Resin composition

By adding organic filler materials to the resin composition of the flexible substrate, combining thermosetting resin and inorganic filler materials, the contradiction between flexibility and adhesion is solved, and a resin composition with high flexibility, low adhesion and good handling is achieved. Suitable for the manufacture of multi-layer flexible substrates.

CN111748175BActive Publication Date: 2024-11-22AJINOMOTO CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010223164.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-27
Filing Date
2020-03-26
Publication Date
2024-11-22
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

When the conventional flexible substrate is fitted with an inorganic filler material, it is difficult to maintain excellent flexibility and low adhesion at the same time, and the handling ability is poor.

Method used

A resin composition including a thermosetting resin, an inorganic filler material, an organic filler material and an adhesive flexible agent is used, and the content of the organic filler material is more than 5%. By optimizing the component ratio and type selection, adhesion is suppressed and treatment properties are improved.

Benefits of technology

While maintaining excellent flexibility, adhesion is significantly suppressed, processing is improved, and a higher folding resistance and lower melt viscosity are achieved in the multi-layer flexible substrate, thereby enhancing pattern buriedness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The problem of the present invention is to provide a resin composition that suppresses adhesion to a low level while maintaining excellent flexibility. The solution of the present invention is a resin composition, which is a resin composition comprising (A) a thermosetting resin, (B) an inorganic filler, (C) an organic filler, and (D) an adhesive flexibilizer, wherein when the non-volatile component in the resin composition is set to 100% by mass, the content of the component (C) is 5% by mass or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition comprising a thermosetting resin and an inorganic filler. Background Art

[0002] In recent years, there has been an increasing demand for semiconductor components that are thinner, lighter, and have a higher mounting density. In order to meet this demand, the use of flexible substrates as base substrates used in semiconductor components has attracted attention. Compared with rigid substrates, flexible substrates can be thinner and lighter. In addition, since flexible substrates are soft and deformable, they can be bent and installed.

[0003] Generally, it is necessary to add a flexible resin component to the insulating material of the flexible substrate, but when adding a flexible resin component, the tackiness (adhesion) sometimes increases and the handling property is poor. In this case, the tackiness can be suppressed by adding an inorganic filler (Patent Document 1), but when the inorganic filler is added at a higher rate, it is difficult to take into account flexibility at the same time.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-95047. Summary of the invention

[0007] Problems to be solved by the invention

[0008] Therefore, an object of the present invention is to provide a resin composition having low tackiness while maintaining excellent flexibility.

[0009] Means for solving problems

[0010] In order to achieve the subject of the present invention, the present inventors conducted intensive research and found that by adding 5% by mass or more of (C) organic filler to a resin composition comprising (A) a thermosetting resin, (D) an adhesive flexibility agent, and (B) an inorganic filler, it is possible to suppress adhesion to a low level while maintaining excellent flexibility, thereby completing the present invention.

[0011] That is, the present invention includes the following contents:

[0012] [1] A resin composition comprising (A) a thermosetting resin, (B) an inorganic filler, (C) an organic filler, and (D) an adhesive flexibilizer, wherein:

[0013] When the non-volatile components in the resin composition are set to 100% by mass, the content of the component (C) is 5% by mass or more;

[0014] [2] The resin composition according to [1] above, wherein the content of the component (B) is 50% by mass or less when the non-volatile component in the resin composition is 100% by mass;

[0015] [3] The resin composition according to [1] or [2], wherein the content of the component (C) is 10% by mass or less when the non-volatile component in the resin composition is 100% by mass;

[0016] [4] The resin composition according to any one of [1] to [3] above, wherein the component (D) is selected from a resin having a polybutadiene structure, a polyrotaxane resin, a polyimide resin, and a maleimide resin having a dimer acid skeleton;

[0017] [5] The resin composition according to any one of [1] to [4] above, wherein the content of the component (D) is 1% by mass or more when the non-volatile component in the resin composition is 100% by mass;

[0018] [6] The resin composition according to any one of [1] to [5] above, wherein (C) the organic filler is a core-shell type graft copolymer particle;

[0019] [7] The resin composition according to [6] above, wherein the monomer component forming the shell portion of the core-shell type graft copolymer particles is a (meth)acrylate;

[0020] [8] The resin composition according to [6] or [7] above, wherein the core particles of the core-shell type graft copolymer particles contain a thermoplastic elastomer;

[0021] [9] The resin composition according to any one of [1] to [8] above, wherein component (A) is an epoxy resin;

[0022]

[10] The resin composition according to any one of [1] to [9] above, further comprising (E) a curing agent;

[0023]

[11] The resin composition according to

[10] above, wherein the component (E) comprises an active ester curing agent;

[0024]

[12] The resin composition according to any one of [1] to

[11] above, wherein the solid content ratio in the resin composition is 95% by mass or less;

[0025]

[13] The resin composition according to any one of [1] to

[12] above, which is used to form an insulating layer of a multi-layer flexible substrate;

[0026]

[14] A cured product, which is a cured product of the resin composition described in any one of [1] to

[13] above;

[0027]

[15] A resin sheet comprising a support and a resin composition layer formed from the resin composition described in any one of [1] to

[13] above and disposed on the support;

[0028]

[16] A multi-layer flexible substrate comprising an insulating layer formed by curing the resin composition described in any one of [1] to

[13] above;

[0029]

[17] A semiconductor device comprising the multilayer flexible substrate described in

[16] above.

[0030] Effects of the Invention

[0031] According to the resin composition of the present invention, it is possible to suppress tackiness to a low level while maintaining excellent flexibility. DETAILED DESCRIPTION

[0032] Hereinafter, the present invention will be described in detail according to the preferred embodiments of the present invention. However, the present invention is not limited to the following embodiments and examples, and can be implemented with arbitrary changes within the scope of the claims of the present invention and their equivalents.

[0033] <Resin composition>

[0034] The resin composition of the present invention comprises (A) a thermosetting resin, (B) an inorganic filler, (C) an organic filler, and (D) an adhesive flexibilizer. When the nonvolatile component in the resin composition is 100% by mass, the content of the component (C) is 5% by mass or more.

[0035] By using such a resin composition, it is possible to suppress tackiness to a low level while maintaining excellent flexibility.

[0036] The resin composition of the present invention may further include any component in addition to (A) a thermosetting resin, (B) an inorganic filler, (C) an organic filler, and (D) an adhesive flexibilizer. As any component, for example, (E) a curing agent, (F) a curing accelerator, (G) other additives, and (H) an organic solvent may be cited. Hereinafter, each component included in the resin composition will be described in detail.

[0037] <(A) Thermosetting resin>

[0038] The resin composition of the present invention contains (A) a thermosetting resin. (A) Thermosetting resin does not contain a resin belonging to component (D). (A) Thermosetting resin can use a known thermosetting resin without particular limitation, and examples thereof include polyester resin, polyurethane resin, polyester polyurethane resin, butyral resin, acrylic resin, cyanate resin, silicone resin, oxetane resin, melamine resin, etc. Among them, epoxy resin is preferred.

[0039] Examples of the epoxy resin include biphenylol epoxy resins, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, bisphenol AF epoxy resins, dicyclopentadiene epoxy resins, trisphenol epoxy resins, naphthol novolac epoxy resins, phenol novolac epoxy resins, tert-butyl-catechol epoxy resins, naphthalene epoxy resins, naphthol epoxy resins, anthracene epoxy resins, glycidylamine epoxy resins, glycidylester epoxy resins, cresol novolac epoxy resins, biphenyl epoxy resins, linear aliphatic epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane epoxy resins, cyclohexanedimethanol epoxy resins, naphthylene ether epoxy resins, trimethylol epoxy resins, and tetraphenylethane epoxy resins. The epoxy resins may be used alone or in combination of two or more.

[0040] For the resin composition, as the epoxy resin, it is preferred to include an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effect of the present invention, relative to 100% by mass of the non-volatile component of the epoxy resin, the proportion of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0041] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as “liquid epoxy resins”) and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as “solid epoxy resins”). The resin composition of the present invention may contain only a liquid epoxy resin or only a solid epoxy resin as the epoxy resin, but preferably contains a liquid epoxy resin and a solid epoxy resin in combination.

[0042] As the liquid epoxy resin, a liquid epoxy resin having two or more epoxy groups in one molecule is preferred.

[0043] As liquid epoxy resins, preferred are bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexanedimethanol type epoxy resins, and glycidyl amine type epoxy resins.

[0044] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene-type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "EPIKOTE 828EL" (bisphenol A-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ZX1059" (a mixture of bisphenol A-type epoxy resin and bisphenol F-type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemicals; "EX-721" (glycidyl ester-type epoxy resin) manufactured by Nagase ChemteX; and "Celloxide 2021P" (alicyclic epoxy resin with an ester skeleton); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel & Sumitomo Chemical Co., Ltd., etc. They can be used alone or in combination of two or more.

[0045] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred.

[0046] As solid epoxy resins, preferred are biphenylol-type epoxy resins, naphthalene-type epoxy resins, naphthalene-type tetrafunctional epoxy resins, cresol novolac-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol-type epoxy resins, biphenyl-type epoxy resins, naphthylene ether-type epoxy resins, anthracene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol AF-type epoxy resins, and tetraphenylethane-type epoxy resins.

[0047] Specific examples of solid epoxy resins include "HP4032H" (naphthalene-type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene-type tetrafunctional epoxy resin) manufactured by DIC Corporation; "N-690" (cresol novolac-type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac-type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", and "HP-7200H" (dicyclopentadiene-type epoxy resin) manufactured by DIC Corporation; Epoxy resin); "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin) manufactured by DIC Corporation; "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000 L", "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YX4000HK" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Corporation "YX7700" manufactured by Mitsubishi Chemical Corporation (a novolac epoxy resin containing a xylene structure); "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd.; "YL7760" manufactured by Mitsubishi Chemical Corporation (a bisphenol AF epoxy resin); "YL7800" manufactured by Mitsubishi Chemical Corporation (a fluorene epoxy resin); "jER1010" manufactured by Mitsubishi Chemical Corporation (a solid bisphenol A epoxy resin); "jER1031S" manufactured by Mitsubishi Chemical Corporation (a tetraphenylethane epoxy resin), etc. These may be used alone or in combination of two or more.

[0048] When a liquid epoxy resin and a solid epoxy resin are used in combination as the epoxy resin, their mass ratio (liquid epoxy resin: solid epoxy resin) is preferably 1:1 to 1:50, more preferably 1:3 to 1:30, and particularly preferably 1:5 to 1:20. By making the mass ratio of the liquid epoxy resin to the solid epoxy resin within the above range, the desired effect of the present invention can be significantly obtained.

[0049] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 50 g / eq. to 3,000 g / eq., further preferably 80 g / eq. to 2,000 g / eq., and further more preferably 110 g / eq. to 1,000 g / eq. By being within the above range, the crosslinking density of the cured product of the resin composition becomes sufficient, and an insulating layer with a small surface roughness can be formed. The epoxy equivalent is the mass of a resin containing 1 equivalent of an epoxy group. The epoxy equivalent can be measured in accordance with JIS K7236.

[0050] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the epoxy resin is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500. The weight average molecular weight of the resin can be measured as a value in terms of polystyrene by gel permeation chromatography (GPC).

[0051] The content of the thermosetting resin (A) is not particularly limited, but when the non-volatile components in the resin composition are set to 100% by mass, it is preferably 5% by mass or more, more preferably 10% by mass or more, further preferably 15% by mass or more, and particularly preferably 20% by mass or more. The upper limit of the content of the thermosetting resin (A) is not particularly limited, but when the non-volatile components in the resin composition are set to 100% by mass, it is preferably 50% by mass or less, more preferably 40% by mass or less, further preferably 30% by mass or less, and particularly preferably 25% by mass or less.

[0052] <(B) Inorganic fillers>

[0053] The resin composition of the present invention contains (B) an inorganic filler.

[0054] (B) The material of the inorganic filler is not particularly limited, and examples thereof include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate, etc., and silica is particularly preferred. As silica, examples thereof include amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. In addition, as silica, spherical silica is preferred. (B) The inorganic filler can be used alone or in combination of two or more.

[0055] (B) The average particle size of the inorganic filler is not particularly limited. From the perspective of obtaining the desired effect of the present invention, it is preferably 10 μm or less, more preferably 5 μm or less, further preferably 3 μm or less, further more preferably 2 μm or less, and particularly preferably 1 μm or less. From the perspective of obtaining the desired effect of the present invention, the lower limit of the average particle size of the inorganic filler is preferably 0.01 μm or more, more preferably 0.05 μm or more, further preferably 0.1 μm or more, further more preferably 0.2 μm or more, and particularly preferably 0.25 μm or more. The average particle size of the inorganic filler can be measured by a laser diffraction-scattering method based on Mie scattering theory. Specifically, it can be measured in the following manner: using a laser diffraction scattering particle size distribution measuring device, a particle size distribution of the inorganic filler is prepared on a volume basis, and the median particle size is used as the average particle size. The sample can be measured using a sample obtained by the following method: 100 mg of inorganic filler and 10 g of methyl ethyl ketone are weighed into a vial and dispersed for 10 minutes using ultrasound. For the sample to be measured, a laser diffraction particle size distribution measuring device is used, and the wavelength of the light source used is set to blue and red, and the volume-based particle size distribution of the inorganic filler is measured in a flow cell mode, and the average particle size is calculated as the median particle size from the obtained particle size distribution. As a laser diffraction particle size distribution measuring device, for example, "LA-960" made by Horiba, Ltd., etc. can be cited.

[0056] Commercially available products of (B) inorganic fillers include, for example, "UFP-30" manufactured by Denki Kagaku Kogyo Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumitomo Metal Materials Corporation; "YC100C", "YA050C", "YA050C-MJE" and "YA010C" manufactured by Admatechs; "UFP-30" manufactured by DENKA Corporation; "Silfil NSS-3N", "Silfil NSS-4N" and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "SC2500SQ", "SO-C4", "SO-C2" and "SO-C1" manufactured by Admatechs; and the like.

[0057] From the viewpoint of improving moisture resistance and dispersibility, the inorganic filler (B) is preferably treated with one or more surface treatment agents such as aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, alkoxysilane compounds, organosilazane compounds, and titanate coupling agents. Commercially available products of the surface treatment agent include, for example, “KBM403” (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM803” (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBE903” (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM573” (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “SZ-31” (hexamethyldisilazane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM103” (phenyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM-4803” (long-chain epoxy-type silane coupling agent) manufactured by Shin-Etsu Chemical Co., Ltd., and “KBM-7103” (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.

[0058] From the viewpoint of improving the dispersibility of the inorganic filler, it is preferred to control the degree of surface treatment performed by the surface treatment agent within a specified range. Specifically, for 100% by mass of the inorganic filler, it is preferred to perform surface treatment with 0.2% by mass to 5% by mass of the surface treatment agent, preferably with 0.2% by mass to 3% by mass, and preferably with 0.3% by mass to 2% by mass.

[0059] The degree of surface treatment by the surface treatment agent can be evaluated by the carbon content per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the carbon content per unit surface area of ​​the inorganic filler is preferably 0.02 mg / m 2 More preferably 0.1 mg / m 2 More preferably, 0.2 mg / m 2 On the other hand, from the viewpoint of preventing the increase of the melt viscosity of the resin composition and the melt viscosity in the sheet form, 1 mg / m 2 Below, more preferably 0.8 mg / m 2 Below, more preferably 0.5 mg / m 2 the following.

[0060] (B) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after washing the surface-treated inorganic filler with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent can be added to the inorganic filler surface-treated with a surface treatment agent, and ultrasonic washing is performed at 25°C for 5 minutes. The supernatant is removed, the solid component is dried, and then the amount of carbon per unit surface area of ​​the inorganic filler is measured using a carbon analyzer. As a carbon analyzer, "EMIA-320V" manufactured by Horiba, Ltd. can be used.

[0061] (B) The specific surface area of ​​the inorganic filler is preferably 1 m 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 3m 2 There is no particular upper limit, but it is preferably 50 m 2 / g or less, more preferably 20m 2 The specific surface area of ​​the inorganic filler can be obtained by adsorbing nitrogen on the surface of the sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech) according to the BET method, and calculating the specific surface area by the BET multipoint method.

[0062] For the content of (B) inorganic filler, when the non-volatile component in the resin composition is set to 100% by mass, from the viewpoint of obtaining a cured product with better flexibility, it is preferably 70% by mass or less, more preferably 60% by mass or less, further preferably 50% by mass or less, and particularly preferably 45% by mass or less. The lower limit of the content of (B) inorganic filler is not particularly limited, and from the viewpoint of obtaining a cured product with sufficient mechanical strength, when the non-volatile component in the resin composition is set to 100% by mass, it is preferably 20% by mass or more, more preferably 30% by mass or more, further preferably 35% by mass or more, and particularly preferably 38% by mass or more.

[0063] <(C) Organic fillers>

[0064] The resin composition of the present invention contains (C) an organic filler. The (C) organic filler does not contain a material that is a component (D). By making the resin composition contain the component (C), the adhesiveness can be reduced and the handling property can be improved.

[0065] (C) The organic filler is present in the resin composition in the form of particles. Examples of the organic filler (C) include rubber particles, polyamide microparticles, silicone particles, etc. In the present invention, rubber particles are preferably used from the viewpoint of significantly obtaining the desired effect of the present invention.

[0066] As the rubber component contained in the rubber particles, for example, polybutadiene, polyisoprene, polychloroprene, ethylene-vinyl acetate copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-isobutylene copolymer, acrylonitrile-butadiene copolymer, isoprene-isobutylene copolymer, isobutylene-butadiene copolymer, ethylene-propylene-diene terpolymer, ethylene-propylene-butene terpolymer and other olefin-based thermoplastic elastomers; thermoplastic elastomers such as acrylic thermoplastic elastomers such as poly(meth)propyl acrylate, poly(meth)butyl acrylate, poly(meth)cyclohexyl acrylate, and poly(meth)octyl acrylate are preferably olefin-based thermoplastic elastomers, and more preferably styrene-butadiene copolymers. Silicone rubbers such as polyorganosiloxane rubbers can be further mixed in the rubber component. For the rubber component contained in the rubber particles, the glass transition temperature is, for example, 0°C or less, preferably -10°C or less, more preferably -20°C or less, and further preferably -30°C or less.

[0067] From the viewpoint of significantly obtaining the desired effect of the present invention, (C) the organic filler is preferably a core-shell particle. The so-called core-shell particle refers to a particle-shaped organic filler formed by "a core particle containing a rubber component as listed above" and "a shell portion covering it with one or more layers". Furthermore, the core-shell particle is preferably a core-shell graft copolymer particle formed by "a core particle containing a rubber component as listed above" and "a shell portion formed by graft copolymerizing a monomer component copolymerizable with the rubber component contained in the core particle". The so-called core-shell type here does not necessarily refer only to those in which the core particle and the shell portion can be clearly distinguished, but also includes those in which the boundary between the core particle and the shell portion is unclear, and the core particle may not be completely covered by the shell portion.

[0068] For the rubber component, in the core-shell type graft copolymer particles, preferably contain 40 mass % or more, more preferably contain 50 mass % or more, further preferably contain 60 mass % or more. The upper limit of the content of the rubber component in the core-shell type graft copolymer particles is not particularly limited, and from the viewpoint of fully coating the core particles with the shell portion, for example, is 95 mass % or less, preferably 90 mass %.

[0069] Examples of the monomer component forming the shell portion of the core-shell graft copolymer particles include (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, and glycidyl (meth)acrylate; (meth)acrylic acid; N-substituted maleimides such as N-methylmaleimide and N-phenylmaleimide; maleimide; α,β-unsaturated carboxylic acids such as maleic acid and itaconic acid; aromatic vinyl compounds such as styrene, 4-vinyltoluene, and α-methylstyrene; (meth)acrylonitrile, etc., preferably (meth)acrylates, more preferably methyl (meth)acrylate.

[0070] Commercially available products of core-shell graft copolymer particles include, for example, "CHT" manufactured by Cheil Industries; "B602" manufactured by UMGABS; "PARALOID EXL2602", "PARALOID EXL2603", "PARALOID EXL2655", "PARALOID EXL2311", "PARALOID EXL2313", "PARALOID XL2315", "PARALOID KM330", "PARALOID KM336P", and "PARALOID KCZ201" manufactured by Dow Chemical Japan; "METABLEN C-223A", "METABLEN E-901", "METABLEN S-2001", "METABLEN W-450A", and "METABLEN SRK-200" manufactured by Mitsubishi Rayon; "Kane Ace M-511", "Kane Ace M-600", and "Kane Ace M-400", "Kane Ace M-580", "Kane Ace MR-01", etc. These may be used alone or in combination of two or more.

[0071] The average particle size (average primary particle size) of the core-shell graft copolymer particles is not particularly limited, but is preferably 20 nm or more, more preferably 50 nm or more, further preferably 80 nm or more, particularly preferably 100 nm or more, and preferably 5,000 nm or less, more preferably 2,000 nm or less, further preferably 1,000 nm or less, and particularly preferably 500 nm or less. The average particle size (average primary particle size) of the core-shell graft copolymer particles can be measured using a zeta potential particle size distribution measuring device or the like.

[0072] When the non-volatile component in the resin composition is set to 100% by mass, the content of (C) organic filler is more than 5.0% by mass, and from the viewpoint of suppressing adhesion as much as possible and then suppressing the usage of (B) inorganic filler as much as possible, obtaining a more flexible cured product, preferably more than 5.5% by mass, more preferably more than 5.8% by mass, further preferably more than 6.0% by mass, and particularly preferably more than 6.2% by mass. From the viewpoint of suppressing viscosity to a low level as much as possible, when the non-volatile component in the resin composition is set to 100% by mass, the upper limit of the content of (C) organic filler is preferably less than 30% by mass, less than 20% by mass, more preferably less than 15% by mass, from the viewpoint of reducing poor porosity and achieving more excellent pattern embedding, more preferably less than 10% by mass, particularly preferably less than 8% by mass.

[0073] <(D) Adhesive Flexibility Agent>

[0074] The resin composition of the present invention contains (D) an adhesive flexibilizer.

[0075] (D) Adhesive flexibilizing agent refers to a component in a flexibilizing agent that imparts flexibility to a cured product of a thermosetting resin and has the property of improving the adhesiveness of the cured product. As for (D) adhesive flexibilizing agent, a wide range of known flexibilizing agents that have the property of improving the adhesiveness of a cured product can be used. Examples of (D) adhesive flexibilizing agents include, but are not limited to, resins having a polybutadiene structure (hereinafter referred to as "polybutadiene resins"), polyrotaxane resins, polyimide resins, and maleimide resins having a dimer acid skeleton.

[0076] The polybutadiene structure includes not only a structure formed by polymerizing butadiene, but also a structure formed by hydrogenating the structure. In addition, for the butadiene structure, only a part of it may be hydrogenated, or all of it may be hydrogenated. In addition, the polybutadiene structure may be included in the main chain or in the side chain in the (D) component.

[0077] Preferred examples of polybutadiene resins include resins containing hydrogenated polybutadiene skeletons, polybutadiene resins containing hydroxyl groups, polybutadiene resins containing phenolic hydroxyl groups, polybutadiene resins containing carboxyl groups, polybutadiene resins containing acid anhydride groups, polybutadiene resins containing epoxy groups, polybutadiene resins containing isocyanate groups, polybutadiene resins containing carbamate groups, polyphenylene ether-polybutadiene resins, etc. Here, the so-called "resin containing hydrogenated polybutadiene skeleton" refers to a resin in which at least a part of the polybutadiene skeleton is hydrogenated, and it is not necessarily a resin in which the polybutadiene skeleton is completely hydrogenated. As resins containing hydrogenated polybutadiene skeletons, for example, epoxy resins containing hydrogenated polybutadiene skeletons can be mentioned. In addition, as polybutadiene resins containing phenolic hydroxyl groups, resins having a polybutadiene structure and having phenolic hydroxyl groups can be mentioned.

[0078] Specific examples of the polybutadiene resin having a polybutadiene structure in the molecule include "BX360" and "BX660" (polyphenylene ether-polybutadiene resin) manufactured by Nippon Kayaku Co., Ltd., "Ricon 657" (epoxy-containing polybutadiene) manufactured by Cray Valley, "Ricon 130MA8", "Ricon 130MA13", "Ricon 130MA20", "Ricon 131MA5", "Ricon 131MA10", "Ricon 131MA17", "Ricon 131MA20", "Ricon 131MA30", "Ricon 131MA40", "Ricon 131MA51", "Ricon 131MA10", "Ricon 131MA17", "Ricon 131MA20", "Ricon 131MA31" and "Ricon 131MA52". 184MA6" (polybutadiene containing anhydride groups), "GQ-1000" (polybutadiene into which hydroxyl groups and carboxyl groups are introduced), "G-1000", "G-2000", "G-3000" (polybutadiene having hydroxyl groups at both ends), "GI-1000", "GI-2000", "GI-3000" (hydrogenated polybutadiene having hydroxyl groups at both ends), "PB3600", "PB4700" (polybutadiene skeleton epoxy compounds) manufactured by Daicel Corporation, "Epofriend A1005", "Epofriend A1010", "Epofriend A1020" (epoxy compounds of block copolymers of styrene, butadiene and styrene), "FCA-061L" (hydrogenated polybutadiene skeleton epoxy compound) manufactured by Nagase ChemteX Co., Ltd., "R-45EPT" (polybutadiene skeleton epoxy compound), etc.

[0079] In addition, as an example of a preferred polybutadiene resin, a linear polyimide butadiene resin (polyimide described in Japanese Unexamined Patent Publication No. 2006-37083 and International Publication No. 2008 / 153208) made of hydroxyl-terminated polybutadiene, a diisocyanate compound and a polyacid or anhydride thereof can also be cited. The content of the polybutadiene structure of the polyimide butadiene resin is preferably 60% to 95% by mass, and more preferably 75% to 85% by mass. The details of the polyimide butadiene resin can be referred to the records of Japanese Unexamined Patent Publication No. 2006-37083 and International Publication No. 2008 / 153208, and the contents are incorporated into this specification.

[0080] From the viewpoint of achieving the desired effects of the present invention, the number average molecular weight of the hydroxy-terminated polybutadiene as a raw material of the polyimide butadiene resin is preferably 500 to 5,000, more preferably 1,000 to 3,000. From the viewpoint of achieving the desired effects of the present invention, the hydroxy-terminated polybutadiene has a hydroxyl equivalent of preferably 250 to 1,250.

[0081] Regarding the diisocyanate compound as a raw material of the polyimide butadiene resin, for example, aromatic diisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, xylylenediisocyanate, and diphenylmethane diisocyanate; aliphatic diisocyanates such as hexamethylene diisocyanate; and alicyclic diisocyanates such as isophorone diisocyanate. Among these, aromatic diisocyanates are preferred, and 2,4-toluene diisocyanate is more preferred.

[0082] Regarding the polybasic acid or its anhydride as a raw material of the above-mentioned polyimide butadiene resin, for example, ethylene glycol ditrimethylolpropane tetracarboxylic acid, pyromellitic acid, benzophenone tetracarboxylic acid, biphenyl tetracarboxylic acid, naphthalene tetracarboxylic acid, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-cyclohexene-1,2-dicarboxylic acid, 3,3'-4,4'-diphenylsulfone tetracarboxylic acid and their anhydrides, tribasic acids such as trimellitic acid and cyclohexanetricarboxylic acid and their anhydrides, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho(1,2-C)furan-1,3-dione, etc. can be mentioned.

[0083] A polyrotaxane resin is a resin having the following structure, wherein the structure has: a plurality of cyclic molecules, a linear axis molecule that is enclosed (inclusion) in a manner that penetrates (passes through) the cyclic molecules, and a capping group that blocks the end of the axis molecule in a manner that prevents the cyclic molecules from falling off (slipping out). The number (inclusion amount) of cyclic molecules in the polyrotaxane resin is not particularly limited, as long as the number of cyclic molecules is within a range of more than 2. For example, when one axis molecule is enclosed in a state that penetrates multiple cyclic molecules, when the amount of cyclic molecules that maximally enclose one axis molecule (maximum inclusion amount) is set to 100%, it is preferably 10% or more, more preferably 15% or more, further preferably 20% or more, preferably 90% or less, more preferably 85% or less, and further preferably 80% or less. The inclusion amount can be determined by the length of the axis molecule and the thickness of the cyclic molecule. For example, when the axial molecule is polyethylene glycol and the cyclic molecule is an α-cyclodextrin molecule, the maximum inclusion amount was experimentally determined (see Macromolecules 1993, 26, 5698-5703).

[0084] As the axis molecule in the polyrotaxane resin, a linear molecule having a molecular weight of 10,000 or more and capable of chemically modifying the end with a capping group can be used. The so-called "linear" means that it is substantially linear, and the axis molecule can have a branched chain as long as the cyclic molecule through which the axis molecule passes can rotate or move. As the axis molecule, for example, polyvinyl alcohol, polyvinyl pyrrolidone, poly (methyl) acrylic cellulose resin, polyacrylamide, polyethylene oxide, polyethylene glycol, polypropylene glycol, polyvinyl acetal resin, polyvinyl methyl ether, polyamine, polyethylene imine, casein, gelatin, starch, polyolefin, polyester, polyvinyl chloride, polystyrene, copolymers such as acrylonitrile-styrene copolymer, acrylic resin, polycarbonate, polyurethane, polyvinyl butyral, polyisobutylene, polytetrahydrofuran, polyamide, polyimide, polydiene, polysiloxane, polyurea, polysulfide, polyphosphazene, polyketone, polyphenylene, polyhalogenated olefins and their derivatives can be cited. Among these, polyethylene glycol chains are preferably used. Two or more of these chains may be mixed in the polyrotaxane resin.

[0085] The length of the axis molecule is not particularly limited as long as the cyclic molecule can rotate or move. The length of the axis molecule can be represented by the weight average molecular weight. As the weight average molecular weight of the axis molecule, it is preferably 3,000 or more, more preferably 4,000 or more, more preferably 5,000 or more, preferably 100,000 or less, more preferably 90,000 or less, and more preferably 85,000 or less. The weight average molecular weight of the axis molecule is the weight average molecular weight measured by gel permeation chromatography (GPC) in terms of polystyrene conversion.

[0086] The axis molecule generally has a structure in which the functional groups of a molecule having functional groups at both ends react and bond with a molecule containing a capping group. Preferred functional groups include amide, hydroxyl, carboxyl, acryloyl, methacryloyl, epoxy, and vinyl groups.

[0087] As the cyclic molecule in the polyrotaxane resin, it is a cyclic molecule that can enclose the axial molecule in a through state, and in order to be able to react with the (E) curing agent, a molecule having at least one reactive group (functional group) can be used. The so-called cyclic molecule refers to a molecule that is substantially cyclic, and the so-called "substantially cyclic" means that it also includes a form that is not completely closed, and its concept also includes: a molecule with a helical structure in which one end of the English letter "C" is not combined with the other end and overlaps. As the cyclic molecule, for example, cyclodextrins, crown ethers, cryptands, macrocyclic amines, calixarene, cyclophane, etc. can be cited. Among these, cyclodextrins are preferred. They can be mixed in two or more species in the polyrotaxane resin.

[0088] Examples of the cyclodextrins include α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, dimethylcyclodextrin, and glucosylcyclodextrin, and derivatives or modified products thereof.

[0089] The cyclic molecule preferably contains a reactive group. As the reactive group, for example, a hydroxyl group, a carboxyl group, an acryloyl group, a methacryloyl group, an epoxy group, a vinyl group, etc. can be cited, among which a hydroxyl group is preferred. By making the cyclic molecule have a reactive group, the cyclic molecules can be cross-linked with each other or the polyrotaxane resin and the thermosetting resin can be cross-linked via a curing agent. In addition, the reactive group of the cyclic molecule on one side can be cross-linked with the reactive group of the cyclic molecule on the other side. Regarding the reactive group, it can have one alone or two or more.

[0090] The reactive group may not be directly bonded to the cyclic molecule. For example, when the cyclic molecule is cyclodextrin, the hydroxyl group of the cyclodextrin itself is a reactive group, and when the hydroxyl group is added to the hydroxyl group, the hydroxyl group of the hydroxypropyl group is also a reactive group. Furthermore, when the ring-opening polymerization of ε-caprolactone is carried out via the hydroxyl group of the hydroxypropyl group, when there is a caprolactone chain, the hydroxyl group at the end opposite to the polyester part of the caprolactone chain is also a reactive group.

[0091] Each cyclic molecule may have one reactive group of a cyclic molecule, or may have two or more reactive groups of a cyclic molecule.

[0092] The weight average molecular weight of the cyclic molecule is preferably 5,000 or more, more preferably 6,000 or more, and even more preferably 7,000 or more, and is preferably 1,500,000 or less, more preferably 1,400,000 or less, and even more preferably 1,350,000 or less. The weight average molecular weight of the cyclic molecule is a weight average molecular weight measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0093] There is no particular limitation on the capping group in the polyrotaxane resin, as long as it is a structure with a relatively large volume to prevent the cyclic molecule from falling off. As the capping group, for example, a cyclodextrin group, adamantyl group, dinitrophenyl group, trityl group, etc. can be cited. Among them, adamantyl group is preferred. These can be present in the polyrotaxane resin alone, or there can be two or more.

[0094] The weight average molecular weight of the polyrotaxane resin as a whole is preferably 10,000 or more, more preferably 15,000 or more, and even more preferably 20,000 or more, and is preferably 1,500,000 or less, more preferably 1,400,000 or less, and even more preferably 1,350,000 or less. The weight average molecular weight of the polyrotaxane resin is a weight average molecular weight measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0095] The hydroxyl value of the polyrotaxane resin is preferably 45 mgKOH / g or more, more preferably 50 mgKOH / g or more, and even more preferably 55 mgKOH / g or more, and is preferably 120 mgKOH / g or less, more preferably 115 mgKOH / g or less, and even more preferably 110 mgKOH / g or less. The hydroxyl value can be measured according to JIS K0070.

[0096] The polyrotaxane resin may be in a liquid state, but is preferably contained in the resin composition in a particle state. The polyrotaxane resin in a particle state is easy to disperse, and the viscosity of the resin composition is easy to reduce.

[0097] The average particle size of the particulate polyrotaxane resin is preferably 100 nm or more, more preferably 500 nm or more, further preferably 800 nm or more, preferably 50,000 nm or less, more preferably 40,000 nm or less, and further preferably 30,000 nm or less. The particulate polyrotaxane resin having such an average particle size will be easily uniformly dispersed in the resin composition, and the viscosity of the resin composition will be easily reduced. The average particle size can be measured by the same method as the measurement of the average particle size in the inorganic filler.

[0098] The polyrotaxane resin can be synthesized by the method described in, for example, International Publication No. 01 / 83566, Japanese Patent Application Publication No. 2005-154675, Japanese Patent No. 4482633, and the like.

[0099] The polyrotaxane resin may be a commercially available product. For example, "SH2400B-007", "SH1310P", "SeRM Super Polymer A1000" and the like manufactured by Advanced Softmaterials Co., Ltd. may be used. These may be used alone or in combination of two or more.

[0100] Polyimide resin is a resin having an imide bond in a repeating unit. Polyimide resins generally include resins obtained by imidization reaction of a diamine compound and tetracarboxylic anhydride. Polyimide resins also include modified polyimide resins such as siloxane-modified polyimide resins.

[0101] The polyimide resin may include, for example, a structure represented by formula (1).

[0102] [Chemical formula 1]

[0103] .

[0104] [Wherein, X 1 represents a tetravalent group obtained by removing two -CO-O-CO- groups from tetracarboxylic dianhydride, X 2 represents a divalent group obtained by removing two -NH2 from a diamine compound, and n represents an integer greater than 2].

[0105] The diamine compound used for preparing the polyimide resin is not particularly limited, and examples thereof include aliphatic diamine compounds and aromatic diamine compounds.

[0106] Examples of the aliphatic diamine compound include linear aliphatic diamine compounds such as 1,2-ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-hexanediamine, 1,5-diaminopentane, and 1,10-diaminodecane; branched aliphatic diamine compounds such as 1,2-diamino-2-methylpropane, 2,3-diamino-2,3-butane, and 2-methyl-1,5-diaminopentane; alicyclic diamine compounds such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,4-diaminocyclohexane, and 4,4′-methylenebis(cyclohexylamine); and dimer acid-type diamines (hereinafter also referred to as “dimer diamines”).

[0107] The so-called dimer acid type diamine refers to a diamine compound obtained by replacing the two terminal carboxylic acid groups (-COOH) of the dimer acid with aminomethyl (-CH2-NH2) or amino group (-NH2). Dimer acid is a known compound obtained by dimerizing unsaturated fatty acids (preferably unsaturated fatty acids with 11 to 22 carbon atoms, particularly preferably unsaturated fatty acids with 18 carbon atoms), and its industrial manufacturing process has been roughly standardized in the industry. For dimer acid, in particular, dimer acid with a carbon number of 36 obtained by dimerizing unsaturated fatty acids with 18 carbon atoms such as oleic acid and linoleic acid, which are cheap and easily available, as the main component can be easily obtained. In addition, for dimer acid, depending on the manufacturing method, the degree of purification, etc., it sometimes contains any amount of monomer acid, trimer acid, other polymerized fatty acids, etc. In addition, although double bonds remain after the polymerization reaction of unsaturated fatty acids, in this specification, the hydride that further undergoes hydrogenation reaction to reduce the unsaturation is also included in the dimer acid. As for the dimer acid type diamine, commercial items are available, for example, PRIAMINE 1073, PRIAMINE 1074, PRIAMINE 1075 manufactured by Croda Japan, VERSAMINE 551, VERSAMINE 552 manufactured by Cognis Japan, etc. are mentioned.

[0108] Examples of the aromatic diamine compound include phenylenediamine compounds, naphthalenediamine compounds, and diphenylamine compounds.

[0109] The so-called phenylenediamine compound refers to a compound formed by a benzene ring having two amino groups, and the benzene ring here may have 1 to 3 substituents. The substituents here are not particularly limited. Specific examples of the phenylenediamine compound include 1,4-phenylenediamine, 1,2-phenylenediamine, 1,3-phenylenediamine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobiphenyl, and 2,4,5,6-tetrafluoro-1,3-phenylenediamine.

[0110] The so-called naphthalene diamine compound refers to a compound formed by a naphthalene ring having two amino groups, and the naphthalene ring here may have 1 to 3 substituents. The substituents here are not particularly limited. Specific examples of the naphthalene diamine compound include 1,5-diaminonaphthalene, 1,8-diaminonaphthalene, 2,6-diaminonaphthalene, and 2,3-diaminonaphthalene.

[0111] The so-called diphenylamine compound refers to a compound containing two aniline structures in the molecule, and further, the two benzene rings in the two aniline structures can each further have 1 to 3 substituents. The substituents here are not particularly limited. The two aniline structures in the diphenylamine compound can be directly bonded and / or bonded via one or two divalent connecting groups having 1 to 100 (preferably 1 to 50, more preferably 1 to 20) backbone atoms selected from carbon atoms, oxygen atoms, sulfur atoms and nitrogen atoms. The diphenylamine compound also includes a compound in which two aniline structures are bonded at two locations.

[0112] Specific examples of the "divalent linking group" in the diphenylamine compound include -NHCO-, -CONH-, -OCO-, -COO-, -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -CH=CH-, -O-, -S-, -CO-, -SO2-, -NH-, -Ph-, -Ph-Ph-, -C(CH3)2-Ph-C(CH3)2-, -O-Ph-O-, -O-Ph-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-C(CH3)2-Ph-O-, -C(CH3)2-Ph-C(CH3)2-,

[0113] [Chemical formula 2]

[0114] wait.

[0115] (where * represents the binding site).

[0116] "Ph" represents 1,4-phenylene, 1,3-phenylene or 1,2-phenylene.

[0117] Specific examples of the diphenylamine compound include 4,4'-diamino-2,2'-bis(trifluoromethyl)-1,1'-biphenyl, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4-aminobenzoic acid 4-aminophenyl ester, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis(4-aminophenyl)propane, 4,4'-(hexafluoroisopropylidene)diphenylamine, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, α,α-bis[4-(4-aminophenoxy)phenyl]-1,3-diisopropylbenzene, α,α-bis[4 -(4-aminophenoxy)phenyl]-1,4-diisopropylbenzene, 4,4'-(9-fluorenylidene)diphenylamine, 2,2-bis(3-methyl-4-aminophenyl)propane, 2,2-bis(3-methyl-4-aminophenyl)benzene, 4,4'-diamino-3,3'-dimethyl-1,1'-biphenyl, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 9,9'- Bis(3-methyl-4-aminophenyl)fluorene, 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane, 4-aminobenzoic acid 5-amino-1,1'-biphenyl-2-yl ester, and the like, preferably 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane and 4-aminobenzoic acid 5-amino-1,1'-biphenyl-2-yl ester.

[0118] As the diamine compound, a commercially available diamine compound may be used, or a diamine compound synthesized by a known method may be used. The diamine compound may be used alone or in combination of two or more.

[0119] The tetracarboxylic anhydride used for preparing the polyimide resin is not particularly limited, and examples thereof include aromatic tetracarboxylic dianhydride and aliphatic tetracarboxylic dianhydride.

[0120] Examples of the aromatic tetracarboxylic dianhydride include pyromellitic dianhydride, naphthalenetetracarboxylic dianhydride, anthracenetetracarboxylic dianhydride, and diphthalic dianhydride. Diphthalic dianhydride is preferred.

[0121] The so-called pyromellitic dianhydride refers to a dianhydride of benzene having four carboxyl groups, and the benzene ring here may have 1 to 3 substituents. Here, there is no particular limitation on the substituent. Specifically, pyromellitic dianhydride, 1,2,3,4-pyromellitic dianhydride, etc. can be cited as pyromellitic dianhydride.

[0122] The so-called naphthalenetetracarboxylic dianhydride refers to a naphthalene dianhydride having four carboxyl groups, and the naphthalene ring here may have 1 to 3 substituents. Here, there is no particular limitation on the substituent. As naphthalenetetracarboxylic dianhydride, specifically, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, etc. can be cited.

[0123] Anthracenetetracarboxylic acid dianhydride refers to an anthracene dianhydride having four carboxyl groups, and the anthracene ring may have 1 to 3 substituents. There are no particular restrictions on the substituents. Specific examples of anthracenetetracarboxylic acid dianhydride include 2,3,6,7-anthracenetetracarboxylic acid dianhydride and the like.

[0124] The so-called diphthalic anhydride refers to a compound containing two phthalic anhydrides in the molecule, and further, the two benzene rings in the two phthalic anhydrides can each have 1 to 3 substituents. Here, there is no particular restriction on the substituent. The two phthalic anhydrides in the diphthalic anhydride can be directly bonded or bonded via a divalent linking group having 1 to 100 (preferably 1 to 50, more preferably 1 to 20) backbone atoms selected from carbon atoms, oxygen atoms, sulfur atoms and nitrogen atoms.

[0125] Specific examples of the divalent linking group include -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2-, -CH(CH3)-, -C(CH3)2-, -O-, -CO-, -SO2-, -Ph-, -O-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-C(CH3)2-Ph-O-, and the like.

[0126] Specific examples of diphthalic dianhydride include 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenyl ethertetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, and 2,3,3',4'-biphenyltetracarboxylic dianhydride. ',4'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 2,3,3',4'-diphenyl sulfone tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenoxyphenyl)sulfone dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethynylene (ethynylidene)-4,4'-diphthalic dianhydride, 2,2'-bis(3,4-dicarboxyphenoxyphenyl)sulfone dianhydride Propylidene-4,4'-diphthalic anhydride, 1,2-ethylene-4,4'-diphthalic anhydride, 1,3-trimethylene-4,4'-diphthalic anhydride, 1,4-tetramethylene-4,4'-diphthalic anhydride, 1,5-pentamethylene-4,4'-diphthalic anhydride, 1,3-bis(3,4-dicarboxyphenyl) Phthalic anhydride, 1,4-bis(3,4-dicarboxyphenyl)phthalic anhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic anhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic anhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride, and the like.

[0127] Specific examples of the aliphatic tetracarboxylic dianhydride include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, cyclohexane-1,2,3,4-tetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride, 3,3',4,4'-bicyclohexyltetracarboxylic dianhydride, carbonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, methylene tetracarboxylic dianhydride, -4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,2-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, thio-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, sulfonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, etc.

[0128] As tetracarboxylic dianhydride, commercially available tetracarboxylic dianhydride may be used, or tetracarboxylic dianhydride synthesized by a known method or a method based thereon may be used. Tetracarboxylic dianhydride may be used alone or in combination of two or more.

[0129] The content of the structure derived from aromatic tetracarboxylic dianhydride relative to the total structure derived from tetracarboxylic dianhydride constituting the polyimide resin is preferably 10 mol % or more, more preferably 30 mol % or more, further preferably 50 mol % or more, further preferably 70 mol % or more, further more preferably 90 mol % or more, and particularly preferably 100 mol %.

[0130] The weight average molecular weight of the polyimide resin is preferably 1,000 to 100,000.

[0131] The maleimide resin having a dimer acid skeleton is, for example, a bismaleimide compound having a hydrocarbon skeleton derived from a dimer acid. The maleimide resin having a dimer acid skeleton is, for example, a bismaleimide compound obtained by imidizing at least a dimer acid type diamine with maleic anhydride, and further includes a bismaleimide compound obtained by imidizing a dimer acid type diamine with tetracarboxylic dianhydride and maleic anhydride.

[0132] The maleimide resin having a dimer acid skeleton is, for example, a bismaleimide compound represented by the following formula (2).

[0133] [Chemical formula 3]

[0134] .

[0135] [Wherein, Y 1 and Y 3 Each independently represents a divalent group obtained by removing two -NH2 from a dimer acid type diamine, and Y 2 represents a tetravalent group obtained by removing two -CO-O-CO- from tetracarboxylic dianhydride, and m represents 0 or 1].

[0136] Specific examples of the maleimide resin having a dimer acid skeleton include "BMI689", "BMI1500", "BMI1700", and "BMI3000" manufactured by DESIGNER MOLECULES Co. These may be used alone or in combination of two or more.

[0137] The content of the adhesive flexibilizer (D) is not particularly limited. From the viewpoint of obtaining a cured product with better flexibility, when the non-volatile component in the resin composition is set to 100% by mass, it is preferably 1% by mass or more, more preferably 5% by mass or more, further preferably 10% by mass or more, and particularly preferably 15% by mass or more. The upper limit of the content of the adhesive flexibilizer (D) is not particularly limited. When the non-volatile component in the resin composition is set to 100% by mass, it is preferably 50% by mass or less, more preferably 40% by mass or less, further preferably 30% by mass or less, and particularly preferably 25% by mass or less.

[0138] <(E) Curing agent>

[0139] The resin composition of the present invention may contain (E) a curing agent as an optional component. The (E) curing agent has a function of curing the (A) thermosetting resin.

[0140] There are no particular restrictions on the curing agent (E). When the thermosetting resin (A) is an epoxy resin, examples thereof include phenolic curing agents, naphthol curing agents, acid anhydride curing agents, active ester curing agents, benzoxazine curing agents, cyanate curing agents, and carbodiimide curing agents, preferably phenolic curing agents, naphthol curing agents, and active ester curing agents. The curing agent (E) preferably includes an active ester curing agent. The curing agent may be used alone or in combination of two or more.

[0141] As phenolic curing agents and naphthol curing agents, from the viewpoint of heat resistance and water resistance, phenolic curing agents with a novolac structure or naphthol curing agents with a novolac structure are preferred. In addition, from the viewpoint of adhesion to the adherend, nitrogen-containing phenolic curing agents or nitrogen-containing naphthol curing agents are preferred, and phenolic curing agents containing triazine skeletons or naphthol curing agents containing triazine skeletons are more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, phenolic novolac resins containing triazine skeletons are preferred. Specific examples of phenol-based curing agents and naphthol-based curing agents include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemicals, "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel & Sumitomo Chemicals Corporation, and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", and "TD-2090-60M" manufactured by DIC Corporation.

[0142] Examples of the acid anhydride curing agent include curing agents having one or more acid anhydride groups in one molecule. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, dicarboxylic anhydride, and the like. Benzophenone tetracarboxylic dianhydride, biphenyl tetracarboxylic dianhydride, naphthalene tetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfone tetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(trimellitic anhydride ester), styrene-maleic acid resin obtained by copolymerization of styrene and maleic acid, etc. Examples of commercially available acid anhydride curing agents include "HNA-100" and "MH-700" manufactured by Shin Nippon Chemical Co., Ltd.

[0143] As active ester curing agent, there is no particular limitation, usually, it is preferred to use phenolic esters, thiophenolic esters, N-hydroxylamine esters, esters of heterocyclic hydroxy compounds, etc., compounds having ester groups with more than 2 high reactive activities in 1 molecule. The active ester curing agent is preferably an active ester curing agent obtained by the condensation reaction of carboxylic acid compounds and / or thiocarboxylic acid compounds with hydroxy compounds and / or thiol compounds. Especially from the viewpoint of improving heat resistance, it is preferably an active ester curing agent obtained by carboxylic acid compounds and hydroxy compounds, and more preferably an active ester curing agent obtained by carboxylic acid compounds and phenolic compounds and / or naphthol compounds. As carboxylic acid compounds, for example benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc. can be cited. Examples of the phenol compound or naphthol compound include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, pyrogallol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the so-called "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing two molecules of phenol on one molecule of dicyclopentadiene.

[0144] Specifically, preferred are active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing acetylated products of phenol novolac, and active ester compounds containing benzoylated products of phenol novolac. Among them, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The so-called "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit composed of phenylene-dicyclopentalene-phenylene.

[0145] Commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000", "HPC-8000H", "HPC-8000-65T", "HPC-8000H-65TM", "EXB-8000L", "EXB-8000L-65M", and "EXB-8000L-65TM" (manufactured by DIC Corporation), which are active ester compounds containing a dicyclopentadiene-type diphenol structure; "EXB9416-70BK", "EXB-8150- 65T" (manufactured by DIC Corporation); "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester compound containing an acetylated product of phenol novolac; "YLH1026" (manufactured by Mitsubishi Chemical Corporation) as an active ester compound containing a benzoylated product of phenol novolac; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester curing agent for an acetylated product of phenol novolac; "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester curing agents for benzoylated products of phenol novolac; and the like.

[0146] Specific examples of the benzoxazine-based curing agent include “JBZ-OP100D” and “ODA-BOZ” manufactured by JFE Chemical Co., Ltd.; “HFB2006M” manufactured by Showa High Molecular Co., Ltd.; and “Pd” and “Fa” manufactured by Shikoku Chemical Industry Co., Ltd.

[0147] Examples of the cyanate curing agent include difunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4,4'-ethylenediphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylene))benzene, bis(4-cyanatephenyl)sulfide, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers obtained by partially triazinizing these cyanate resins. Specific examples of cyanate curing agents include "PT30" and "PT60" manufactured by Lonza Japan (both are phenol novolac-type multifunctional cyanate resins), "BA230", and "BA230S75" (prepolymers obtained by triazinizing part or all of bisphenol A dicyanate to form a trimer), etc.

[0148] Specific examples of the carbodiimide-based curing agent include "V-03" and "V-07" manufactured by Nisshinbo Chemical Co., Ltd.

[0149] When the resin composition contains (E) a curing agent, the amount ratio of the (A) thermosetting resin to the (E) curing agent is preferably in the range of 1:0.2 to 1:2, more preferably 1:0.3 to 1:1.5, and even more preferably 1:0.4 to 1:1.2, in terms of the ratio of [the total number of reactive groups of the thermosetting resin]:[the total number of reactive groups of the curing agent]. Here, the reactive group of the curing agent refers to an active hydroxyl group, an active ester group, etc., which varies depending on the type of the curing agent. The reactive group of the thermosetting resin refers to an epoxy group, etc., which varies depending on the type of the thermosetting resin.

[0150] When the resin composition contains (E) a curing agent, its content is not particularly limited. When the non-volatile component in the resin composition is set to 100% by mass, it is preferably 0.1% by mass or more, more preferably 1% by mass or more, further preferably 3% by mass or more, and particularly preferably 4% by mass or more. The upper limit of the content of the (E) curing agent is not particularly limited. When the non-volatile component in the resin composition is set to 100% by mass, it is preferably 30% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, and particularly preferably 10% by mass or less.

[0151] <(F) Curing accelerator>

[0152] The resin composition of the present invention may contain (F) a curing accelerator as an optional component. The (F) curing accelerator has a function of accelerating the curing rate of the (A) thermosetting resin.

[0153] There are no particular restrictions on the curing accelerator (F). When the thermosetting resin (A) is an epoxy resin, examples thereof include phosphorus curing accelerators, amine curing accelerators, imidazole curing accelerators, guanidine curing accelerators, and metal curing accelerators. Among them, phosphorus curing accelerators, amine curing accelerators, imidazole curing accelerators, and metal curing accelerators are preferred, and amine curing accelerators are more preferred. The curing accelerators may be used alone or in combination of two or more.

[0154] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate.

[0155] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine (DMAP), benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, and 4-dimethylaminopyridine is preferred.

[0156] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1') imidazole compounds such as 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, and adducts of imidazole compounds with epoxy resins.

[0157] As the imidazole-based curing accelerator, a commercially available item may be used, and examples thereof include "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0158] Examples of the guanidine-based curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanidine, 1-ethylbiguanidine, 1-n-butylbiguanidine, 1-n-octadecylbiguanidine, 1,1-dimethylbiguanidine, 1,1-diethylbiguanidine, 1-cyclohexylbiguanidine, 1-allylbiguanidine, 1-phenylbiguanidine, and 1-(o-tolyl)biguanidine.

[0159] As metal curing accelerators, organic metal complexes or organic metal salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin can be cited. As specific examples of organic metal complexes, organic cobalt complexes such as cobalt acetylacetonate (II), cobalt acetylacetonate (III), organic copper complexes such as copper acetylacetonate (II), organic zinc complexes such as zinc acetylacetonate (II), organic iron complexes such as iron acetylacetonate (III), organic nickel complexes such as nickel acetylacetonate (II), and organic manganese complexes such as manganese acetylacetonate (II) can be cited. As organic metal salts, for example, zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, zinc stearate, etc. can be cited.

[0160] When the resin composition contains (F) a curing accelerator, its content is not particularly limited. When the non-volatile component in the resin composition is set to 100% by mass, it is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, further preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more. The upper limit of the content of the (F) curing accelerator is not particularly limited. When the non-volatile component in the resin composition is set to 100% by mass, it is preferably 2% by mass or less, more preferably 1% by mass or less, further preferably 0.5% by mass or less, and particularly preferably 0.3% by mass or less.

[0161] <(G) Other additives>

[0162] The resin composition of the present invention may further contain any additive as a non-volatile component. Examples of such additives include thermoplastic resins such as phenoxy resins, polyvinyl acetal resins, polyolefin resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyetheretherketone resins, and polyester resins; organometallic compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as siloxane; thickeners such as Benton and montmorillonite; silicone-based defoamers, acrylic defoamers, and fluorine-based defoamers. Defoamers such as defoamers and vinyl resin defoamers; UV absorbers such as benzotriazole UV absorbers; adhesion enhancers such as urea silane; adhesion enhancers such as silane coupling agents, triazole adhesion imparting agents, tetrazole adhesion imparting agents, and triazine adhesion imparting agents; antioxidants such as hindered phenol antioxidants and hindered amine antioxidants; fluorescent whitening agents such as stilbene derivatives; flame retardants such as phosphorus flame retardants (such as phosphate compounds, phosphazene compounds, phosphonic acid compounds, and red phosphorus), nitrogen flame retardants (such as melamine sulfate), halogen flame retardants, and inorganic flame retardants (such as antimony trioxide). One additive can be used alone, or two or more additives can be used in combination at any ratio. If it is a person skilled in the art, the content of (G) other additives can be appropriately set.

[0163] <(H) Organic solvent>

[0164] The resin composition of the present invention may contain any organic solvent as a volatile component in addition to the non-volatile components mentioned above. As the (H) organic solvent, any known organic solvent may be used as appropriate, and the type thereof is not particularly limited as long as it is an organic solvent that can dissolve at least a portion of the non-volatile components. As the (H) organic solvent, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, and diphenyl ether; alcohol solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, and carbitol acetate (ethyl diglycol Ether ester solvents such as acetate, diethylene glycol monoethyl ether acetate), γ-butyrolactone, methoxypropionic acid methyl ester; ester alcohol solvents such as methyl lactate, ethyl lactate, 2-hydroxyisobutyric acid methyl ester; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, trimethylbenzene, etc. The organic solvent may be used alone or in combination of two or more in any ratio.

[0165] For the content of (H) organic solvent, from the viewpoint of effectively drying the resin composition, it can be set in a manner that the mass ratio of non-volatile components relative to the total mass of the resin composition, that is, the solid content ratio, is preferably 30% by mass or more, more preferably 35% by mass or more, further preferably 40% by mass or more, and particularly preferably 45% by mass or more. The upper limit of the solid content ratio is not particularly limited, and from the viewpoint of the handleability of the resin composition, it can be preferably 100% by mass or less, more preferably 95% by mass or less, further preferably 92% by mass or less, and particularly preferably 90% by mass or less.

[0166] <Method for producing resin composition>

[0167] The resin composition of the present invention can be manufactured in the following manner, for example: in any order and / or partially or entirely simultaneously, (A) thermosetting resin, (B) inorganic filler, (C) organic filler, (D) adhesive flexibilizer, (E) curing agent used as required, (F) curing accelerator used as required, (G) other additives used as required, (H) organic solvent used as required are added to any reaction vessel and mixed. In addition, in the process of adding each component and mixing, the temperature can be appropriately set, and heating and / or cooling can be performed temporarily or throughout. In addition, in the process of adding each component and mixing, stirring or vibration can be performed. In addition, when adding and mixing or afterwards, stirring devices such as mixers can be used to stir the resin composition so that it is evenly dispersed.

[0168] <Characteristics of resin composition>

[0169] The resin composition of the present invention contains not only (A) a thermosetting resin, (D) an adhesive flexibilizer, and (B) an inorganic filler, but also 5% by mass or more of (C) an organic filler, and thus can suppress tackiness to a low level while maintaining excellent flexibility.

[0170] The resin composition of the present invention contains the adhesive flexibilizer (D) and thus has sufficient flexibility. Therefore, for example, when a cured layer of the resin composition having a thickness of 40 μm, a width of 15 mm, and a length of 110 mm is subjected to an MIT folding test under the conditions of a load of 2.5 N, a bending angle of 90 degrees, a bending speed of 175 times / min, and a bending radius of 1.0 mm in accordance with JIS C-5016, the number of foldings can be preferably 3,000 times or more, more preferably 5,000 times or more, further preferably 7,000 times or more, and particularly preferably 8,000 times or more.

[0171] For the resin composition of the present invention, for example, the minimum melt viscosity of the resin composition measured under the conditions of a starting temperature of 60°C to 200°C, a heating rate of 5°C / min, a vibration frequency of 1 Hz, and a deformation of 1 deg can be preferably 40,000 poise or less, preferably 30,000 poise or less, preferably 20,000 poise or less, and preferably 10,000 poise or less.

[0172] The resin composition of the present invention contains (C) an organic filler. For example, the layered resin composition is tested using a probe tack tester with a probe diameter of 5 mm and a load of 1 kgf / cm 2The adhesion force measured under the conditions of a contact speed of 0.5 mm / sec, a stretching speed of 0.5 mm / sec, a holding time of 10 seconds, and a temperature of 80°C is preferably 2.0 N or less, more preferably 1.8 N or less, further preferably 1.7 N or less, and particularly preferably 1.6 N or less.

[0173] In addition, the resin composition of the present invention has the characteristics that void defects can be suppressed and pattern embedding properties are more excellent, especially when the content of the (C) organic filler is 10% by mass or less.

[0174] <Resin Sheet>

[0175] The resin sheet of the present invention includes a support and a resin composition layer formed from the resin composition of the present invention and provided on the support.

[0176] The thickness of the resin composition layer is preferably 200 μm or less, more preferably 150 μm or less, further preferably 100 μm or less, and particularly preferably 70 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, and can usually be 1 μm or more, 1.5 μm or more, 2 μm or more, etc.

[0177] Examples of the support include films made of plastic materials, metal foils, and release papers, and films made of plastic materials and metal foils are preferred.

[0178] When a film formed of a plastic material is used as a support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes referred to as "PET") and polyethylene naphthalate (hereinafter sometimes referred to as "PEN"), polycarbonate (hereinafter sometimes referred to as "PC"), acrylic polymers such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0179] When a metal foil is used as a support, examples of the metal foil include copper foil and aluminum foil, preferably copper foil. The copper foil may be a foil made of a single metal such as copper or an alloy of copper and other metals (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).

[0180] The surface of the support that contacts the resin composition layer may be subjected to matte treatment, corona treatment, or antistatic treatment.

[0181] In addition, as a support, a support with a release layer having a release layer on the surface bonded to the resin composition layer can be used. As a release agent for the release layer of the support with a release layer, for example, one or more release agents selected from alkyd resins, polyolefin resins, polyurethane resins, and silicone resins can be cited. The support with a release layer can use commercial products, for example, PET films having a release layer with an alkyd resin-based release agent as the main component, i.e., "SK-1", "AL-5", "AL-7" manufactured by Lintec Co., Ltd., "Lumirror T60" manufactured by Toray Industries, "Purex" manufactured by Teijin Co., Ltd., "Unipeel" manufactured by UNITIKA Co., Ltd., etc. can be cited.

[0182] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the thickness of the entire support with a release layer is preferably in the above range.

[0183] In one embodiment, the resin sheet may further include other layers as needed. As the other layers, for example, a protective film selected according to the support and disposed on the surface of the resin composition layer that is not bonded to the support (i.e., the surface on the opposite side of the support) can be cited. The thickness of the protective film is not particularly limited, for example, 1 μm to 40 μm. By laminating the protective film, dust and the like can be prevented from adhering to the surface of the resin composition layer, or damage can be prevented from occurring on the surface of the resin composition layer.

[0184] The resin sheet can be produced by directly coating the resin composition on a support using a die coater or the like, or by coating a resin varnish prepared by dissolving the resin composition in an organic solvent on a support and drying the varnish to form a resin composition layer.

[0185] Examples of the organic solvent that can be used when applying the mixture on the support include the same organic solvents as those listed in the description of the organic solvent (H) above. The organic solvent may be used alone or in combination of two or more.

[0186] Drying can be carried out by known methods such as heating and blowing hot air. The drying conditions are not particularly limited, and the drying is carried out in a manner such that the content of the organic solvent in the resin composition layer is 10% by mass or less, preferably 5% by mass or less. Although it varies with the boiling point of the organic solvent in the resin composition or resin varnish, for example, when a resin composition or resin varnish containing 30% to 60% by mass of an organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0187] The resin sheet can be stored by winding it into a roll. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0188] <Laminated Sheet>

[0189] The laminated sheet is a sheet made by laminating multiple layers of resin composition layers and curing. The laminated sheet contains multiple layers of insulating layers as a cured product of the resin composition layer. Usually, the number of resin composition layers laminated to make the laminated sheet is consistent with the number of insulating layers contained in the laminated sheet. The number of specific insulating layers per laminated sheet is usually more than 2, preferably more than 3, particularly preferably more than 5, preferably less than 20, more preferably less than 15, and particularly preferably less than 10.

[0190] The laminated sheet is a sheet used by bending (folding in half) with one surface facing the other. The minimum bending radius of the laminated sheet is not particularly limited, but is preferably 0.1 mm or more, more preferably 0.2 mm or more, further preferably 0.3 mm or more, preferably 5 mm or less, more preferably 4 mm or less, and particularly preferably 3 mm or less.

[0191] Holes may be formed in each insulating layer included in the laminated sheet, and the holes can function as through holes or through holes in the multi-layer flexible substrate.

[0192] For the laminated sheet, in addition to the insulating layer, it can also further include any element. For example, the laminated sheet can have a conductor layer as an arbitrary element. The conductor layer can usually be partially formed on the surface of the insulating layer or between the insulating layers. The conductor layer usually functions as a wiring in the multilayer flexible substrate.

[0193] The conductor material used in the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor material may be a single metal or an alloy. As an alloy, for example, an alloy of two or more metals selected from the above group (for example, nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy) can be cited. Among them, from the viewpoint of versatility, cost, ease of patterning, etc. of forming the conductor layer, chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper as a single metal is preferred; and alloys such as nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy. Among them, single metals of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper are more preferred; and nickel-chromium alloy, and single metal of copper is further preferred.

[0194] The conductor layer may be a single-layer structure or a multi-layer structure including two or more single metal layers or alloy layers formed of different types of metals or alloys. When the conductor layer is a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0195] The conductor layer may be patterned so as to function as wiring.

[0196] The thickness of the conductor layer depends on the design of the multi-layer flexible substrate, and is preferably 3 μm to 35 μm, more preferably 5 μm to 30 μm, further preferably 10 μm to 20 μm, and particularly preferably 15 μm to 20 μm.

[0197] The thickness of the laminated sheet is preferably 100 μm or more, more preferably 150 μm or more, particularly preferably 200 μm or more, and is preferably 2,000 μm or less, more preferably 1,000 μm or less, particularly preferably 500 μm or less.

[0198] <Method for producing laminated sheet>

[0199] The laminated sheet can be manufactured using a manufacturing method including the following steps: (a) a step of preparing a resin sheet; and (b) a step of using the resin sheet and laminating and curing a plurality of resin composition layers. The order of laminating and curing the resin composition layers is arbitrary as long as the desired laminated sheet can be obtained. For example, after all the multi-layer resin composition layers are laminated, the laminated multi-layer resin composition layers can be cured together. In addition, for example, each time another resin composition layer is laminated on a certain resin composition layer, the laminated resin composition layer can be cured.

[0200] A preferred embodiment of step (b) is described below. In the embodiments described below, for the purpose of distinction, the resin composition layers are appropriately denoted with symbols in the form of "first resin composition layer" and "second resin composition layer", and further, on the insulating layer obtained by curing these resin composition layers, the same as the resin composition layer, the insulating layer is also denoted with symbols in the form of "first insulating layer" and "second insulating layer".

[0201] In a preferred embodiment, step (b) comprises the following steps:

[0202] (II) a step of curing the first resin composition layer to form a first insulating layer,

[0203] (VI) a step of laminating a second resin composition layer on the first insulating layer,

[0204] (VII) a step of curing the second resin composition layer to form a second insulating layer. In addition, step (b) may further include any of the following steps as required:

[0205] (I) a step of laminating a first resin composition layer on a sheet-like supporting substrate,

[0206] (III) a step of opening a hole in the first insulating layer,

[0207] (IV) a step of roughening the first insulating layer,

[0208] (V) forming a conductor layer on the first insulating layer;

[0209] Hereinafter, each step will be described.

[0210] Step (I) is a step of laminating the first resin composition layer on the sheet-like supporting substrate before step (II). The sheet-like supporting substrate is a removable member, and for example, a plate-like, sheet-like, or film-like member can be used.

[0211] The lamination of the sheet-like support substrate and the first resin composition layer can be implemented by vacuum lamination. In the vacuum lamination method, the heating and pressing temperature is preferably 60°C to 160°C, more preferably in the range of 80°C to 140°C, the heating and pressing pressure is preferably 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the heating and pressing time is preferably 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably implemented under reduced pressure conditions with a pressure of 26.7hPa or less.

[0212] Lamination can be performed by a commercially available vacuum laminator. Examples of the commercially available vacuum laminator include a vacuum pressure laminator manufactured by Meiki Mfg. Co., Ltd., a vacuum applicator manufactured by Nikko-Materials Co., Ltd., and a batch vacuum pressure laminator.

[0213] When using a resin sheet, the lamination of the sheet-like support substrate and the first resin composition layer can be performed by, for example, pressing the resin sheet from the support body side, and heating and pressing the first resin composition layer of the resin sheet to the sheet-like support substrate. As a member (hereinafter sometimes appropriately referred to as a "heating and pressing member") for heating and pressing the resin sheet to the sheet-like support substrate, for example, a heated metal plate (SUS end plate, etc.) or a metal roller (SUS roller) can be cited. It is preferred that the heating and pressing member is not directly pressed to the resin sheet, but is pressed across an elastic material such as heat-resistant rubber so that the first resin composition layer fully follows the surface unevenness of the sheet-like support substrate.

[0214] After lamination, the first resin composition layer can be smoothed by, for example, pressing with a heating and pressing member under normal pressure (under atmospheric pressure). For example, when a resin sheet is used, the resin sheet is pressed with a heating and pressing member from the support side, so that the first resin composition layer of the resin sheet can be smoothed. The pressing conditions of the smoothing treatment can be set to the same conditions as the heating and pressing conditions of the above-mentioned lamination. The smoothing treatment can be performed using a commercially available laminator. The lamination and smoothing treatment can be performed continuously using the above-mentioned commercially available vacuum laminator.

[0215] Step (II) is a step of curing the first resin composition layer to form a first insulating layer. The heat curing conditions of the first resin composition layer are not particularly limited, and any conditions used when forming an insulating layer of a printed wiring board can be applied.

[0216] Generally, specific heat curing conditions vary depending on the type of resin composition. For example, the curing temperature is preferably 120°C to 240°C, more preferably 150°C to 220°C, and further preferably 170°C to 210°C. In addition, the curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 110 minutes, and further preferably 20 minutes to 100 minutes.

[0217] Before the first resin composition layer is thermally cured, the first resin composition layer may be preheated at a temperature lower than the curing temperature. For example, before the first resin composition layer is thermally cured, the first resin composition layer may be preheated at a temperature of 50° C. or higher and lower than 120° C. (preferably 60° C. or higher and 115° C. or lower, more preferably 70° C. or higher and 110° C. or lower) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and further preferably 15 minutes to 100 minutes).

[0218] Step (III) is a step of drilling holes in the first insulating layer. Through this step (III), holes such as through holes and through holes can be formed in the first insulating layer. The drilling can be carried out using, for example, a drill, laser, plasma, etc., depending on the composition of the resin composition. The size and shape of the hole can be appropriately set according to the design of the multilayer flexible substrate.

[0219] Step (IV) is a step of roughening the first insulating layer. Usually, smear removal is also performed in step (IV). Therefore, the roughening treatment is sometimes referred to as smear removal treatment. Examples of the roughening treatment include a swelling treatment using a swelling solution, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing solution.

[0220] The swelling liquid is not particularly limited, and examples thereof include alkaline aqueous solutions such as sodium hydroxide aqueous solution and potassium hydroxide aqueous solution. Examples of commercially available swelling liquids include "Swelling Dip Securiganth P" and "Swelling Dip Securiganth SBU" manufactured by ATOTECH JAPAN. The swelling treatment using the swelling liquid can be performed, for example, by immersing the cured body in a swelling liquid at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 minutes to 15 minutes.

[0221] As the oxidant, there is no particular limitation, and an alkaline permanganate solution formed by dissolving permanganate in an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution can be cited. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. As commercially available oxidants, alkaline permanganate solutions such as "Concentrate Compact P", "Concentrate Compact CP", and "Dosing Solution Securiganth P" manufactured by ATOTECH JAPAN can be cited. The roughening treatment using the oxidant can be performed by immersing the cured body in an oxidant solution heated to 60°C to 80°C for 10 minutes to 30 minutes.

[0222] In addition, an acidic aqueous solution can be used as a neutralizing solution. As a commercially available product, for example, "Reduction Solution Securiganth P" manufactured by ATOTECH JAPAN Co., Ltd. can be cited. The treatment with the neutralizing solution can be carried out by immersing the solidified body in a neutralizing solution at 30°C to 80°C for 5 minutes to 30 minutes. In view of operability, etc., it is preferred to immerse the solidified body in a neutralizing solution at 40°C to 70°C for 5 minutes to 20 minutes.

[0223] The arithmetic mean roughness (Ra) of the surface of the roughened first insulating layer is preferably 400 nm or less, more preferably 300 nm or less, and further preferably 200 nm or less. The lower limit is not particularly limited and may be 30 nm or more, 40 nm or more, or 50 nm or more.

[0224] Step (V) is a step of forming a conductor layer on the first insulating layer as needed. Regarding the method for forming the conductor layer, for example, a plating method, a sputtering method, a vapor deposition method, etc. can be cited, among which a plating method is preferred. As a preferred example, a method of plating on the surface of the first insulating layer using an appropriate method such as a semi-additive method and a full-additive method to form a conductor layer having a desired wiring pattern can be cited. Among them, from the viewpoint of simplicity of production, a semi-additive method is preferred.

[0225] The following is an example of forming a conductor layer using a semi-additive method. First, a plating seed layer is formed on the surface of a first insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a portion of the plating seed layer corresponding to a desired wiring pattern. A metal layer is formed on the exposed plating seed layer by electrolytic plating, and then the mask pattern is removed. Then, the unnecessary plating seed layer is removed by etching or other treatments to form a conductor layer having a desired wiring pattern.

[0226] In step (II), a first insulating layer is obtained, and if necessary, steps (III), (IV), and (V) are performed, and then step (VI) is performed. Step (VI) is a step of laminating a second resin composition layer on the first insulating layer. The lamination of the first insulating layer and the second resin composition layer can be performed by the same method as the lamination of the sheet-like supporting substrate and the first resin composition layer in step (I).

[0227] However, when the first resin composition layer is formed using a resin sheet, the support of the resin sheet is removed before step (VI). The support may be removed between step (I) and step (II), between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V).

[0228] After step (VI), step (VII) is performed. Step (VII) is a step of curing the second resin composition layer to form a second insulating layer. The curing of the second resin composition layer can be performed by the same method as the curing of the first resin composition layer in step (II). Thus, a laminated sheet including a multilayer insulating layer such as a first insulating layer and a second insulating layer can be obtained.

[0229] In addition, in the method according to the aforementioned embodiment, as necessary, a step (VIII) of opening a hole on the second insulating layer, a step (IX) of roughening the second insulating layer, and a step (X) of forming a conductor layer on the second insulating layer may be performed. The opening of the second insulating layer in step (VIII) may be performed by the same method as the opening of the first insulating layer in step (III). In addition, the roughening of the second insulating layer in step (IX) may be performed by the same method as the roughening of the first insulating layer in step (IV). Furthermore, the formation of the conductor layer on the second insulating layer in step (X) may be performed by the same method as the formation of the conductor layer on the first insulating layer in step (V).

[0230] In the aforementioned embodiment, the embodiment of manufacturing a laminated sheet by stacking and curing of two layers of resin composition layers such as the first resin composition layer and the second resin composition layer is described, but a laminated sheet can also be manufactured by stacking and curing of more than three layers of resin composition layers. For example, in the method related to the aforementioned embodiment, the stacking and curing of the resin composition layer performed by steps (VI) to (VII), and the opening of the insulating layer performed by steps (VIII) to (X) as needed, the roughening treatment of the insulating layer, and the formation of the conductor layer on the insulating layer can be repeatedly implemented to manufacture a laminated sheet. Thus, a laminated sheet comprising more than three layers of insulating layers can be obtained.

[0231] Furthermore, the method according to the above-mentioned embodiment may include any steps other than the above-mentioned steps. For example, when step (I) is performed, a step of removing the sheet-like supporting substrate may be performed.

[0232] <Multilayer flexible substrate>

[0233] The multilayer flexible substrate includes a laminated sheet. The multilayer flexible substrate may include only the laminated sheet, or may include not only the laminated sheet but also any other member. Examples of the other members include electronic components and cover films.

[0234] The multilayer flexible substrate can be manufactured by a manufacturing method including a method for manufacturing the above-mentioned laminated sheet. Therefore, the multilayer flexible substrate can be manufactured by a manufacturing method including the following steps: (a) a step of preparing a resin sheet, and (b) a step of using the resin sheet and laminating and curing a plurality of resin composition layers.

[0235] The method for manufacturing a multilayer flexible substrate may include not only the aforementioned steps but also any other steps. For example, the method for manufacturing a multilayer flexible substrate having an electronic component may include the step of joining the electronic component to a laminated sheet. Regarding the joining conditions between the laminated sheet and the electronic component, any conditions may be adopted under which the terminal electrodes of the electronic component and the conductor layer as wiring provided on the laminated sheet can be connected to each other. In addition, for example, the method for manufacturing a multilayer flexible substrate having a cover film may include the step of laminating the laminated sheet with the cover film.

[0236] The aforementioned multi-layer flexible substrate can usually be used by being bent in a manner that one surface of the laminated sheet included in the multi-layer flexible substrate faces each other. For example, the multi-layer flexible substrate is accommodated in a housing of a semiconductor device in a state where the multi-layer flexible substrate is bent and reduced in size. In addition, for example, in a semiconductor device having a bendable movable portion, the multi-layer flexible substrate is provided in the movable portion.

[0237] <Semiconductor devices>

[0238] The semiconductor device includes the aforementioned multi-layer flexible substrate. The semiconductor device includes, for example, a multi-layer flexible substrate and a semiconductor chip mounted on the multi-layer flexible substrate. In most semiconductor devices, the multi-layer flexible substrate can be bent in a manner such that one surface of the stacked sheets included in the multi-layer flexible substrate faces each other and is accommodated in a housing of the semiconductor device.

[0239] Examples of the semiconductor device include various semiconductor devices that can be used in electrical products (eg, computers, mobile phones, digital cameras, and televisions) and vehicles (eg, motorcycles, cars, trains, ships, and aircraft).

[0240] The semiconductor device described above can be manufactured, for example, by a manufacturing method including the steps of preparing a multilayer flexible substrate, bending the multilayer flexible substrate so that one surface of a laminated sheet faces each other, and housing the bent multilayer flexible substrate in a housing. Example

[0241] Hereinafter, the present invention will be specifically described by way of examples. However, the present invention is not limited by the following examples. In the following description, unless otherwise clearly stated, the "parts" and "%" indicating the amount respectively indicate "parts by mass" and "% by mass". In addition, unless otherwise clearly stated, the operations described below are performed in an environment of normal temperature and pressure.

[0242] <Synthesis Example 1: Synthesis of polybutadiene resin containing phenolic hydroxyl group>

[0243] 69 g of difunctional hydroxy-terminated polybutadiene ("G-3000" manufactured by Nippon Soda Co., Ltd., number average molecular weight = 3000, hydroxyl equivalent = 1800 g / eq.), 40 g of aromatic hydrocarbon mixed solvent ("Ipzole 150" manufactured by Idemitsu Petrochemical Co., Ltd.), and 0.005 g of dibutyltin laurate were added to a reaction container and mixed to uniformly dissolve. After becoming uniform, the temperature was raised to 60° C., and 8 g of isophorone diisocyanate ("IPDI" manufactured by Evonik Degussa Japan Co., Ltd., isocyanate equivalent = 113 g / eq.) was further added while stirring, and the reaction was carried out for about 3 hours.

[0244] Next, 23 g of cresol novolac resin ("KA-1160" manufactured by DIC Corporation, hydroxyl equivalent = 117 g / eq.) and 60 g of ethyl diglycol acetate (manufactured by Daicel Corporation) were added to the reactant, and the mixture was heated to 150° C. while stirring, and the reaction was carried out for about 10 hours. The FT-IR spectra at 2250 cm -1The disappearance of the NCO peak was confirmed. The disappearance of the NCO peak was considered the end point of the reaction, and the reactants were cooled to room temperature. Then, the reactants were filtered with a 100-mesh filter cloth to obtain an elastomer having a butadiene structure and phenolic hydroxyl groups (polybutadiene resin containing phenolic hydroxyl groups: non-volatile components 50% by mass). The number average molecular weight of the elastomer is 5900, and the glass transition temperature is -7°C.

[0245] <Synthesis Example 2: Synthesis of polyimide resin 1>

[0246] In a 500 ml separable flask equipped with a nitrogen inlet pipe and a stirring device, 9.13 g (30 mmol) of 5-amino-1,1'-biphenyl-2-yl 4-aminobenzoate, 15.61 g (30 mmol) of 4,4'-(4,4'-isopropyldiphenyloxy)diphthalic dianhydride, 94.64 g of N-methyl-2-pyrrolidone, 0.47 g (6 mmol) of pyridine, and 10 g of toluene were added, and an imidization reaction was carried out for 4 hours at 180° C. under a nitrogen atmosphere while excluding toluene from the system during the process, thereby obtaining a polyimide solution (non-volatile content 20% by mass) containing polyimide resin 1. In the polyimide solution, no precipitation of the synthesized polyimide resin 1 was observed.

[0247] <Synthesis Example 3: Synthesis of polyimide resin 2>

[0248] A reaction vessel equipped with a stirrer, a water separator, a thermometer and a nitrogen inlet tube was charged with 65.0 g of aromatic tetracarboxylic dianhydride ("BisDA-1000" manufactured by SABIC JAPAN, 4,4'-(4,4'-isopropyldiphenyloxy) diphthalic dianhydride), 266.5 g of cyclohexanone, and 44.4 g of methylcyclohexane, and the solution was heated to 60°C. Next, 43.7 g of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan) and 5.4 g of 1,3-bis(aminomethyl)cyclohexane were added dropwise, and then an imidization reaction was carried out at 140°C for 1 hour. Thus, a polyimide solution (non-volatile component 30% by mass) containing polyimide resin 2 was obtained. In addition, the weight average molecular weight of polyimide resin 2 was 25,000.

[0249] <Synthesis Example 4: Synthesis of polyimide resin 3>

[0250] Prepare a 500 mL detachable flask equipped with a water quantitative receiver connected to a reflux condenser, a nitrogen inlet tube, and a stirrer. Add 20.3 g of 4,4'-oxydiphthalic anhydride (ODPA), 200 g of γ-butyrolactone, 20 g of toluene, and 29.6 g of 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane to the flask, stir at 45°C for 2 hours under a nitrogen stream, and react. Next, the reaction solution was heated, and the condensation water was removed azeotropically with toluene under a nitrogen stream while being maintained at about 160°C. It was confirmed that "a predetermined amount of water was accumulated in the water quantitative receiver" and "no water outflow was observed". After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. The mixture was then cooled to obtain a polyimide solution (non-volatile content 20% by mass) containing polyimide resin 3. The obtained polyimide resin 3 had a repeating unit represented by the following formula (X1) and a repeating unit represented by the following formula (X2). The weight average molecular weight of the polyimide resin 3 was 12,000.

[0251] [Chemical formula 4]

[0252] .

[0253] [Chemical formula 5]

[0254] .

[0255] <Example 1>

[0256] A mixed solvent of 5 parts of a biphenylol epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Corporation, with an epoxy equivalent of about 185 g / eq.), 5 parts of a naphthalene epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd., with an epoxy equivalent of about 332 g / eq.), 10 parts of a bisphenol AF epoxy resin ("YL7760" manufactured by Mitsubishi Chemical Corporation, with an epoxy equivalent of about 238 g / eq.), 2 parts of a cyclohexane epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical Corporation, with an epoxy equivalent of about 135 g / eq.), 40 parts of a polybutadiene resin containing a phenolic hydroxyl group obtained in Synthesis Example 1 (non-volatile content 50% by mass), and 10 parts of cyclohexanone was heated and dissolved while stirring. After cooling to room temperature, 4 parts of a cresol novolac curing agent containing a triazine skeleton ("LA-3018-50P" manufactured by DIC Corporation, a 2-methoxypropanol solution with a hydroxyl equivalent of about 151 and a non-volatile content of 50%), 6 parts of an active ester curing agent ("EXB-8000L-65M" manufactured by DIC Corporation, an MEK solution with an active group equivalent of about 220 and a non-volatile content of 65% by mass), and spherical silica ("SC2500SQ" manufactured by Yaduma Corporation, with an average particle size of 0.5 μm and a specific surface area of ​​11.2 m 2 / g, 100 parts of silica (a material surface-treated with 1 part of N-phenyl-3-aminopropyltrimethoxysilane ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.) 40 parts, core-shell graft copolymer rubber particles ("EXL2655" manufactured by Dow Chemical Japan Co., Ltd.) 6 parts, and 0.2 parts of an amine curing accelerator (4-dimethylaminopyridine (DMAP)) were uniformly dispersed using a high-speed rotary mixer, and then filtered using a cartridge filter ("SHP020" manufactured by ROKITECHNO Co., Ltd.) to prepare a resin composition.

[0257] <Example 2>

[0258] A resin composition was prepared by the same operation as in Example 1 except that 100 parts of the polyimide solution (non-volatile content 20% by mass) obtained in Synthesis Example 2 was used instead of 40 parts of the polybutadiene resin (non-volatile content 50% by mass) containing a phenolic hydroxyl group obtained in Synthesis Example 1.

[0259] <Example 3>

[0260] A resin composition was prepared by the same operation as in Example 1 except that 66.7 parts of the polyimide solution (non-volatile content 30% by mass) obtained in Synthesis Example 3 was used instead of 40 parts of the polybutadiene resin (non-volatile content 50% by mass) containing phenolic hydroxyl groups obtained in Synthesis Example 1.

[0261] <Example 4>

[0262] A resin composition was prepared by the same operation as in Example 1 except that 100 parts of the polyimide solution (non-volatile content 20% by mass) obtained in Synthesis Example 4 was used instead of 40 parts of the polybutadiene resin (non-volatile content 50% by mass) containing a phenolic hydroxyl group obtained in Synthesis Example 1.

[0263] <Example 5>

[0264] A resin composition was prepared by the same operation as in Example 1, except that 40 parts of a resin containing a polybutadiene structure (manufactured by Nippon Kayaku Co., Ltd., "BX360", a block copolymer of polyphenylene ether and polybutadiene, a toluene solution with a non-volatile content of 50% by mass) was used instead of 40 parts of the polybutadiene resin containing phenolic hydroxyl groups (non-volatile content of 50% by mass) obtained in Synthesis Example 1.

[0265] <Example 6>

[0266] A resin composition was prepared in the same manner as in Example 1 except that 20 parts of a bismaleimide resin (“BMI689” manufactured by DM Co.) was used instead of 40 parts of the phenolic hydroxyl group-containing polybutadiene resin (non-volatile content: 50% by mass) obtained in Synthesis Example 1.

[0267] <Example 7>

[0268] A resin composition was prepared by the same operation as in Example 1, except that 50 parts of a polyrotaxane resin (a 40% solution of methyl ethyl ketone of "SH1310P" manufactured by Advanced Softmaterials, in which the axial molecule comprises a polyethylene glycol chain and the cyclic molecule comprises a cyclodextrin) was used instead of 40 parts of the polybutadiene resin containing a phenolic hydroxyl group (50% by mass of non-volatile matter) obtained in Synthesis Example 1.

[0269] <Example 8>

[0270] A resin composition was prepared in the same manner as in Example 1 except that the amount of the core-shell type graft copolymer rubber particles ("EXL2655" manufactured by Dow Chemical Japan Co., Ltd.) used in Example 1 was changed from 6 parts to 12 parts.

[0271] <Comparative Example 1>

[0272] A resin composition was prepared by performing the same operations as in Example 1, except that the amount of spherical silica ("SC2500SQ" manufactured by Yaduma Co., Ltd., a surface-treated material) used in Example 1 was changed from 40 parts to 70 parts, and the amount of core-shell graft copolymer rubber particles ("EXL2655" manufactured by Dow Chemical Japan Co., Ltd.) used was changed from 6 parts to 5 parts.

[0273] <Comparative Example 2>

[0274] A resin composition was prepared by the same operation as in Example 1 except that 6 parts of the core-shell type graft copolymer rubber particles ("EXL2655" manufactured by Dow Chemical Japan Co., Ltd.) of Example 1 were not used.

[0275] <Comparative Example 3>

[0276] A resin composition was prepared by the same operation as in Example 1 except that 42 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, solid content 30% by mass) was used instead of 40 parts of a polybutadiene resin containing a phenolic hydroxyl group (non-volatile content 50% by mass) obtained in Synthesis Example 1.

[0277] <Test Example 1: Evaluation of flexibility (MIT folding resistance)>

[0278] The resin composition of each embodiment and comparative example was uniformly applied on a release-treated surface of a PET film (38 μm thick) treated with an alkyd release agent using a die coater so that the thickness of the resin composition layer after drying became 40 μm, and dried at 80 to 120° C. (100° C. on average) for 6 minutes to obtain a resin sheet.

[0279] The obtained resin sheet was laminated on a polyimide film (UPILEX S, manufactured by Ube Industries, Ltd.) using an intermittent vacuum pressurizing laminator (MVLP-500 manufactured by Meiki Seisakusho Co., Ltd.). For lamination, the pressure was reduced for 30 seconds to a pressure of 13 hPa or less, and then the pressure was pressed at 120° C. for 30 seconds at a pressure of 0.74 MPa to obtain a resin sheet with a protective film. Then, the PET film was peeled off from the resin sheet with a protective film, and the resin composition was cured under curing conditions of 190° C. and 90 minutes, and the polyimide film was peeled off to obtain a cured product sample.

[0280] The obtained solidified sample was cut into test pieces with a width of 15 mm and a length of 110 mm. The MIT test device (manufactured by Toyo Seiki Seisaku-sho, Ltd., MIT folding fatigue tester "MIT-DA") was used to measure the number of folding times of the solidified body until it broke under the measurement conditions of a load of 2.5 N, a bending angle of 90 degrees, a bending radius of 1.0 mm, and a bending speed of 175 times / minute in accordance with JIS C-5016. It should be noted that 5 samples were measured, and the average value of the top three samples from largest to smallest was calculated. The case where the number of folding times was less than 8,000 times was evaluated as "×", and the case where the number of folding times was more than 8,000 times was evaluated as "○".

[0281] <Test Example 2: Evaluation of Pattern Embedding Property and Flatness>

[0282] <Test Example 2-1: Measurement of minimum melt viscosity>

[0283] The minimum melt viscosity was measured using a dynamic viscoelasticity measuring device ("Rheosol-G3000" manufactured by UBM Co., Ltd.) for the resin composition layer of the resin sheet obtained in Test Example 1. For 1 g of the sample resin composition collected from the resin composition layer, the temperature was raised from a starting temperature of 60°C to 200°C at a heating rate of 5°C / min using a parallel plate having a diameter of 18 mm, and the dynamic viscoelastic modulus was measured under the measurement conditions of a measurement temperature interval of 2.5°C, a vibration frequency of 1 Hz, and a deformation of 1 degree, and the minimum melt viscosity (poise) was measured.

[0284] <Test Example 2-2: Measurement of Adhesive Strength>

[0285] The protective film was peeled off from the resin sheet with a protective film obtained in Test Example 1, and the resin composition layer was subjected to a probe viscosity tester (TESTER Industries, Ltd., "TE-6002") using a glass probe with a diameter of 5 mm and a load of 1 kgf / cm 2 , contact speed 0.5 mm / sec, tensile speed 0.5 mm / sec, holding time 10 sec, temperature 80° C. Adhesion force (N) was evaluated as “×” when it was greater than 1.6 N, and as “○” when it was less than 1.6 N.

[0286] <Test Example 2-3: Evaluation of Pattern Embedding Property and Void>

[0287] As the inner layer circuit board, a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness of 18 μm, substrate thickness of 0.15 mm, "HL832NSF LCA" manufactured by Mitsubishi Gas Chemical Co., Ltd., size of 255*340 mm) having a circuit conductor (copper) formed in a 1 mm square wiring pattern (residual copper rate of 59%) on both sides was prepared. The copper surface was roughened with "CZ8201" manufactured by MEC Co., Ltd. on both sides of the inner layer circuit board (copper etching amount of 0.5 μm).

[0288] The resin sheet obtained in Test Example 1 was laminated on both sides of the inner layer circuit board using an intermittent vacuum pressurizing laminator (2-Stage Buildup Laminator, CVP700, manufactured by Nikko-Materials Co., Ltd.) in such a manner that the resin composition layer was in contact with the inner layer circuit board. Lamination was performed by reducing the pressure for 30 seconds to a pressure of 13 hPa or less, and then pressing at 130° C. and a pressure of 0.74 MPa for 45 seconds. Next, hot pressing was performed at 120° C. and a pressure of 0.5 MPa for 75 seconds.

[0289] The inner layer circuit board laminated with the resin sheet was placed in an oven at 100°C for post-heat curing for 30 minutes at 100°C, and then moved to an oven at 180°C for post-heat curing for 30 minutes at 180°C to form an insulating layer. This was referred to as an "evaluation substrate".

[0290] The support was peeled off from the evaluation substrate, and the surface of the insulating layer was observed with a micro optical microscope. Regarding pattern embedding, the case where it was fully embedded was evaluated as "○", and the case where it was insufficiently embedded was evaluated as "×". Regarding pores, the case where no pores were generated was evaluated as "○", and the case where pores were generated was evaluated as "×".

[0291] The amounts of nonvolatile components used in the resin compositions of Examples and Comparative Examples, and the measurement results and evaluation results of the Test Examples are shown in Table 1 below.

[0292] [Table 1]

[0293] .

[0294] It is known that by using a resin composition comprising (A) a thermosetting resin, (B) an inorganic filler, 5% by mass or more of (C) an organic filler, and (D) an adhesive flexibilizer, it is possible to suppress adhesion to a low level while maintaining excellent flexibility. It is known that, in particular, when (C) the organic filler is 10% by mass or less, poor porosity can be suppressed and excellent pattern embedding properties can be achieved.

Claims

1. A resin composition comprising (A) an epoxy resin, (B) an inorganic filler, (C) core-shell particles, (D) an adhesive flexibilizer, and (E) a curing agent, in, When the nonvolatile component in the resin composition is 100 mass %, the content of the component (B) is 20 mass % or more and 50 mass % or less, When the nonvolatile components in the resin composition are set to 100% by mass, the content of the component (C) is 5% by mass or more. When the nonvolatile components in the resin composition are set to 100% by mass, the content of the component (D) is 1% by mass or more. (B) component contains silicon dioxide, (D) component is selected from a resin having a polybutadiene structure, a polyrotaxane resin, a polyimide resin, and a maleimide resin having a dimer acid skeleton, The component (E) contains an active ester curing agent.

2. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100 mass %, the content of the component (A) is 5 mass % or more and 50 mass % or less.

3. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100 mass %, the content of the component (A) is 20 mass % or more and 25 mass % or less.

4. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (B) is 45% by mass or less.

5. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (B) is 38% by mass or more.

6. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (C) is 6.2% by mass or more.

7. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (C) is 30% by mass or less.

8. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (C) is 10% by mass or less.

9. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (C) is 8% by mass or less.

10. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (D) is 15% by mass or more.

11. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100% by mass, the content of the component (D) is 50% by mass or less.

12. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100 mass %, content of the component (D) is 25 mass % or less.

13. The resin composition according to claim 1, wherein (C) The core-shell type particles are core-shell type graft copolymer particles.

14. The resin composition according to claim 13, wherein The monomer component forming the shell portion of the core-shell type graft copolymer particles is a (meth)acrylic acid ester.

15. The resin composition according to claim 13, wherein The core particles of the core-shell type graft copolymer particles contain a thermoplastic elastomer.

16. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100 mass %, the content of the component (E) is 0.1 mass % or more and 30 mass % or less.

17. The resin composition according to claim 1, wherein When the nonvolatile matter in the resin composition is 100 mass %, the content of the component (E) is 4 mass % or more and 10 mass % or less. 18 . The resin composition according to claim 1 , further comprising (F) a curing accelerator.

19. The resin composition according to claim 18, wherein When the nonvolatile matter in the resin composition is 100 mass %, content of the component (F) is 0.001 mass % or more and 2 mass % or less.

20. The resin composition according to claim 18, wherein When the nonvolatile matter in the resin composition is 100 mass %, content of the component (F) is 0.1 mass % or more and 0.3 mass % or less.

21. The resin composition according to claim 1, wherein The solid content ratio in the resin composition is 95% by mass or less.

22. The resin composition according to claim 1, which is used to form an insulating layer of a multi-layer flexible substrate. 23 . A cured product, which is a cured product of the resin composition according to claim 1 .

24. A resin sheet comprising: Support body, and A resin composition layer formed from the resin composition according to any one of claims 1 to 22, provided on the support. 25 . A multi-layer flexible substrate comprising an insulating layer formed by curing the resin composition according to claim 1 . 26 . A semiconductor device comprising the multi-layer flexible substrate according to claim 25 .