Semiconductor structure and preparation method
By forming a liner layer and an isolation layer on the semiconductor substrate, filling the dielectric layer in steps and etching to form a second trench, the problems of edge notches and voids in the shallow trench isolation structure are solved, and rectangular cross-section and optimized side are realized The wall angle improves the isolation effect and product yield.
Patent Information
- Application Number
- CN201811147153.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-09-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2038-09-29
AI Technical Summary
The existing shallow trench isolation structure has poor isolation effects in edge notches, voids and side wall angles, which affects device performance and yield.
By forming a first trench, a liner layer and an isolation layer on the semiconductor substrate, the dielectric layer is filled in step and a second trench is formed by etching to avoid edge notches and voids, ensuring a rectangular cross-section and optimizing sidewall angle.
A shallow groove structure with no holes and optimized isolation effect is achieved, improving product yield and isolation performance.
Smart Images

Figure CN110970345B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to a semiconductor structure and a preparation method thereof. Background Art
[0002] At present, shallow trench isolation (STI) structures are widely used in the isolation process of semiconductor technology nodes of 0.25um and below. Among them, the defects or parameters that affect the performance of shallow trench isolation structures mainly include edge gaps (divot), voids (void) and sidewall angles.
[0003] like Figure 1 As shown, it is a cross-sectional schematic diagram of a shallow trench isolation structure obtained by using the prior art. A silicon dioxide dielectric layer 102 is filled in the groove formed on the silicon substrate 101 to form a shallow trench isolation structure. In the subsequent process, it is generally necessary to use wet etching to remove the thermal oxide layer on the surface of the silicon substrate, which will simultaneously etch the silicon dioxide dielectric layer 102 in the groove and form an edge notch 102a at the edge of the groove. The edge notch 102a will form an additional leakage current channel in the subsequent process, affecting the isolation effect and even causing device failure. In addition, the top width a1 of the shallow trench isolation structure obtained under the prior art is generally greater than the bottom width a2, that is, the cross-section of the entire shallow trench isolation structure is an inverted trapezoid, and the range of its sidewall angle α is generally between 80° and 89°. Considering the electrical isolation effect between devices, when the sidewall angle α is closer to 90° or even equal to 90°, the isolation effect of the shallow trench isolation structure is better, and the excessive inclination of the sidewall angle α is also easy to cause the shallow trench isolation structure to produce defects due to stress in the subsequent chemical mechanical polishing process. However, due to the limitations of the existing dielectric layer deposition process, when the sidewall angle α is close to 90°, it is easier to generate void defects 102 b in the silicon dioxide dielectric layer 102 , which will adversely affect the isolation effect, and further affect the device performance and product yield.
[0004] Therefore, it is necessary to propose a new semiconductor structure and preparation method to solve the above problems. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a semiconductor structure and a preparation method thereof, so as to solve the problem of poor isolation effect of the shallow trench isolation structure in the prior art.
[0006] To achieve the above object and other related objects, the present invention provides a method for preparing a semiconductor structure, comprising the following steps:
[0007] 1) providing a semiconductor substrate, and forming a first trench in the semiconductor substrate;
[0008] 2) forming a liner layer at least on the sidewall of the first trench;
[0009] 3) forming an isolation layer on the upper surface of the liner layer, wherein the isolation layer at least covers the side and top of the liner layer;
[0010] 4) filling the first trench with a first dielectric layer;
[0011] 5) etching and removing a portion of the first dielectric layer to form a second trench, wherein the depth of the second trench is less than the depth of the first trench; and
[0012] 6) Filling the second trench with a second dielectric layer, wherein the second dielectric layer at least fills up the second trench.
[0013] As a preferred solution of the present invention, the cross-sectional shape of the first groove formed in step 1) includes a rectangle.
[0014] As a preferred solution of the present invention, the top width of the cross section of the second groove formed in step 5) is greater than the bottom width.
[0015] As a preferred solution of the present invention, the depth range of the first groove formed in step 1) is between
[0016] As a preferred solution of the present invention, the depth range of the second groove formed in step 5) is between
[0017] As a preferred solution of the present invention, in step 1), the step of forming the first trench in the semiconductor substrate comprises the following steps:
[0018] 1-1) sequentially forming a first barrier layer, a second barrier layer and a third barrier layer on the surface of the semiconductor substrate;
[0019] 1-2) performing patterning on the first barrier layer, the second barrier layer and the third barrier layer, wherein the patterns formed by the first barrier layer, the second barrier layer and the third barrier layer are the same;
[0020] 1-3) using the third barrier layer as a hard mask layer, and forming the first trench in the semiconductor substrate by etching;
[0021] As a preferred embodiment of the present invention, the following steps are also included after step 6):
[0022] 7) using the second barrier layer as a grinding stop layer, and removing the third barrier layer and the second dielectric layer above the second barrier layer by chemical mechanical grinding;
[0023] 8) using the first barrier layer as an etching stop layer and removing the second barrier layer by dry etching;
[0024] 9) Removing the first barrier layer by wet etching.
[0025] As a preferred embodiment of the present invention, the semiconductor substrate includes a silicon substrate, the first barrier layer includes a silicon dioxide barrier layer, the second barrier layer includes a polysilicon barrier layer, the third barrier layer includes a silicon nitride barrier layer, and the liner layer includes a silicon dioxide layer; the liner layer formed in step 2) is also located on the side wall of the second barrier layer to form a groove structure at the side wall position of the first barrier layer.
[0026] As a preferred solution of the present invention, the isolation layer formed in step 3) fills up the groove structure.
[0027] The present invention also provides a semiconductor structure, comprising:
[0028] Semiconductor substrate;
[0029] A first trench formed in the semiconductor substrate;
[0030] A liner layer formed on a sidewall of the first trench;
[0031] an isolation layer, located in the first groove and covering at least the side and top of the liner layer;
[0032] A first dielectric layer is located in the first trench, and a thickness of the first dielectric layer is less than a depth of the first trench;
[0033] a second trench located in the first trench and above the first dielectric layer and the isolation layer; and
[0034] The second dielectric layer is located in the second trench.
[0035] As a preferred solution of the present invention, the cross-sectional shape of the first groove includes a rectangle.
[0036] As a preferred solution of the present invention, the upper surface of the second dielectric layer is at least flush with the top of the isolation layer.
[0037] As a preferred solution of the present invention, the top width of the cross section of the second groove is greater than the bottom width.
[0038] As described above, the present invention provides a semiconductor structure and a preparation method, which have the following beneficial effects:
[0039] The present invention introduces a new semiconductor shallow trench isolation structure, uses an isolation layer to cover a protective liner layer and the side wall of a dielectric layer at the edge of the trench, thereby avoiding the formation of edge notch defects; adopts a preparation method of step-by-step filling of the dielectric layer to obtain a shallow trench isolation structure without void defects and with a rectangular cross-section, thereby improving the isolation effect of the shallow trench isolation structure and increasing the product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 A schematic cross-sectional view of a shallow trench isolation structure obtained in the prior art is shown.
[0041] Figure 2 Shown is a flow chart of a method for preparing a semiconductor structure provided in Embodiment 1 of the present invention.
[0042] Figures 3 to 13 It is a cross-sectional schematic diagram showing each step of a method for preparing a semiconductor structure provided in the first embodiment of the present invention.
[0043] Component number description
[0044] 101 Silicon substrate
[0045] 102 Silicon dioxide dielectric layer
[0046] 102a Edge chip
[0047] 102b Void defect
[0048] 201 Semiconductor substrate
[0049] 201a First groove
[0050] 201b Second groove
[0051] 202 cushion layer
[0052] 203 Isolation Layer
[0053] 203a Protective structure
[0054] 204 first dielectric layer
[0055] 204a Hollow
[0056] 205 Second dielectric layer
[0057] 206 First barrier layer
[0058] 206a Groove structure
[0059] 207 Second barrier layer
[0060] 208 Third barrier layer
[0061] 209 photoresist layer
[0062] 209a Anti-reflective coating
[0063] a1 top width
[0064] a2 bottom width
[0065] α Sidewall angle
[0066] S1-S6 Steps 1)-6) of the method for preparing a semiconductor structure provided in the first embodiment of the present invention DETAILED DESCRIPTION
[0067] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0068] See also Figures 2 to 13 It should be noted that the illustrations provided in this embodiment are only schematic illustrations of the basic concept of the present invention. Although the illustrations only show components related to the present invention and are not drawn according to the number, shape and size of components in actual implementation, the form, quantity and proportion of each component in actual implementation may be changed arbitrarily, and the component layout may also be more complicated.
[0069] Embodiment 1
[0070] See also Figures 2 to 13 The present invention provides a method for preparing a semiconductor structure, comprising the following steps:
[0071] 1) providing a semiconductor substrate 201, and forming a first trench 201a in the semiconductor substrate 201;
[0072] 2) forming a liner layer 202 on the sidewall of the first trench 201a;
[0073] 3) forming an isolation layer 203 on the upper surface of the liner layer 202, wherein the isolation layer 203 at least covers the side surface and the top of the liner layer 202;
[0074] 4) Filling the first trench 201 a with a first dielectric layer 204 , wherein the first dielectric layer 204 at least covers the isolation layer 203 ;
[0075] 5) etching and removing a portion of the first dielectric layer 204 to form a second trench 201b, wherein the depth of the second trench 201b is less than the depth of the first trench 201a; and
[0076] 6) Filling the second trench 201 b with a second dielectric layer 205 , wherein the second dielectric layer 205 at least fills up the second trench 201 b .
[0077] In step 1), refer to Figure 2 The S1 step and Figure 5 , providing a semiconductor substrate 201, and forming a first trench 201a in the semiconductor substrate 201. Optionally, as Figure 5 As shown, the cross-sectional shape of the first trench 201a formed in this embodiment is rectangular, which can make the cross-sectional shape of the shallow trench isolation structure finally obtained rectangular, thereby improving the isolation effect of the shallow trench isolation structure. It should be pointed out that the cross-sectional shape of the trench obtained in the present invention is rectangular, which means that the sidewalls of the trench are vertical and the bottom of the trench is flat, and it does not require the cross-sectional shape to strictly conform to a rectangle in the geometric sense. Optionally, the optional depth range of the first trench 201a is between The preferred depth is The semiconductor substrate 201 includes a silicon substrate, and the first trench 201a is formed by dry etching, and the process gas of the dry etching includes etching gases such as Cl2 and SF6. In this embodiment, a first barrier layer 206, a second barrier layer 207 and a third barrier layer 208 are formed on the surface of the semiconductor substrate 201, and the above layers are patterned, and the patterns formed by the first barrier layer 206, the second barrier layer 207 and the third barrier layer 208 are the same. The patterned third barrier layer 208 is used as a hard mask layer to etch the semiconductor substrate 201 and form the first trench 201a.
[0078] In step 2), refer to Figure 2 The S2 step and Figure 6 , a liner layer 202 is formed at least on the sidewall of the first trench 201a. Figure 6 As shown, in the present embodiment, a liner layer 202 is formed on the sidewall and the bottom of the first trench 201a. In other embodiments of the present invention, the liner layer 202 may also be formed only on the sidewall of the first trench 201a. The first barrier layer 206 includes a silicon dioxide barrier layer, the second barrier layer 207 includes a polysilicon barrier layer, the third barrier layer 208 includes a silicon nitride barrier layer, the liner layer 202 includes a silicon dioxide layer, and the method for forming the liner layer 202 includes a thermal oxidation process. When the liner layer 202 is formed on the sidewall of the first trench 201a, the liner layer 202 is also formed on the sidewall of the second barrier layer 207, and a groove structure 206a is formed on the sidewall of the first barrier layer 206. Optionally, the thermal oxidation process is a dry oxygen oxidation process, the oxidation temperature is 800 to 1100°C, and the thickness of the liner layer 202 ranges from 200 to 1100°C. Preferably It should be noted that, in other embodiments, the third barrier layer 208 may also include a silicon dioxide layer, or a composite layer composed of silicon nitride and silicon dioxide.
[0079] In step 3), refer to Figure 2 The S3 steps and Figure 7 , an isolation layer 203 is formed on the upper surface of the liner layer 202, and the isolation layer 203 at least covers the side and top of the liner layer 202. In this embodiment, the isolation layer 203 completely covers the liner layer 202 from the side and top, fills the groove structure 206a, and also covers the liner layer 202 on the side wall of the second barrier layer 207 and the top and side wall of the third barrier layer 208; the isolation layer 203 includes a linear silicon nitride layer, and the thickness of the linear silicon nitride layer ranges from Preferably The linear silicon nitride layer is formed by chemical vapor deposition. Since the isolation layer 203 is a silicon nitride layer and covers the liner layer 202 composed of silicon dioxide, the liner layer 202 can be protected from being etched in the subsequent wet process of etching silicon dioxide, thereby avoiding edge divot defects in the shallow trench isolation structure.
[0080] In step 4), refer to Figure 2 The S4 step and Figure 8 , filling the first trench 201a with a first dielectric layer 204. Optionally, the first dielectric layer 204 comprises a silicon dioxide layer, and the silicon dioxide layer is formed by chemical vapor deposition. Figure 8 It can be seen that, since the cross section of the first trench 201a is rectangular, and its top width is equal to the bottom width, when the first dielectric layer 204 is filled by chemical vapor deposition, since the deposition rate at the top of the trench is higher than that at the bottom of the trench, the first dielectric layer 204 will be closed prematurely at the top of the first trench 201a during the filling process, and a cavity 204a will be formed in the first trench 201a. The cavity 204a will seriously affect the isolation performance of the shallow trench isolation structure, so the prior art generally cannot adopt a shallow trench isolation structure with a rectangular cross section, which is also the technical difficulty improved and overcome by the present invention.
[0081] In step 5), refer to Figure 2 S5 steps and Fig. 9 After etching away a portion of the first dielectric layer 204, a second trench 201b is formed, and the depth of the second trench 201b is less than the depth of the first trench 201a. Fig. 9As shown, in this embodiment, a portion of the first dielectric layer 204 is removed by etching, and the isolation layer 203 located on the top and sidewall of the third barrier layer 208, as well as the liner layer 202 and the isolation layer 203 located on the sidewall of the second barrier layer 207 are also removed. Optionally, the etching includes a wet etching process, and the etching solution used in the wet etching process is a mixed solution of hydrofluoric acid and ammonium fluoride, the volume ratio of the hydrofluoric acid to the ammonium fluoride ranges from 1:10 to 1:20, preferably 1:20, and the mixed solution has a selectivity of at least 37:1 for etching silicon dioxide to silicon nitride. Since the mixed solution has a high selectivity for silicon nitride when etching silicon dioxide, after the second trench 201b is formed by etching, the isolation layer 203 at the recess structure 206a will not be etched away, so that it can cover and protect the liner layer 202 located thereunder. As for the isolation layer 203 located on the surface of the liner layer 202 on the sidewall of the second barrier layer 207 and on the top and sidewall of the third barrier layer 208, they can be removed or retained during the etching process, and do not affect the structure of the present invention to protect the liner layer 202. Optionally, the depth of the second trench 201b is 1 / 4 to 3 / 4 of the depth of the first trench 201a, and the depth range of the second trench 201b is between Preferably If a cavity 204a is formed in the first dielectric layer 204 in step 4), the cavity 204a needs to be completely exposed by etching so as to fill the cavity 204a in the subsequent dielectric filling step. In other embodiments of the present invention, a dry etching process may be used to remove part of the first dielectric layer 204, and it is also necessary to ensure that the silicon dioxide has a high selectivity to silicon nitride so that the isolation layer 203 at the groove structure 206a will not be etched away.
[0082] In step 6), refer to Figure 2 S6 steps and Fig.10 , a second dielectric layer 205 is filled in the second trench 201b, and the second dielectric layer 205 at least fills the second trench 201b. Fig. 9 As shown, the top width of the cross section of the second groove 201b is greater than the bottom width, and has a shape of being wide at the top and narrow at the bottom, and having a shallow depth. Fig.10 When the second dielectric layer 205 is filled in the Figure 8The cavity 204a generated in the first trench 201a having a rectangular cross-section. Optionally, the second dielectric layer 205 comprises a silicon dioxide layer, and the silicon dioxide layer is formed by chemical vapor deposition. The present invention obtains a shallow trench isolation structure with a rectangular cross-section and no void defects by introducing a secondary filling process. In other embodiments of the present invention, if the depth-to-width ratio of the trench is high, the number of filling processes may not be limited to two times, and the filling-etching steps may be repeated multiple times until a trench isolation structure without void defects is obtained.
[0083] As an example, in step 1), the step of forming the first trench 201a in the semiconductor substrate 201 includes the following steps:
[0084] 1-1) sequentially forming a first barrier layer 206, a second barrier layer 207 and a third barrier layer 208 on the surface of the semiconductor substrate 201;
[0085] 1-2) performing patterning on the first barrier layer 206, the second barrier layer 207 and the third barrier layer 208, wherein the patterns formed by the first barrier layer 206, the second barrier layer 207 and the third barrier layer 208 are the same;
[0086] 1-3) using the third barrier layer 208 as an etching barrier layer, and forming the first trench in the semiconductor substrate 201 by etching;
[0087] As an example, after step 6), the following steps are also included:
[0088] 7) using the second barrier layer 207 as a grinding stop layer, and removing the third barrier layer 208 and the second dielectric layer 205 above the second barrier layer 207 by chemical mechanical grinding;
[0089] 8) Using the first barrier layer 206 as an etching stop layer, removing the second barrier layer 207 by dry etching;
[0090] 9) Remove the first barrier layer 206 by wet etching.
[0091] In step 1-1), refer to Figure 3 , sequentially forming a first barrier layer 206, a second barrier layer 207 and a third barrier layer 208 on the surface of the semiconductor substrate 201. Optionally, the first barrier layer 206 comprises a silicon dioxide barrier layer, which is a thermal oxide layer grown by a dry oxygen oxidation process, and the oxidation temperature is 800-1100° C. The thickness of the first barrier layer 206 ranges from Preferably The second barrier layer 207 comprises a polysilicon barrier layer, which is grown by chemical vapor deposition and has a thickness ranging from Preferably The third barrier layer 208 comprises a silicon nitride barrier layer, the silicon nitride barrier layer is grown by chemical vapor deposition, and has a thickness ranging from Preferably
[0092] In steps 1-2), refer to Figure 3 and Figure 4 , the first barrier layer 206, the second barrier layer 207 and the third barrier layer 208 are patterned, and the patterns formed by the first barrier layer 206, the second barrier layer 207 and the third barrier layer 208 are the same. Optionally, the patterning process includes photolithography and etching processes. The anti-reflection coating 209a and the photoresist layer 209 are sequentially coated on the surface of the third barrier layer 208, wherein the thickness of the anti-reflection coating 209a ranges from The thickness of the photoresist layer 209 ranges from The patterned photoresist layer 209 is obtained through exposure and development process, such as Figure 1 As shown. With the photoresist layer 209 as an etching barrier layer, the anti-reflection coating 209a, the third barrier layer 208, the second barrier layer 207 and the first barrier layer 206 are dry-etched in sequence to obtain the patterned first barrier layer 206, the second barrier layer 207 and the third barrier layer 208. Optionally, CF4, CHF3 or the like is used as an etching gas to etch the third barrier layer 208; Cl2, SF6, HBr or the like is used as an etching gas to etch the second barrier layer 207; CF4, CHF3 or the like is used as an etching gas to etch the first barrier layer 206.
[0093] In steps 1-3), refer to Figure 4 and Figure 5 , the first groove 201a is formed in the semiconductor substrate 201 by etching with the third barrier layer 208 as an etching barrier layer. Optionally, after the patterned first barrier layer 206, the second barrier layer 207 and the third barrier layer 208 are formed, the residual photoresist layer 209 and the anti-reflective coating 209a are removed by ashing and wet cleaning steps. The exposed semiconductor substrate 201 is dry-etched with the third barrier layer 208 as an etching barrier layer to form the first groove 201a. When the dry etching is used to etch the semiconductor substrate 201, it is necessary to maintain a high selectivity for the third barrier layer 208 as an etching barrier layer, and after the dry etching, the cross section of the formed first groove 201a is rectangular.
[0094] In step 7), refer to Fig.11 , using the second barrier layer 207 as a grinding stop layer, chemical mechanical polishing is used to remove the third barrier layer 208 and the second dielectric layer 205 above the second barrier layer 207. Optionally, the chemical mechanical polishing has different grinding resistances when grinding the second barrier layer 207, the third barrier layer 208 and the second dielectric layer 205, and the motor torques generated are also different. Therefore, the grinding end point can be judged by the change of the motor torque. When grinding to the second barrier layer 207, the grinding process is terminated in time and accurately stops on the second barrier layer 207. After the chemical mechanical polishing, the surface of the second barrier layer 207 is flush with the surface of the second dielectric layer 205 filled in the second groove 201b.
[0095] In step 8), refer to Fig.12 , using the first barrier layer 206 as an etching stop layer, the second barrier layer 207 is removed by dry etching. Optionally, Cl2, SF6, HBr, etc. are used as etching gases to remove the second barrier layer 207 by dry etching. The dry etching has a high selectivity for the silicon dioxide layer, so the second dielectric layer 205 is almost not etched, and the dry etching can stop on the first barrier layer 206.
[0096] In step 9), refer to Fig.13 , the first barrier layer 206 is removed by wet etching. Since after preparing the shallow trench isolation structure, it is also necessary to form an active area and other device structures on the surface of the semiconductor substrate 201, it is necessary to completely remove the first barrier layer 206 on the surface of the semiconductor substrate 201. Optionally, the first barrier layer 206 comprises a silicon dioxide barrier layer, and the first barrier layer 206 is removed by wet etching, and the wet etching may use a chemical solution such as DHF. The isolation layer 203 filled at the groove structure 206a in step 3) forms a protective structure 203a after removing the first barrier layer 206. The protective structure 203a covers and protects the liner layer 202 of the lower layer and part of the side wall of the second dielectric layer 205 filled in the second trench 201b, so that it will not be etched by the wet chemical solution, thereby avoiding the formation of edge gap (divot) defects.
[0097] Embodiment 2
[0098] See also Figure 5 , Fig. 9 and Fig.13 The present invention also provides a semiconductor structure, comprising:
[0099] Semiconductor substrate 201;
[0100] A first trench 201a is formed in the semiconductor substrate 201;
[0101] A liner layer 202 formed on the sidewall of the first trench 201a;
[0102] An isolation layer 203, located in the first trench 201a and covering at least the side and top of the liner layer 202;
[0103] A first dielectric layer 204 is located in the first trench 201a, and a thickness of the first dielectric layer 204 is less than a depth of the first trench 201a;
[0104] The second trench 201b is located in the first trench 201a and above the first dielectric layer 204 and the isolation layer 203; and
[0105] The second dielectric layer 205 is located in the second trench 201b.
[0106] In this embodiment, if Fig.13 As shown, a semiconductor substrate 201 is formed with Figure 5 The first trench 201a is marked in FIG. A liner layer 202 is formed on the sidewall and bottom of the first trench 201a. The side and top of the liner layer 202 are covered with an isolation layer 203. The first dielectric layer 204 is formed in the first trench 201a, and its thickness is less than the depth of the first trench 201a. The first dielectric layer 204 and the isolation layer 203 are formed as shown in FIG. Fig. 9 The second trench 201 b marked in FIG. 1 is filled with a second dielectric layer 205 .
[0107] Optionally, the semiconductor substrate 201 includes a silicon substrate, the liner layer 202 includes a silicon dioxide layer, the isolation layer 203 includes a silicon nitride layer, and the first dielectric layer 204 and the second dielectric layer 205 include silicon dioxide layers. The isolation layer 203 covers and protects the liner layer 202 and a portion of the sidewall of the second dielectric layer 205 filled in the second trench 201b from the top and side, so that the liner layer 202 and the second dielectric layer 205 filled in the second trench 201b will not be corroded by the wet process solution for etching silicon dioxide, thereby avoiding the formation of edge divot defects.
[0108] As an example, the cross-sectional shape of the first groove 201a includes a rectangle. Figure 5The first trench 201a can be formed by dry etching the semiconductor substrate 201. By introducing the first trench 201a with a rectangular cross-section, the cross-section of the resulting shallow trench isolation structure can be made rectangular, thereby improving the isolation effect of the shallow trench isolation structure.
[0109] As an example, the upper surface of the second dielectric layer 205 is at least flush with the top of the isolation layer 203. In this embodiment, the upper surface of the second dielectric layer 205 is higher than the top of the isolation layer 203, which can leave an etching margin for the second dielectric layer 205 in the subsequent wet etching process to prevent the top and exposed sidewalls of the second dielectric layer 205 from generating recessed defects due to etching.
[0110] As an example, the top width of the cross section of the second groove 201b is greater than the bottom width. In this embodiment, the first groove 201a and the second groove 201b are formed successively by etching and filling processes. Since the existing dielectric layer filling process is easy to form a void defect in a rectangular groove structure, by introducing the second groove 201b with a wide top and narrow bottom cross-section structure, it is ensured that there is no void defect in the second groove 201b after the second dielectric layer 205 is filled.
[0111] In summary, the present invention provides a semiconductor structure and a preparation method, the preparation method comprising: 1) providing a semiconductor substrate, forming a first trench in the semiconductor substrate; 2) forming a liner layer at least on the sidewall of the first trench; 3) forming an isolation layer on the upper surface of the liner layer, the isolation layer at least covering the side and top of the liner layer; 4) filling the first dielectric layer in the first trench; 5) etching and removing part of the first dielectric layer to form a second trench, the depth of the second trench being less than the depth of the first trench; 6) filling the second trench with a second dielectric layer, the second dielectric layer at least filling the second trench. The present invention also provides a semiconductor structure, comprising: a semiconductor substrate; a first trench, formed in the semiconductor substrate; a liner layer, formed on the sidewall of the first trench; an isolation layer, located in the first trench, and at least covering the side and top of the liner layer; a first dielectric layer, located in the first trench, the thickness of the first dielectric layer being less than the depth of the first trench; a second trench, located in the first trench, and located above the first dielectric layer and the isolation layer; a second dielectric layer, located in the second trench. The present invention avoids the formation of edge notch defects by using an isolation layer to cover the protective liner layer and the side wall of the dielectric layer at the edge of the groove; and adopts a preparation method of step-by-step filling of the dielectric layer to obtain a shallow trench isolation structure with no void defects and a rectangular cross-section, thereby improving the isolation effect and increasing the product yield.
[0112] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a semiconductor structure, characterized in that: The steps include: 1) providing a semiconductor substrate, and sequentially forming a first barrier layer, a second barrier layer, and a third barrier layer on the surface of the semiconductor substrate; performing patterning on the first barrier layer, the second barrier layer, and the third barrier layer, wherein the patterns formed by the first barrier layer, the second barrier layer, and the third barrier layer are the same; Using the third barrier layer as a hard mask layer, forming a first trench in the semiconductor substrate by etching; 2) forming a liner layer at least on the sidewall of the first trench; 3) forming an isolation layer on the upper surface of the liner layer, wherein the isolation layer at least covers the side and top of the liner layer; 4) filling the first trench with a first dielectric layer, wherein the first dielectric layer at least covers the isolation layer; 5) etching and removing a portion of the first dielectric layer to form a second trench, wherein the depth of the second trench is less than the depth of the first trench; and 6) filling the second trench with a second dielectric layer, wherein the second dielectric layer at least fills up the second trench; The semiconductor substrate includes a silicon substrate, the first barrier layer includes a silicon dioxide barrier layer, the second barrier layer includes a polysilicon barrier layer, the third barrier layer includes a silicon nitride barrier layer, and the liner layer includes a silicon dioxide layer; the liner layer formed in step 2) is also located on the side wall of the second barrier layer to form a groove structure at the side wall position of the first barrier layer; the isolation layer fills the groove structure.
2. The method for preparing a semiconductor structure according to claim 1, characterized in that: The cross-sectional shape of the first groove formed in step 1) includes a rectangle.
3. The method for preparing a semiconductor structure according to claim 1, characterized in that: The second trench formed in step 5) has a cross-section whose top width is greater than its bottom width.
4. The method for preparing a semiconductor structure according to claim 1, characterized in that: The depth of the first groove formed in step 1) ranges from 5. The method for preparing a semiconductor structure according to claim 1, characterized in that: The depth of the second groove formed in step 5) ranges from 6. The method for preparing a semiconductor structure according to claim 1, characterized in that: After step 6), the following steps are also included: 7) using the second barrier layer as a grinding stop layer, and removing the third barrier layer and the second dielectric layer above the second barrier layer by chemical mechanical grinding; 8) using the first barrier layer as an etching stop layer and removing the second barrier layer by dry etching; 9) Removing the first barrier layer by wet etching.
7. A semiconductor structure, characterized in that: include: Semiconductor substrate; A first trench formed in the semiconductor substrate; A liner layer formed on a sidewall of the first trench; an isolation layer, located in the first groove and covering at least the side and top of the liner layer; A first dielectric layer is located in the first trench, and a thickness of the first dielectric layer is less than a depth of the first trench; A second trench is located in the first trench and above the first dielectric layer and the isolation layer; and A second dielectric layer, located in the second trench; A protection structure covers the liner layer and a portion of the sidewall of the second dielectric layer filled in the second trench.
8. The semiconductor structure according to claim 7, characterized in that: A cross-sectional shape of the first groove includes a rectangle.
9. The semiconductor structure according to claim 7, characterized in that: The upper surface of the second dielectric layer is at least flush with the top of the isolation layer.
10. The semiconductor structure according to claim 7, characterized in that: A top width of a cross section of the second groove is greater than a bottom width.