Wafer, semiconductor device and method for manufacturing the same

By forming a trench in the dicing area of ​​the semiconductor device that is deeper than the wafer's allowable test circuit and filling it with a protective layer, the problem of cracks caused by dicing is solved and the yield and stability of the chip are improved.

CN111293047BActive Publication Date: 2024-10-15CHANGXIN MEMORY TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811393018.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-11-21
Publication Date
2024-10-15
Estimated Expiration
2038-11-21

AI Technical Summary

Technical Problem

In the manufacturing process of semiconductor integrated circuits, cutting metal circuits can easily lead to cracks in the cutting lanes, affecting the yield and stability of the effective circuits in the chip.

Method used

Form a trench in the cutting area and fill the trench with a protective layer. The depth of the trench is greater than or equal to the depth of the wafer acceptance test circuit. The test pads are exposed through photolithography technology to reduce cutting stress and buffer the occurrence of cracks. .

Benefits of technology

It effectively reduces the stress during cutting, reduces the occurrence and expansion of cracks, and improves the yield and stability of the chip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111293047B_ABST
    Figure CN111293047B_ABST
Patent Text Reader

Abstract

The present disclosure provides a wafer, a semiconductor device and a manufacturing method thereof, and relates to the field of semiconductor technology. The wafer includes: a substrate; a dielectric layer, located on a side surface away from the substrate; a wafer acceptance test circuit, formed in the dielectric layer, and the wafer acceptance test circuit includes a metal interconnection layer; a groove, formed in the dielectric layer and located on the side of the wafer acceptance test circuit, and the groove is filled with a protective layer; wherein the depth of the groove is greater than or equal to the depth of the wafer acceptance test circuit. When the chip is cut along the cutting road area, the protective layer material is elastic, which can buffer the stress problem when the chip is cut, reduce the generation of cracks, and when cracks occur, the groove and the filled protective layer material can prevent the cracks from expanding, thereby improving the yield and stability of the chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a wafer, a semiconductor device and a method for manufacturing the same. Background Art

[0002] During the manufacturing process of semiconductor integrated circuits, wafers need to undergo a wafer acceptance test (WAT). In semiconductor manufacturing design, independent circuits are usually placed in the cutting path area to test the electrical properties of the chip and monitor whether there are problems in the manufacturing process. These circuits include metal oxide field effect transistors (MOS), vias, metal circuits, etc. The WAT test is an electrical test of the test structure on the wafer after the manufacturing process is completed.

[0003] After the WAT test, the chip needs to be cut with a diamond knife during the packaging process to perform the dicing step. If the metal circuit is cut, it is easy to pull the metal circuit and cause cracks in the cutting path, which will affect the yield and stability of the effective circuit in the chip. If the crack is too large, the effective circuit in the chip will be more easily damaged, affecting the chip yield.

[0004] Therefore, it is necessary to provide a new technical solution to improve one or more problems existing in the above solutions.

[0005] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0006] The purpose of the present disclosure is to provide a wafer, a semiconductor device and a method for manufacturing the same, which can at least to some extent overcome the technical problem of cracking caused by cutting due to the limitations and defects of the related art.

[0007] According to one aspect of the present disclosure, a wafer is provided, comprising a die region and a scribe line region, wherein the scribe line region comprises:

[0008] substrate;

[0009] A dielectric layer, located on a side surface away from the substrate;

[0010] A wafer acceptance test circuit is formed in the dielectric layer, and the wafer acceptance test circuit includes a metal interconnect layer;

[0011] A groove is formed in the dielectric layer and is located on the side of the wafer acceptance test circuit, and the groove is filled with a protective layer;

[0012] Wherein, the depth of the groove is greater than or equal to the depth of the wafer acceptance test circuit.

[0013] In one embodiment, the scribe line area further includes a test pad, and the test pad is located on the dielectric layer.

[0014] In one embodiment, the trench surrounds the wafer acceptance test circuit.

[0015] In one embodiment, the groove has a notch perpendicular to the cutting direction.

[0016] In one embodiment, the protective layer includes one or more of polyimide and tetraethyl orthosilicate.

[0017] In one embodiment, the width of the trench is 1-10 microns, and / or the horizontal distance between the trench and the WAT circuit is 1-10 microns.

[0018] In one embodiment, the depth of the trench is greater than the depth of the wafer acceptance test circuit by more than 100 nm.

[0019] In one embodiment, the longitudinal section of the groove is rectangular or inverted trapezoidal.

[0020] In one embodiment, the groove is rectangular, circular or elliptical in a top view.

[0021] In one embodiment, the top view of the groove is in the shape of a multi-layer rectangle, a multi-layer circle, or a multi-layer ellipse.

[0022] According to another aspect of the present disclosure, a semiconductor device is provided, comprising the above-mentioned wafer.

[0023] According to another aspect of the present disclosure, there is provided a method for manufacturing a semiconductor device, comprising:

[0024] providing a substrate;

[0025] forming a dielectric layer including a wafer acceptance test circuit on the substrate;

[0026] forming a test pad on the dielectric layer including the wafer acceptance test circuit;

[0027] forming a groove in the dielectric layer and located at a side of the wafer acceptance test circuit, wherein a depth of the groove is greater than or equal to a depth of the wafer acceptance test circuit;

[0028] depositing a protective layer in the trench;

[0029] forming an opening on the protective layer by photolithography so as to expose the test pad;

[0030] Wherein, the wafer acceptance test circuit and the groove are located in a dicing road area.

[0031] In one embodiment, the protective layer includes one or more of polyimide and tetraethyl orthosilicate.

[0032] In one embodiment, the width of the groove is 1-10 microns; and / or the horizontal distance between the groove and the wafer acceptance test circuit is 1-10 microns.

[0033] In one embodiment, the longitudinal section of the groove is rectangular or inverted trapezoidal.

[0034] In one embodiment, the groove is rectangular, circular or elliptical in a top view.

[0035] In one embodiment, the top view of the groove is in the shape of a multi-layer rectangle, a multi-layer circle, or a multi-layer ellipse.

[0036] In one embodiment, the depth of the trench is greater than the depth of the wafer acceptance test circuit by more than 100 nm.

[0037] By forming a groove located at the side of the WAT circuit in the cutting road area, and filling the groove with a protective layer, when the chip is cut along the cutting road area, the stress problem during chip cutting can be buffered and the generation of cracks can be reduced.

[0038] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0040] Figure 1A A flowchart showing a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0041] Figure 1B A flow chart showing a method of forming a dielectric layer including a WAT ​​circuit on a substrate in one embodiment of the present disclosure is shown;

[0042] Figure 1C A flow chart showing a method for forming a trench by a mask-photolithography process in one embodiment of the present disclosure;

[0043] Figure 2A-2GA cross-sectional view showing various stages in a method for manufacturing a semiconductor device according to another embodiment of the present disclosure;

[0044] Figure 3 A top view of a semiconductor device in one embodiment of the present disclosure is shown;

[0045] Figure 4 A top view of a semiconductor device in another embodiment of the present disclosure is shown;

[0046] Figure 5 A top view of a semiconductor device in another embodiment of the present disclosure is shown;

[0047] Figure 6 A top view of a semiconductor device in another embodiment of the present disclosure is shown;

[0048] Figure 7 A longitudinal cross-sectional view of a semiconductor device in one embodiment of the present disclosure is shown;

[0049] Figure 8 A longitudinal cross-sectional view of a semiconductor device in another embodiment of the present disclosure is shown;

[0050] Fig. 9 A schematic diagram of a longitudinal cross-sectional view of a semiconductor device in another embodiment of the present disclosure is shown. DETAILED DESCRIPTION

[0051] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided so that the disclosure will be more comprehensive and complete and to fully convey the concepts of the example embodiments to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.

[0052] In addition, the accompanying drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same reference numerals in the drawings represent the same or similar parts, and thus their repeated description will be omitted.

[0053] In the related art, an independent WAT circuit can be placed in the cutting path area to test the electrical properties of the chip. The WAT circuit may include a metal interconnect layer in a dielectric layer on a substrate, and a test pad formed on the dielectric layer. The present disclosure provides an improved semiconductor device, such as Figure 2GAs shown, the semiconductor device includes a cutting path area 205, which includes a substrate 201, a dielectric layer 202 located on the substrate 201, a WAT ​​circuit 203 formed in the dielectric layer 202, and a groove 206 formed in the dielectric layer 202 and located on the side of the WAT circuit 203, wherein the communication has an opening on the surface of the dielectric layer, and the groove 206 is filled with a protective layer 207; wherein the depth of the groove 206 is greater than or equal to the depth of the WAT circuit 203, that is, a side of the groove 206 close to the substrate 201 is lower than or equal to a side of the metal layer of the WAT circuit 203 close to the substrate 201.

[0054] The method for forming the semiconductor device is described below with reference to the accompanying drawings.

[0055] Figure 1A A flowchart showing a method for manufacturing a semiconductor device according to an embodiment of the present disclosure is shown.

[0056] like Figure 1A As shown, in step S102, a substrate is provided.

[0057] In an exemplary embodiment of the present disclosure, the substrate can be a silicon substrate such as a silicon epitaxial wafer, silicon on an insulating layer, or a substrate of other semiconductor materials such as GaN, and the substrate can be an intrinsic semiconductor substrate, or an N-type doped or P-type doped semiconductor substrate, which is not limited in the embodiment of the present disclosure.

[0058] Step S104: forming a dielectric layer including a WAT ​​circuit on the substrate.

[0059] In an exemplary embodiment of the present disclosure, the material of the dielectric layer may be one or more of silicon oxide, silicon nitride or silicon oxynitride. In a specific implementation, the dielectric layer may be formed by chemical vapor deposition, atomic layer deposition, etc. It is understood that the dielectric layer may be a single insulating material layer, or may be formed by stacking multiple insulating material layers of the same or different materials.

[0060] In an exemplary embodiment of the present disclosure, the WAT circuit may be one or more metal layers. The multiple metal layers may realize electrical connection between two metal layers through conductive pillars. The material of the metal layer and the material of the conductive pillar may be the same, so that they are easy to form in a unified process. The material of the metal layer may be one of metals such as copper, aluminum, tungsten, gold, etc., or an alloy material of the above metal materials.

[0061] Combination Figure 1B A method for forming a dielectric layer including a WAT ​​circuit on a substrate in one embodiment is described.

[0062] like Figure 1BAs shown, in step S1041, a first dielectric layer is deposited on a substrate. The deposition method may be chemical vapor deposition, atomic layer deposition, or the like.

[0063] Step S1042, forming a photoresist layer on the first dielectric layer by a spraying method.

[0064] Step S1043, performing exposure and development through a corresponding mask plate to transfer the pattern of the mask plate to the dielectric layer.

[0065] Step S1044, by etching, the opening portion not covered and protected by the photoresist is removed to form a groove. The etching method can be dry etching, wet etching or plasma etching.

[0066] Step S1045, depositing a conductive material in the groove. The deposition method may be physical vapor deposition or electroplating.

[0067] Step S1046, flattening the surface by a polishing process to form a metal layer. The polishing process may be chemical mechanical polishing.

[0068] Step S1047 , forming a second dielectric layer on the first dielectric layer to cover the first dielectric layer.

[0069] By repeating the above steps, multiple metal layers can be formed.

[0070] If two metal layers need to be connected via a conductive column, exposure and development can be performed on the dielectric layer between the two metal layers to form a through hole, and then metal is deposited to form a conductive column to electrically connect the two metal layers.

[0071] Step S106: forming a test pad on the dielectric layer including the WAT circuit.

[0072] In an exemplary embodiment of the present disclosure, the test pad can be formed by the following method: depositing a metal layer on the surface of the dielectric layer, forming a photoresist layer on the metal layer, transferring the pattern to the metal layer by photolithography technology, and etching to form the required test pad. The test pad can be connected to the metal layer below through a conductive column.

[0073] Step S108 , forming a groove located at the side of the WAT circuit in the dielectric layer, wherein the depth of the groove is greater than or equal to the depth of the WAT circuit.

[0074] The grooves can be formed by a mask-photolithography process. Figure 1C As shown, the mask lithography process may include:

[0075] Step S1081, forming a photoresist layer on the surfaces of the dielectric layer and the test pad;

[0076] Step S1082, performing exposure through a corresponding mask plate to transfer the pattern of the mask plate to the photoresist layer;

[0077] Step S1083, through development, the photoresist layer is exposed to form a groove area, and the groove is located at the side of the WAT circuit;

[0078] Step S1084, forming a groove by etching, wherein the etching can be dry etching, wet etching or plasma etching;

[0079] Step S1085, removing the photoresist layer to obtain a trench structure.

[0080] Step S110, depositing a protective layer in the groove. A protective layer is formed in the groove and on the surface of the test pad and the dielectric layer. The method of forming the protective layer can be chemical vapor deposition, atomic layer deposition, etc. The material of the protective layer can be one or more combinations of materials such as polyimide and tetraethyl orthosilicate (TEOS).

[0081] Step S112: forming an opening on the protection layer by photolithography to expose the test pad.

[0082] In an exemplary embodiment of the present disclosure, the test pad may be exposed by the following photolithography technology: a photoresist layer is formed on the protection layer, a pattern is transferred to the protection layer by the photolithography technology, and the exposed protection layer is etched to expose the test pad.

[0083] In the above embodiment, in the cutting path area, a groove is formed on the side of the WAT circuit, and a protective layer is filled in the groove. In this way, when the chip is cut along the cutting path area, the protective layer is elastic, which can buffer the stress problem during chip cutting and reduce the occurrence of cracks. When cracks occur, the protective layer material filled in the groove can prevent the cracks from expanding, thereby improving the yield and stability of the chip.

[0084] Figure 2A-2G Cross-sectional views showing various stages in a method for manufacturing a semiconductor device according to another embodiment of the present disclosure.

[0085] like Figure 2A As shown, a substrate 201 is provided.

[0086] like Figure 2B As shown, a dielectric layer 202 including a WAT ​​circuit 203 is formed on a substrate 201 .

[0087] like Figure 2C As shown, a test pad 204 is formed on the dielectric layer. The test pad 204 is generally located above the WAT circuit 203.

[0088] like Figure 2D As shown, a photoresist 209 is coated on the dielectric layer 202, and a trench pattern is photolithographically processed.

[0089] like Figure 2E As shown, the trench 206 is formed by etching, and the photoresist 209 is removed.

[0090] like Figure 2F As shown, a protection layer 207 is deposited on the trench 206 and the dielectric layer 202 .

[0091] like Figure 2G As shown, the protection layer 207 is exposed and developed, thereby exposing the test pad 204 for testing.

[0092] In the above embodiment, the WAT circuit 203 , the test pad 204 and the groove 206 are all located in the scribe line region, that is, in the region between the scribe lines 205 .

[0093] A semiconductor device formed by a semiconductor manufacturing method similar to the above is Figure 2G As shown, the semiconductor device includes a scribe line region, wherein the scribe line region includes: a substrate; a dielectric layer located on the substrate; a WAT ​​circuit formed in the dielectric layer; a groove formed in the dielectric layer and surrounding the WAT circuit, the groove having an opening on a surface of the dielectric layer away from the substrate, and a protective layer filled in the groove; wherein the depth of the groove is greater than or equal to the depth of the WAT circuit. In one embodiment, the depth of the groove may be greater than the depth of the WAT circuit by 100 nm. In one embodiment, the wafer includes a grain region and a scribe line region as described above.

[0094] Figure 3 FIG. 2 shows a top view of a semiconductor device in one embodiment of the present disclosure. Figure 3 As shown, the top view of the groove 206 is a closed rectangle, which surrounds the WAT circuit 204. In one embodiment, the distance d1 between the groove 206 and the WAT circuit is 1-10 microns, for example, the distance d1 between the groove 206 and the WAT circuit can be 3 microns, 5 microns or 7 microns; in one embodiment, the width of the groove 206 is 1-10 microns, for example, the width of the groove 206 can be 3 microns, 5 microns or 7 microns.

[0095] Figure 4 FIG. 2 shows a top view of a semiconductor device in another embodiment of the present disclosure. Figure 4 As shown, the top view of the trench 206 is circular, which surrounds the WAT circuit 204. In one embodiment, the distance between the trench 206 and the WAT circuit is 1-10 microns, for example, the distance between the trench 206 and the WAT circuit can be 3 microns, 5 microns or 7 microns.

[0096] Figure 5 FIG. 2 shows a top view of a semiconductor device in another embodiment of the present disclosure. Figure 5 As shown, the top view of the groove 206 is a non-closed rectangle, which includes an opening 31 perpendicular to the cutting direction.

[0097] Figure 6 FIG. 2 shows a top view of a semiconductor device in another embodiment of the present disclosure. Figure 6 As shown, the top view of the groove 206 presents two non-closed circles, which include openings 32 perpendicular to the cutting direction.

[0098] The protective layer has an opening perpendicular to the cutting direction, thus forming an unclosed protective layer. In this way, there is no protective layer along the cutting direction of the diamond knife, which prevents the protective layer from warping or rolling up, while the protective layer in the groove can still prevent the expansion of cracks. In addition, the multi-layer protective groove can better prevent the cracks from extending into the chip.

[0099] In some embodiments, the top view of the groove 206 may be an ellipse or other shapes.

[0100] Figure 7 FIG. 2 shows a longitudinal cross-sectional view of a semiconductor device in one embodiment of the present disclosure. Figure 7 As shown, the groove 206 is rectangular along a longitudinal section perpendicular to the substrate, and its opening 41 is located on the surface of the dielectric layer away from the substrate.

[0101] Figure 8 A longitudinal cross-sectional view of a semiconductor device in another embodiment of the present disclosure is shown. Figure 8 As shown, the groove 206 is in an inverted trapezoidal shape along the longitudinal section perpendicular to the substrate, and its opening 41 is located on the surface of the dielectric layer away from the substrate. In one embodiment, the bottom width of the groove close to the substrate side is between 1-10 microns, for example, the bottom width of the groove close to the substrate side is 3 microns, 5 microns or 7 microns. The opening width of the groove away from the substrate side is between 2-12 microns, for example, the opening width of the groove away from the substrate side can be 4 microns, 6 microns, 8 microns or 10 microns, and the opening width is greater than the bottom width.

[0102] It should be pointed out that for inverted trapezoidal grooves, when filling the protective layer, the protective layer is more likely to fill the grooves completely; in addition, during cutting, cracks often start to occur from the top, so the width of the protective layer above is wider, which makes it easier to prevent the cracks from reaching the chip area.

[0103] In addition, it should be noted that when actually etching the groove, the bottom of the formed rectangle or inverted trapezoid is usually not horizontal, but presents a certain curvature. Fig. 9 As shown, the bottom of the groove has a curvature, and is shaped like an inverted trapezoid or an inverted triangle.

[0104] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.

Claims

1. A wafer comprising a die region and a scribe line region, characterized in that: The cutting road area includes: substrate; A dielectric layer, located on a side surface away from the substrate; A wafer acceptance test circuit is formed in the dielectric layer, and the wafer acceptance test circuit includes a metal interconnect layer; A groove is formed in the dielectric layer, the groove surrounds the wafer acceptance test circuit, the groove has an opening perpendicular to the cutting direction, the groove is filled with a protective layer, the protective layer is elastic, and the protective layer in the groove has an opening perpendicular to the cutting direction to form an unsealed protective layer so that there is no protective layer on the path along the cutting direction; Wherein, the depth of the groove is greater than or equal to the depth of the wafer acceptance test circuit.

2. The wafer according to claim 1, characterized in that The scribe line area also includes a test pad, and the test pad is located on the dielectric layer.

3. The wafer according to any one of claims 1 to 2, characterized in that: The protective layer includes one or more of polyimide and tetraethyl orthosilicate.

4. The wafer according to any one of claims 1 to 2, characterized in that: The width of the groove is 1-10 microns, and / or the horizontal distance between the groove and the wafer acceptance test circuit is 1-10 microns.

5. The wafer according to any one of claims 1 to 2, characterized in that: The longitudinal section of the groove is rectangular or inverted trapezoidal.

6. A semiconductor device, characterized in that: Comprising a wafer according to any one of claims 1-5.

7. A method for manufacturing a semiconductor device, characterized in that: include: providing a substrate; forming a dielectric layer including a wafer acceptance test circuit on the substrate; forming a test pad on the dielectric layer including the wafer acceptance test circuit; forming a groove surrounding the wafer acceptance test circuit in the dielectric layer, wherein the depth of the groove is greater than or equal to the depth of the wafer acceptance test circuit, and the groove has an opening perpendicular to the cutting direction; Depositing a protective layer in the groove, wherein the protective layer is elastic and has an opening in the groove perpendicular to the cutting direction to form an unsealed protective layer so that there is no protective layer on the path along the cutting direction; forming an opening on the protective layer on the dielectric layer by photolithography so as to expose the test pad; Wherein, the wafer acceptance test circuit and the groove are located in a dicing road area.

8. The method for manufacturing a semiconductor device according to claim 7, wherein: The protective layer includes one or more of polyimide and tetraethyl orthosilicate.

9. The method for manufacturing a semiconductor device according to claim 7 or 8, characterized in that: The width of the groove is 1-10 microns; and / or the horizontal distance between the groove and the wafer acceptance test circuit is 1-10 microns.