Method for preparing iron-based composite phosphate polyanion positive electrode material based on iron phosphate solution method
By combining the iron phosphate solution method and spray drying method, the problems of low solubility of iron phosphate and high product heterogeneous phases were solved, and high-efficiency and low-cost iron-based composite phosphate polyanionic cathode material was prepared, improving rate performance and production Efficiency, suitable for industrial production.
Patent Information
- Application Number
- CN202411335317.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-15
AI Technical Summary
The existing preparation method of iron-based composite phosphate polyanionic cathode material has the problems of low solubility of iron phosphate in water, many products with poor product performance, resulting in high production costs and low efficiency, making it difficult to meet industrial needs.
The iron-based composite phosphate polyanionic positive electrode material is prepared by mixing the phosphorus source, sodium source, transition metal M source, carbon source and reducing agent in water, stirring evenly, and calcining it. The reducing agent is used to improve the dissolution of iron phosphate. The ball matte grinding process is omitted, and the spherical powder is prepared by spray drying to control particle size and morphology.
It improves the crystallinity and phase purity of the product, improves the electrochemical performance, especially the rate performance, simplifies the process flow, reduces costs, and is suitable for industrial production.
Smart Images

Figure CN118954466A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrode material preparation, and in particular relates to a method for preparing an iron-based composite phosphate polyanion positive electrode material based on an iron phosphate solution method. Background Art
[0002] At present, the trend of replacing traditional fossil fuels with sustainable and clean energy such as wind and solar energy is in full swing. Therefore, how to store highly intermittent and non-dispatchable energy has become an important issue that needs to be solved urgently. Among various energy storage technologies, lithium-ion batteries (LIBs) can provide both outstanding energy and high reliability. Lithium-ion batteries have the characteristics of high density and high output power, and are considered to be an indispensable energy source for portable electronic devices and electric vehicles. However, limited lithium reserves and increased mining difficulty cannot meet the greater demand for lithium-ion batteries in large-scale energy storage systems (EES). In recent years, sodium-ion batteries (SIBs) have become ideal candidates for EES due to their abundant sodium resources and low cost.
[0003] In the past few years, polyanion-type sodium battery cathode materials based on iron-based composite phosphate polyanion cathodes have been widely developed. Among them, sodium iron pyrophosphate (Na4Fe3(PO4)2(P2O7), referred to as NFPP) has a high voltage platform of 3.2V, a low volume change (less than 4%) when used as a sodium ion battery cathode, and a theoretical capacity of 129mAhg -1 The advantages of this material are low price, environmental friendliness, and easy synthesis. The disadvantages are extremely low electronic and ionic conductivity, which limits its capacity and power density and requires nano-sizing and carbon coating modification.
[0004] A more researched idea is to compound the iron-based composite phosphate polyanion positive electrode with carbon, such as compounding with carbon nanotubes, reduced graphene oxide, and using template block surfactant F127 to obtain nano-sized iron-based composite phosphate polyanion positive electrode / carbon particles, etc. However, these methods are cumbersome, costly, difficult to scale up, and cannot meet the needs of actual applications.
[0005] At present, the iron source for the domestic production of iron-based composite phosphate polyanion positive electrodes is mainly ferric nitrate. The obtained iron-based composite phosphate polyanion positive electrode has good phase formation and no impurities, but there are problems such as nitrogen emission and low yield, which cannot be mass-produced in industry. The synthesis route with iron phosphate as raw material is low in cost and green and easy to scale up, but due to the low solubility of iron phosphate in water, sodium iron phosphate impurities are often generated in the process of synthesizing pure phase iron-based composite phosphate polyanion positive electrode, resulting in poor rate performance and capacity attenuation. In order to ensure the final phase formation and morphology of the iron-based composite phosphate polyanion positive electrode, it is usually necessary to obtain a pure phase through a long reaction or other harsh conditions, and then optimize the particle size through a variety of processes such as ball milling, sand milling, and spraying, which greatly increases the production cost and reduces the production efficiency. Therefore, it is necessary to develop a new simple, convenient, green and safe method for preparing an iron-based composite phosphate polyanion positive electrode suitable for industrial production using iron phosphate as raw material to solve the above problems. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing an iron-based composite phosphate polyanion positive electrode material based on an iron phosphate solution method, so as to solve the problems of low solubility of iron phosphate in water, multiple impurities in the product and poor rate performance.
[0007] To achieve the above object, the present invention provides a method for preparing an iron-based composite phosphate polyanion positive electrode material, comprising: x The stoichiometric ratio of P element, sodium element and M element in (PO4)2P2O7 is to prepare a phosphorus source, a sodium source and a transition metal M source, mix the sodium source, the phosphorus source, the transition metal M source, the carbon source and the reducing agent in water, stir them uniformly, then collect a powder sample, calcine the powder sample, and obtain an iron-based composite phosphate polyanion positive electrode material;
[0008] Wherein, the transition metal M source contains at least iron phosphate, and x satisfies the condition that Na4M x The positive and negative valence of (PO4)2P2O7 is balanced; the total amount of the carbon source and the reducing agent added is 55% to 220% of the molar amount of the transition metal M source, and the content of the carbon source is at least 50% of the molar amount of the transition metal M source.
[0009] Further, the reducing agent includes at least one of an inorganic reducing agent and an organic reducing agent; the inorganic reducing agent includes at least one of ammonium hydrochloride, aluminum powder, and lithium aluminum hydride; the organic reducing agent includes at least one of ethanol, citric acid, triethyl citrate, gluconic acid, ascorbic acid, and tartaric acid;
[0010] The reducing agent is preferably an organic reducing agent, and more preferably comprises at least one or two of ascorbic acid and triethyl citrate.
[0011] Furthermore, the carbon source is one or more of graphene, carbon nanotubes, graphite, carbon powder, citric acid, glucose, sucrose, acetic acid, tartaric acid, ascorbic acid, and benzoic acid; preferably, it contains at least one or more of citric acid, tartaric acid, and ascorbic acid.
[0012] Furthermore, the amount of the carbon source added is 50% to 150% of the molar amount of the transition metal M source; for example, 55%, 60%, 70%, 80%, 90%, 100%, 120%, 130%, 140%, etc.; the amount of the reducing agent added is 5% to 70% of the molar amount of the transition metal M source, for example, 8%, 10%, 12%, 15%, 20%, 25%, 30%, 40%, 50%, 60%, etc.
[0013] In some embodiments, the carbon source is citric acid and / or tartaric acid, and the reducing agent is ascorbic acid or triethyl citrate.
[0014] Further, the transition metal M source also includes one or more of vanadium salts, titanium salts, manganese salts, cobalt salts, nickel salts, copper salts, and zinc salts; wherein the salt is sulfate and its hydrate, chloride and its hydrate, acetate and its hydrate, or oxalate and its hydrate;
[0015] The amount of the transition metal M source other than iron phosphate is 5% to 30% of the molar amount of the iron phosphate.
[0016] Furthermore, the sodium source includes at least one of an inorganic sodium salt, an organic sodium salt, a sodium oxide, and sodium hydroxide; the inorganic sodium salt includes at least one of trisodium phosphate, sodium pyrophosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium bicarbonate, and sodium carbonate; the organic sodium salt includes at least one of sodium acetate, sodium tartrate, sodium oxalate, sodium formate, sodium benzoate, and sodium citrate; the sodium oxide includes at least one of sodium peroxide and sodium oxide.
[0017] Furthermore, the phosphorus source includes at least one of phosphoric acid, phosphates and pyrophosphates; the phosphates include at least one of trisodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; the pyrophosphates include at least one of sodium pyrophosphate, sodium acid pyrophosphate and ammonium pyrophosphate.
[0018] Furthermore, the calcination includes: first heating the temperature from room temperature to 250-350°C at a heating rate of 2-5°C / min, and keeping the temperature for 1-6 hours; then heating the temperature to 450-700°C at a heating rate of 2-5°C / min, and keeping the temperature for 6-20 hours.
[0019] Furthermore, the feed rate of the spray drying is 2-10 mL / min, the air inlet temperature is 100-150° C., and the air outlet temperature is 50-70° C.
[0020] Furthermore, the sintering gas atmosphere is one of argon, nitrogen, argon-hydrogen mixed gas, and nitrogen-hydrogen mixed gas.
[0021] The present invention also provides an iron-based composite phosphate polyanion positive electrode material, which is prepared by any of the preparation methods described above.
[0022] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0023] 1. The preparation method of the iron-based composite phosphate polyanion positive electrode material provided by the present invention uses low-cost and safe iron phosphate as the iron source, and under the action of a reducing agent, the iron phosphate becomes a soluble system in an aqueous solution, so that the reaction reaches atomic-level mixing, omitting processes such as ball milling and sand milling, and preparing the positive electrode material of the iron-based composite phosphate polyanion positive electrode by spray drying in a very short time, which solves the problem of uneven multi-phase mixing of raw materials during mixing. The prepared carbon-coated iron-based composite phosphate polyanion positive electrode material has significantly improved crystallinity and phase purity, and the electrochemical performance is also improved to a certain extent, especially the rate performance.
[0024] 2. The iron-based composite phosphate polyanion positive electrode spherical powder synthesized by the solution method of the present invention has a regular morphology and a controllable product particle size. The introduction of the reducing agent greatly accelerates the reaction process, forms a pure phase in a shorter time, greatly improves production efficiency, and reduces costs.
[0025] 3. The iron-based composite phosphate polyanion positive electrode prepared by the present invention can easily introduce other transition metal elements to increase the voltage platform.
[0026] 4. The raw materials used in the present invention include iron phosphate, other transition metal salts, sodium source, phosphorus source, carbon source, reducing agent, etc., which are cheap, easily available and widely distributed. The preparation process is green, simple and easy to scale up, and can provide an optional route for the pilot production of iron-based composite phosphate polyanion positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a SEM image of the iron-based composite phosphate polyanion positive electrode material obtained in Example 1 of the present invention;
[0028] Figure 2 Another SEM image of the iron-based composite phosphate polyanion cathode material obtained in Example 1 of the present invention;
[0029] Figure 3 This is a SEM image of the iron-based composite phosphate polyanion positive electrode material obtained in Example 5 of the present invention;
[0030] Figure 4The left picture in the middle is a physical picture of the solution in Example 1 after stirring for 4 hours, and the right picture is a physical picture of the solution in Example 5 after stirring for 32 hours;
[0031] Figure 5 This is the XRD pattern of the iron-based composite phosphate polyanion positive electrode material obtained in Example 1 of the present invention;
[0032] Figure 6 This is a comparison diagram of the first cycle charge and discharge of Example 1 and Example 5 of the present invention;
[0033] Figure 7 A comparison chart of the discharge capacity ratios of Example 1 and Example 5 of the present invention;
[0034] Figure 8 A comparison chart of the discharge capacity ratio of Example 1 and Example 6;
[0035] Fig. 9 This is a discharge capacity rate performance diagram of Example 2 of the present invention;
[0036] Fig.10 This is a first cycle charge and discharge curve diagram of Example 3 of the present invention;
[0037] Fig.11 This is the first cycle charge and discharge curve diagram of Example 4 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0039] The present invention provides a method for preparing an iron-based composite phosphate polyanion positive electrode material, comprising: mixing a transition metal salt, a sodium source, a phosphorus source, a carbon source and a reducing agent in water, stirring at room temperature for 4 to 24 hours to form a uniform solution, then spray drying to obtain a powder sample, and calcining the powder sample in a specific gas atmosphere to obtain the iron-based composite phosphate polyanion positive electrode material; wherein the transition metal salt contains at least iron phosphate, and the total addition amount of the carbon source and the reducing agent is 55% to 220% of the molar amount of the transition metal salt.
[0040] When the selected carbon source has reducing properties or the selected reducing agent is an organic reducing agent, the amount ratio of the carbon source to the reducing agent is not particularly limited, preferably the amount of the carbon source added is 50% to 150% of the molar amount of the transition metal salt, and the amount of the reducing agent added is 5% to 70% of the molar amount of the transition metal salt. The carbon source is preferably a compound that can be complexed with the transition metal, such as a carboxyl compound, which can synergistically promote the dissolution of iron phosphate under the action of the reducing agent.
[0041] When the selected carbon source is not reducing, the amount of the reducing agent added is 5% to 70% of the molar amount of the transition metal salt, preferably 20 to 60%.
[0042] The content of transition metal salt in the obtained homogeneous solution is 10-50 g / L, preferably 20-40 g / L. The total content (solid content) of raw materials in the homogeneous solution is 80-200 g / L, preferably 100-180 g / L, more preferably 120-160 g / L.
[0043] The transition metal salt, sodium source and phosphorus source satisfy the stoichiometric ratio of Na4Fe3(PO4)2(P2O7). When the chemical formula contains transition metals other than iron, iron is converted into other transition metals according to the valence. For example, Na4Fe2Co(PO4)2(P2O7), Na4Fe2Mn(PO4)2(P2O7), etc.
[0044] Example 1
[0045] A sodium ion positive electrode active material, specifically an iron-based composite phosphate polyanion positive electrode, whose chemical formula is Na4Fe3(PO4)2(P2O7), and the preparation method of the positive electrode active material is:
[0046] The raw materials are ferric phosphate, sodium pyrophosphate, sodium bicarbonate, citric acid and ascorbic acid; among them, sodium pyrophosphate is both a sodium source and a phosphorus source, ferric phosphate is an iron source and a phosphorus source, sodium bicarbonate is a supplementary sodium source, citric acid is a carbon source, and ascorbic acid is a supplementary carbon source and a reducing agent.
[0047] 10.9718 g of ferric phosphate, 3.6229 g of sodium pyrophosphate, 3.8223 g of sodium bicarbonate, 21.0138 g of citric acid, 2.202 g of ascorbic acid and 300 mL of water were uniformly mixed and stirred at room temperature for 4 h to form a clear transparent solution. Figure 4 The above solution was spray dried at an inlet air temperature of 120°C and an outlet air temperature of 60°C, and the obtained light green powder was calcined at 300°C for 3h in an argon atmosphere, and then calcined at 500°C for 10h to obtain a black iron-based composite phosphate polyanion positive electrode sample. The XRD pattern is shown in Figure 5 shown.
[0048] The positive electrode material prepared in this embodiment was mixed with SuperP and polyvinylidene fluoride (PVDF) in a mass ratio of 7:2:1 and added with an appropriate amount of NMP to form a homogenous mixture. The black slurry was coated on aluminum foil using a 150μm four-sided preparation device, and the positive electrode material pole piece was made after drying, punching and pressing. Metal sodium was used as the negative electrode pole piece, glass fiber was used as the separator, and the electrolyte was 1M NaClO4 inEC+PC+FEC (EC:PC:FEC=10:10:1 volume ratio), and the button battery was assembled in a glove box with water and oxygen below 0.01ppm.
[0049] Example 2
[0050] A sodium ion positive electrode active material, specifically an iron-based composite phosphate polyanion positive electrode, whose chemical formula is Na4Fe3(PO4)2(P2O7), and the preparation method of the positive electrode active material is:
[0051] The raw materials are ferric phosphate, trisodium phosphate, sodium carbonate, tartaric acid and triethyl citrate; among them, trisodium phosphate is both a sodium source and a phosphorus source, ferric phosphate is an iron source and a phosphorus source, sodium carbonate is a supplementary sodium source, tartaric acid is a carbon source, and triethyl citrate is a carbon source and a reducing agent.
[0052] 10.9718g of iron phosphate, 3.3238g of trisodium phosphate, 2.4112g of sodium carbonate, 18.5453g of tartaric acid, and 300mL of water were uniformly mixed and stirred at room temperature for 12h to form a clear transparent solution. The solution was spray dried at an inlet air temperature of 120°C and an outlet air temperature of 60°C. The obtained light green powder was calcined at 300°C for 3h in an argon atmosphere and continued to be calcined at 500°C for 10h to obtain a black iron-based composite phosphate polyanion positive electrode sample. The button cell was assembled in a glove box with water and oxygen below 0.01ppm, and the specific assembly parameters were the same as those in Example 1.
[0053] Example 3
[0054] A positive electrode active material, specifically an iron-based composite phosphate polyanion positive electrode, whose chemical formula is Na4Fe2Mn(PO4)2(P2O7), and a preparation method of the positive electrode active material is:
[0055] The raw materials are ferric phosphate, manganese acetate dihydrate, sodium pyrophosphate, citric acid and ascorbic acid; among them, sodium pyrophosphate is both a sodium source and a phosphorus source, ferric phosphate is an iron source and a phosphorus source, citric acid is a carbon source, and ascorbic acid is a carbon source and a reducing agent.
[0056] 7.3145g of iron phosphate, 3.3512g of manganese acetate dihydrate, 6.6475g of sodium pyrophosphate, 23.5475g of citric acid, 4.404g of ascorbic acid and 300mL of water were uniformly mixed and stirred at room temperature for 24h to form a clear transparent solution. The above solution was spray dried at an inlet air temperature of 120°C and an outlet air temperature of 60°C. The obtained powder was calcined at 300°C for 3h in an argon atmosphere and continued to be calcined at 550°C for 10h to obtain a black iron-based composite phosphate polyanion positive electrode sample. The button cell was assembled in a glove box with water and oxygen below 0.01ppm, and the specific assembly parameters were the same as those in Example 1.
[0057] Example 4
[0058] A positive electrode active material, specifically an iron-based composite phosphate polyanion positive electrode, whose chemical formula is Na4Fe2Co(PO4)2(P2O7), and a preparation method of the positive electrode active material is:
[0059] The raw materials are ferric phosphate, cobalt acetate tetrahydrate, sodium pyrophosphate, citric acid and ascorbic acid; among them, sodium pyrophosphate is both a sodium source and a phosphorus source, ferric phosphate is an iron source and a phosphorus source, citric acid is a carbon source, and ascorbic acid is a carbon source and a reducing agent.
[0060] 7.3145g of iron phosphate, 3.1125g of cobalt acetate tetrahydrate, 6.6475g of sodium pyrophosphate, 23.5475g of citric acid, 4.404g of ascorbic acid and 300mL of water were uniformly mixed and stirred at room temperature for 24h to form a clear transparent solution. The above solution was spray dried at an inlet air temperature of 120°C and an outlet air temperature of 60°C. The obtained powder was calcined at 300°C for 3h in an argon atmosphere and continued to be calcined at 650°C for 10h to obtain a black iron-based composite phosphate polyanion positive electrode sample. The button cell was assembled in a glove box with water and oxygen below 0.01ppm, and the specific assembly parameters were the same as those in Example 1.
[0061] Example 5
[0062] A sodium ion positive electrode active material, specifically an iron-based composite phosphate polyanion positive electrode, whose chemical formula is Na4Fe3(PO4)2(P2O7), and the preparation method of the positive electrode active material is:
[0063] The raw materials are ferric phosphate, sodium pyrophosphate, sodium bicarbonate and citric acid; among them, sodium pyrophosphate is both a sodium source and a phosphorus source, ferric phosphate is an iron source and a phosphorus source, sodium bicarbonate is a supplementary sodium source, and citric acid is a carbon source and a reducing agent.
[0064] 10.9718 g of ferric phosphate, 3.6229 g of sodium pyrophosphate, 3.8223 g of sodium bicarbonate, 23.6405 g of citric acid and 300 mL of water were uniformly mixed and stirred at room temperature for 32 h. Figure 4 As shown in the middle right figure. The mixed solution was sand-milled for 2 hours to obtain a mixed solution with smaller particles, spray-dried at an inlet air temperature of 120°C and an outlet air temperature of 60°C, and the obtained green powder was calcined at 300°C for 3 hours in an argon atmosphere, and continued to be calcined at 500°C for 10 hours to obtain a black iron-based composite phosphate polyanion positive electrode sample. The button battery was assembled in a glove box with water and oxygen below 0.01ppm, and the specific assembly parameters were the same as those in Example 1.
[0065] Example 6
[0066] A sodium ion positive electrode active material, specifically an iron-based composite phosphate polyanion positive electrode, whose chemical formula is Na4Fe3(PO4)2(P2O7), and the preparation method of the positive electrode active material is:
[0067] The raw materials are ferric phosphate, sodium pyrophosphate, sodium bicarbonate and citric acid; among them, sodium pyrophosphate is both a sodium source and a phosphorus source, ferric phosphate is an iron source and a phosphorus source, sodium bicarbonate is a supplementary sodium source, and citric acid is a carbon source.
[0068] 10.9718g of iron phosphate, 3.6229g of sodium pyrophosphate, 3.8223g of sodium bicarbonate, 21.0138g of carbon source and 300mL of water were uniformly mixed, stirred at room temperature for 24h, the mixed solution was sand-milled for 2h to obtain a mixed solution with smaller particles, spray-dried at an inlet air temperature of 120°C and an outlet air temperature of 60°C, and the obtained green powder was calcined at 300°C for 3h in an argon atmosphere, and continued to be calcined at 500°C for 10h to obtain a black iron-based composite phosphate polyanion positive electrode sample. The button cell was assembled in a glove box with water and oxygen below 0.01ppm, and the specific assembly parameters were the same as those in Example 1.
[0069] like Figure 1-3 As shown, it can be seen that the iron-based composite phosphate polyanion positive electrode material prepared in Example 1 is a regular spherical particle with good dispersibility, while the material prepared in Example 5 is obviously lumped together. Figure 4 It can be seen that when citric acid is used as both a carbon source and a reducing agent, the solubility of ferric phosphate is not as good as that when ascorbic acid is used. The color difference of the mixture formed in the aqueous solution indicates that the type of reducing agent plays an important role in the dissolution and reaction of the mixture.
[0070] from Figure 7It can be seen that when ascorbic acid is replaced by citric acid, the rate performance of the obtained iron-based composite phosphate polyanion positive electrode sample is reduced, the battery specific capacity at low rate is not much different, and its specific capacity at high rate is significantly reduced compared with Example 1. Example 6 removes ascorbic acid compared with Example 1. Figure 8 It can be seen that its rate performance is further reduced, and the specific capacity at high rate is lower than that of Examples 1 and 5. It can be seen that in the preparation system of the present invention, the type of reducing agent also has an important influence on the product performance. When the reducing agent is preferably used as the reducing agent, the rate performance is better.
[0071] from Figure 9-11 It can be seen that other iron-based composite phosphate polyanion positive electrode materials prepared in the present invention also have good electrical properties.
[0072] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an iron-based composite phosphate polyanion positive electrode material, It is characterized in that include: Press Na 4 M x (PO 4 ) 2 P 2 O 7 A phosphorus source, a sodium source and a transition metal M source are prepared according to the stoichiometric ratio of the P element, the sodium element and the M element, the sodium source, the phosphorus source, the transition metal M source, the carbon source and the reducing agent are mixed and stirred evenly in water, and then a powder sample is collected, and the powder sample is calcined to obtain an iron-based composite phosphate polyanion positive electrode material; Wherein, the transition metal M source comprises at least iron phosphate, and x satisfies Na 4 M x (PO 4 ) 2 P 2 O 7 The total amount of the carbon source and the reducing agent added is 55% to 220% of the molar amount of the transition metal M source, and the content of the carbon source is at least 50% of the molar amount of the transition metal M source.
2. The method for preparing the iron-based composite phosphate polyanion positive electrode material according to claim 1, It is characterized in that The reducing agent includes at least one of an inorganic reducing agent and an organic reducing agent; the inorganic reducing agent includes at least one of ammonium hydrochloride, aluminum powder, and lithium aluminum hydride; the organic reducing agent includes at least one of ethanol, citric acid, triethyl citrate, gluconic acid, ascorbic acid, and tartaric acid; The reducing agent is preferably an organic reducing agent, and more preferably comprises at least one or two of ascorbic acid and triethyl citrate.
3. The method for preparing the iron-based composite phosphate polyanion positive electrode material according to claim 2, It is characterized in that The carbon source is one or more of graphene, carbon nanotubes, graphite, carbon powder, citric acid, glucose, sucrose, acetic acid, tartaric acid, ascorbic acid, and benzoic acid; preferably, it contains at least one or more of citric acid, tartaric acid, and ascorbic acid.
4. A method for preparing an iron-based composite phosphate polyanion cathode material according to any one of claims 1 to 3, It is characterized in that The added amount of the carbon source is 50% to 150% of the molar amount of the transition metal M source; the added amount of the reducing agent is 5% to 70% of the molar amount of the transition metal M source.
5. The method for preparing the iron-based composite phosphate polyanion positive electrode material according to claim 1, It is characterized in that The transition metal M source also includes one or more of vanadium salts, titanium salts, manganese salts, cobalt salts, nickel salts, copper salts, and zinc salts; wherein the salt is sulfate and its hydrate, chloride and its hydrate, acetate and its hydrate, or oxalate and its hydrate; The amount of the transition metal M source other than iron phosphate is 5% to 30% of the molar amount of the iron phosphate.
6. The method for preparing the iron-based composite phosphate polyanion positive electrode material according to claim 1, It is characterized in that The sodium source includes at least one of an inorganic sodium salt, an organic sodium salt, a sodium oxide, and sodium hydroxide; the inorganic sodium salt includes at least one of trisodium phosphate, sodium pyrophosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium bicarbonate, and sodium carbonate; the organic sodium salt includes at least one of sodium acetate, sodium tartrate, sodium oxalate, sodium formate, sodium benzoate, and sodium citrate; the sodium oxide includes at least one of sodium peroxide and sodium oxide; And / or, the phosphorus source includes at least one of phosphoric acid, phosphates and pyrophosphates, the phosphates include at least one of trisodium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; the pyrophosphates include at least one of sodium pyrophosphate, sodium acid pyrophosphate and ammonium pyrophosphate.
7. The method for preparing the iron-based composite phosphate polyanion positive electrode material according to claim 1, It is characterized in that The calcination comprises: firstly heating the temperature from room temperature to 250-350°C at a heating rate of 2-5°C / min and keeping the temperature for 1-6h; and then heating the temperature to 450-700°C at a heating rate of 2-5°C / min and keeping the temperature for 6-20h.
8. The method for preparing the iron-based composite phosphate polyanion positive electrode material according to claim 1, It is characterized in that The powder sample is obtained by spray drying, the feed rate of the spray drying is 2-10 mL / min, the air inlet temperature is 100-150° C., and the air outlet temperature is 50-70° C.
9. The method for preparing the iron-based composite phosphate polyanion positive electrode material according to claim 1, It is characterized in that The calcination gas atmosphere is one of argon, nitrogen, argon-hydrogen mixed gas, and nitrogen-hydrogen mixed gas.
10. An iron-based composite phosphate polyanion cathode material, It is characterized in that The invention is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing Na4Fe3 (PO4) 2 (P2O7) by homogeneous phase method and application
CN113060713A
Iron-based phosphate-based polyanion positive electrode material as well as preparation and application thereof
CN116553505A
Preparation method of composite sodium ferric phosphate
CN117208880A
Pure-phase iron-based mixed phosphate sodium ion battery positive electrode material as well as preparation and application thereof
CN117735505A
Method for synthesizing ferric sodium pyrophosphate positive electrode material by using ferric phosphate
CN118062820A