic dianhydride
[0045] Examples of tetracarboxylic dianhydrides used in the synthesis of polyamic acid include aliphatic tetracarboxylic dianhydrides, alicyclic tetracarboxylic dianhydrides, and aromatic tetracarboxylic dianhydrides. Specific examples of these include aliphatic tetracarboxylic dianhydrides such as 1,2,3,4-butanetetracarboxylic dianhydride;
[0046] Examples of the alicyclic tetracarboxylic dianhydride include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentanetetracarboxylic dianhydride, and cyclohexanetetracarboxylic dianhydride.
[0047] Examples of the aromatic tetracarboxylic dianhydride include pyromellitic dianhydride, 4,4′-(hexafluoroisopropylidene)diphthalic anhydride, ethylene glycol dianhydrotrimellitate, 4,4′-carbonyldiphthalic anhydride, 4,4′-oxydiphthalic anhydride, propane-1,3-diylbis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylate), etc. In addition, the tetracarboxylic dianhydride described in Japanese Patent Laid-Open No. 2010-97188 can be used. In addition, as the tetracarboxylic dianhydride, one type can be used alone or two or more types can be used in combination.
[0048] ·Diamine compounds
[0049] Examples of the diamine compound used in the synthesis of polyamic acid include aliphatic diamines, alicyclic diamines, aromatic diamines, diaminoorganosiloxanes, etc. Specific examples of these diamines include aliphatic diamines such as m-xylylenediamine, 1,3-propylenediamine, and hexamethylenediamine;
[0050] Examples of the alicyclic diamine include 1,4-diaminocyclohexane and 4,4′-methylenebis(cyclohexylamine);
[0051] Examples of the aromatic diamines include hexadecyloxy-2,4-diaminobenzene, octadecyloxy-2,4-diaminobenzene, octadecyloxy-2,5-diaminobenzene, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-3,5-diaminobenzene, cholestanyloxy-2,4-diaminobenzene, cholestanyloxy-2,4-diaminobenzene, 3,5-diaminobenzoic acid cholestanyl ester, 3,5-diaminobenzoic acid cholestanyl ester, 3,5-diaminobenzoic acid octyl ester, ester, 3,6-bis(4-aminobenzoyloxy)cholestane, 3,6-bis(4-aminophenoxy)cholestane, 2,4-diamino-N,N-diallylaniline, 4-(4′-trifluoromethoxybenzoyloxy)cyclohexyl-3,5-diaminobenzoate, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-butylcyclohexane, 3,5-diaminobenzoic acid=5ξ-cholestane-3-yl, the following formula (E-1):
[0052] [Chemistry 3]
[0053]
[0054] (In formula (E-1), X I and X II are independently a single bond, -O-, *-COO- or *-OCO- (wherein "*" indicates the I Bond of I is an alkanediyl group having 1 to 3 carbon atoms, R IIis a single bond or an alkanediyl group having 1 to 3 carbon atoms, a is 0 or 1, b is an integer of 0 to 2, c is an integer of 1 to 20, and d is 0 or 1. (wherein a and b are not 0 at the same time)
[0055] The compound represented by the above, and the side chain type diamine such as the diamine having a photo-alignment group in the side chain:
[0056] p-phenylenediamine, 4,4′-diaminodiphenylmethane, 4-aminophenyl-4-aminobenzoate, 4,4′-diaminoazobenzene, 3,5-diaminobenzoic acid, 1,5-bis(4-aminophenoxy)pentane, 1,2-bis(4-aminophenoxy)ethane, bis[2-(4-aminophenyl)ethyl]adipic acid, N,N-bis(4-aminophenyl)methylamine, 1,4-bis-(4-aminophenyl)-piperazine, N,N′-bis(4-aminophenyl)-benzidine, 2,2′-dimethyl-4,4′-diaminobiphenyl, 2,2′-bis(trifluoromethyl)-4,4′-diaminobiphenyl, 4,4′-diaminodiphenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis(4-aminophenyl) Main chain type diamines such as 1,4-bis(4-aminophenyl)hexafluoropropane, 4,4′-(phenylene diisopropylidene) dianiline, 1,4-bis(4-aminophenoxy)benzene, 4,4′-bis(4-aminophenoxy)biphenyl, 4,4′-[4,4′-propane-1,3-diylbis(piperidin-1,4-diyl)]diphenylamine, 4,4′-diaminobenzanilide, 4,4′-diaminostilbene, 4,4′-diaminodiphenylamine, 1,3-bis(4-aminophenethyl)urea, 1,3-bis(4-aminobenzyl)urea, 1,4-bis(4-aminophenyl)-piperazine, N-(4-aminophenylethyl)-N-methylamine, N,N′-bis(4-aminophenyl)-N,N′-dimethylbenzidine, and diamines having a photo-alignment group in the main chain;
[0057] Examples of the diaminoorganosiloxane include 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, and in addition thereto, diamines described in JP-A-2010-97188 can be used.
[0058] Synthesis of polyamic acid
[0059] Polyamic acid can be obtained by reacting tetracarboxylic dianhydride and diamine compound, optionally with a molecular weight modifier (such as acid monoanhydride or monoamine, etc.). The ratio of tetracarboxylic dianhydride and diamine compound used in the synthesis reaction of polyamic acid is preferably 0.2 to 2 equivalents of the anhydride group of tetracarboxylic dianhydride relative to 1 equivalent of the amino group of the diamine compound.
[0060] The synthesis reaction of polyamic acid is preferably carried out in an organic solvent. The reaction temperature at this time is preferably -20°C to 150°C, and the reaction time is preferably 0.1 hour to 24 hours. As the organic solvent used in the reaction, for example, aprotic polar solvents, phenolic solvents, alcohols, ketones, esters, ethers, halogenated hydrocarbons, hydrocarbons, etc. can be cited. A particularly preferred organic solvent is preferably one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphoric triamide, metacresol, dimethyl phenol and halogenated phenol as a solvent, or a mixture of one or more of these organic solvents and other organic solvents (such as butyl cellosolve, diethylene glycol diethyl ether, etc.). The amount (a) of the organic solvent used is preferably set to an amount in which the total amount (b) of tetracarboxylic dianhydride and diamine is 0.1% by mass to 50% by mass relative to the total amount (a+b) of the reaction solution.
[0061] (Polyamic acid ester)
[0062] Polyamic acid esters can be obtained, for example, by the following methods: [I] a method of reacting the polyamic acid obtained by the synthesis reaction with an esterifying agent; [II] a method of reacting a tetracarboxylic acid diester with a diamine compound; [III] a method of reacting a tetracarboxylic acid diester dihalide with a diamine compound, etc. The polyamic acid ester contained in the liquid crystal aligning agent may have only an amic acid ester structure, or may be a partially esterified product in which an amic acid structure and an amic acid ester structure coexist.
[0063] (Polyimide)
[0064] Polyimide can be obtained, for example, by imidizing the polyamic acid synthesized in the manner described above by dehydration and ring closure. From the viewpoint of making the solubility in water or a water-soluble organic solvent better, the imidization rate of the polyimide is preferably 80% or less, more preferably 50% or less. The lower limit of the imidization rate is not particularly limited, preferably 20% or more, more preferably 30% or more. In addition, the imidization rate is expressed as a percentage of the number of imide ring structures relative to the total number of amic acid structures and the number of imide ring structures of the polyimide. A part of the imide ring may also be an isoimide ring.
[0065] The dehydration ring-closure of polyamic acid is preferably carried out by the following method, that is, polyamic acid is dissolved in an organic solvent, a dehydrating agent and a dehydration ring-closure catalyst are added to the solution, and heating is performed as needed. In the method, as a dehydrating agent, for example, anhydrides such as acetic anhydride, propionic anhydride, and trifluoroacetic anhydride can be cited. Relative to 1 mol of the amic acid structure of polyamic acid, the amount of the dehydrating agent used is preferably set to 0.01 mol to 20 mol. As a dehydration ring-closure catalyst, for example, tertiary amines such as pyridine, trimethylpyridine, dimethylpyridine, and triethylamine can be used. Relative to 1 mol of the dehydrating agent used, the amount of the dehydration ring-closure catalyst used is preferably set to 0.01 mol to 10 mol. As an organic solvent used in the dehydration ring-closure reaction, an organic solvent exemplified as an organic solvent used in the synthesis of polyamic acid can be cited. The reaction temperature of the dehydration ring-closure reaction is preferably 0°C to 180°C. The reaction time is preferably 1.0 hour to 120 hours.
[0066] (Photo-aligning group)
[0067] The polymer (P) may be a polymer having a photo-alignment group. In the above case, the organic film formed using the liquid crystal alignment agent may be given a liquid crystal alignment ability by a photo-alignment method, which is preferred in this regard. Here, the photo-alignment group refers to a functional group that can impart anisotropy to the film by a photo-isomerization reaction, a photo-dimerization reaction, a photo-Fries rearrangement reaction, or a photolysis reaction using light irradiation.
[0068] Specific examples of the photo-alignment group include: an azobenzene-containing group containing azobenzene or a derivative thereof as a basic skeleton, a cinnamic acid structure-containing group containing cinnamic acid or a derivative thereof (cinnamic acid structure) as a basic skeleton, a chalcone-containing group containing chalcone or a derivative thereof as a basic skeleton, a benzophenone-containing group containing benzophenone or a derivative thereof as a basic skeleton, a coumarin-containing group containing coumarin or a derivative thereof as a basic skeleton, a cyclobutane-containing structure containing cyclobutane or a derivative thereof as a basic skeleton, a stilbene-containing group using stilbene or a derivative thereof as a basic skeleton, a phenyl benzoate-containing group containing phenyl benzoate or a derivative thereof as a basic skeleton, and the like. Among these, the photo-aligning group is preferably at least one selected from the group consisting of an azobenzene-containing group, a cinnamic acid structure-containing group, a chalcone-containing group, a stilbene-containing group, a cyclobutane-containing structure, and a phenyl benzoate-containing group. In terms of high sensitivity to light and easy introduction into a polymer, a cinnamic acid structure-containing group or a cyclobutane-containing structure is preferred.
[0069] The polymer with a photo-orientation group can be obtained, for example, by using the polymerization of a monomer with a photo-orientation group. The proportion of the photo-orientation group in the polymer (A) (i.e., the proportion of the photo-orientation group in the polymer (P)) is appropriately set according to the type of the photo-orientation group in order to give the desired liquid crystal orientation ability to the coating film, for example, in the case of a base containing a cinnamic acid structure, relative to all constituent units of the polymer with the photo-orientation group, preferably set to 5 mol% or more, more preferably set to 10 mol% to 80 mol%. In the case where the photo-orientation group is a cyclobutane-containing structure, relative to all constituent units of the polymer with the photo-orientation group, it is preferred that the proportion of the photo-orientation group is set to 10 mol% or more, more preferably set to 15 mol% to 80 mol%.
[0070] Regarding the solution viscosity of the polymer used in the preparation of the liquid crystal alignment agent, when a solution with a concentration of 10% by mass is prepared, it is preferably a solution viscosity of 10mPa·s to 800mPa·s, and more preferably a solution viscosity of 15mPa·s to 500mPa·s. In addition, the solution viscosity (mPa·s) is a value obtained by measuring a polymer solution with a concentration of 10% by mass prepared using a good solvent for the polymer (γ-butyrolactone, N-methyl-2-pyrrolidone, etc.) at 25°C using an E-type rotational viscometer.
[0071] The weight average molecular weight (Mw) of the polymer (A) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, more preferably 2,000 to 300,000. In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of Mw to the number average molecular weight (Mn) in terms of polystyrene measured by GPC is preferably 7 or less, more preferably 5 or less.
[0072] (Base (B))
[0073] The base (B) is a cation (M) containing a typical metal element or a transition metal element. n+ ) and a counterion.
[0074] Examples of the counter ions possessed by the base (B) include halide ions, inorganic acid ions, and organic acid ions. Specific examples of these include halide ions, fluoride ions (F - ), chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - )wait;
[0075] Examples of inorganic acid ions include hydroxide ions, bicarbonate ions, carbonate ions, sulfate ions, hydrogensulfate ions, phosphate ions, hydrogenphosphate ions, dihydrogenphosphate ions, phosphinate ions, nitrate ions, borate ions, sulfite ions, hypochlorite ions, perchlorate ions, thiocyanate ions, and hydrofluorate ions;
[0076] Examples of the organic acid ion include acetate ion, trimethylacetate ion, trifluoroacetate ion, trifluoromethanesulfonate ion, tetraphenylborate ion, alkoxide ions having 1 to 10 carbon atoms (methoxy ion, ethoxy ion, propoxy ion, n-butoxy ion, tert-butoxy ion, 2-methyl-2-butoxy ion, etc.), propionate ion, butyrate ion, formate ion, lactate ion, citrate ion, succinate ion, oxalate ion, tartrate ion, fumarate ion, maleate ion, malonate ion, aniline ion, benzoate ion, glycine ion, pyridinium ion, phenol ion, anilinosulfonate ion, thiocarboxylate ion, methylsulfinate ion, methylsulfate ion, ethylsulfate ion, amidesulfate ion, valerate ion, and dodecylbenzenesulfonate ion.
[0077] In terms of obtaining a liquid crystal alignment film with higher liquid crystal orientation, the base (B) is preferably a weak base. Here, in this specification, the so-called weak base refers to a salt of a weak acid with a pKa of 4 or more in water at 25°C. As weak acids with a pKa of 4 or more, there are: carboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, and benzoic acid; alcohols with 1 to 10 carbon atoms such as methanol, ethanol, propanol, n-butanol, tert-butanol, and 2-methyl-2-butanol; inorganic acids such as boric acid, carbonic acid, and formic acid. In the case where the counter ion is a weak acid ion, it is particularly preferred to be an ion derived from one of the groups consisting of an inorganic acid and an alcohol with 1 to 10 carbon atoms.
[0078] As the base (B), it is preferred to use a salt of an alkali metal and a weak acid in order to improve the liquid crystal orientation, transparency, and solvent resistance of the alignment film to be obtained in a balanced manner.
[0079] The base (B) is preferably used in an amount of 10 to 150 mol parts, more preferably 20 to 120 mol parts, and even more preferably 20 to 100 mol parts, relative to 100 mol parts of all monomer units of the polymer (A). In addition, the base (B) may be used alone or in combination of two or more.
[0080] (Solvent)
[0081] The liquid crystal aligning agent disclosed in the present invention is an aqueous polymer composition containing water as a solvent component. In this case, the amount of organic solvent used can be reduced, and a liquid crystal aligning agent with better environmental and safety aspects can be obtained, which is preferred.
[0082] As the solvent component, water can be used alone, but from the viewpoint of making the polymer more soluble in the solvent and having good coating properties on the substrate, it is preferred to prepare a mixed solvent of a water-soluble solvent having a lower surface tension than water (hereinafter also referred to as "solvent Q") and water, and particularly preferred is a mixed solvent of water and alcohol.
[0083] As solvent Q, preferably, a compound in which the hydrogen atom of a chain hydrocarbon in which methylene can be replaced by -O- or -COO- is substituted by a hydroxyl group, for example, alcohols such as methanol, ethanol, n-propanol, isopropanol, diacetone alcohol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, butyl cellosolve (ethylene glycol monobutyl ether), propylene glycol monoethyl ether, 1-hexanol, and 4-methyl-2-pentanol; esters such as ethyl lactate and butyl lactate. When solvent Q is used in combination, the proportion of water used is preferably set to 20% by mass or more, more preferably set to 40% to 95% by mass, and further preferably set to 60% to 90% by mass, relative to the total amount of the solvent contained in the liquid crystal aligning agent.
[0084] As the solvent, a solvent other than water and solvent Q (hereinafter also referred to as "other organic solvent") may be used in combination. Examples of other organic solvents include aprotic polar solvents such as N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, 3-butoxy-N,N-dimethylpropionamide, and 3-methoxy-N,N-dimethylpropionamide;
[0085] Ketone solvents such as 4-hydroxy-4-methyl-2-pentanone, diisobutyl ketone, ethylene carbonate, and propylene carbonate;
[0086] Ether solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diisoamyl ether, tetrahydrofuran, etc.;
[0087] Ester solvents such as butyl acetate, methyl methoxypropionate, ethyl ethoxypropionate, isoamyl propionate, isoamyl isobutyrate, and propylene glycol diacetate;
[0088] Hydrocarbon solvents such as cyclopentanone and cyclohexanone, etc. In addition, as other organic solvents, these may be used alone or in combination of two or more.
[0089] The content ratio of other organic solvents is preferably 30 mass % or less, more preferably 20 mass % or less, further preferably 5 mass % or less, with respect to the total amount of the solvent contained in the liquid crystal aligning agent.
[0090] (Other ingredients)
[0091] The liquid crystal aligning agent of the present disclosure contains at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester and polyimide, a base having a typical metal element or a transition metal element, and water, and may contain components other than these components (hereinafter also referred to as "other components").
[0092] As other components, in addition to the solvents described above, for example, epoxy-containing compounds (such as N,N,N′,N′-tetraglycidyl-m-xylene diamine, N,N,N′,N′-tetraglycidyl-4,4′-diaminodiphenylmethane, etc.), functional silane compounds (such as 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, etc.), antioxidants, metal chelate compounds, curing catalysts, curing accelerators, surfactants, fillers, dispersants, photosensitizers, etc. The proportion of other components can be appropriately selected according to each compound within the range that does not impair the effects of the present invention.
[0093] In addition, in order to obtain polymer (P), it is preferably carried out in the following manner: polymer (A) is separated from the reaction solution, and after being purified as needed, it is mixed with alkali (B) in a solvent containing water. When preparing a liquid crystal alignment agent, it can also be carried out by the following method: polymer (A) and alkali (B) are pre-mixed in a solvent containing water, and then the obtained polymer solution is diluted with a solvent and adjusted to the desired concentration, and other components prepared as needed are added. Alternatively, a liquid crystal alignment agent of a desired concentration can be obtained by mixing polymer (A), alkali (B) and other components prepared as needed in a solvent containing water.
[0094] The solid content concentration in the liquid crystal alignment agent (the ratio of the total mass of the components other than the solvent of the liquid crystal alignment agent to the total mass of the liquid crystal alignment agent) is appropriately selected in consideration of viscosity, volatility, etc., preferably in the range of 1% to 10% by mass. When the solid content concentration is less than 1% by mass, the film thickness of the coating is too small, and it is difficult to obtain a good liquid crystal alignment film. On the other hand, when the solid content concentration exceeds 10% by mass, the film thickness of the coating is too large, and it is difficult to obtain a good liquid crystal alignment film. In addition, the viscosity of the liquid crystal alignment agent increases, and there is a tendency for the coating property to decrease.
[0095] 《Liquid crystal alignment film, liquid crystal element and optical film》
[0096] The liquid crystal element and the optical film of the present disclosure include a liquid crystal alignment film formed using the liquid crystal alignment agent described above.
[0097] (Liquid crystal element)
[0098] The liquid crystal element disclosed in the present invention can be effectively applied to various purposes due to the high transparency of the liquid crystal alignment film. Specifically, it can be used as: clocks, portable game consoles, word processors, notebook personal computers, car navigation systems, camcorders, personal digital assistants (PDAs), digital cameras, mobile phones, smart phones, various monitors, liquid crystal televisions, information displays and other display devices, or dimming devices (dimming films), etc.
[0099] When used as a liquid crystal display device, the operation mode of the liquid crystal is not particularly limited. Specifically, for example, the operation mode of the liquid crystal is: twisted nematic (TN) type, super twisted nematic (STN) type, vertical alignment type (including vertical alignment-multidomain vertical alignment (VA-MVA) type, vertical alignment-patterned vertical alignment (VA-PVA) type, etc.), in-plane switching (IPS) type, fringe field switching (FFS) type, optically compensated bend (OCB) type, etc.
[0100] The following is a description of a method for producing a liquid crystal display element. The liquid crystal display element can be produced, for example, by a method including the following steps 1 to 3. In step 1, the substrate used varies depending on the desired operation mode. In steps 2 and 3, each operation mode is common.
[0101] (Step 1: Formation of coating film)
[0102] First, a liquid crystal alignment agent is applied to the substrate, and the applied surface is preferably heated to form a coating film on the substrate. As a substrate, for example, a transparent substrate comprising the following materials can be used: glass such as float glass and soda glass; plastics such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, and poly (alicyclic olefin). As a transparent conductive film disposed on one side of the substrate, a NESA film (a registered trademark of PPG, USA) containing tin oxide (SnO2) and an indium tin oxide (Indium Tin Oxide, ITO) film containing indium oxide-tin oxide (In2O3-SnO2) can be used. In the case of manufacturing a TN type, STN type or VA type liquid crystal element, two substrates provided with a patterned transparent conductive film are used. On the other hand, in the case of manufacturing an IPS type or FFS type liquid crystal element, a substrate provided with an electrode and an opposing substrate without an electrode are used, and the electrode comprises a transparent conductive film or a metal film patterned into a comb-tooth shape. As the metal film, for example, a film containing a metal such as chromium can be used. The liquid crystal aligning agent is applied to the substrate on the electrode formation surface, preferably by offset printing, spin coating, roll coater, flexographic printing or inkjet printing.
[0103] After applying the liquid crystal alignment agent, it is preferred to perform preheating (prebaking) for the purpose of preventing the applied liquid crystal alignment agent from sagging. The prebaking temperature is preferably 30°C to 200°C, and the prebaking time is preferably 0.25 minutes to 10 minutes. Afterwards, a calcination (post-baking) process is performed for the purpose of completely removing the solvent and, if necessary, thermally imidizing the amide acid structure possessed by the polymer. The calcination temperature (post-baking temperature) is preferably 80°C to 300°C, and the post-baking time is preferably 5 minutes to 200 minutes. The film thickness of the film formed in the above manner is preferably 0.001μm to 1μm. After applying the liquid crystal alignment agent on the substrate, the organic solvent is removed to form a liquid crystal alignment film or a coating film that becomes a liquid crystal alignment film.
[0104] (Process 2: Orientation Treatment)
[0105] In the case of manufacturing TN type, STN type, IPS type or FFS type liquid crystal display elements, a treatment (orientation treatment) is implemented to impart liquid crystal orientation ability to the coating film formed in the process 1. Thus, the orientation ability of the liquid crystal molecules is imparted to the coating film to form a liquid crystal orientation film. As an orientation treatment, for example, it can be listed as: a friction treatment in which a roller wound with a cloth containing fibers such as nylon, rayon, and cotton is used to rub the coating film in a fixed direction; or a light orientation treatment in which a coating film formed on a substrate using a liquid crystal orientation agent is irradiated with light to impart liquid crystal orientation ability to the coating film. On the other hand, in the case of manufacturing a vertically oriented liquid crystal element, the coating film formed in the process 1 can be directly used as a liquid crystal orientation film, or an orientation treatment (rubbing treatment, light orientation treatment, etc.) can be applied to the coating film. The liquid crystal orientation agent suitable for a vertically oriented liquid crystal display element can also be applied to a polymer sustained alignment (PSA) type liquid crystal display element.
[0106] In the case where the liquid crystal alignment agent contains a polymer having a photo-orientation group, it is preferred to form a liquid crystal alignment film using a photo-orientation method. In the above case, a uniform liquid crystal orientation can be imparted to the photosensitive organic film while suppressing the generation of static electricity and dust, and precise control of the liquid crystal orientation direction can also be achieved, which is preferred in this regard. The light irradiation for light orientation can be carried out using the following methods: a method for irradiating the coating after the post-baking process, a method for irradiating the coating after the pre-baking process and before the post-baking process, and a method for irradiating the coating during the heating process of the coating in at least any one of the pre-baking process and the post-baking process. As the radiation irradiated to the coating, for example, ultraviolet rays and visible rays containing light with a wavelength of 150nm to 800nm can be used. Preferably, ultraviolet rays containing light with a wavelength of 200nm to 400nm can be used. In the case where the radiation is polarized light, it can be linearly polarized light or partially polarized light. In the case where the radiation used is linearly polarized light or partially polarized light, the irradiation can be carried out from a direction perpendicular to the substrate surface, from an inclined direction, or in combination. In the case of non-polarized radiation, the irradiation direction is set to an oblique direction.
[0107] Examples of the light source include a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, and an excimer laser. The radiation dose is preferably 400 J / m 2 ~50,000J / m 2 , more preferably 1,000 J / m 2 ~20,000J / m 2After irradiation with light for imparting alignment ability, the substrate surface may be washed with water, an organic solvent (such as methanol, isopropanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated.
[0108] The surface of the liquid crystal alignment film formed on the substrate is preferably subjected to a passivation treatment (passivation treatment). The above treatment is preferred because it can further improve the solvent resistance of the liquid crystal alignment film. The passivation treatment is performed by making the film surface have a valence ratio of M to that of the polymer (P). n+ Thus, the M of the polymer (P) is n+ Converted into metal ions with a higher valence, forming a passivation film on the membrane surface. n+ In the case of a monovalent cation, for example, a salt of a divalent or higher valent cation such as calcium hydroxide, barium hydroxide, magnesium hydroxide, or strontium hydroxide can be preferably used.
[0109] (Step 3: Construction of Liquid Crystal Cell)
[0110] Next, two substrates formed with liquid crystal alignment films in the above manner are prepared, and a liquid crystal cell is manufactured by arranging liquid crystal between the two substrates arranged opposite to each other. When manufacturing a liquid crystal cell, for example, the following methods can be cited: (1) two substrates are arranged opposite to each other with a gap (spacer) between them in a manner that the liquid crystal alignment films face each other, and the peripheral portions of the two substrates are bonded together using a sealant, and the liquid crystal is injected into the cell gap divided by the substrate surface and the sealant, and then the injection hole is sealed; (2) a sealant is applied to a specified position on one of the substrates formed with a liquid crystal alignment film, and then liquid crystal is dripped at a specified number of locations on the surface of the liquid crystal alignment film, and then another substrate is bonded in a manner that the liquid crystal alignment films face each other, and the liquid crystal is diffused over the entire surface of the substrate (liquid crystal dripping (one drop filling, ODF) method), etc. It is ideal that the manufactured liquid crystal cell is further heated until the temperature at which the liquid crystal used obtains an isotropic phase, and then slowly cooled to room temperature, thereby removing the flow orientation when the liquid crystal is filled.
[0111] As a sealant, for example, an epoxy resin containing a hardener and alumina balls as a spacer can be used. As a spacer, a photo spacer, a bead spacer, etc. can be used. As liquid crystals, nematic liquid crystals and smectic liquid crystals can be listed, wherein nematic liquid crystals are preferred. In addition, cholesteric liquid crystals, chiral auxiliary agents, ferroelectric liquid crystals, etc. can also be added to nematic liquid crystals or smectic liquid crystals for use.
[0112] Next, a polarizing plate is attached to the outer surface of the liquid crystal cell as needed. Examples of the polarizing plate include a polarizing plate formed by sandwiching a polarizing film called "H film" between cellulose acetate protective films, or a polarizing plate containing the H film itself. The "H film" absorbs iodine while stretching and orienting polyvinyl alcohol. In this way, a liquid crystal display element is obtained.
[0113] (Optical Film)
[0114] As an optical film, for example, when manufacturing a phase difference film, first, the liquid crystal orientation agent prepared above is applied to the substrate, and it is preferred to heat (bake) the coated surface to form a coating. As a substrate, it is preferably a transparent substrate comprising synthetic resins such as triacetyl cellulose (TAC), polyethylene terephthalate, polybutylene terephthalate, polyether sulfone, polyamide, polyimide, polymethyl methacrylate, and polycarbonate. As a coating to a substrate, for example, it can be carried out by a rod coater method, a spinner method, a printing method, an inkjet method, a roller coater method, etc. The baking temperature is preferably 40°C to 150°C, and more preferably 80°C to 140°C. The heating time is preferably 0.1 minutes to 15 minutes, and more preferably 1 minute to 10 minutes.
[0115] Next, the coating film formed on the substrate is irradiated with light to impart liquid crystal orientation capability to the coating film. As the irradiated light, for example, ultraviolet rays and visible light rays containing light with a wavelength of 150nm to 800nm can be cited. Among these, ultraviolet rays containing light with a wavelength of 300nm to 400nm are preferred. The irradiated light may be polarized light or non-polarized light. As polarized light, it is preferred to use light containing linear polarization.
[0116] When the light used is polarized light, the light irradiation can be performed from a direction perpendicular to the substrate surface or from an inclined direction, or a combination of these. When irradiating non-polarized light, it is necessary to irradiate from an inclined direction relative to the substrate surface. The irradiation amount of light is preferably set to 0.1 mJ / cm 2 Above and less than 1,000mJ / cm 2 , more preferably 1 mJ / cm 2 ~500mJ / cm 2 The coating film (liquid crystal alignment film) after light irradiation is preferably subjected to a passivation treatment (passivation treatment) in order to further improve solvent resistance. The description of the passivation treatment is the same as that of the method for producing a liquid crystal display element.
[0117] Next, a polymerizable liquid crystal is applied to the coating film after light irradiation in the manner described above and hardened. Thus, a coating film (liquid crystal layer) containing a polymerizable liquid crystal is formed. The polymerizable liquid crystal used herein is a liquid crystal compound or liquid crystal composition polymerized by at least one of heating and light irradiation. The polymerizable liquid crystal may also be a mixture of multiple liquid crystal compounds. The polymerizable liquid crystal may also be a composition further containing a known polymerization initiator, a suitable solvent, etc.
[0118] When the polymerizable liquid crystal as described above is applied to the formed liquid crystal alignment film, for example, an appropriate coating method such as a bar coater method, a roll coater method, a spinner method, a printing method, an inkjet method, etc. can be used.
[0119] Next, the coating of the polymerizable liquid crystal formed in the manner described above is subjected to one or more treatments selected from heating and light irradiation, thereby hardening the coating to form a liquid crystal layer. The heating temperature of the coating is appropriately selected according to the type of polymerizable liquid crystal used. For example, when using RMS03-013C manufactured by Merck, it is preferably heated at a temperature in the range of 40°C to 80°C. The heating time is preferably 0.5 minutes to 5 minutes. As the irradiation light, non-polarized ultraviolet light with a wavelength in the range of 200nm to 500nm can be preferably used. As the irradiation amount of light, it is preferably set to 50mJ / cm 2 ~10,000mJ / cm 2 , more preferably 100 mJ / cm 2 ~5,000mJ / cm 2 .
[0120] The thickness of the formed liquid crystal layer is appropriately set according to the desired optical characteristics. For example, in the case of manufacturing a 1 / 2 wavelength plate for visible light with a wavelength of 540nm, the thickness of the formed retardation film is selected so that the phase difference becomes 240nm to 300nm; if it is a 1 / 4 wavelength plate, the thickness is selected so that the phase difference becomes 120nm to 150nm.
[0121] The phase difference film obtained in the manner described can be preferably used as a phase difference film of a liquid crystal display element. The driving mode of the applied liquid crystal display element is not limited, for example, it can be applied to various known modes such as TN type, STN type, IPS type, FFS type, VA type, etc. The phase difference film is used by attaching the surface of the substrate side of the phase difference film to the outer surface of the polarizing plate arranged on the visible side of the liquid crystal display element. Therefore, it is preferably set to the following embodiment: the substrate of the phase difference film is set to a TAC-based or acrylic substrate, so that the substrate of the phase difference film also functions as a protective film of the polarizing film.
[0122] [Example]
[0123] Hereinafter, the present invention will be further specifically described by way of examples, but the present invention is not limited to these examples.
[0124] In the following examples, the weight average molecular weight Mw, number average molecular weight Mn, solution viscosity of the polymer solution, and imidization ratio of the polyimide were measured by the following method. The required amount of the raw material compound and the polymer used in the following examples was ensured by repeatedly performing the synthesis under the synthesis ratio shown in the following synthesis example as needed.
[0125] [Weight average molecular weight Mw and number average molecular weight Mn of polymer]
[0126] Mw and Mn are polystyrene-equivalent values measured by GPC under the following conditions.
[0127] Column: TSK gel GRCXLII manufactured by Tosoh
[0128] Solvent: N,N-dimethylformamide
[0129] Temperature: 40℃
[0130] Pressure: 68kgf / cm 2
[0131] [Solution viscosity of polymer solution]
[0132] The solution viscosity (mPa·s) of the polymer solution was measured at 25° C. using an E-type rotational viscometer.
[0133] [Imidization ratio of polyimide]
[0134] The imidized polymer was dried under reduced pressure at room temperature, dissolved in deuterated dimethyl sulfoxide, and measured at room temperature using tetramethylsilane as a reference substance. 1 The imidization ratio was determined by H-nuclear magnetic resonance (NMR) using the following mathematical formula (I).
[0135] Imidization rate (%) = (1-A 1 / A 2 ×α)×100…(I)
[0136] (In formula (I), A 1 A is the peak area of protons originating from NH groups appearing near the chemical shift of 10 ppm, 2 is the peak area derived from other protons, and α is the ratio of the number of other protons in the polymer precursor (polyamic acid) to one proton of the NH group).
[0137] The compounds used in the Examples are shown below. In addition, the compound represented by the formula (X) may be simply abbreviated as "compound (X)" below.
[0138] [Chemistry 4]
[0139]
[0140] [Synthesis example 1]
[0141] 47.4 g (0.15 mol) of compound (a-1) and 52.6 g (0.15 mol) of compound (b-1) were dissolved in 566 g of N-methyl-2-pyrrolidone (NMP), and the reaction was carried out at 60°C for 6 hours to obtain a polyamic acid solution containing 15% by mass. The weight average molecular weight Mw of the obtained polyamic acid is 45,000. After the reaction, the reaction solution was added dropwise to 3000 g of water to precipitate polyamic acid (resin). After filtering and separating with a 100-mesh filter, the precipitate was washed with methanol and dried at 40°C under reduced pressure for 15 hours to obtain 85 g of polyamic acid solid. 50 g of the obtained solid was put into a flask, and 340 g of water and 10 g (0.18 mol) of potassium hydroxide were added, and the mixture was stirred at 20° C. for 12 hours to dissolve the solid, thereby obtaining a polyamic acid solution (PA-1) having a solid content concentration of 15% by mass.
[0142] [Synthesis example 2]
[0143] 61.3g (0.14 mol) of compound (a-2) and 38.7g (0.14 mol) of compound (b-2) were dissolved in 566g of NMP, and the reaction was carried out at 60°C for 6 hours to obtain a polyamic acid solution containing 15% by mass. The weight average molecular weight Mw of the obtained polyamic acid is 70,000. After the reaction, the reaction solution was added dropwise to 3000g of water to precipitate the polyamic acid (resin). After filtering and separating with a 100-mesh filter, the precipitate was washed with methanol and dried at 40°C for 15 hours under reduced pressure to obtain 92g of a polyamic acid solid. 50g of the obtained solid was placed in a flask, 425g of water and 25g (0.30 mol) of sodium bicarbonate were added, and the solution was dissolved by stirring at 20°C for 12 hours to obtain a polyamic acid solution (PA-2) having a solid content concentration of 15% by mass.
[0144] [Synthesis example 3]
[0145] 61.3g (0.14 mol) of compound (a-2) and 48.1g (0.14 mol) of compound (b-3) were dissolved in 566g of NMP, and the reaction was carried out at 60°C for 6 hours to obtain a polyamic acid solution containing 15% by mass. The weight average molecular weight Mw of the obtained polyamic acid is 65,000. After the reaction, the reaction solution was added dropwise to 3000g of water to precipitate polyamic acid (resin). After filtering and separating with a 100-mesh filter, the precipitate was washed with methanol and dried at 40°C for 15 hours under reduced pressure to obtain 80g of a polyamic acid solid. 50g of the obtained solid was placed in a flask, 470g of water and 33g (0.14 mol) of cesium pivalate were added, stirred at 20°C for 12 hours and dissolved to obtain a polyamic acid solution (PA-3) having a solid content concentration of 15% by mass.
[0146] [Synthesis Example 4]
[0147] 19.61g (0.1 mol) of cyclobutanetetracarboxylic dianhydride and 21.23g (0.1 mol) of 4,4′-diamino-2,2′-dimethylbiphenyl were dissolved in 367.6g of NMP and reacted at room temperature for 6 hours. The reaction mixture was injected into a large amount of excess methanol to precipitate polyamic acid (resin). After filtering and separating with a 100-mesh filter, the precipitate was washed with methanol and dried at 40°C for 15 hours under reduced pressure to obtain 35g of polyamic acid solid. 20g of the obtained solid was placed in a flask, 200g of water and 15g (0.11 mol) of potassium carbonate were added, and the mixture was stirred at 20°C for 12 hours to dissolve, and a polyamic acid solution (PA-4) having a solid content concentration of 15% by mass was obtained.
[0148] [Synthesis example 5]
[0149] A polyamic acid solution (PA-5) having a solid content concentration of 15% by mass was obtained in the same manner as in Synthesis Example 4 except that 15 g (0.14 mol) of sodium 2-methyl-2-butoxide was used instead of potassium carbonate.
[0150] [Synthesis example 6]
[0151] 2,3,5-tricarboxycyclopentyl acetic acid dianhydride 224g (1.0 mole), p-phenylenediamine 54g (0.5 mole), and 3,5-diaminobenzoic acid cholesteryl ester 260g (0.5 mole) were dissolved in 2900g of NMP and reacted at 60°C for 6 hours to obtain a polyamic acid solution having a solution viscosity of 320mPa s. 300g of the obtained polymer solution was added dropwise to 3000g of water to precipitate polyamic acid (resin). After separation by filtration using a 100-mesh filter, the precipitate was washed with methanol and dried at 40°C for 15 hours under reduced pressure to obtain 40g of a polyamic acid solid. The obtained solid 20g was placed in a flask, 130g of water and 3g (0.13 mole) of lithium hydroxide were added, stirred at 20°C for 12 hours and dissolved to obtain a polyamic acid solution (PA-6) having a solid content concentration of 15% by mass.
[0152] [Synthesis Example 7]
[0153] 224g (1.0 mol) of 2,3,5-tricarboxycyclopentylacetic acid dianhydride, 108g (1.0 mol) of p-phenylenediamine, and 7.8g (0.015 mol) of 3,5-diaminobenzoic acid cholesteryl ester were dissolved in 3039g of NMP and reacted at 60°C for 6 hours to obtain a polyamic acid solution with a solution viscosity of 260mPa·s. Then, 2700g of NMP was added to the obtained polyamic acid solution, 396g of pyridine and 306g of acetic anhydride were added, and dehydration and ring closure were carried out at 110°C for 4 hours. After the imidization reaction, the solvent in the system was replaced with new γ-butyrolactone to obtain a solid content concentration of 9.0% by mass, a solid content concentration of 10% by mass, a solution viscosity of 250mPa·s, and an imidization rate of about 51% of 3,000g of polymer solution. 300g of the obtained polymer solution was added dropwise to 3000g of water to precipitate polyamic acid (resin). After separation by filtration with a 100-mesh filter, the precipitate was washed with methanol and dried at 40°C for 15 hours under reduced pressure to obtain 25g of a polyamic acid solid. 20g of the obtained solid was put into a flask, 130g of water and 3g (0.08 mole) of sodium hydroxide were added, and the mixture was stirred for 12 hours at 20°C and dissolved to obtain a polyamic acid solution (PA-7) having a solid content concentration of 15% by mass.
[0154] [Synthesis example 8]
[0155] A polyamic acid solution (PR-1) (solid content concentration: 15.8% by mass) was obtained by performing synthesis in the same manner as in Synthesis Example 2 except that 30 g (0.30 mol) of triethylamine was used instead of sodium hydrogen carbonate.
[0156] [Synthesis Example 9]
[0157] According to the method described in paragraphs
[0134] and
[0150] of JP-A-2016-224151, an acrylic copolymer aqueous solution (PR-2) was obtained.
[0158] [Synthesis Example 10]
[0159] According to the method described in paragraph
[0041] of Japanese Patent Application Laid-Open No. 08-087017, a polyamic acid aqueous solution (PR-3) was obtained.
[0160] [Example 1]
[0161] 1. Preparation of Liquid Crystal Alignment Agent
[0162] Distilled water (WT) as a solvent was added to the polyamic acid solution (PA-1) having a solid content concentration of 15% by mass obtained in Synthesis Example 1 as a polymer component, and the solid content concentration was 3% by mass. Then, the obtained solution was filtered using a filter with a pore size of 1 μm to prepare a liquid crystal aligning agent (A-1).
[0163] 2. Production of optical films
[0164] The liquid crystal alignment agent (A-1) prepared above was applied to the triacetyl cellulose film using a bar coater, and baked in an oven at 120°C for 2 minutes to form a coating film with a thickness of 0.1 μm. Next, the coating film surface was irradiated with polarized ultraviolet light containing a bright line of 313 nm at a rate of 10 mJ / cm2 perpendicularly from the normal line of the substrate surface using a Hg-Xe lamp and a Glan-Taylor prism. 2 , a liquid crystal alignment film was prepared. Next, the polymerizable liquid crystal (RMS03-013C, manufactured by Merck) was filtered using a filter with a pore size of 0.2 μm and coated on the surface of the liquid crystal alignment film using a rod coater. Next, after baking in an oven set at 50°C for 1 minute, a Hg-Xe lamp was used to irradiate the polymerizable liquid crystal with 1,000 mJ / cm of non-polarized ultraviolet light containing a bright line of 365 nm. 2 The optically anisotropic film formed on the liquid crystal alignment film had a film thickness of 1.0 μm.
[0165] 3. Evaluation of liquid crystal orientation
[0166] For the optical film obtained above, the liquid crystal orientation was observed by visual observation and polarizing microscope under cross nicol. The situation where the liquid crystal orientation was good under visual observation and no abnormal region was observed under polarizing microscope was evaluated as "good (A)"; the situation where the liquid crystal orientation was good under visual observation but abnormal region was observed under polarizing microscope was evaluated as "acceptable (B)"; the situation where abnormal liquid crystal orientation was observed under visual observation was evaluated as "poor (C)". As a result, in the embodiment 1, the liquid crystal orientation was evaluated as "acceptable (B)".
[0167] 4. Transparency Evaluation
[0168] For the optical film produced above, the transparency is evaluated by measuring the haze. The measurement is performed using a spectroscopic haze meter (manufactured by Tokyo Denshoku Co., Ltd.). The lower the haze value, the better the transparency. When the haze value is 2% or less, it is judged as "good (A)"; when the haze value is greater than 2% and less than 4%, it is judged as "acceptable (B)"; when the haze value is greater than 4%, it is judged as "poor (C)". In Example 1, the transparency is "good (A)".
[0169] 5. Evaluation of solvent resistance
[0170] The liquid crystal alignment agent (A-1) prepared above is coated on a glass substrate using a spinner, and after pre-baking on a hot plate at 120°C for 2 minutes, the thickness of the formed coating is measured by a stylus film thickness meter. Secondly, cyclopentanone is applied to the formed coating by a spinner, dried on a hot plate at 120°C for 2 minutes, and the film thickness is measured again. At this time, the smaller the change in film thickness, the better the solvent resistance. When the film thickness change rate is less than 3%, it is judged as "good (A)"; when the film thickness change rate is greater than 3% and less than 20%, it is judged as "acceptable (B)"; when the film thickness change rate is greater than 20%, it is judged as "poor (C)". In Example 1, the solvent resistance is "good (A)".
[0171] [Example 2 to Example 8 and Comparative Example 1 to Comparative Example 3]
[0172] Except for changing the type and amount of the polymer solution and the solvent, and the solid content concentration as described in Table 1 below, liquid crystal aligning agents (A-2) to (A-7) and liquid crystal aligning agents (R-1) to (R-3) were prepared in the same manner as in Example 1. In addition, when a solvent other than distilled water was added, the water introduced from the polyamic acid solution prepared in Synthesis Examples 1 to 10 was considered, and the final solvent composition was prepared in a manner of the mass ratio described in Table 1 below.
[0173] Moreover, evaluation was performed similarly to Example 1 except having changed the following points in Example 1 using each obtained liquid crystal aligning agent.
[0174] Regarding Example 2 and Example 3
[0175] Except having used the liquid crystal aligning agent (A-2) or the liquid crystal aligning agent (A-3) instead of the liquid crystal aligning agent (A-1), it carried out various evaluations similar to Example 1.
[0176] Regarding Example 4 and Example 5
[0177] In addition to using the liquid crystal aligning agent (A-4) or the liquid crystal aligning agent (A-5) instead of the liquid crystal aligning agent (A-1), the coating film surface was irradiated with polarized ultraviolet rays including a bright line of 254 nm at 10,000 J / m from the normal line of the substrate surface using a Hg-Xe lamp and a Glan Taylor prism. 2 Various evaluations were performed in the same manner as in Example 1 except for this point.
[0178] About Example 6
[0179] Various evaluations were performed in the same manner as in Example 1 except that a liquid crystal aligning agent (A-6) was used instead of the liquid crystal aligning agent (A-1), the coating film surface was not irradiated with polarized ultraviolet rays, and RMS03-015 (manufactured by Merck) was used as the polymerizable liquid crystal.
[0180] About Example 7
[0181] Except that the liquid crystal orientation agent (A-7) was used instead of the liquid crystal orientation agent (A-1), and that the coating formed by using the liquid crystal orientation agent was given liquid crystal orientation ability by friction treatment instead of photo-orientation treatment, various evaluations were performed in the same manner as in Example 1. The friction treatment was performed as follows. Using a friction machine having a roller wound with a rayon cloth, the coating surface was rubbed at a roller rotation speed of 400 rpm, a platform movement speed of 3 cm / second, and a hair press length of 0.4 mm, and then ultrasonically washed in ultrapure water for 1 minute and dried in a clean oven at 100°C for 10 minutes.
[0182] About Example 8
[0183] Various evaluations were performed in the same manner as in Example 1 except that a liquid crystal aligning agent (A-2) was used instead of the liquid crystal aligning agent (A-1) and the coating film (liquid crystal aligning film) after the polarized ultraviolet ray irradiation was immersed in a 1% aqueous solution of strontium hydroxide to perform a passivation treatment.
[0184] · About Comparative Example 1 and Comparative Example 2
[0185] Except having used the liquid crystal aligning agent (R-1) or the liquid crystal aligning agent (R-2) instead of the liquid crystal aligning agent (A-1), it carried out various evaluations similar to Example 1.
[0186] About Comparative Example 3
[0187] Various evaluations were performed in the same manner as in Example 1, except that the liquid crystal aligning agent (R-3) was used instead of the liquid crystal aligning agent (A-7) and that the coating film formed using the liquid crystal aligning agent was given liquid crystal aligning ability by rubbing treatment instead of photo-alignment treatment. The rubbing treatment was performed under the same conditions as in Example 7.
[0188] [Table 1]
[0189]
[0190] In Table 1, the abbreviations of the solvents are as follows.
[0191] CHN: Cyclohexanone
[0192] PGME: Propylene glycol monomethyl ether
[0193] WT: distilled water
[0194] MEOH: Methanol
[0195] THF: Tetrahydrofuran
[0196] NPA: n-propanol
[0197] IPA: Isopropyl alcohol
[0198] Various evaluation results of Examples 1 to 8 and Comparative Examples 1 to 3 are summarized in Table 2 below.
[0199] [Table 2]
[0200] Orienting agent type Liquid crystal orientation Transparency Solvent resistance Example 1 A-1 B A A Example 2 A-2 A A A Example 3 A-3 A A A Example 4 A-4 A A A Example 5 A-5 A A A Example 6 A-6 B A B Example 7 A-7 B A A Example 8 A-2 A A A Comparative Example 1 R-1 B C C Comparative Example 2 R-2 B C C Comparative Example 3 R-3 A C C
[0201] As is clear from Table 2, the evaluations of liquid crystal orientation, transparency, and solvent resistance in Examples 1 to 8 were all "A" or "B". In contrast, the transparency and solvent resistance in the comparative examples were inferior to those in the examples.
Claims
1. A liquid crystal aligning agent comprising a polymer having a partial structure represented by the following formula (1), wherein the polymer has a group containing a cinnamic acid structure, In formula (1), R 1 is a hydrogen atom or a monovalent organic group, X 1 is a tetravalent organic group, X 2 is a divalent organic group; M n+ is a monovalent cation of an alkali metal element; m1 is 1 or 2, m2 is 0 or 1, and satisfies m1+m2=2, The liquid crystal alignment agent contains a water-containing solvent, and the proportion of water in the solvent is more than 50%.
2. A liquid crystal alignment agent, comprising: A polymer selected from at least one of the group consisting of polyamic acid, polyamic acid ester and polyimide, wherein the polymer has a group containing a cinnamic acid structure; Bases, having an alkali metal element; and A water-containing solvent, wherein the proportion of water in the solvent is 50% or more. 3 . A liquid crystal alignment film, formed using the liquid crystal alignment agent according to claim 1 . 4 . An optical film comprising the liquid crystal alignment film according to claim 3 . 5 . A liquid crystal element comprising the liquid crystal alignment film according to claim 3 .
6. A method for manufacturing a liquid crystal alignment agent, comprising mixing at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester and polyimide, a base having an alkali metal element, and a water-containing solvent, wherein the proportion of water in the solvent is greater than 50%; the polymer has a group containing a cinnamic acid structure.
7. A method for manufacturing a liquid crystal alignment film, comprising: The step of applying the liquid crystal alignment agent according to claim 1 or 2 to a pair of substrates respectively to form a coating film on the pair of substrates; as well as A step of passivating the surfaces of the pair of substrates on which the coating film is formed The passivation treatment is performed by bringing the membrane surface into contact with a base having a valence greater than that of the n-valent cations possessed by the polymer.
8. A method for manufacturing a liquid crystal element, comprising: A step of applying the liquid crystal alignment agent according to claim 1 or 2 to a pair of substrates, respectively, and forming a liquid crystal alignment film by irradiating light; as well as A step of arranging the pair of substrates on which the liquid crystal alignment films are formed so that the liquid crystal alignment films face each other with a liquid crystal layer interposed therebetween to construct a liquid crystal cell.
Citation Information
Patent Citations
Production of liquid crystal display element
JP1996087017A
Liquid crystal aligning agent and liquid crystal display element
JP2010097188A
Aqueous solvent-based liquid crystal aligning agent, liquid crystal alignment film and phase difference material
JP2016224151A
Liquid crystal alignment agent
JP1998218992A
Liquid crystal orientated film, optical compensation sheet, STN-type liquid crystal display device and orientating discotic liquid crystalline molecule
JP2001089657A