A method for preparing ferric orthophosphate using ferrous phosphate

By grinding and washing ferrous phosphate multiple times, combined with flash evaporation treatment, the problems of high cost and unstable quality of the existing ferrous phosphate production process are solved, and high-purity, low-cost ferrous phosphate preparation is achieved, with superior processing performance and Electrochemical properties.

CN111825071BActive Publication Date: 2024-10-29SHANDONG LUBEI ENTERPRISE GROUP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010720309.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-24
Publication Date
2024-10-29
Estimated Expiration
2040-07-24

AI Technical Summary

Technical Problem

The existing ferric phosphate production process has high costs, high energy consumption, complex processes and unstable product quality, resulting in many shortcomings in the production of ferric phosphate.

Method used

By grinding ferrous phosphate, controlling its particle size, and using hydrogen peroxide for full reaction, combined with multiple washing and flash evaporation treatments, to ensure a stable iron-phosphorus ratio and uniform particle size of ferrous phosphate, further through electrochemical testing and negative pressure air transport Quick drying to achieve the preparation of high-purity iron orthophosphate.

Benefits of technology

The iron-phosphorus ratio stability and particle size controllability of ferric phosphate are achieved, the production cost is reduced, the processing performance and electrochemical performance of the product are improved, the impurity removal efficiency reaches more than 90%, and the product reaches 99.9% high purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111825071B_ABST
    Figure CN111825071B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing ferric orthophosphate using ferrous phosphate, wherein ferrous phosphate slurry is ground, and the particle size of the material after grinding is controlled; ferrous phosphate slurry is mixed with phosphoric acid and a slightly excessive amount of hydrogen peroxide, and the temperature is raised and matured after sufficient reaction; the cooled ferric phosphate slurry is filtered and washed by a plate and frame filter press; the washed filter cake is dried by a flash dryer to obtain ferric phosphate dihydrate, and then crystal water is removed by a new rotary kiln to obtain ferric orthophosphate. The method provided by the present invention can prepare ferric orthophosphate with a particle size of 2-4 μm, and the prepared ferric orthophosphate material has a higher bulk density, and the synthesized lithium iron phosphate has better electrochemical properties, and has a good application prospect in the field of lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical industry, and in particular to a method for preparing ferric orthophosphate by utilizing ferrous phosphate. Background Art

[0002] Iron phosphate is the raw material for lithium iron phosphate, the positive electrode material of lithium batteries. With the development and utilization of new energy in my country, the demand for it is increasing. Iron phosphate can also be used as a catalyst and in the manufacture of ceramics.

[0003] After a lot of searching, we know that: Chinese invention patent: application number [CN201110072970.9], publication number [CN102153061A] A method for synthesizing an orthophosphate iron material, the present invention relates to a method for synthesizing an orthophosphate iron material. The present invention belongs to the technical field of lithium ion positive electrode materials. A method for synthesizing an orthophosphate iron material, the steps are: 1) making a hollow sphere template: oil with a carbon-hydrogen bond and a water-soluble surfactant without metal ions are stirred in an aqueous solution for 0.1-10 hours to form an emulsion; the weight ratio of the oil and the surfactant is 1:1-9, accounting for 0.1-5% of the total weight of the solution; 2) orthophosphate iron precipitation: with this emulsion, in an acidic solution in the presence of phosphate and trivalent iron salt, the pH value of the solution is adjusted to form an orthophosphate iron precipitate; the precipitate is attached to the emulsion microsphere, forming a structure with iron phosphate on the outside and the emulsion microsphere as the core; 3) orthophosphate iron microsphere treatment: the emulsion microsphere is filtered and dried, and then calcined at high temperature to form a hollow / shell structure microsphere orthophosphate iron material. The invention has the advantages of simple process, convenient operation, stable iron orthophosphate microspheres, large rate discharge capacity and low temperature capacity.

[0004] At present, the production process of ferric phosphate is the synthesis of iron salt and phosphate or the direct production of iron powder and phosphoric acid. It has the disadvantages of high production cost and energy consumption, complex production process, and high impurities, resulting in poor product quality stability. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing ferric orthophosphate by using ferrous phosphate, which solves the problems raised by the background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing ferric orthophosphate using ferrous phosphate, comprising the following process flow:

[0007] Step S1: grinding the ferrous phosphate slurry, sending the ground slurry to a storage tank after sand grinding, and cooling it through a cold water coil for standby use;

[0008] Step S2: pumping the ferrous phosphate slurry and phosphoric acid into a weighing and metering tank respectively, adding a certain amount of ferrous phosphate slurry into the reactor through the weighing and metering tank, adding a certain amount of water, phosphoric acid and hydrogen peroxide respectively, and after sufficient reaction, heating and aging through the outer half-tube steam, discharging the material into the cooling tank for cooling, and then pumping it to the water washing feed tank;

[0009] Step S3: The cooled iron phosphate slurry is separated into solid and liquid by a filter press to remove phosphate in the slurry. After five washings until the conductivity is qualified, the filter cake is slurried and pumped to the kiln tail storage tank; the filtrate is pumped to the CN filter for sedimentation separation, the upper clear liquid overflows into the clear liquid tank, the thick slurry enters the thick slurry tank, and then pumped to the water washing feed tank;

[0010] Step S4: removing part of the free water in the ferric phosphate solution through a diaphragm pressing plate frame to increase the solid content of the ferric phosphate; and controlling the flash drying feed amount.

[0011] Step S5: The iron phosphate filter cake of the filter plate frame is dried by the flash evaporator to remove moisture. After the flash drying and the feeding of the silo are completed, according to the discharge time of the rotary kiln, after the thick material layer reaches the last temperature zone, the speed of the rotary kiln is increased to above 13Hz, and the frequency conversion of the induced draft fan is turned to the maximum, and the thin material layer is quickly transported out by negative pressure air delivery;

[0012] Step S6: removing crystal water from the dihydrate ferric phosphate that has been flash-dried to have no free water at 580-600 degrees, testing the electrochemical properties of the anhydrous ferric phosphate after cooling, and preparing the ingredients for ferric orthophosphate synthesis.

[0013] Preferably, in steps S1 and S2, the ferrous phosphate is sand-ground to a particle size of less than 4 microns, and the amount of phosphoric acid and hydrogen peroxide added is calculated according to the iron content and phosphoric acid content in the slurry, and pumped into the ferrous phosphate synthesis kettle.

[0014] Preferably, in step S3, the iron phosphate is separated by a filter press and then washed five times until the conductivity is qualified.

[0015] Preferably, in steps S4 and S5, the ferric phosphate is passed through a diaphragm pressing plate frame to remove part of the moisture to increase the solid content, and then dried by a flash evaporation main machine to remove the moisture.

[0016] Preferably, in step S6, the ferric phosphate dihydrate that is flash dried to be free of free water is subjected to a temperature of 580-600 degrees to remove crystal water.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] In the grinding process described in the present invention, the particle size of the ferrous phosphate after grinding is controlled, so that the oxidation process of the final ferrous phosphate product is controllable and the particle size is uniform. By adding a slight excess of hydrogen peroxide, the complete reaction of the oxidation process is guaranteed, so that the iron-phosphorus ratio of the ferrous phosphate product is stable. The particle size of the ferrous phosphate prepared by this method is controllable, the iron-phosphorus ratio is stable and high, and the lithium iron phosphate used for production has the advantages of excellent processing performance and stable electrical properties; the present invention makes full use of ferrous sulfate resources, removes titanium, calcium, magnesium, zinc, manganese and other ions at a relatively low cost, and the impurity removal efficiency reaches more than 90%, and obtains a high-purity food-grade ferric orthophosphate with a content of more than 99.9%. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The figure is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] See also Figure 1 The present invention provides a method for preparing ferric orthophosphate by using ferrous phosphate. A method for preparing ferric orthophosphate by using ferrous phosphate includes the following process flow:

[0022] Step S1: grinding the ferrous phosphate slurry, sending the ground slurry to a storage tank after sand grinding, and cooling it through a cold water coil for standby use;

[0023] Step S2: pumping the ferrous phosphate slurry and phosphoric acid into a weighing and metering tank respectively, adding a certain amount of ferrous phosphate slurry into the reactor through the weighing and metering tank, adding a certain amount of water, phosphoric acid and hydrogen peroxide respectively, and after sufficient reaction, heating and aging through the outer half-tube steam, discharging the material into the cooling tank for cooling, and then pumping it to the water washing feed tank;

[0024] Step S3: The cooled iron phosphate slurry is separated into solid and liquid by a filter press to remove phosphate in the slurry. After five washings until the conductivity is qualified, the filter cake is slurried and pumped to the kiln tail storage tank; the filtrate is pumped to the CN filter for sedimentation separation, the upper clear liquid overflows into the clear liquid tank, the thick slurry enters the thick slurry tank, and then pumped to the water washing feed tank;

[0025] Step S4: removing part of the free water in the ferric phosphate solution through a diaphragm pressing plate frame to increase the solid content of the ferric phosphate; and controlling the flash drying feed amount.

[0026] Step S5: The iron phosphate filter cake of the filter plate frame is dried by the flash evaporator to remove moisture. After the flash drying and the feeding of the silo are completed, according to the discharge time of the rotary kiln, after the thick material layer reaches the last temperature zone, the speed of the rotary kiln is increased to above 13Hz, and the frequency conversion of the induced draft fan is turned to the maximum, and the thin material layer is quickly transported out by negative pressure air delivery;

[0027] Step S6: removing crystal water from the dihydrate ferric phosphate that has been flash-dried to have no free water at 580-600 degrees, testing the electrochemical properties of the anhydrous ferric phosphate after cooling, and preparing the ingredients for ferric orthophosphate synthesis.

[0028] In the embodiment of the present invention, further, in steps S1 and S2, the ferrous phosphate is sand-ground to a particle size of less than 4 microns, and the amount of phosphoric acid and hydrogen peroxide added is calculated according to the iron content and phosphoric acid content in the slurry, and pumped into the ferrous phosphate synthesis kettle.

[0029] In the embodiment of the present invention, further, in step S3, the iron phosphate is separated by a filter press and then washed five times until the conductivity is qualified.

[0030] In the embodiment of the present invention, further, in steps S4 and S5, the ferric phosphate is passed through a diaphragm pressing plate frame to remove part of the moisture to increase the solid content, and then the ferrous phosphate is dried by a flash evaporation main machine to remove the moisture.

[0031] In the embodiment of the present invention, further, in step S6, the ferric phosphate dihydrate which has been flash dried to be free of free water is subjected to a temperature of 580-600 degrees to remove crystal water.

[0032] At the same time, a flash drying method for iron phosphate is provided, and the specific process steps are as follows:

[0033] (1) Grinding the ferrous phosphate slurry, sending the ground slurry to a storage tank after sand milling, cooling it through a cold water coil and then setting it aside for use.

[0034] (2) The ferrous phosphate slurry and phosphoric acid are pumped into a weighing and metering tank respectively, and a certain amount of ferrous phosphate slurry is added into the reactor through the weighing and metering tank, and a certain amount of water, phosphoric acid and hydrogen peroxide are added respectively. After sufficient reaction, the slurry is heated and matured through steam in the outer half pipe, discharged into the cooling tank for cooling, and then pumped into the water washing feed tank.

[0035] (3) Before batching, take the slurry from the high-level tank under stirring to analyze the Fe content.

[0036] (4) The cooled iron phosphate slurry is separated into solid and liquid by a filter press to remove the phosphate in the slurry. After five washings until the conductivity is qualified, the filter cake is slurried and pumped to the kiln tail storage tank; the filtrate is pumped to the CN filter for sedimentation separation, the upper clear liquid overflows into the clear liquid tank, the thick slurry enters the thick slurry tank, and finally pumped to the water washing feed tank.

[0037] (5) removing part of the free water in the iron phosphate solution by means of a diaphragm pressing plate frame, thereby increasing the solid content of the iron phosphate; and drying the iron phosphate filter cake on the filter plate frame by means of a flash evaporation main machine to remove the water.

[0038] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing ferric orthophosphate using ferrous phosphate, characterized in that: The process includes the following: Step S1: grinding the ferrous phosphate slurry, sending the ground slurry to a storage tank after sand grinding, and cooling it through a cold water coil for standby use; Step S2: pumping the ferrous phosphate slurry and phosphoric acid into a weighing and metering tank respectively, adding a certain amount of ferrous phosphate slurry into the reactor through the weighing and metering tank, adding a certain amount of water, phosphoric acid and hydrogen peroxide respectively, and after sufficient reaction, heating and aging through the outer half-tube steam, discharging the material into the cooling tank for cooling, and then pumping it to the water washing feed tank; Step S3: The cooled iron phosphate slurry is separated into solid and liquid by a filter press to remove phosphate in the slurry. After five washings until the conductivity is qualified, the filter cake is slurried and pumped to the kiln tail storage tank; the filtrate is pumped to the CN filter for sedimentation separation, the upper clear liquid overflows into the clear liquid tank, the thick slurry enters the thick slurry tank, and then pumped to the water washing feed tank; Step S4: removing part of the free water in the iron phosphate solution through a diaphragm pressing plate frame to increase the solid content of the iron phosphate; controlling the flash drying feed amount; Step S5: The iron phosphate filter cake of the filter plate frame is dried by the flash evaporator to remove moisture. After the flash drying and the feeding of the silo are completed, according to the discharge time of the rotary kiln, after the thick material layer reaches the last temperature zone, the speed of the rotary kiln is increased to above 13Hz, and the frequency conversion of the induced draft fan is turned to the maximum, and the thin material layer is quickly transported out by negative pressure air delivery; Step S6: removing crystal water from the dihydrate ferric phosphate which has been flash-dried to have no free water at 580-600 degrees, testing the electrochemical properties of the anhydrous ferric phosphate after cooling, and preparing the ingredients for ferric orthophosphate synthesis.

2. The method for preparing ferric orthophosphate by using ferrous phosphate according to claim 1, characterized in that: In steps S1 and S2, the ferrous phosphate is sand-ground to a particle size of less than 4 microns, and the amount of phosphoric acid and hydrogen peroxide added is calculated according to the iron content and phosphoric acid content in the slurry, and pumped into the ferrous phosphate synthesis kettle.

3. The method for preparing ferric orthophosphate by using ferrous phosphate according to claim 1, characterized in that: In step S3, the iron phosphate is separated by a filter press and then washed five times until the conductivity is qualified.

4. The method for preparing ferric orthophosphate by using ferrous phosphate according to claim 1, characterized in that: In steps S4 and S5, the iron phosphate is passed through a diaphragm pressing plate frame to remove part of the moisture to increase the solid content, and then dried by a flash evaporation main machine to remove the moisture.

5. The method for preparing ferric orthophosphate by using ferrous phosphate according to claim 2, characterized in that: In step S6, the ferric phosphate dihydrate which has been flash dried to have no free water is subjected to a temperature of 580-600 degrees to remove crystal water.

Citation Information

Patent Citations

  • Method for synthesizing ferric phosphate material

    CN102153061A

  • Method for synthesizing ferric phosphate material

    CN102153061B

  • Method for producing battery-grade ferric orthophosphate from titanium dioxide solid waste

    CN108584902A