A punch, a die and a stretching process for stretching a battery can body

Through the variable wall thickness stretching process that combines step punches and molds, the contradiction between the wall thickness of the battery can and the reliability of the roll seal is solved, saving materials and improving the energy density and reliability of the battery pack.

CN112157175BActive Publication Date: 2024-10-01SUZHOU SLAC PRECISION EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010964743.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-15
Publication Date
2024-10-01
Estimated Expiration
2040-09-15

AI Technical Summary

Technical Problem

The welding process of the existing battery tank body results in poor reliability and stability, and the space utilization rate after rolling is low, which cannot effectively solve the contradiction between the tank wall thickness and the reliability of the rolling seal.

Method used

Using a stretching process that combines a step punch and a die, and through a stretching process with variable wall thickness, a battery tank body with a thinner wall thickness in the middle section and thicker wall thickness at both ends is designed. This is achieved by using a combination of step punches and thinning rings. Variable wall thickness of the tank, combined with compressed gas assisted demolding.

Benefits of technology

It saves materials, improves the sealing strength and space utilization, reduces the cost of materials, and enhances the energy density and reliability of the battery pack.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112157175B_ABST
    Figure CN112157175B_ABST
Patent Text Reader

Abstract

A punch, a die and a stretching process for stretching a battery can body, characterized by: a specially designed step punch as a punch, at least one thinning ring as a die, and a can body variable wall thickness stretching process. The variable wall thickness stretching process belongs to thinning stretching, when a sheet or plate is formed and stretched at least once to obtain a cup-shaped stretched part, and then through thinning stretching, especially variable wall thickness stretching using a step punch and at least one thinning ring, a variable wall thickness battery can body is finally obtained with a thin middle section and thick walls at one or both axial ends. This variable wall thickness battery can body can reduce the amount of material used in the middle section of the can body on the one hand, and on the other hand, can ensure the sealing strength of one or both ends of the can body. Therefore, the contradiction between the amount of material used and the sealing strength caused by the thickness of the battery can body is well solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of can body processing, and in particular to a punch and a die for stretching a battery can body and a stretching process thereof. Background Art

[0002] New energy vehicles use battery packs as the power source of the entire vehicle. The battery packs are equipped with multiple battery cells. The battery cell is the smallest unit that constitutes the new energy battery system. It is composed of a positive electrode, a negative electrode and an electrolyte. The outer shell of the battery cell is a battery can. Multiple assembled battery cells are gathered and arranged in the battery pack with their axes parallel.

[0003] The battery can is composed of a can body and a can cover. In the prior art, the can body is usually processed by cold pressing, and the formed can body and the can cover are then welded together. However, the reliability and stability of the welded ends of the battery can are poor, and are prone to problems such as breakage, poor contact, and poor explosion-proof performance. In addition, after the welded battery cans are assembled into battery cells, the can bodies cannot be closely arranged due to the presence of welds, resulting in low space utilization in the battery pack.

[0004] If the can body and end cover can be sealed by the rolling process, the adverse effects of welding can be avoided. However, there is currently no stretching process for the body of a rolled battery can, and the stretching process used for other types of cans can usually only stretch a can body with the same wall thickness. Therefore, when designing a rolled and sealed battery can, it is necessary to pay attention to the wall thickness of the battery can body: if the can wall is too thick, it will not only increase the material cost, but also increase the weight of the battery pack, resulting in a decrease in the overall energy density of the battery pack; if the can wall is too thin, there will be problems such as the can end is easy to tear during the rolling process or it is not firm during use after the rolling process. Therefore, if a variable wall thickness battery can body can be manufactured with a thinner wall thickness in the middle section (saving materials) and a thicker wall thickness at both ends (providing rolling strength), it is the best solution to solve the wall thickness problem of the battery can body.

[0005] In view of this, how to design a punch, a die and a stretching process for stretching a battery can body, so as to produce a battery can body with variable wall thickness that saves materials and provides high-reliability sealing, is the research topic of the present invention. Summary of the invention

[0006] The present invention provides a punch and a die for stretching a battery can body and a stretching process thereof, the purpose of which is to solve the contradiction between the amount of material used and the reliability of sealing caused by the thickness of the battery can body wall.

[0007] In order to achieve the above-mentioned purpose, the technical solution adopted by the punch of the present invention is: a punch for stretching the body of a battery can, the innovation of which lies in: the punch is a step punch, the main body of which is a cylinder, the step punch has a thick rod segment, at least one end of the thick rod segment in the axial direction is provided with a thin rod segment, the difference between the radius of the thick rod segment and the radius of the thin rod segment is less than or equal to 0.3 mm, and the ratio of the radius of the two is less than or equal to 101:100; the thin rod segment and the thick rod segment are transitioned by at least one conical surface or / and curved surface, and the ratio of the radius difference between the thick rod segment and the thin rod segment to the axial projection length of the conical surface or / and curved surface is less than 0.2.

[0008] In order to achieve the above-mentioned purpose, the technical solution adopted by the mold of the present invention is: a mold for stretching the battery can body, the mold is composed of a male mold and a female mold, and its innovation lies in:

[0009] The punch is composed of a step punch, the main body of which is a cylinder, with a thick rod segment on the step punch, and a thin rod segment on at least one axial end of the thick rod segment, the difference between the radius of the thick rod segment and the radius of the thin rod segment is less than or equal to 0.3 mm, and the ratio of the radii of the two is less than or equal to 101:100; the thin rod segment and the thick rod segment are transitioned by at least one conical surface and / or curved surface, and the ratio of the radius difference between the thick rod segment and the thin rod segment to the axial projection length of the conical surface and / or curved surface is less than 0.2.

[0010] The die is composed of at least one thinning ring, which is coaxially arranged with the step punch; the difference between the inner diameter of the thinning ring and the diameter of the thick rod section of the step punch is less than twice the wall thickness of the can body to be thinned.

[0011] The relevant contents in the above mold technical solution are explained as follows:

[0012] 1. In the above die solution, it is preferred that the die is composed of at least two thinning rings, the at least two thinning rings are coaxially arranged with the step punch, and the inner diameters of the at least two thinning rings are arranged to decrease in sequence along the punching direction.

[0013] 2. In the above mold solution, it is preferred that the ratio of the wall thickness of the thinned part corresponding to the thick rod segment after thinning by the thinning ring to the diameter of the thick rod segment is 1:30.

[0014] To achieve the above-mentioned purpose, the technical solution adopted by the stretching process of the present invention is: a battery can body stretching process, including thinning stretching, the number of thinning stretching is at least one, and its innovation is: the thinning stretching includes at least one variable wall thickness stretching for the thin-wall section and the thick-wall section of the can body, and the variable wall thickness stretching is completed by using a stamping device through the following mold:

[0015] The mold is composed of a punch and a die, the punch is composed of a step punch, the main body of the step punch is a cylinder, a thick rod segment is provided on the step punch, at least one axial end of the thick rod segment is provided with a thin rod segment, the difference between the radius of the thick rod segment and the radius of the thin rod segment is less than or equal to 0.3 mm, and the ratio of the radii of the two is less than or equal to 101:100; the thin rod segment and the thick rod segment are transitioned by at least one conical surface and / or curved surface, and the ratio of the radius difference between the thick rod segment and the thin rod segment to the axial projection length of the conical surface and / or curved surface is less than 0.2.

[0016] The die is composed of at least one thinning ring, which is coaxially arranged with the step punch; the difference between the inner diameter of the thinning ring and the diameter of the thick rod section of the step punch is less than twice the wall thickness of the can body to be thinned.

[0017] During the variable wall thickness stretching process, the step punch drives the stretched part to pass through each thinning ring in sequence, and then demolds to obtain a thinned part. The thinned part includes a thin-walled section corresponding to the thick rod section of the step punch and a thick-walled section corresponding to the thin rod section of the step punch, the thick-walled section is located at one or both ends of the thinned part in the axial direction, and there is at least one conical surface or / and curved surface transition between the thin-walled section and the thick-walled section.

[0018] The relevant contents in the above-mentioned stretching process technical solution are explained as follows:

[0019] 1. In the above-mentioned stretching process scheme, for the stretching of the battery can body, sheets or plates (such as aluminum alloy plates or aluminum alloy sheets) are usually used as raw materials (but aluminum alloy ingots are not excluded as raw materials), and then the battery can body is obtained by at least one forming stretching and at least one thinning stretching. In the present invention, the forming stretching refers to the stretching process of changing the stretched piece from a sheet to a cup-shaped stretched piece (usually called a "punch cup"), and the forming stretching also includes the stretching process of changing the punch cup diameter and the punch cup length. The thinning stretching refers to the stretching process of thinning the wall thickness of the cup-shaped stretched piece. There are usually two stretching conditions for thinning stretching. The first is a stretching process in which only the wall thickness is changed, the inner diameter remains unchanged, and the outer diameter is reduced. The second is a stretching process in which the inner diameter, the outer diameter, and the wall thickness are changed. According to the prior art, in order to stretch a metal sheet into the shape of a battery can body, at least one forming stretching and one thinning stretching are theoretically required. When multiple forming stretches are combined with multiple thinning stretches, the thinning stretch can be cross-combined with the forming stretch in the process order, that is, the forming stretch is performed first, followed by the thinning stretch, then the forming stretch, and finally the thinning stretch. When a forming stretch is combined with one or more thinning stretches, the forming stretch is usually performed first. When multiple forming stretches are combined with a thinning stretch, the first stretch should usually be the forming stretch, and the thinning stretch can be arranged at the end, or between the remaining forming stretches. In fact, the order of forming stretching and thinning stretching is relatively flexible, except that the first stretching should be the forming stretching, and the remaining stretching order is relatively flexible, which can be confirmed according to the material properties, the shape and size of the stretched object and other parameters, which are all prior arts known to those skilled in the art. In the present invention, the variable wall thickness stretching refers to a stretching process in which the wall thickness of the same stretched part changes with different thicknesses during a single stretching process. For example, in the present invention, the wall thickness of the middle section of the stretched battery can body is thinner, while the wall thickness at both ends or one end is relatively thicker. From the perspective of the stretching process, variable wall thickness stretching should be a special case of thinning stretching. Since the innovation of the present invention lies in the variable wall thickness stretching in the thinning stretching, and the forming stretching belongs to the existing public technology for the stretching of the battery can body, when describing the prior art in the invention stretching process technical scheme, only the thinning stretching is mentioned, and the forming stretching is not mentioned. This is understandable to those skilled in the art and is also the expression allowed by the Patent Law.

[0020] 2. In the above-mentioned stretching process scheme, it is preferred that the die is composed of at least two thinning rings, which are coaxially arranged with the step punch, and the inner diameters of the at least two thinning rings are arranged to decrease in sequence along the punching direction. The two thinning rings actually realize the secondary stretching process in one stretching action, which is less likely to cause stretching fracture than one thinning ring, thereby improving the stretching yield. In practical applications, the number of thinning rings can be determined based on many factors such as the geometric size of the battery can body, material properties, material thickness, and yield control.

[0021] 3. In the above-mentioned stretching process scheme, it is preferred that the ratio of the wall thickness of the thinned part after thinning by the thinning ring corresponding to the thick rod segment to the diameter of the thick rod segment is 1:30. This requirement not only helps to optimize the stretching of the battery can body, but also further highlights the advantages of the variable wall thickness battery can body, and controls the battery can body to be easily elastically demoulded after the variable wall thickness position stretching.

[0022] 4. In the above-mentioned stretching process scheme, it is preferred that the step punch is provided with a gas delivery hole along the central axis, and the gas delivery hole is connected to a compressed gas device; in variable wall thickness stretching, after the step punch completes the stretching action, the compressed gas device outputs gas to the bottom of the thinned part through the gas delivery hole to demould the thinned part.

[0023] 5. In the above-mentioned stretching process scheme, the punching equipment can be a punch press, or a stretching machine, or other mechanical equipment and hydraulic equipment that can achieve a stretching stroke. Among them, the stretching machine can be a horizontal stretching machine or a vertical stretching machine. The step punch of the horizontal stretching machine realizes the stretching action in the horizontal direction, and the step punch of the vertical stretching machine realizes the stretching action in the vertical direction. In order to ensure the accuracy of the stretching action, a punch guide device can also be set on the stretching machine to guide the step punch to stretch along the stretching direction.

[0024] 6. In the above-mentioned stretching process scheme, the ratio of the radius difference between the thick rod segment and the thin rod segment to the projection length of the conical surface or curved surface in the axial direction is less than 0.2 in order to control the slope of the transition conical surface and / or the curvature of the transition curved surface. This requirement mainly depends on the size and material properties of the battery can body. If the projection length of the conical surface or curved surface in the axial direction is too long, the beneficial effect of the step structure will be weakened, and the material saving will be insufficient; if the projection length is too short, the resistance to thinning and stretching will be large, which is easy to cause tensile fracture, directly leading to an increase in the defective rate.

[0025] 8. In the above-mentioned stretching process, in order to ensure the stretching quality and production efficiency during the variable wall thickness stretching process, the punching speed of the step punch is less than 400 times per minute.

[0026] The design principle and beneficial effects of the present invention are:

[0027] The present invention is specially designed with variable wall thickness stretching in the battery can body stretching process. Variable wall thickness stretching belongs to thinning stretching. When the sheet or plate is stretched at least once to obtain a cup-shaped stretching piece, it is then subjected to thinning stretching, especially variable wall thickness stretching using a step punch and at least one thinning ring to finally obtain a variable wall thickness battery can body with a thin wall in the middle section and thick wall at one or both axial ends. This variable wall thickness battery can body can reduce the amount of material used on the one hand, and can also ensure the sealing strength of one or both ends of the can body on the other hand.

[0028] Due to the application of the above technical solution, the present invention has the following advantages and effects compared with the prior art:

[0029] 1. Compared with the existing cold-pressing process for preparing battery can bodies, the present invention solves the contradiction between the amount of material used and the strength of the roll-sealing caused by the thickness of the battery can body. Existing battery cans all use can bodies with equal wall thickness. When one or both ends of the can body and the can lid are sealed by the roll-sealing process, in order to ensure the strength of the can body end closure, the can body wall thickness can only meet certain thickness requirements, and the wall thickness of the middle section of the can body can only meet the requirements of the ends. However, from the perspective of the thickness requirements of the middle section of the can body itself, it can be further thinned, but due to the limitations of process technology, the effect of saving materials cannot be achieved. The present invention uses a variable wall thickness stretching process to break through this limitation, thereby solving this contradiction well.

[0030] 2. In the variable wall thickness stretching, the present invention creatively designs a step punch used as a punch for the battery can body: the step punch includes a thick rod segment, at least one of the two axial ends of the thick rod segment is connected with a thin rod segment, and the thin rod segment corresponds to the axial end of the can body to be stretched. Through reverse extrusion stretching, a thick wall segment is formed at the top and / or bottom of the battery can body, and a thin wall segment is formed in the middle of the battery can body.

[0031] This technical feature has a significant effect. First, the connection method between the battery can body and the can cover produced by the stretching process of the present invention can be applied to the rolling process (equivalent to the rolling of the can body and the cover of the can). Compared with the welding seal in the prior art, the rolling seal is not only highly reliable, but also saves the arrangement space of the battery can, which is beneficial to improve the space utilization rate in the battery pack. Secondly, compared with the conventional can body with equal wall thickness, the variable wall thickness can body obtained by the stretching process of the present invention has a thick wall section at the end and a thin wall section in the middle, which can not only effectively avoid the tearing of the can end during the rolling process, but also effectively improve the reliability during use. Secondly, the thin-wall section of the can body can effectively reduce the material used, thereby reducing the material cost, and is also beneficial to reduce the weight of the can body and increase the internal volume of the can body, thereby improving the energy density of the overall battery pack.

[0032] 3. In the present invention, the arrangement of multiple thinning rings can improve production efficiency and reduce equipment costs, and the design of multiple thinning rings is also generally applicable to metal can materials with different ductility properties.

[0033] 4. In the present invention, the process and structural restrictions of matching the step punch with the thinning ring size are designed, which not only helps to further highlight the advantages of the variable wall thickness battery can body, but also helps to control the elastic demoulding of the battery can body.

[0034] 5. In the present invention, preferably, a gas delivery hole is provided on the punch along the central axis thereof, and the gas delivery hole is connected to a compressed gas device for ventilation after the stretching action is completed, so as to achieve air-assisted elastic demoulding with good demoulding effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Attached Figure 1 It is a schematic structural diagram of a first punching machine equipped with a punching die in the present invention;

[0036] Attached Figure 2 It is a schematic diagram of the structure of a second punching machine equipped with a punching die in the present invention;

[0037] Attached Figure 3 It is a schematic diagram of the structure of a stretching machine equipped with a punch die in the present invention;

[0038] Attached Figure 4 It is a structural schematic diagram of the step punch in the present invention;

[0039] Attached Figure 5 for Figure 4 A partial enlarged view of

[0040] Attached Figure 6 It is a schematic diagram of the structure of the sheet material during the process of forming the battery can body of the present invention;

[0041] Attached Figure 7 It is a structural schematic diagram of the cup punching member in the process of forming the battery can body of the present invention;

[0042] Attached Figure 8 It is a structural schematic diagram of the re-drawing member in the process of forming the battery can body of the present invention;

[0043] Attached Fig. 9 It is a schematic structural diagram of the thinned parts during the formation of the battery can body of the present invention.

[0044] In the above drawings: 1. First punch; 2. Sheet material; 3. Cup punch; 4. First punch die; 5. Second punch; 6. Redrawn piece; 7. Second punch die; 8. Stretching machine; 9. Thinning piece; 10. Step punch; 11. Thin rod section; 12. Thick rod section; 13. Conical surface; 14. Thinning ring; 15. Punch guide; 16. Thin wall section; 17. Thick wall section. DETAILED DESCRIPTION

[0045] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0046] Embodiment: A battery can body stretching process

[0047] Please refer to the attached Figure 1 To Attachment Fig. 9 A battery can body stretching process is used to stretch a variable wall thickness can body suitable for end sealing, that is, the can body has a thin wall section 16 in the middle axial direction and thick wall sections 17 at both ends. The process includes the following stretching steps:

[0048] The first step: cup punching (this step belongs to forming and stretching), such as Figure 1 , Figure 6 and Figure 7 As shown, the sheet material 2 is punched and formed by a first punching machine 1 through a first punching die 4 to obtain a cup-shaped punched cup part 3.

[0049] Step 2: Re-draw (this step belongs to forming stretching), such as Figure 2 , Figure 7 and Figure 8 As shown, the cup part 3 is punched and formed by a second punch press 5 through a second die 7 to obtain a cup-shaped re-drawn part 6, the inner diameter of which is smaller than the inner diameter of the cup part 3, and the height of which is greater than the height of the cup part 3.

[0050] The third step: thinning (this step belongs to variable wall thickness stretching in thinning stretching), such as Figure 3 , Figure 8 and Fig. 9 As shown, the re-drawn part 6 is subjected to variable wall thickness stretching by a stretching machine 8 through a step punch 10 used as a punch and three thinning rings 14 used as a die to obtain a thinned part 9; the three thinning rings 14 are coaxially arranged with the step punch 10, respectively, and in the thinning step, the step punch 10 sequentially passes through each thinning ring 14. In this embodiment, the punching speed of the step punch 10 is less than 400 times per minute.

[0051] like Figure 4 and Figure 5 As shown, the main body of the step punch 10 is a cylinder, and the step punch 10 has a thick rod segment 12, and thin rod segments 11 are provided at both ends of the thick rod segment 12 in the axial direction. In this embodiment, the difference between the radius of the thick rod segment 12 and the radius of the thin rod segment 11 is less than or equal to 0.3 mm, and the radius ratio of the two is less than or equal to 101:100. The thin rod segment 11 and the thick rod segment 12 are transitioned by at least one conical surface 13 (this embodiment uses one conical surface 13, or two conical surfaces), and the ratio of the radius difference between the thick rod segment 12 and the thin rod segment 11 to the axial projection length of the conical surface 13 is less than 0.2.

[0052] The three thinning rings 14 are coaxially arranged with the step punch 10, and the inner diameters of the three thinning rings 14 are arranged to decrease in sequence along the punching direction. The difference between the inner diameter of the thinning ring 14 and the diameter of the thick rod section 12 of the step punch 10 is less than twice the wall thickness of the can body to be thinned.

[0053] like Fig. 9 As shown, during the variable wall thickness stretching process, the step punch 10 drives the stretched part to pass through each thinning ring 14 in sequence, and then demolds to obtain a thinned part 9. The thinned part 9 includes a thin-walled section 16 corresponding to the thick rod section 12 of the step punch 10 and a thick-walled section 17 corresponding to the thin rod section 11 of the step punch 10. The thick-walled section 17 is located at both ends of the thinned part 9 in the axial direction, and there is a conical transition between the thin-walled section 16 and the thick-walled section 17. In this embodiment, the ratio of the wall thickness of the thinned part 9 after thinning by the thinning ring 14 corresponding to the thick rod section 12 to the diameter of the thick rod section 12 is 1:30. In this embodiment, the raw material of the battery can body is aluminum alloy, specifically aluminum alloy sheet or aluminum alloy plate.

[0054] like Figure 3 As shown, in this embodiment, the stretching machine 8 is a horizontal stretching machine, and the step punch 10 is stretched in the horizontal direction. The stretching machine 8 is also provided with a punch guide device 15 to guide the step punch 10 to stretch in the horizontal direction.

[0055] In this embodiment, a gas delivery hole is provided on the step punch 10 along the central axis, and the gas delivery hole is connected to a compressed gas device. In the variable wall thickness stretching, after the step punch 10 completes the stretching action, the compressed gas device outputs gas to the bottom of the thinning part 9 through the gas delivery hole to demold the thinning part 9.

[0056] The following is an explanation of other implementations and structural changes of the present invention:

[0057] 1. In the above embodiments, a conical surface transition is provided between the thin-walled section 16 and the thick-walled section 17. However, the present invention is not limited thereto, and two or three conical surfaces may be used for transition, one or two curved surfaces may be used for transition, or even a combination of a conical surface and a curved surface may be used for transition. These changes may be determined and selected according to specific circumstances, which are easily understood and accepted by those skilled in the art.

[0058] 2. In the above embodiment, the punching speed of the step punch 10 is less than 400 times per minute. However, the present invention is not limited thereto, and the punching speed of the step punch 10 can be set to be greater than or equal to 400 times per minute. However, whether the production efficiency can be improved in this way depends on whether the stretching effect and the yield rate can meet the corresponding requirements.

[0059] 3. In the above embodiment, three thinning rings 14 are used to form the concave mold, but the present invention is not limited to this. Theoretically, at least one thinning ring 14 is used, preferably two thinning rings 14 are used, and in this embodiment, three thinning rings 14 are used as the best. A larger number of thinning rings can also be used. In practical applications, the number of thinning rings can be determined based on many factors such as the geometric size of the battery can body, material properties, material thickness, and yield control. This is understandable and acceptable to those skilled in the art.

[0060] 4. In the above embodiments, the raw material of the battery can body is preferably aluminum alloy, such as aluminum alloy sheet or aluminum alloy plate, or aluminum alloy ingot. However, the present invention is not limited to the selection of aluminum alloy as the raw material, and other materials may also be selected, such as stainless steel, copper, copper alloy and other metal materials suitable for stretching.

[0061] 5. In the above embodiments, the "first punch" and the "second punch" are two punches, but the present invention is not limited thereto. The "first punch" and the "second punch" can also be the same punch. In this case, when implemented, the first punch die can be installed on the punch first, the sheet material can be punched to form a cup-shaped punched cup part, and then the first punch die can be removed, and the second punch die can be installed on the punch, and the punched cup part can be punched to form a re-drawn part with a smaller diameter; or a progressive die can be used on the same punch. This is easy to understand and accept by those skilled in the art.

[0062] 6. In the above embodiments, thin rod segments are connected to both ends of the thick rod segment of the step punch in the axial direction, and correspondingly, thick wall segments are provided at both ends of the thinning member, but the present invention is not limited thereto. The thin rod segment can also be provided at only one end of the thick rod segment of the step punch in the axial direction, and the corresponding end of the thinning member forms a thick wall segment, which is easily understood and accepted by those skilled in the art.

[0063] 7. In the above embodiments, the stretching machine is a horizontal stretching machine, and the stretching action of the step punch is arranged in the horizontal direction. However, the present invention is not limited to this. For example, the stretching machine can also be a vertical stretching machine, and accordingly, the stretching action of the step punch is arranged in the vertical direction, but this vertical stretching machine has a higher requirement for the space height of the machine platform. This is easy to understand and accept by those skilled in the art.

[0064] 8. In the above embodiment, the battery can body can be formed by sequentially passing through a cupping step, a re-drawing step and a thinning step. However, the present invention is not limited to this. The battery can body stretching process of the present invention may include multiple re-drawing steps and multiple thinning steps. In the present invention, the cupping step belongs to forming stretching, and the re-drawing step also belongs to forming stretching. The forming stretching refers to the stretching process of changing the stretched piece from a sheet into a cup-shaped stretched piece (usually called "cupping"), and the forming stretching also includes the stretching process of changing the cup diameter and cup length. The essence of forming stretching is mainly to make a relatively variable stretching for the shape and outer dimensions of the stretched piece. In the present invention, the thinning step belongs to thinning stretching, and the thinning step in the above embodiment is essentially variable wall thickness stretching. In fact, in this embodiment, equal wall thickness thinning stretching can also be arranged, and the stretching can be arranged before the variable wall thickness stretching step, and even the equal wall thickness thinning stretching can be arranged between two forming stretching steps. In fact, the order of forming stretching and thinning stretching is relatively flexible, except that the first stretching should be forming stretching, and the remaining stretching order can even be arranged alternately with the re-drawing step and the thinning step. In practice, it can be confirmed based on parameters such as material properties, shape and size of the object being stretched, etc., which are all existing technologies known to those skilled in the art.

[0065] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A punch for stretching the battery can body, Features: The punch is a step punch (10), the main body of which is a cylinder. The step punch (10) has a thick rod section (12), and thin rod sections (11) are provided at two axial ends of the thick rod section (12). The difference between the radius of the thick rod section (12) and the radius of the thin rod section (11) is less than or equal to 0.3 mm, and the ratio of the two radii is less than or equal to 101:100; the thin rod section (11) and the thick rod section (12) are transitioned by at least one conical surface (13) or / and a curved surface, and the ratio of the radius difference between the thick rod section (12) and the thin rod section (11) to the axial projection length of the conical surface (13) or / and the curved surface is less than 0.

2.

2. A battery can body stretching die, the die consisting of a male die and a female die, Features: The punch is composed of a step punch (10), the main body of the step punch (10) is a cylinder, the step punch (10) has a thick rod section (12), and thin rod sections (11) are provided at both ends of the thick rod section (12) in the axial direction, the difference between the radius of the thick rod section (12) and the radius of the thin rod section (11) is less than or equal to 0.3 mm, and the ratio of the two radii is less than or equal to 101:100; the thin rod section (11) and the thick rod section (12) are transitioned through at least one conical surface (13) or / and a curved surface, and the ratio of the radius difference between the thick rod section (12) and the thin rod section (11) to the axial projection length of the conical surface (13) or / and the curved surface is less than 0.2; The die is composed of at least two thinning rings (14), the at least two thinning rings (14) are coaxially arranged with the step punch (10), and the inner diameters of the at least two thinning rings (14) are arranged to decrease in sequence along the punching direction; the difference between the inner diameter of the thinning ring (14) and the diameter of the thick rod section (12) of the step punch (10) is less than twice the wall thickness of the can body to be thinned; and the ratio of the wall thickness of the thinned part (9) corresponding to the thick rod section (12) after being thinned by the thinning ring (14) to the diameter of the thick rod section (12) is 1:

30.

3. A battery can body stretching process, comprising thinning and stretching, wherein the number of thinning and stretching is at least one, Features: The thinning and stretching includes at least one wall thickness changing stretching for the thin-walled section (16) and the thick-walled section (17) of the can body, and the wall thickness changing stretching is performed by using a stamping device (8) through the following dies: The die is composed of a punch and a die, the punch is composed of a step punch (10), the main body of the step punch (10) is a cylinder, the step punch (10) is provided with a thick rod segment (12), thin rod segments (11) are provided at two axial ends of the thick rod segment (12), the difference between the radius of the thick rod segment (12) and the radius of the thin rod segment (11) is less than or equal to 0.3 mm, and the ratio of the two radii is less than or equal to 101:100; the thin rod segment (11) and the thick rod segment (12) are transitioned by at least one conical surface (13) or / and a curved surface, and the ratio of the radius difference between the thick rod segment (12) and the thin rod segment (11) to the axial projection length of the conical surface (13) or / and the curved surface is less than 0.2; The die is composed of at least two thinning rings (14), the at least two thinning rings (14) are coaxially arranged with the step punch (10), and the inner diameters of the at least two thinning rings (14) are arranged to decrease in sequence along the punching direction; the difference between the inner diameter of the thinning ring (14) and the diameter of the thick rod section (12) of the step punch (10) is less than twice the wall thickness of the can body to be thinned; the ratio of the wall thickness of the thinned part (9) corresponding to the thick rod section (12) after being thinned by the thinning ring (14) to the diameter of the thick rod section (12) is 1:30; During the variable wall thickness stretching process, the step punch (10) drives the stretched part to pass through each thinning ring (14) in sequence, and then demoulds to obtain a thinned part (9); The thinning member (9) comprises a thin-walled section (16) corresponding to the thick rod section (12) of the step punch (10) and a thick-walled section (17) corresponding to the thin rod section (11) of the step punch (10), the thick-walled section (17) being located at two axial ends of the thinning member (9), and at least one conical surface or / and curved surface transition is provided between the thin-walled section (16) and the thick-walled section (17).

4. The battery can body stretching process according to claim 3, Features: The step punch (10) is provided with a gas delivery hole axially extending along the central axis, the gas delivery hole being connected to a compressed gas device; during variable wall thickness stretching, after the step punch (10) completes the stretching action, the compressed gas device outputs gas to the bottom of the thinned part (9) through the gas delivery hole, so as to demould the thinned part (9).

5. The battery can body stretching process according to claim 3, Features: The raw material of the battery can body is aluminum alloy.

6. The battery can body stretching process according to claim 5, Features: The raw material of the battery can body is aluminum alloy sheet or aluminum alloy plate.