Rechargeable lithium battery
By using sheet-shaped polyethylene particles and inorganic particles in the negative electrode functional layer in rechargeable lithium batteries, combined with specific electrolyte solutions and positive electrode active materials, the problem of thermal runaway of lithium batteries during short circuit and overcharge and discharge is solved, and the battery performance is improved. stability and cycle life, achieving higher safety and capacity retention.
Patent Information
- Application Number
- CN202010360725.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-03
- Filing Date
- 2020-04-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-04-30
AI Technical Summary
Existing rechargeable lithium batteries are prone to thermal runaway and explosion due to internal short circuit, overcharge and over-discharge, which pose safety risks, and their stability and cycle life characteristics are insufficient.
The negative electrode functional layer contains flaky polyethylene particles and inorganic particles, and the electrolyte solution is combined with propionate and carbonate solvents to optimize the impregnation performance of the electrolyte solution, and materials such as LiCoO2 and LiFePO4 are used in the positive active material layer to form Closed cell function to improve battery stability and safety.
Significantly improves the physical and thermal safety of lithium batteries, extends the cycle life characteristics at room temperature and high temperature, enhances the battery's capacity retention rate, and effectively suppresses heat release during abnormal operations, achieving excellent physical stability and safety sex.
Smart Images

Figure CN111883818B_ABST
Abstract
Description
[0001] This application claims priority to and the benefit of Korean Patent Application No. 10-2019-0052568 filed on May 3, 2019, in the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The present disclosure relates to a rechargeable lithium battery. Background Art
[0003] Portable information devices such as cellular phones, notebook computers, smart phones, etc. or electric vehicles have used rechargeable lithium batteries that have high energy density and are easy to carry as driving power sources. In addition, research has recently been actively conducted on using rechargeable lithium batteries as power sources or power storage devices for hybrid vehicles or electric vehicles by utilizing high energy density characteristics.
[0004] One of the main research tasks of such rechargeable lithium batteries is to improve the safety of rechargeable batteries. For example, if a rechargeable lithium battery releases heat and an electrolyte decomposition reaction and thermal runaway occur due to internal short circuit, overcharge and over discharge, the internal pressure inside the battery may rise rapidly, causing the battery to explode. Among them, when an internal short circuit of a rechargeable lithium battery occurs, there is a high risk of explosion because the high electrical energy stored in each electrode is conducted in the short-circuited positive and negative electrodes.
[0005] In addition to the damage to the rechargeable lithium battery, the explosion may also cause fatal injuries to the user. Therefore, it is urgent to develop a technology that can improve the stability of rechargeable lithium batteries. Summary of the invention
[0006] Embodiments provide a rechargeable lithium battery having improved stability and improved electrolyte impregnation.
[0007] An embodiment provides a rechargeable lithium battery, comprising: a negative electrode, comprising a negative electrode active material layer and a negative electrode functional layer disposed on the negative electrode active material layer; a positive electrode, comprising a positive electrode active material layer; and an electrolyte solution, wherein the negative electrode functional layer comprises flaky polyethylene particles, the electrolyte solution comprises a lithium salt and a non-aqueous organic solvent, and the non-aqueous organic solvent comprises about 60 volume % to about 80 volume % of a propionate solvent and about 20 volume % to about 40 volume % of a carbonate solvent.
[0008] The propionate-based solvent may include at least one selected from methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0009] The carbonate-based solvent may include at least one selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, and methyl butyl carbonate.
[0010] The electrolyte solution may further include an additive, and the additive may be included in an amount of about 3 wt % to about 20 wt % based on the total amount of the electrolyte solution.
[0011] The flaky polyethylene particles may have a particle size of about 1 μm to about 8 μm.
[0012] The ratio of the major axis length to the minor axis length of the flaky polyethylene particles may be about 1 to about 5.
[0013] The flake-shaped polyethylene particles may have a thickness of about 0.2 μm to about 4 μm.
[0014] The negative electrode functional layer may also optionally include inorganic particles and a binder.
[0015] The total amount of the flaky polyethylene particles and the inorganic particles:the amount of the binder may be in a weight ratio of about 80:20 to about 99:1.
[0016] The flaky polyethylene particles and the inorganic particles may be included in a weight ratio of 95:5 to 10:90.
[0017] The negative electrode functional layer may have a thickness of about 1 μm to about 10 μm.
[0018] A ratio between a thickness of the negative electrode active material layer and a thickness of the negative electrode functional layer may be about 50:1 to about 10:1.
[0019] The positive electrode active material layer may include a first positive electrode active material including at least one composite oxide of a metal selected from cobalt, manganese, nickel, and combinations thereof and lithium, and a second positive electrode active material including a compound represented by Chemical Formula 1.
[0020] [Chemical formula 1]
[0021] Li a Fe 1-x M x PO4
[0022] In Chemical Formula 1, 0.90≤a≤1.8, 0≤x≤0.7, and M is Mn, Co, Ni, or a combination thereof.
[0023] The first positive electrode active material may include LiCoO2, Li b M 1 1-y1-z1 M 2 y1 M3 z1 O2(0.9≤b≤1.8, 0≤y1≤1, 0≤z1≤1, 0≤y1+z1≤11, M 1 、M 2 and M 3 is independently one of a metal selected from Ni, Co, Mn, Al, Sr, Mg or La and a combination thereof.
[0024] The second positive active material may include LiFePO 4 .
[0025] The positive electrode active material layer may further include a positive electrode functional layer disposed on the positive electrode active material layer.
[0026] The first positive electrode active material may be included in the positive electrode active material layer, and the second positive electrode active material may be included in at least one of the positive electrode active material layer and the positive electrode functional layer.
[0027] The first positive active material and the second positive active material may be included in a weight ratio of about 97:3 to about 80:20.
[0028] The first positive active material may be included in an amount of about 70 wt % to about 99 wt % based on the total amount of the positive active material layer, and the second positive active material may be included in an amount of about 1 wt % to about 30 wt % based on the total amount of the positive active material layer.
[0029] When the reaction rate increases with temperature, an incipient pore closing function can be achieved, thereby ensuring the stability of the rechargeable lithium battery.
[0030] By improving the impregnation properties of the electrolyte solution, it is possible to provide a rechargeable lithium battery having improved room temperature and high temperature cycle-life characteristics and high temperature storage characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The structure of a rechargeable lithium battery according to an embodiment is schematically shown.
[0032] Figure 2 is a scanning electron microscope (SEM) image of polyethylene spherical particles in a dispersed state.
[0033] Figure 3 is a SEM photograph of the flaky polyethylene particles according to Example 1-1.
[0034] Figure 4 is a graph analyzing the particle size distribution of the flake-shaped polyethylene particles included in the negative electrode functional layer compositions according to Example 1-1, Example 1-2, and Example 1-3. DETAILED DESCRIPTION
[0035] Hereinafter, embodiments of the present invention are described in detail with reference to the accompanying drawings. In the following description of the present disclosure, well-known functions or constructions will not be described in order to clarify the present disclosure.
[0036] In order to clearly illustrate the present disclosure, descriptions and relationships are omitted, and the same or similar configuration elements are denoted by the same reference numerals throughout the disclosure.
[0037] In addition, since the size and thickness of each configuration shown in the drawings are arbitrarily illustrated for better understanding and ease of description, the present disclosure is not limited thereto.
[0038] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, the element can be directly on the other element or intervening elements may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0039] A rechargeable lithium battery according to an embodiment includes: a negative electrode including a negative electrode active material layer and a negative electrode functional layer disposed on the negative electrode active material layer; a positive electrode including a positive electrode active material; an electrolyte solution, the negative electrode functional layer including flaky polyethylene particles, the electrolyte solution including a lithium salt and a non-aqueous organic solvent, and the non-aqueous organic solvent includes about 60 volume % to about 80 volume % of a propionate solvent and about 20 volume % to about 40 volume % of a carbonate solvent.
[0040] Hereinafter, a rechargeable lithium battery according to embodiments is described with reference to the accompanying drawings. Figure 1 The structure of a rechargeable lithium battery according to an embodiment is schematically shown. Figure 1 , a cylindrical rechargeable lithium battery is shown as an example of the rechargeable lithium battery, but the rechargeable lithium battery according to the present invention is not limited thereto but may have a square, coin, button, or pouch shape.
[0041] Reference Figure 1 According to an embodiment, a rechargeable lithium battery 100 includes a battery cell, a battery case 120 configured to accommodate the battery cell, and a sealing member 140 that seals the battery case 120. The battery cell includes a negative electrode 112, a positive electrode 114 facing the negative electrode 112, a separator 113 disposed between the negative electrode 112 and the positive electrode 114, and an electrolyte for a rechargeable lithium battery (not shown) impregnating the negative electrode 112, the positive electrode 114, and the separator 113.
[0042] The negative electrode 112 includes a negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector, and a negative electrode functional layer disposed on the negative electrode active material layer.
[0043] The negative electrode current collector may include one selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0044] The negative electrode active material layer may be disposed on the negative electrode current collector and may include a negative electrode active material, and optionally a negative electrode conductive material and a negative electrode binder.
[0045] The negative electrode active material may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / de-doping lithium, or a transition metal oxide.
[0046] Examples of materials that can reversibly intercalate / deintercalate lithium ions may include carbonaceous materials, i.e., carbon-based negative electrode active materials commonly used in rechargeable lithium batteries. Examples of carbon-based negative electrode active materials may be crystalline carbon, amorphous carbon, or combinations thereof. Crystalline carbon may be graphite (such as natural graphite or artificial graphite that is amorphous, plate-like, flaky, spherical, or fibrous), and amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbonization products, calcined coke, etc.
[0047] The lithium metal alloy includes an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.
[0048] The material capable of doping / de-doping lithium may be a silicon-based material or a tin-based material, for example, Si, SiO x (0 < x < 2), Si-Q alloy (where Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, but not Si), Si-carbon composite, Sn, SnO2, Sn-R alloy (where R is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, but not Sn), Sn-carbon composite, etc. At least one of these materials may be mixed with SiO2. The element Q and the element R may be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0049] The transition metal oxide may include lithium titanium oxide.
[0050] In the negative electrode active material layer, an amount of the negative electrode active material is about 95 wt % to about 99 wt % based on the total amount of the negative electrode active material layer.
[0051] The negative electrode active material layer may further optionally include a negative electrode conductive material and a negative electrode binder.
[0052] The negative electrode conductive material is used to impart conductivity to the negative electrode, and as long as the conductive material is an electronic conductive material that does not cause chemical changes in the battery, the material can be used. Examples of conductive materials may include carbon-based materials (such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials including metal powders or metal fibers of copper, nickel, aluminum, silver, etc., conductive polymers (such as polyphenylene derivatives), or mixtures thereof.
[0053] The negative electrode conductive material may be included in an amount of about 1 wt % to about 5 wt % based on the total weight of the negative electrode active material layer.
[0054] The negative electrode binder improves the binding properties between the negative electrode active material particles and the binding properties between the negative electrode active material particles and the current collector. The negative electrode binder can be a non-water-soluble binder, a water-soluble binder, an amphiphilic binder (water-soluble / non-water-soluble binder), or a combination thereof.
[0055] The non-water-soluble binder may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0056] The water-soluble binder can be styrene-butadiene rubber, a polymer containing ethylene oxide, polyvinyl pyrrolidone, acrylated styrene-butadiene rubber, polyvinyl alcohol, sodium polyacrylate, a copolymer of propylene and C2 to C8 olefins, a copolymer of (meth)acrylic acid and (meth)acrylic acid alkyl ester, or a combination thereof.
[0057] The amphiphilic adhesive may be an acrylated styrenic rubber.
[0058] When a water-soluble binder is used as a negative electrode binder, a cellulose compound may also be used as a thickener to provide viscosity. The cellulose compound includes one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or an alkali metal salt thereof. The alkali metal may be Na, K, or Li. The thickener may be included in an amount of about 0.1 to about 3 parts by weight based on 100 parts by weight of the negative electrode active material.
[0059] The amount of the negative electrode binder may be about 1 wt % to about 5 wt % based on the total weight of the negative electrode active material layer.
[0060] The negative electrode functional layer is provided on the negative electrode active material layer, and the negative electrode functional layer includes sheet-like polyethylene particles.
[0061] Reference Figure 2 and Figure 3 Describe the shape of the flake polyethylene pellets. Figure 2 This is a scanning electron microscope (SEM) photograph of polyethylene spherical particles in a dispersed state. Figure 3 This is a SEM photo of polyethylene flake particles. Figure 2 and Figure 3 , flake polyethylene particles will have a shape that is significantly different from spherical polyethylene particles.
[0062] Therefore, when the flake polyethylene particles of the example are used, a thin and wide functional layer can be formed compared with spherical particles, and there can be an advantage of rapidly melting the flake polyethylene particles to block ion passages in a wide area.
[0063] The flaky polyethylene particles may have a melting point (T ) of about 90° C. to about 160° C. (eg, about 110° C. to about 140° C.). m ), the melting point can be determined by differential scanning calorimetry (DSC) according to ISO 11357-3. In addition, for example, the flaky polyethylene particles may have a weight average molecular weight of about 300 g / mole (mol) to about 10,000 g / mol (specifically, about 2,000 g / mol to about 6,000 g / mol). When the polyethylene particles have a melting point and a weight average molecular weight within the range, a shut-down function (or closed cell function) may be achieved before an internal short circuit of a battery during thermal runaway caused by abnormal operation of the battery.
[0064] Generally, polyethylene can be divided into HDPE (high density polyethylene, density: about 0.94 g / cc to about 0.965 g / cc), MDPE (medium density polyethylene, density: about 0.925 g / cc to about 0.94 g / cc), LDPE (low density polyethylene, density: about 0.91 g / cc to about 0.925 g / cc), VLDPE (very low density polyethylene, density: about 0.85 g / cc to about 0.91 g / cc), etc. according to density. Flaky polyethylene particles can be prepared, for example, by using polyethylene polymers (such as HDPE, MDPE and LDPE) alone or as a mixture of two or more.
[0065] The particle size of the flaky polyethylene particles included in the negative electrode functional layer may be about 1 μm to about 8 μm, specifically, about 2 μm to about 6 μm. On the other hand, the ratio of the major axis length to the minor axis length of the flaky polyethylene particles (hereinafter referred to as the ratio of the major axis length to the minor axis length) may be about 1 to about 5, specifically, about 1.1 to about 4.5, for example, about 1.2 to about 3.5. In addition, the thickness of the flaky polyethylene particles may be about 0.2 μm to about 4 μm, specifically, about 0.3 μm to about 2.5 μm, or, for example, about 0.3 μm to about 1.5 μm. When the flaky polyethylene particles have a size, a ratio of the major axis length to the minor axis length and a thickness within the range, the performance of the battery is ensured by minimizing the transfer impedance of lithium ions, and the heat release of the battery can also be suppressed in the early stage by enhancing the closed-cell function.
[0066] The particle size of the flaky polyethylene particles may be an average particle size (D50) at a volume ratio of 50% in a cumulative particle size distribution curve.
[0067] As used herein, when no definition is otherwise provided, the average particle size (D50) can be measured by methods known to those of ordinary skill in the art. For example, the average particle size can be measured by a particle size analyzer or by a TEM (transmission electron microscope) or SEM (scanning electron microscope) photograph.
[0068] Alternatively, a dynamic light scattering measurement device is used to perform data analysis and the number of particles is counted for each size range. From this, the D50 value can be easily obtained by calculation.
[0069] More precisely, the particle size of the flaky polyethylene particles can be determined by dynamic light scattering measurement methods. Specifically, the size can be measured by analysis of the light scattering properties of the particles according to ISO 13320. For non-spherical particles, the size distribution is reported for which the predicted scattering pattern of the volume sum of spherical particles matches the measured scattering pattern.
[0070] The negative electrode functional layer includes sheet polyethylene and optionally additional inorganic particles and a binder. The closed-cell function of the sheet polyethylene can suppress the heat release of the battery in the early stage, the electrical insulation of the inorganic particles can prevent the short circuit between the positive electrode and the negative electrode, and the binder can play a role in bonding the sheet polyethylene to the inorganic particles and also bonding them to the negative electrode active material layer. Therefore, the physical / thermal safety and stability of the rechargeable lithium battery and the room temperature / high temperature cycle life characteristics can be improved.
[0071] Inorganic particles may include, for example, Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, SrTiO3, BaTiO3, Mg(OH)2, boehmite, or a combination thereof, but are not limited thereto. In addition to inorganic particles, organic particles may also be included, for example, acrylic compounds, imide compounds, amide compounds, or a combination thereof, but the organic particles are not limited thereto.
[0072] The inorganic particles may be spherical, plate-like, cubic or amorphous. The average particle size (D50) of the inorganic particles may be from about 1 nm to about 2500 nm, for example, from about 100 nm to about 2000 nm, or from about 200 nm to about 1000 nm, or from about 300 nm to about 800 nm.
[0073] When the negative electrode functional layer further includes inorganic particles, the flaky polyethylene particles and the inorganic particles may be included in a weight ratio of about 95:5 to about 10:90 (specifically, about 70:30 to about 30:70). When the flaky polyethylene particles and the inorganic particles are used within the range, the cycle life characteristics and output characteristics of the battery can be ensured.
[0074] The binder may be the same as the binder used as the negative electrode binder, but is not limited thereto.
[0075] When the negative electrode functional layer also includes inorganic particles and a binder, the total amount of flaky polyethylene particles and inorganic particles: the amount of binder (i.e., the ratio of the total amount of flaky polyethylene particles and inorganic particles to the amount of binder) can be about 80:20 to about 99:1 by weight, specifically, about 85:15 to about 97:3 by weight.
[0076] The thickness of the negative electrode functional layer may be about 1 μm to about 10 μm, specifically, about 3 μm to about 10 μm. In addition, the ratio of the thickness of the negative electrode active material layer to the thickness of the negative electrode functional layer may be about 50:1 to about 10:1, specifically, about 30:1 to about 10:1. When the thickness of the negative electrode functional layer and the ratio of the thickness of the negative electrode functional layer are within the above range, physical stability and thermal stability can be significantly improved while maintaining excellent cycle life characteristics.
[0077] The electrolyte solution includes a nonaqueous organic solvent, a lithium salt, and optionally an additive.
[0078] The nonaqueous organic solvent serves as a medium for transmitting ions participating in an electrochemical reaction of a battery. The nonaqueous organic solvent according to an embodiment includes a propionate-based solvent and a carbonate-based solvent.
[0079] Examples of carbonate solvents include chain carbonates (such as dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl butyl carbonate and ethyl methyl carbonate (MEC)) and cyclic carbonates (such as ethylene carbonate (EC), propylene carbonate (PC) and butylene carbonate (BC)).
[0080] The propionate-based solvent may include at least one of methyl propionate, ethyl propionate, propyl propionate, butyl propionate, and the like.
[0081] According to an embodiment, the non-aqueous organic solvent may include about 60 volume % to about 80 volume % of a propionate solvent and about 20 volume % to about 40 volume % of a carbonate solvent. For example, the amount of the propionate solvent is greater than or equal to about 60 volume %, greater than or equal to about 61 volume %, greater than or equal to about 62 volume %, greater than or equal to about 63 volume %, greater than or equal to about 64 volume %, greater than or equal to about 65 volume %, greater than or equal to about 66 volume %, greater than or equal to about 67 volume %, greater than or equal to about 68 volume %, greater than or equal to about 69 volume %, or greater than or equal to about 70 volume % and less than or equal to about 80 volume %, less than or equal to about 79 volume %, less than or equal to about 78 volume %, less than or equal to about 77 volume %, less than or equal to about 76 volume %, less than or equal to about 75 volume %, less than or equal to about 74 volume %, less than or equal to about 73 volume %. %, less than or equal to about 72% by volume, or less than or equal to about 71% by volume, for example, the amount of the carbonate solvent is greater than or equal to about 20% by volume, greater than or equal to about 21% by volume, greater than or equal to about 22% by volume, greater than or equal to about 23% by volume, greater than or equal to about 24% by volume, greater than or equal to about 25% by volume, greater than or equal to about 26% by volume, greater than or equal to about 27% by volume, greater than or equal to about 28% by volume, greater than or equal to about 29% by volume, or greater than or equal to about 30% by volume and less than or equal to about 40% by volume, less than or equal to about 39% by volume, less than or equal to about 38% by volume, less than or equal to about 37% by volume, less than or equal to about 36% by volume, less than or equal to about 35% by volume, less than or equal to about 34% by volume, less than or equal to about 33% by volume, less than or equal to about 32% by volume, or less than or equal to about 31% by volume.
[0082] For example, the nonaqueous organic solvent may include ethylene carbonate in an amount of about 5 volume % to about 20 volume %, about 7 volume % to about 18 volume %, about 9 volume % to about 16 volume %, or about 11 volume % to about 16 volume %.
[0083] The nonaqueous organic solvent may include propylene carbonate in an amount of about 5 volume % to about 20 volume %, about 7 volume % to about 18 volume %, about 9 volume % to about 16 volume %, or about 11 volume % to about 16 volume %.
[0084] The non-aqueous organic solvent may include ethyl propionate in an amount of about 25 volume % to about 50 volume %, about 25 volume % to about 45 volume %, about 25 volume % to about 42 volume %, or about 29 volume % to about 41 volume %.
[0085] The non-aqueous organic solvent may include propyl propionate in an amount of about 25 volume % to about 50 volume %, about 25 volume % to about 45 volume %, about 25 volume % to about 42 volume %, or about 29 volume % to about 41 volume %.
[0086] Generally, when the amount of carbonate solvents in the electrolyte solution increases, the viscosity of the electrolyte solution increases, and thus the capacity characteristics of the battery deteriorate, and when the amount of propionate solvents in the electrolyte solution increases, the dissociation degree of the electrolyte salt decreases, and thus the capacity characteristics or cycle life characteristics deteriorate. Specifically, for a rechargeable battery including a negative electrode functional layer according to an embodiment, since the lithium channel is restricted during normal operation of the battery, the impregnation of the electrolyte solution may deteriorate, but when the propionate solvent and the carbonate solvent are included in the range, the viscosity of the electrolyte solution and the dissociation degree of the electrolyte salt can be appropriately adjusted, so that the impregnation of the electrolyte solution can be improved, and as a result, the capacity characteristics and cycle life characteristics of the battery can be improved.
[0087] The nonaqueous organic solvent according to an embodiment may further include an organic solvent in addition to the carbonate-based solvent and the propionate-based solvent.
[0088] Organic solvent can be, for example, esters, ethers, ketones, alcohols or aprotic solvents. Esters can include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, γ-butyrolactone, decalactone, valerolactone, mevalonolactone, caprolactone, etc. Ether solvents can include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. Ketone solvents can be cyclohexanone, etc. Alcohol solvents can include ethanol, isopropanol, etc. Aprotic solvents can include nitrile (such as, R-CN (wherein R is C2 to C20 straight chain, branched or cyclic hydrocarbon group, double bond, aromatic ring or ether bond)), amide (such as, dimethylformamide, etc.), dioxolane (such as, 1,3-dioxolane, etc.), sulfolane, etc.
[0089] These organic solvents may be used alone or in combination of two or more. In the case of mixing two or more, the mixing ratio may be appropriately adjusted according to the desired battery performance, which is widely understood by those skilled in the art.
[0090] In addition to the propionate solvent and the carbonate solvent, the non-aqueous organic solvent according to the embodiment may also include an aromatic hydrocarbon organic solvent. In this case, the total amount of the propionate solvent and the carbonate solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of about 1:1 to about 30:1.
[0091] As the aromatic hydrocarbon organic solvent, an aromatic hydrocarbon compound represented by Chemical Formula 2 may be used.
[0092] [Chemical formula 2]
[0093]
[0094] In Chemical Formula 2, R1 to R6 are the same or different and are selected from hydrogen, halogen, C1 to C10 alkyl, halogenated alkyl, and combinations thereof.
[0095] Specific examples of aromatic hydrocarbon organic solvents can be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluoroform, Benzene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0096] Lithium salts can be used as non-aqueous electrolytes for rechargeable lithium batteries. Lithium salts dissolved in organic solvents provide lithium ions to the battery, allowing the rechargeable lithium battery to operate essentially, and improve the transport of lithium ions between the positive electrode and the negative electrode.
[0097] Examples of lithium salts include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide: LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein, x and y are natural numbers), at least one supporting salt of LiCl, LiI and LiB(C2O4)2 (lithium di(oxalato)borate: LiBOB).
[0098] The concentration of the lithium salt may be in the range of about 0.1 M to about 2.0 M. When the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to optimal electrolyte conductivity and viscosity.
[0099] The electrolyte solution may further include vinylene carbonate, an ethylene carbonate-based compound of Chemical Formula 3, a nitrile-based compound, or a combination thereof as an additive to improve the cycle life of the battery.
[0100] [Chemical formula 3]
[0101]
[0102] In Chemical Formula 3, R7 and R8 may be the same or different and may be selected from hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2) and a fluorinated C1 to C5 alkyl group, wherein at least one of R7 and R8 is selected from a halogen group, a cyano group (CN), a nitro group (NO2) and a fluorinated C1 to C5 alkyl group, with the proviso that R7 and R8 are not both hydrogen.
[0103] Examples of the ethylene carbonate-based compound may include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, fluoroethylene carbonate, and the like.
[0104] Examples of the nitrile compound may include valeronitrile (GN), succinonitrile (SN), adiponitrile (AN), 3,3′-thio-dipropionitrile (TPN), 1,2,3-hexanitrile, 1,2,4-hexanitrile, 1,2,5-hexanitrile, 1,2,6-hexanitrile, 1,3,4-hexanitrile, 1,3,5-hexanitrile, 1,3,6-hexanitrile, and 1,4,5-hexanitrile.
[0105] In the case of further using such cycle life improving additives, their amounts may be appropriately adjusted. The additives may be included in an amount of, for example, about 3 wt % to about 20 wt %, or about 5 wt % to about 18 wt %, based on the total weight of the electrolyte solution.
[0106] The positive electrode includes a positive electrode current collector layer and a positive electrode active material layer provided on at least one surface of the positive electrode current collector layer.
[0107] The positive electrode current collector layer is used to support the positive electrode active material. As the positive electrode current collector layer, for example, aluminum foil, nickel foil or a combination thereof can be used, but it is not limited thereto.
[0108] The positive electrode active material layer may include a first positive electrode active material including at least one composite oxide of a metal selected from cobalt, manganese, nickel, and combinations thereof and lithium, and a second positive electrode active material including a compound represented by Chemical Formula 1.
[0109] [Chemical formula 1]
[0110] Li a Fe 1-x M x PO4
[0111] In Chemical Formula 1, 0.90≤a≤1.8, 0≤x≤0.7, and M is Mn, Co, Ni, or a combination thereof.
[0112] The first positive electrode active material may include LiCoO2, Li b M 1 1-y1-z1 M 2 y1 M 3 z1 O2 (0.9≤.91-z, 0.91-z, 0.91-z, 0.91-z1 mass 1, M 1 、M 2 and M 3 is independently one of a metal selected from Ni, Co, Mn, Al, Sr, Mg or La and a combination thereof.
[0113] For example, the first positive active material may include LiCoO 2 , but is not limited thereto.
[0114] For example, M 1 Can be Ni, M 2 and M 3 It may independently be a metal such as Co, Mn, Al, Sr, Mg or La.
[0115] More specifically, M 1 Can be Ni, M2 It can be Co, M 3 It may be Mn or Al, but is not limited thereto.
[0116] The second positive active material may include, for example, LiFePO 4 .
[0117] The average particle size of the first positive active material may be about 10 μm to about 30 μm, specifically, about 10 μm to about 25 μm, for example, about 13 μm to about 20 μm. In addition, the average particle size of the second positive active material may be about 300 nm to about 700 nm, specifically, about 300 nm to about 600 nm, for example, about 300 nm to about 500 nm. When the average particle size of the first positive active material and the second positive active material is within the above range, the energy density can be increased to achieve a high-capacity rechargeable lithium battery.
[0118] The rechargeable lithium battery according to an embodiment of the present invention has both a positive electrode active material layer including a first positive electrode active material and a second positive electrode active material and a negative electrode functional layer disposed on the negative electrode, so that the heat increase rate due to thermal / physical shock can be reduced, and the flaky polyethylene particles can melt and help to completely block the ion channel.
[0119] According to an embodiment, the positive electrode active material layer may further include a positive electrode functional layer disposed on the positive electrode active material layer.
[0120] The first positive electrode active material may be included in the positive electrode active material layer, and the second positive electrode active material may be included in at least one of the positive electrode active material layer and the positive electrode functional layer.
[0121] In an embodiment, the first positive active material and the second positive active material may be included in a weight ratio of about 97:3 to about 80:20, for example, may be included in a weight ratio of about 95:5 to about 85:15.
[0122] The amount of the first positive active material may be about 70 wt % to about 99 wt %, more specifically about 85 wt % to about 99 wt %, about 85 wt % to about 95 wt % or about 85 wt % to about 93 wt % based on the total amount of the positive active material layer.
[0123] When the amount of the first positive electrode active material satisfies the above range, the safety of the battery may be improved without reducing the capacity.
[0124] In addition, based on the total amount of the positive electrode active material layer, the amount of the second positive electrode active material can be about 1wt% to about 30wt%, more specifically, about 1wt% to about 15wt%, about 5wt% to about 15wt% or about 7wt% to about 15wt%. When the amount of the second positive electrode active material meets the above range, the safety of the battery can be improved without reducing the capacity.
[0125] The positive electrode active material layer may further optionally include a positive electrode conductive material and a positive electrode binder.
[0126] The amount of the positive conductive material and the positive binder may be about 1 wt % to about 5 wt %, respectively, based on the total weight of the positive active material layer.
[0127] The positive electrode conductive material is used to impart conductivity to the positive electrode, and the type of the positive electrode conductive material is the same as that of the negative electrode conductive material described above.
[0128] The positive electrode binder firmly adheres to the positive electrode active material and is also used to well attach the positive electrode active material to the current collector. Examples of the positive electrode binder may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0129] The separator 113 may be disposed between the positive electrode 114 and the negative electrode 112. The separator 113 may be, for example, selected from glass fiber, polyester, polyethylene, polypropylene, polytetrafluoroethylene, or a combination thereof. The separator 113 may have the form of a nonwoven fabric or a woven fabric. For example, in a rechargeable lithium battery, polyolefin polymer separators such as polyethylene and polypropylene are mainly used. In order to ensure heat resistance or mechanical strength, a coated separator including a ceramic component or a polymer material may be used. Optionally, the separator may have a single-layer structure or a multilayer structure.
[0130] Hereinafter, the above aspects of the present disclosure are explained in more detail with reference to examples. However, these examples are exemplary, and the present disclosure is not limited thereto.
[0131] Example
[0132] Example 1-1
[0133] LiCoO2 and LiFePO4 were mixed in a weight ratio of 9:1 to prepare a positive electrode active material, and 95wt% of the positive electrode active material, 3wt% of a polyvinylidene fluoride binder, and 2wt% of a Ketjen black conductive material were mixed in an N-methylpyrrolidone solvent to prepare a positive electrode active material slurry. The positive electrode active material slurry was coated on both surfaces of an aluminum current collector, and then dried and compressed to manufacture a positive electrode having a positive electrode active material layer.
[0134] 98 wt% of artificial graphite, 0.8 wt% of carboxymethyl cellulose and 1.2 wt% of styrene-butadiene rubber were mixed in pure water to prepare a negative electrode active material slurry. The negative electrode active material slurry was coated on both surfaces of a copper current collector, and then dried and compressed to manufacture a negative electrode having a negative electrode active material layer.
[0135] The negative electrode functional layer composition was prepared by mixing 48 wt % of flaky polyethylene (PE) particles (average particle size (D50): 2 μm, major axis length / minor axis length: about 2, thickness: about 0.6 μm), 47 wt % of alumina (average particle size: 0.7 μm) and 5 wt % of an acrylated styrene rubber binder in an alcohol solvent.
[0136] The negative electrode having the negative electrode functional layer is manufactured by coating the negative electrode functional layer composition on the surface of the negative electrode, and then drying and compressing it.
[0137] A positive electrode, a polyethylene (PE) / polypropylene (PP) multilayer separator, and a negative electrode having a coating layer including flaky PE particles are sequentially stacked to manufacture an electrode assembly, and an electrolyte solution is injected therein to manufacture a rechargeable lithium battery cell.
[0138] An electrolyte solution was prepared by mixing ethylene carbonate (EC): propylene carbonate (PC): ethyl propionate (EP): propyl propionate (PP) in a volume ratio of 10:10:40:40, adding 1.0 M electrolyte LiPF6 thereto, and then adding 3 wt % of fluoroethylene carbonate (FEC), 1 wt % of vinyl carbonate (VC) and 2 wt % of succinonitrile (SN) thereto based on the total weight of the electrolyte solution.
[0139] Example 1-2
[0140] A rechargeable lithium battery cell was manufactured according to the same method as Example 1-1, except that flaky PE particles (average particle size: 4 μm, major axis length / minor axis length: about 2.4, thickness: about 0.6 μm) were used instead of the flaky polyethylene (PE) particles (average particle size (D50): 2 μm, major axis length / minor axis length: about 2, thickness: about 0.6 μm) of Example 1-1 to form the negative electrode functional layer.
[0141] Example 1-3
[0142] A rechargeable lithium battery cell was manufactured according to the same method as Example 1-1, except that flaky PE particles (average particle size: 6 μm, major axis length / minor axis length: about 2.4, thickness: about 0.6 μm) were used instead of the flaky polyethylene (PE) particles (average particle size (D50): 2 μm, major axis length / minor axis length: about 2, thickness: about 0.6 μm) of Example 1-1 to form the negative electrode functional layer.
[0143] Example 2-1 to Example 2-3
[0144] Rechargeable lithium battery cells were manufactured in the same manner as Examples 1-1 to 1-3, respectively, except that EC:PC:EP:PP was mixed in a volume ratio of 15:15:30:40 instead of the solvents of Examples 1-1 to 1-3.
[0145] Example 3-1 to Example 3-3
[0146] Rechargeable lithium battery cells were manufactured in the same manner as Examples 1-1 to 1-3, respectively, except that a solvent prepared by mixing EC:PC:EP:PP at a volume ratio of 20:20:30:30 was used instead of the solvents of Examples 1-1 to 1-3.
[0147] Figure 4 is a graph analyzing the particle size distribution of the flake-shaped polyethylene particles included in the negative electrode functional layer compositions according to Example 1-1, Example 1-2, and Example 1-3.
[0148] Comparative Example 1
[0149] A rechargeable lithium battery cell was manufactured in the same method as Example 1-1, except that a solvent prepared by mixing EC:EMC:DEC in a volume ratio of 30:50:20 was used instead of the solvent of Example 1-1.
[0150] Comparative Example 2
[0151] A rechargeable lithium battery cell was manufactured in the same method as Example 1-1, except that a solvent prepared by mixing EC:EP at a volume ratio of 50:50 was used instead of the solvent of Example 1-1.
[0152] Comparison Example 3
[0153] A rechargeable lithium battery cell was manufactured in the same method as Example 1-1, except that a solvent prepared by mixing EC:PC:EP:PP in a volume ratio of 20:30:25:25 was used instead of the solvent of Example 1-1.
[0154] Comparison Example 4
[0155] A rechargeable lithium battery cell was manufactured in the same method as Example 1-1, except that a solvent prepared by mixing EC:PC:EP:PP in a volume ratio of 5:5:45:45 was used instead of the solvent of Example 1-1.
[0156] Comparative Example 5
[0157] Rechargeable lithium battery cells were manufactured in the same manner as in Example 1-1, respectively, except that the negative electrode functional layer was not included in the negative electrode.
[0158] Evaluation example
[0159] Impregnation properties of electrolyte solution
[0160] The negative electrode plates according to Examples 1-1 to 1-3, Examples 2-1 and 3-1, and Comparative Examples 1 to 4 were cut into a size of 3 cm×6 cm, respectively, and then immersed in each electrolyte solution prepared in the Examples and Comparative Examples for 300 seconds, and then the amount of the electrolyte solution impregnated into the negative electrode was measured in a quantitative method. The results are shown in Table 1. The measurement was performed using an Attension Sigma device.
[0161] (Table 1)
[0162]
[0163] Referring to Table 1, compared with the negative electrodes of Comparative Examples 1 to 4, the negative electrodes of Examples 1-1 to 1-3, 2-1, and 3-1 maintained the impregnation property in the electrolyte solution within an appropriate range.
[0164] Cycle life characteristics at room temperature / high temperature
[0165] The rechargeable lithium battery cells of Examples 1-1 to 1-3, Examples 2-1 to 2-3, Examples 3-1 to 3-3, and Comparative Examples 1 to 4 were charged at 4.4V at a rate of 0.5C / 0.5C at room temperature (25°C) and a high temperature of 45°C, and then discharged down to 3.0V, which was regarded as one cycle and repeated for 300 cycles, and then the capacity retention rate of the battery cells was measured. The results are shown in Table 2.
[0166] (Table 2)
[0167]
[0168]
[0169] Referring to Table 2, compared with the rechargeable lithium battery cells of Comparative Examples 1 to 4, the rechargeable lithium battery cells of Examples 1-1 to 1-3, Examples 2-1 to 2-3, and Examples 3-1 to 3-3 exhibited excellent room temperature capacity retention and high temperature capacity retention after 300 cycles. Specifically, Comparative Examples 2 and 4, which included an excessive amount of propionate solvent in an organic solvent, exhibited a decrease in the degree of dissociation of the electrolyte salt, and thus exhibited a deterioration in the room temperature / high temperature capacity retention, while Comparative Examples 1 and 3, which included an excessive amount of carbonate solvent in an organic solvent, exhibited an increase in the viscosity of the electrolyte solution and deterioration in the impregnation of the electrolyte solution, and thus exhibited insufficient capacity characteristics and capacity retention. On the other hand, Examples 1-1 to 1-3 and Examples 2-1 to 2-3, which included propionate solvents and carbonate solvents within the preferred range, exhibited greatly improved capacity retention.
[0170] Safety Assessment of Rechargeable Lithium Battery Cells
[0171] The puncture test, drop test, and collision test of the rechargeable lithium battery cells manufactured in Example 1-1 and Comparative Example 5 were performed, and the results of evaluating physical safety are shown in Table 3. On the other hand, the physical safety evaluation criteria are as described in Table 4.
[0172] (Table 3)
[0173] puncture fall collision Example 1-1 L2 L2 L2 Comparative Example 5 L5 L4 L5
[0174] (Table 4)
[0175] Level Standard event L0 No events L1 Leakage, external temperature <150℃ L2 External temperature <200℃ L3 Smoke, external temperature>200℃ L4 flame L5 explode
[0176] Referring to Tables 3 and 4, the rechargeable lithium battery cell of Example 1-1 effectively inhibited the ion channel during the thermal runaway caused by the physical impact and closed at the early stage as expected, and exhibited excellent physical safety, compared with the rechargeable lithium battery cell of Comparative Example 5. Therefore, the rechargeable lithium battery cell according to the embodiment can effectively realize the closed-cell function and maintain excellent battery characteristics.
[0177] In the above, some examples of the present invention have been described and illustrated, however, it is obvious to those skilled in the art that the present invention is not limited to the described examples, and various modifications and variations can be made without departing from the spirit and scope of the present invention. Therefore, the examples so modified or varied themselves will not be understood separately from the technical ideas and aspects of the present invention, and the modified embodiments are within the scope of the claims of the present invention.
[0178] <Description of symbols>
[0179] 100: Rechargeable lithium battery
[0180] 112: Negative electrode
[0181] 113: Diaphragm
[0182] 114: Positive electrode
[0183] 120: Battery housing
[0184] 140: Sealing member
Claims
1. A rechargeable lithium battery, comprising: A negative electrode, comprising a negative electrode active material layer and a negative electrode functional layer disposed on the negative electrode active material layer; A positive electrode, including a positive electrode active material layer; as well as Electrolyte solution, The negative electrode functional layer includes flaky polyethylene particles. The ratio of the major axis length to the minor axis length of the flaky polyethylene particles is 1 to 5. The electrolyte solution includes a lithium salt and a non-aqueous organic solvent, and The non-aqueous organic solvent includes 60 volume % to 80 volume % of a propionate-based solvent and 20 volume % to 40 volume % of a carbonate-based solvent.
2. The rechargeable lithium battery according to claim 1, wherein The propionate solvent includes at least one selected from methyl propionate, ethyl propionate, propyl propionate and butyl propionate.
3. The rechargeable lithium battery according to claim 1, wherein The carbonate solvent includes at least one selected from ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate and methyl butyl carbonate.
4. The rechargeable lithium battery according to claim 1, wherein The electrolyte solution also includes additives, and The additive is included in an amount of 3 wt % to 20 wt % based on the total amount of the electrolyte solution.
5. The rechargeable lithium battery according to claim 1, wherein The flake-shaped polyethylene particles have a particle size of 1 μm to 8 μm.
6. The rechargeable lithium battery according to claim 1, wherein: The ratio of the major axis length to the minor axis length of the flaky polyethylene particles is 1.1 to 4.
5.
7. The rechargeable lithium battery according to claim 1, wherein: The flake-shaped polyethylene particles have a thickness of 0.2 μm to 4 μm.
8. The rechargeable lithium battery according to claim 1, wherein The negative electrode functional layer further includes inorganic particles and a binder.
9. The rechargeable lithium battery according to claim 8, wherein: The ratio of the total amount of the flaky polyethylene particles and the inorganic particles to the amount of the binder is 80:20 to 99:1 by weight.
10. The rechargeable lithium battery according to claim 8, wherein: The flaky polyethylene particles and the inorganic particles are included in a weight ratio of 95:5 to 10:
90.
11. The rechargeable lithium battery according to claim 1, wherein: The negative electrode functional layer has a thickness of 1 μm to 10 μm.
12. The rechargeable lithium battery according to claim 1, wherein: The ratio between the thickness of the negative electrode active material layer and the thickness of the negative electrode functional layer is 50:1 to 10:
1.
13. The rechargeable lithium battery according to claim 1, wherein: The positive electrode active material layer includes a first positive electrode active material and a second positive electrode active material, the first positive electrode active material includes at least one of a composite oxide of a metal selected from cobalt, manganese, nickel and a combination thereof and lithium, and the second positive electrode active material includes a compound represented by Chemical Formula 1, [Chemical formula 1] Li a Fe 1-x M x PO4 In Chemical Formula 1, 0.90≤a≤1.8, 0≤x≤0.7, and M is Mn, Co, Ni, or a combination thereof.
14. The rechargeable lithium battery according to claim 13, wherein: The first positive electrode active material includes LiCoO2, Li b M 1 1-y1-z1 M 2 y1 M 3 z1 O2 and a combination thereof, wherein 0.9≤b≤1.8, 0≤y1≤1, 0≤z1≤1, 0≤y1+z1≤1, M 1 、M 2 and M 3 independently a metal selected from Ni, Co, Mn, Al, Sr, Mg or La.
15. The rechargeable lithium battery according to claim 13, wherein: The second positive electrode active material includes LiFePO4.
16. The rechargeable lithium battery according to claim 13, wherein: The positive electrode active material layer further includes a positive electrode functional layer disposed on the positive electrode active material layer.
17. The rechargeable lithium battery according to claim 16, wherein: The first positive electrode active material is included in the positive electrode active material layer, and The second positive electrode active material is included in at least one of the positive electrode active material layer and the positive electrode functional layer.
18. The rechargeable lithium battery according to claim 13, wherein: The first positive electrode active material and the second positive electrode active material are included in a weight ratio of 97:3 to 80:
20.
19. The rechargeable lithium battery according to claim 13, wherein: The first positive electrode active material is included in an amount of 70 wt % to 99 wt % based on the total amount of the positive electrode active material layer, and The second positive active material is included in an amount of 1 wt % to 30 wt % based on the total amount of the positive active material layer.