A GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate and a method for preparing the same
By preparing a GaN/two-dimensional AlN heterojunction rectifier on a silicon substrate, the problems of insufficient frequency and efficiency of existing rectifiers in high-frequency and high-efficiency applications are solved, and a two-dimensional electron gas with high concentration and mobility is achieved. Improved the stability and reverse leakage performance of the rectifier.
Patent Information
- Application Number
- CN202010346191.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-04-27
AI Technical Summary
Existing rectifiers suffer from insufficient frequency and efficiency improvements in high-frequency, high-efficiency applications. In particular, the polarization intensity of AlGaN heterojunctions is difficult to control, making it difficult to meet the needs of the new generation of microwave RF systems.
A GaN/two-dimensional AlN heterojunction rectifier on a silicon substrate is used, by sequentially stacking a silicon substrate, a GaN buffer layer, a carbon-doped semi-insulating GaN layer, a two-dimensional AlN layer, an undoped GaN layer, and an undoped InGaN layer. layer and SiNx passivation layer, and set up mesa isolation grooves and Schottky contact electrodes, and use low-temperature pulse laser deposition technology and plasma-enhanced chemical vapor deposition method to prepare the rectifier.
It achieves ultra-high concentration and mobility of two-dimensional electron gas, greatly improves frequency and efficiency, has good stability and reliability of the rectifier, and has excellent reverse leakage performance, making it suitable for the application of high-frequency devices.
Smart Images

Figure CN111430457B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of rectifiers, and in particular to a GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate and a preparation method thereof. Background Art
[0002] Space wireless energy transmission technology has been a very active research hotspot in recent years. It has advantages that contact energy transmission modes do not have, such as strong environmental affinity, green environmental protection, and safe transmission. Rectifiers, as an indispensable part of space wireless energy transmission systems, are widely used in military and civilian fields such as satellite systems, aerospace vehicles, and household appliances. At present, most rectifiers use the first-generation semiconductor Si. However, Si is an indirect bandgap semiconductor with a small bandgap width and a small breakdown field strength, so it is difficult to apply to high-frequency devices. As a representative of the third-generation semiconductor, group III nitrides have the characteristics of high breakdown voltage, large bandgap width, high thermal conductivity, high electron saturation rate, and high carrier mobility, so they have great potential in the preparation of rectifiers. At present, rectifiers prepared based on group III nitrides mostly use AlGaN / GaN heterostructures. The polarization effect of the GaN / AlGaN heterojunction will produce a two-dimensional electron gas with high surface density and high electron mobility at the interface, which can realize the preparation of radio frequency devices with a theoretical frequency of THz. However, since the polarization strength of the AlGaN heterojunction is difficult to control, too thick an AlGaN layer will lead to relaxation, and too thin an AlGaN layer will reduce its quality and uniformity, making it difficult to meet the high-frequency and high-efficiency application requirements of the new generation of microwave radio frequency systems. Therefore, designing a new heteroepitaxial structure with greater polarization strength is the key to achieving high-frequency and high-efficiency rectifier devices. The thickness of two-dimensional AlN is only a few atomic layers, so the stress and polarization strength it is subject to are greater than those of AlGaN. Therefore, the GaN / two-dimensional AlN heterostructure can produce a two-dimensional electron gas with ultra-high concentration and ultra-high mobility, thereby achieving a significant increase in frequency and efficiency. Summary of the invention
[0003] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the object of the present invention is to provide a GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate and a preparation method thereof, which has the advantages of high compatibility with existing production means and easy implementation.
[0004] The purpose of the present invention is achieved by one of the following technical solutions.
[0005] A GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate comprises a silicon substrate, a GaN buffer layer, a carbon-doped semi-insulating GaN layer, a two-dimensional AlN layer, a non-doped GaN layer, a non-doped InGaN layer and a SiNx passivation layer stacked in sequence, and also comprises a mesa isolation groove and a Schottky contact electrode arranged on one side of the non-doped InGaN layer, wherein the mesa isolation groove contacts the non-doped GaN layer, the non-doped InGaN layer, the SiNx passivation layer and the Schottky contact electrode, and the Schottky contact electrode contacts the mesa isolation groove and the non-doped GaN layer.
[0006] As a preferred solution of the present invention, the thickness of the GaN buffer layer is 650-900nm.
[0007] As a preferred embodiment of the present invention, the doping concentration of the carbon-doped semi-insulating GaN layer is 5.0×10 18 ~6.0×10 18 cm -3 , thickness is 80~180 nm.
[0008] As a preferred embodiment of the present invention, the thickness of the two-dimensional AlN layer is 2 to 4 atomic layers.
[0009] As a preferred embodiment of the present invention, the thickness of the two-dimensional AlN layer is 2 atomic layers.
[0010] As a preferred solution of the present invention, the thickness of the undoped GaN layer is 350-550 nm.
[0011] As a preferred solution of the present invention, the thickness of the non-doped InGaN layer is 50-200 nm.
[0012] As a preferred solution of the present invention, in the SiNx passivation layer, x=1.29-1.51.
[0013] As a preferred embodiment of the present invention, the depth of the mesa isolation groove (8) is 1.2-1.5 μm; and the thickness of the Schottky contact electrode (9) is 220-250 nm.
[0014] As a preferred solution of the present invention, the depth of the mesa isolation groove is 1.5 μm; the thickness of the Schottky contact electrode is 250 nm.
[0015] The method for preparing a GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate as described in any one of the above items comprises the following steps:
[0016] (1) A GaN buffer layer, a carbon-doped semi-insulating GaN layer, a two-dimensional AlN layer, an undoped GaN layer, and an undoped InGaN layer are sequentially grown on a silicon substrate to obtain a rectifier epitaxial wafer;
[0017] (2) placing the rectifier epitaxial wafer obtained in step (1) in acetone and anhydrous ethanol for ultrasonic treatment in turn, taking it out and washing it with deionized water and then drying it with nitrogen;
[0018] (3) Transferring the Schottky contact pattern to the rectifier epitaxial wafer: uniformly spin-coating photoresist on the rectifier epitaxial wafer obtained in step (2), then placing it in a photolithography machine for exposure, and finally cleaning the epitaxial wafer with a developer to reveal the pattern;
[0019] (4) using reactive ion etching to etch a groove along the Schottky contact electrode pattern in the rectifier epitaxial wafer to obtain an ohmic contact electrode;
[0020] (5) Preparation of Schottky contact electrode: placing the rectifier epitaxial wafer with the ohmic contact electrode pattern groove obtained in step (4) into an electron beam evaporation device, then evacuating the chamber and bombarding the metal target with an electron gun to deposit the metal on the surface of the epitaxial wafer. After the evaporation is completed, the epitaxial wafer is annealed;
[0021] (6) Immerse the rectifier epitaxial wafer in the degumming solution and rinse it with deionized water. Then, place the epitaxial wafer in acetone for ultrasonic treatment and blow dry it with nitrogen.
[0022] (7) Aligning the rectifier epitaxial wafer by the alignment mark in the mask, repeating step (3), photolithography and developing at the corresponding position, preparing the device ohmic contact electrode pattern and cleaning;
[0023] (8) Preparation of ohmic contact electrode: repeating steps (5) and (6), depositing electrode metal, annealing and cleaning, and completing the preparation of ohmic contact electrode;
[0024] (9) Preparation of silicon nitride passivation layer: placing the rectifier epitaxial wafer obtained in step (8) into a plasma enhanced chemical vapor deposition device, then heating, evacuating, introducing carrier gas and reaction gas, and finally depositing SiNx passivation on the surface of the epitaxial wafer;
[0025] (10) Repeat step (3) to expose and develop the ohmic contact electrode and the Schottky contact electrode to expose the SiNx on the two electrodes;
[0026] (11) Using a wet etching method, the exposed SiNx is etched away, and finally step (6) is repeated to remove the photoresist and SiNx passivation layer remaining on the surface of the rectifier epitaxial wafer;
[0027] (12) Aligning the mask alignment marks, repeating steps (3) and (4), transferring the mesa isolation pattern to the surface of the epitaxial wafer and etching grooves on the surface;
[0028] (13) placing the rectifier epitaxial wafer obtained in step (12) into a plasma-assisted chemical vapor deposition device, repeating step (8), and depositing a SiNx passivation layer in the groove etched in step (12);
[0029] (14) Repeat step (11) to remove excess photoresist on the surface of the epitaxial wafer, and then remove residual photoresist and SiNx on the surface of the rectifier epitaxial wafer by soaking in a degumming solution and ultrasonic cleaning to complete the preparation of the GaN / two-dimensional AlN heterojunction rectifier on the silicon substrate.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The two-dimensional AlN / GaN thin film heterostructure of the present invention can generate a two-dimensional electron gas with ultra-high concentration and electron mobility, thereby achieving a significant increase in frequency and efficiency. The electron gas concentration of the rectifier prepared in Example 1 is as high as 10 14 cm -2 , and the mobility is as high as 3000 cm 2 / V·s.
[0032] (2) The defect density of the material film of the present invention is small. The half-width of the GaN (0002) x-ray rocking curve of the GaN film of Example 1 is 0.09°.
[0033] (3) The stability and reliability of the rectifier of the present invention are very good. The turn-on voltage of Example 1 is 0.75 V, and the calculated specific on-resistance R ON is 8.8 mΩ / sq.
[0034] (4) The reverse leakage performance of the rectifier of the present invention is very good. Under a reverse bias voltage of -20 V, the leakage current of the rectifier prepared in Example 1 was measured to be -0.0003 A. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a cross-sectional schematic diagram of the preparation of the rectifier chip according to Example 1 of the present invention.
[0036] Figure 2 3 is a graph of the GaN (0002) x-ray rocking curve of Example 1 of the present invention.
[0037] Figure 3 The rectifier forward direction of the embodiment 1 of the present invention is JV Graph.
[0038] Figure 4 The rectifier reverse current of the embodiment 1 of the present invention is IV Graph. DETAILED DESCRIPTION
[0039] The specific implementation of the present invention is further described below in conjunction with the examples and drawings, but the implementation of the present invention is not limited thereto.
[0040] The structure of the rectifier of the present invention is as follows Figure 1 As shown, it includes a silicon substrate 1, a GaN buffer layer 2, a carbon-doped semi-insulating GaN layer 3, a two-dimensional AlN layer 4, an undoped GaN layer 5, an undoped InGaN layer 6 and a SiNx passivation layer 7 stacked in sequence, and also includes a mesa isolation groove 8 and a Schottky contact electrode 9 arranged on one side of the undoped InGaN layer 6, wherein the mesa isolation groove 8 is in contact with the undoped GaN layer 5, the undoped InGaN layer 6, the SiNx passivation layer 7 and the Schottky contact electrode 9, and the Schottky contact electrode 9 is in contact with the mesa isolation groove 8 and the undoped GaN layer 5.
[0041] Example 1
[0042] The method for preparing a rectifier chip suitable for working under AC frequency on a silicon substrate of this embodiment:
[0043] (1) A rectifier epitaxial wafer is grown on a silicon substrate using low-temperature pulsed laser deposition technology, including a GaN buffer layer 2 grown on a silicon substrate 1, and a carbon-doped semi-insulating GaN layer 3 grown on the GaN buffer layer 2, with a doping concentration of 5.9×10 18 cm -3 , a non-doped two-dimensional AlN layer 4 grown on a carbon-doped semi-insulating GaN layer 3, a non-doped GaN layer 5 grown on the non-doped two-dimensional AlN layer 4, and a non-doped InGaN layer 6 grown on the non-doped GaN layer; the GaN buffer layer has a thickness of 800nm, the carbon-doped semi-insulating GaN layer has a thickness of 80nm; the non-doped two-dimensional AlN layer has a thickness of 2 atomic layers; the non-doped GaN layer has a thickness of 450nm; the non-doped InGaN layer has a thickness of 120nm;
[0044] (2) The rectifier epitaxial wafer was placed in acetone and anhydrous ethanol for ultrasonic treatment for 5 min, then washed with deionized water and dried with nitrogen;
[0045] (3) Spin-coat the cleaned rectifier epitaxial wafer with positive photoresist, model AZ5214, with a thickness of 0.3 μm, place the epitaxial wafer coated with photoresist on a hot plate for pre-baking for 45 seconds, then place it in a photolithography machine for exposure, with an exposure time of 5 seconds, then immerse the exposed epitaxial wafer in a developer, model RZX3038, for 60 seconds to make the pattern on the epitaxial wafer appear, and rinse the epitaxial wafer with deionized water and blow dry with nitrogen; finally, place the epitaxial wafer on a hot plate for baking to harden the film, with a baking time of 45 seconds;
[0046] (4) Using reactive ion etching, a groove is etched along the Schottky contact electrode pattern in the rectifier epitaxial wafer, and the groove depth is 250 nm;
[0047] (5) Place the rectifier epitaxial wafer with the ohmic contact electrode pattern grooves obtained in step (4) into an electron beam evaporation device and reduce the vacuum degree of the chamber to 2×10 -5 Pa, followed by sequential evaporation of electrode metals MoS2 / Ni / Au. After the evaporation, the rectifier epitaxial wafer was annealed at 400°C for 55 minutes;
[0048] (6) Immerse the rectifier epitaxial wafer with the prepared ohmic contact electrode in the degumming solution for 70 minutes, take it out, rinse it with deionized water, and place it in acetone for 5 minutes of ultrasonic treatment, then take it out, rinse it with deionized water and blow it dry with nitrogen;
[0049] (7) Aligning the rectifier epitaxial wafer through the alignment marks in the mask plate, repeating step (3), photolithography and developing at the corresponding position, and preparing the device Schottky contact electrode pattern area exposed on the rectifier epitaxial wafer;
[0050] (8) Preparation of ohmic contact electrode 9 for rectifier epitaxial wafer after photolithography. Place the rectifier epitaxial wafer with device ohmic contact pattern into electron beam evaporation equipment and evacuate the chamber to a vacuum degree of 2×10 -5 Pa, then sequentially evaporate the ohmic contact electrode materials Ti / Al / Ni / Au. Finally, repeat step (6) to remove the photoresist and evaporated metal remaining on the surface of the epitaxial wafer;
[0051] (9) The SiNx passivation layer 7 is prepared by plasma enhanced chemical vapor deposition. The rectifier epitaxial wafer with the prepared electrode is placed in a plasma enhanced chemical vapor deposition device. The temperature of the device is raised to 800°C and the vacuum degree of the chamber is evacuated to 2×10 -5 Pa, deposition time 75 min;
[0052] (10) Repeat step (3) and prepare a mask plate on the surface of the epitaxial wafer by photolithography and development to expose the SiNx (x=1.33~1.5) on the ohmic contact electrode and the Schottky contact electrode pattern;
[0053] (11) Use a wet etching method to etch away the exposed SiNx passivation layer, remove it and rinse it with deionized water, and finally repeat step (6) to remove the residual photoresist and SiNx on the surface of the epitaxial wafer by soaking in a degumming solution and ultrasonic cleaning;
[0054] (12) Aligning through the mask alignment mark, repeating steps (3) and (4), preparing a mesa isolation pattern on the surface of the epitaxial wafer by photolithography and development, and using a reactive ion etching device to perform groove etching on the surface of the rectifier epitaxial wafer obtained in step (12) to a depth of 1.5 μm, and finally cleaning the surface of the epitaxial wafer with deionized water and drying it with nitrogen;
[0055] (13) Preparation of mesa isolation passivation layer: Place the rectifier epitaxial wafer into a plasma-assisted chemical vapor deposition device, repeat the process of step (9), and deposit a SiNx passivation layer in the etched groove of the rectifier epitaxial wafer for 75 min;
[0056] (14) Repeat step (11) to remove the excess SiNx layer on the surface of the rectifier epitaxial wafer. Then repeat step (6) to remove the residual SiNx and photoresist on the surface of the rectifier epitaxial wafer to complete the preparation of the GaN / two-dimensional AlN heterojunction rectifier on the silicon substrate.
[0057] The GaN (0002) x-ray rocking curve of the GaN film of the rectifier prepared in this embodiment is as follows: Figure 2 As shown, the half-height width is 0.09°. JV Curve like Figure 3 As shown, the turn-on voltage is 0.75 V, and the specific on-resistance R is calculated. ON The device has good stability and reliability under high power conditions. IV Curve like Figure 4 As shown in FIG. 1 , under a reverse bias voltage of -20 V, the leakage current of the device is -0.0003 A, and the reverse leakage performance is very good. At the same time, the electron gas concentration of the rectifier prepared in this embodiment is measured to be as high as 10 14 cm -2 , and the mobility is as high as 3000 cm 2 / V·s.
[0058] Example 2
[0059] The method for preparing a rectifier chip suitable for working under AC frequency on a silicon substrate of this embodiment:
[0060] (1) A rectifier epitaxial wafer is grown on a silicon substrate using low-temperature pulsed laser deposition technology, including a GaN buffer layer 2 grown on a silicon substrate 1, and a carbon-doped semi-insulating GaN layer 3 grown on the GaN buffer layer 2, with a doping concentration of 5.9×10 18 cm -3, a non-doped two-dimensional AlN layer 4 grown on a carbon-doped semi-insulating GaN layer 3, a non-doped GaN layer 5 grown on the non-doped two-dimensional AlN layer 4, and a non-doped InGaN layer 6 grown on the non-doped GaN layer; the GaN buffer layer has a thickness of 650nm, the carbon-doped semi-insulating GaN layer has a thickness of 120 nm; the non-doped two-dimensional AlN layer has a thickness of 3 atomic layers; the non-doped GaN layer has a thickness of 350nm; the non-doped InGaN layer has a thickness of 50nm;
[0061] (2) The rectifier epitaxial wafer was placed in acetone and anhydrous ethanol for ultrasonic treatment for 5 min, then washed with deionized water and dried with nitrogen;
[0062] (3) Spin-coat the cleaned rectifier epitaxial wafer with positive photoresist, model AZ5214, with a thickness of 0.3 μm, place the epitaxial wafer coated with photoresist on a hot plate for pre-baking for 45 seconds, then place it in a photolithography machine for exposure, with an exposure time of 3 seconds, then immerse the exposed epitaxial wafer in a developer, model RZX3038, for 45 seconds to make the pattern on the epitaxial wafer appear, and rinse the epitaxial wafer with deionized water and blow dry with nitrogen; finally, place the epitaxial wafer on a hot plate for baking to harden the film, with a baking time of 45 seconds;
[0063] (4) Using reactive ion etching, a groove is etched along the Schottky contact electrode pattern in the rectifier epitaxial wafer, and the groove depth is 250 nm;
[0064] (5) Place the rectifier epitaxial wafer with the ohmic contact electrode pattern grooves obtained in step (4) into an electron beam evaporation device and reduce the vacuum degree of the chamber to 3.5×10 -5 Pa, followed by sequential evaporation of electrode metals MoS2 / Ni / Au. After the evaporation, the rectifier epitaxial wafer is annealed at 700°C for 90 minutes;
[0065] (6) Immerse the rectifier epitaxial wafer with the prepared ohmic contact electrode in the degumming solution for 40 minutes, take it out, rinse it with deionized water, and place it in acetone for 5 minutes of ultrasonic treatment, then take it out, rinse it with deionized water and blow it dry with nitrogen;
[0066] (7) Aligning the rectifier epitaxial wafer through the alignment mark in the mask plate, repeating the photolithography process in step (3), photolithography and developing at the corresponding position, and preparing the device Schottky contact electrode pattern area exposed on the rectifier epitaxial wafer;
[0067] (8) Preparation of ohmic contact electrode 9 for rectifier epitaxial wafer after photolithography. Place the rectifier epitaxial wafer with device ohmic contact pattern into electron beam evaporation equipment and evacuate the chamber to a vacuum degree of 3.5×10 -5Pa, followed by sequential evaporation of ohmic contact electrode materials Ti / Al / Ni / Au. After evaporation, the rectifier epitaxial wafer is annealed at 700°C for 90 minutes. Finally, step (6) is repeated to remove the residual photoresist and evaporated metal on the surface of the epitaxial wafer;
[0068] (9) The SiNx passivation layer 7 is prepared by plasma enhanced chemical vapor deposition. The rectifier epitaxial wafer with the prepared electrode is placed in a plasma enhanced chemical vapor deposition device. The temperature of the device is raised to 800°C and the vacuum degree of the chamber is evacuated to 3.5×10 -5 Pa, deposition time 75 min;
[0069] (10) Repeat step (3) and prepare a mask plate on the surface of the epitaxial wafer by photolithography and development to expose the SiNx (x=1.33~1.5) on the ohmic contact electrode and the Schottky contact electrode pattern;
[0070] (11) Use a wet etching method to etch away the exposed SiNx passivation layer, remove it and rinse it with deionized water, and finally repeat step (6) to remove the remaining photoresist and SiNx on the surface of the epitaxial wafer;
[0071] (12) Aligning through the mask alignment mark, repeating steps (3) and (4), preparing a mesa isolation pattern on the surface of the epitaxial wafer by photolithography and development, and performing groove etching on the surface with an etching depth of 1.5 μm, and finally cleaning the surface of the epitaxial wafer with deionized water and drying it with nitrogen;
[0072] (13) Preparation of mesa isolation passivation layer: Place the rectifier epitaxial wafer into a plasma-assisted chemical vapor deposition device, repeat the process of step (9), and deposit a SiNx passivation layer in the etched groove of the rectifier epitaxial wafer for 75 min;
[0073] (14) Repeat step (11) to remove the excess SiNx layer on the surface of the rectifier epitaxial wafer. Then repeat step (6) to remove the residual SiNx and photoresist on the surface of the rectifier epitaxial wafer, and finally complete the preparation of the GaN / two-dimensional AlN heterojunction rectifier on the silicon substrate.
[0074] The GaN (0002) x-ray rocking curve half-width of the GaN film prepared in this embodiment is 0.09°. JV The turn-on voltage in the curve is 0.78V, and the calculated specific on-resistance R ON 9.1 mΩ / sq, so the stability and reliability of the device are very good under high power working conditions. IVIn the curve, under the reverse bias voltage of -20 V, the leakage current of the device is -0.0003 A, so the reverse leakage performance is very good. At the same time, it is measured that the electron gas concentration of the rectifier prepared in this embodiment is as high as 10 14 cm -2 , and the mobility is as high as 2900cm 2 / V·s.
[0075] Example 3
[0076] The method for preparing a rectifier chip suitable for working under AC frequency on a silicon substrate of this embodiment:
[0077] (1) A rectifier epitaxial wafer is grown on a silicon substrate using low-temperature pulsed laser deposition technology, including a GaN buffer layer 2 grown on a silicon substrate 1 and a carbon-doped semi-insulating GaN layer 3 grown on the GaN buffer layer 2, with a doping concentration of 5.9×10 18 cm -3 , a non-doped two-dimensional AlN layer 4 grown on a carbon-doped semi-insulating GaN layer 3, a non-doped GaN layer 5 grown on the non-doped two-dimensional AlN layer 4, and a non-doped InGaN layer 6 grown on the non-doped GaN layer; the buffer layer has a thickness of 900nm, the carbon-doped semi-insulating GaN layer has a thickness of 180nm; the non-doped two-dimensional AlN layer has a thickness of 4 atomic layers; the non-doped GaN layer has a thickness of 550nm; the non-doped InGaN layer has a thickness of 200nm;
[0078] (2) The rectifier epitaxial wafer was placed in acetone and anhydrous ethanol for ultrasonic treatment for 8 minutes, then washed with deionized water and dried with nitrogen;
[0079] (3) Spin-coat the cleaned rectifier epitaxial wafer with positive photoresist, model AZ5214, with a thickness of 0.9 μm, place the epitaxial wafer coated with photoresist on a hot plate for pre-baking for 45 seconds, then place it in a photolithography machine for exposure, with an exposure time of 7 seconds, then immerse the exposed epitaxial wafer in a developer, model RZX3038, for 45 seconds to make the pattern on the epitaxial wafer appear, and rinse the epitaxial wafer with deionized water and blow dry with nitrogen; finally, place the epitaxial wafer on a hot plate for baking to harden the film, with a baking time of 45 seconds;
[0080] (4) Using reactive ion etching, a groove is etched along the Schottky contact electrode pattern in the rectifier epitaxial wafer, with a groove depth of 250 nm;
[0081] (5) Place the rectifier epitaxial wafer with the ohmic contact electrode pattern grooves obtained in step (4) into an electron beam evaporation device and reduce the vacuum degree of the chamber to 5.5×10 -5Pa, followed by sequential evaporation of electrode metals MoS2 / Ni / Au. After the evaporation, the rectifier epitaxial wafer is annealed at 700°C for 90 minutes;
[0082] (6) Immerse the rectifier epitaxial wafer with the prepared ohmic contact electrode in the degumming solution for 95 minutes, take it out, rinse it with deionized water, and place it in acetone for 8 minutes of ultrasonic treatment, then take it out, rinse it with deionized water and blow it dry with nitrogen;
[0083] (7) Aligning the rectifier epitaxial wafer through the alignment mark in the mask plate, repeating the photolithography process in step (3), photolithography and developing at the corresponding position, and preparing the device Schottky contact electrode pattern area exposed on the rectifier epitaxial wafer;
[0084] (8) Preparation of ohmic contact electrode 9 for the rectifier epitaxial wafer after photolithography: Place the rectifier epitaxial wafer with the device ohmic contact pattern into an electron beam evaporation device and evacuate the chamber to a vacuum degree of 5.5×10 -5 Pa, followed by sequential evaporation of ohmic contact electrode materials Ti / Al / Ni / Au. Finally, repeat step (6) to remove the remaining photoresist and evaporated metal on the surface of the epitaxial wafer;
[0085] (9) The SiNx passivation layer 7 is prepared by plasma enhanced chemical vapor deposition. The rectifier epitaxial wafer with the prepared electrode is placed in a plasma enhanced chemical vapor deposition device. The temperature of the device is raised to 800°C and the vacuum degree of the chamber is evacuated to 1×10 -5 Pa, deposition time 110 min;
[0086] (10) Repeat the process of step (3), prepare a mask plate on the surface of the epitaxial wafer by photolithography and development, and expose the SiNx (x=1.33~1.5) on the ohmic contact electrode and the Schottky contact electrode pattern;
[0087] (11) Use a wet etching method to etch away the exposed SiNx passivation layer, remove it and rinse it with deionized water, and finally repeat step (6) to remove the remaining photoresist and SiNx on the surface of the epitaxial wafer;
[0088] (12) Aligning through the mask alignment mark, repeating steps (3) and (4), preparing a mesa isolation pattern on the surface of the epitaxial wafer by photolithography and development, and etching a groove on the surface with an etching depth of 1.5 μm, and finally cleaning the surface of the epitaxial wafer with deionized water and drying it with nitrogen;
[0089] (13) Preparation of mesa isolation passivation layer: The rectifier epitaxial wafer is placed in a plasma-assisted chemical vapor deposition device, and the process of step (9) is repeated to deposit a SiNx passivation layer in the etched groove of the rectifier epitaxial wafer. The deposition time is 110 min.
[0090] (14) After using the wet etching process in step (11) to remove the excess SiNx layer on the surface of the rectifier epitaxial wafer, the process in step (6) is used to remove the residual SiNx and photoresist on the surface of the rectifier epitaxial wafer by soaking in a degumming solution and ultrasonic cleaning, and finally the preparation of the GaN / two-dimensional AlN heterojunction rectifier on the silicon substrate is completed.
[0091] The GaN (0002) x-ray rocking curve half-width of the GaN film prepared in this embodiment is 0.095°. JV The turn-on voltage in the curve is 0.80V, and the calculated specific on-resistance R ON The device has good stability and reliability under high power conditions. IV In the curve, under the reverse bias voltage of -20 V, the leakage current of the device is -0.00035 A, so the reverse leakage performance is very good. At the same time, it is measured that the electron gas concentration of the rectifier prepared in this embodiment is as high as 10 14 cm -2 , and the mobility is as high as 3000 cm 2 / V·s.
[0092] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate, It is characterized in that The invention comprises a silicon substrate (1), a GaN buffer layer (2), a carbon-doped semi-insulating GaN layer (3), a two-dimensional AlN layer (4), an undoped GaN layer (5), an undoped InGaN layer (6) and a SiNx passivation layer (7) which are stacked in sequence, and also comprises a mesa isolation groove (8) and a Schottky contact electrode (9) arranged on one side of the undoped InGaN layer (6), wherein the mesa isolation groove (8) is in contact with the undoped GaN layer (5), the undoped InGaN layer (6), the SiNx passivation layer (7) and the Schottky contact electrode (9), and the Schottky contact electrode (9) is in contact with the mesa isolation groove (8) and the undoped GaN layer (5).
2. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 1, It is characterized in that The thickness of the GaN buffer layer (2) is 650-900 nm.
3. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 1, It is characterized in that The doping concentration of the carbon-doped semi-insulating GaN layer (3) is 5.0×10 18 ~6.0×10 18 cm -3 , thickness is 80~180 nm.
4. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 1, It is characterized in that The thickness of the two-dimensional AlN layer (4) is 2 to 4 atomic layers.
5. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 4, It is characterized in that The thickness of the two-dimensional AlN layer (4) is 2 atomic layers.
6. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 1, It is characterized in that The thickness of the non-doped GaN layer (5) is 350-550 nm.
7. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 1, It is characterized in that The thickness of the non-doped InGaN layer (6) is 50-200 nm.
8. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 1, It is characterized in that In the SiNx passivation layer (7), x=1.29-1.
51.
9. The GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate according to claim 1, It is characterized in that The depth of the mesa isolation groove (8) is 1.2-1.5 μm; the thickness of the Schottky contact electrode (9) is 220-250 nm.
10. A method for preparing a GaN / two-dimensional AlN heterojunction rectifier on a silicon substrate as claimed in any one of claims 1 to 9, It is characterized in that The following steps are involved: (1) A GaN buffer layer, a carbon-doped semi-insulating GaN layer, a two-dimensional AlN layer, an undoped GaN layer, and an undoped InGaN layer are sequentially grown on a silicon substrate to obtain a rectifier epitaxial wafer; (2) placing the rectifier epitaxial wafer obtained in step (1) in acetone and anhydrous ethanol for ultrasonic treatment in turn, taking it out and washing it with deionized water and then drying it with nitrogen; (3) Transferring the Schottky contact pattern to the rectifier epitaxial wafer: uniformly spin-coating photoresist on the rectifier epitaxial wafer obtained in step (2), then placing it in a photolithography machine for exposure, and finally cleaning the epitaxial wafer with a developer to reveal the pattern; (4) using reactive ion etching to etch a groove along the Schottky contact electrode pattern in the rectifier epitaxial wafer to obtain an ohmic contact electrode; (5) Preparation of Schottky contact electrode: placing the rectifier epitaxial wafer with the ohmic contact electrode pattern groove obtained in step (4) into an electron beam evaporation device, then evacuating the chamber and bombarding the metal target with an electron gun to deposit the metal on the surface of the epitaxial wafer. After the evaporation is completed, the epitaxial wafer is annealed; (6) Immerse the rectifier epitaxial wafer in the degumming solution and rinse it with deionized water. Then, place the epitaxial wafer in acetone for ultrasonic treatment and blow dry it with nitrogen. (7) Aligning the rectifier epitaxial wafer by the alignment mark in the mask, repeating step (3), photolithography and developing at the corresponding position, preparing the device ohmic contact electrode pattern and cleaning; (8) Preparation of ohmic contact electrode: repeating steps (5) and (6), depositing electrode metal, annealing and cleaning, and completing the preparation of ohmic contact electrode; (9) Preparation of silicon nitride passivation layer: placing the rectifier epitaxial wafer obtained in step (8) into a plasma enhanced chemical vapor deposition device, then heating, evacuating, introducing carrier gas and reaction gas, and finally depositing SiNx passivation on the surface of the epitaxial wafer; (10) Repeat step (3) to expose and develop the ohmic contact electrode and the Schottky contact electrode to expose the SiNx on the two electrodes; (11) Using a wet etching method, the exposed SiNx is etched away, and finally step (6) is repeated to remove the photoresist and SiNx passivation layer remaining on the surface of the rectifier epitaxial wafer; (12) Aligning the mask alignment marks, repeating steps (3) and (4), transferring the mesa isolation pattern to the surface of the epitaxial wafer and etching grooves on the surface; (13) placing the rectifier epitaxial wafer obtained in step (12) into a plasma-assisted chemical vapor deposition device, repeating step (8), and depositing a SiNx passivation layer in the groove etched in step (12); (14) Repeat step (11) to remove excess photoresist on the surface of the epitaxial wafer, and then remove residual photoresist and SiNx on the surface of the rectifier epitaxial wafer by soaking in a degumming solution and ultrasonic cleaning to complete the preparation of the GaN / two-dimensional AlN heterojunction rectifier on the silicon substrate.
Citation Information
Patent Citations
Two-dimensional ALN material and preparation method and application thereof
CN108321076A
GaN / two-dimensional AlN heterojunction rectifier on silicon substrate
CN212010980U
Heterojunction field effect transistor and manufacturing method thereof
US20090045439A1
GAN fin-typed transistor having high linearity and high electron mobility, and manufacturing method thereof
WO2018103606A1