Lithium-ion secondary battery

By forming a carbon compound coating layer containing acidic functional groups on the surface of the positive electrode active material particles of the lithium-ion secondary battery, and using a polar solvent with a high dielectric constant in the non-aqueous electrolyte, the insufficient load characteristics of the lithium-ion secondary battery are solved. The problem is that more efficient lithium-ion embedding and deintercalation is achieved, improving battery performance.

CN112262492BActive Publication Date: 2024-11-05MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980039335.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-13
Filing Date
2019-05-31
Publication Date
2024-11-05
Estimated Expiration
2039-05-31

AI Technical Summary

Technical Problem

The existing lithium-ion secondary batteries have shortcomings in improving load characteristics, especially due to the electrical conductivity and wetting properties of olivine lithium phosphate, which leads to the inadequate improvement of load characteristics.

Method used

The coating layer containing carbon compounds is formed on the surface of the positive electrode active material particles, and an acid functional group is added to the coating layer. A polar solvent with a relative dielectric constant of 20 or more is used in the non-aqueous electrolyte is formed to improve electron conduction and wettability to improve load characteristics.

Benefits of technology

Through this method, the load characteristics of the lithium-ion secondary battery are significantly improved, the DC resistivity is reduced, and the intercalation and deintercalation efficiency of lithium ions is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112262492B_ABST
    Figure CN112262492B_ABST
Patent Text Reader

Abstract

A lithium ion secondary battery (100) comprises: a positive electrode (11) having a positive electrode active material capable of inserting and removing lithium ions; a negative electrode (12) having a negative electrode active material capable of inserting and removing lithium ions; a separator (13) disposed between the positive electrode (11) and the negative electrode (12); and a non-aqueous electrolyte (14) comprising a polar solvent having a relative dielectric constant of 20 or more. A coating layer comprising a carbon compound is formed on the surface of positive electrode active material particles constituting the positive electrode active material, and the coating layer comprises an acidic functional group. The amount of the acidic functional group in the composite composed of the positive electrode active material and the coating layer is 0.004 mmol / g or more and 0.0062 mmol / g or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium ion secondary battery. Background Art

[0002] Lithium ion secondary batteries are widely used as power sources for small electronic devices and power sources for driving vehicles, for example, due to their high energy density.

[0003] As one of such lithium ion secondary batteries, a lithium ion secondary battery using olivine-type lithium phosphate as a positive electrode active material is disclosed in Patent Document 1. In addition, Patent Document 1 describes the following: In view of the poor electronic conductivity of olivine-type lithium phosphate, a carbon composite of olivine-type lithium phosphate is used as a positive electrode active material, and the thickness of the positive electrode active material layer is optimized, thereby achieving a balance between load characteristics and battery capacity.

[0004] Patent Document 2 describes a lithium ion secondary battery in which a conductive path composed of carbon is constructed inside positive electrode active material particles containing olivine-type lithium phosphate in order to improve the conductivity of olivine-type lithium phosphate.

[0005] Patent Document 1: Japanese Patent No. 3997702

[0006] Patent Document 2: Japanese Patent Application Publication No. 2003-203628 Summary of the invention

[0007] However, as in the lithium ion secondary battery described in Patent Document 1, simply optimizing the thickness of the positive electrode active material layer does not change the conductivity of each positive electrode active material particle, so there is still room for improvement in load characteristics.

[0008] In addition, in Patent Document 2, there is no description of the detailed state of carbon constituting the conductive path, so it is unclear whether the conductive path is sufficient. Therefore, when the conductive path constructed inside the positive electrode active material particle is insufficient, it cannot be said that the load characteristics are sufficiently improved.

[0009] In addition, it is known that when the wettability of nonaqueous electrolyte to positive electrode active material is poor, the load characteristic decreases. However, in patent documents 1 and 2, the wettability of nonaqueous electrolyte to positive electrode active material is not considered at all, and it can be considered that if only the necessary conditions shown in patent documents 1 and 2 are met, sufficient load characteristics may not be obtained sometimes.

[0010] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a lithium ion secondary battery capable of improving load characteristics.

[0011] The lithium ion secondary battery of the present invention is characterized by comprising:

[0012] A positive electrode having a positive electrode active material capable of inserting and extracting lithium ions;

[0013] A negative electrode having a negative electrode active material capable of inserting and extracting lithium ions;

[0014] a separator, disposed between the positive electrode and the negative electrode; and

[0015] A non-aqueous electrolyte comprising a polar solvent having a relative dielectric constant of 20 or more;

[0016] A coating layer containing a carbon compound is formed on the surface of the positive electrode active material particles constituting the positive electrode active material, and the coating layer contains an acidic functional group.

[0017] The amount of the acidic functional group in the composite composed of the positive electrode active material and the coating layer is 0.004 mmol / g or more and 0.0062 mmol / g or less.

[0018] The coating layer may account for 0.1 wt % or more and 5 wt % or less in the composite.

[0019] In addition, the specific surface area of ​​the composite can be 9.0 m 2 / g or above.

[0020] The positive electrode active material may be a material having a chemical formula of Li x M y P z O 4-δ (Among them, 0.5 <x / y<1.5,y / z> 1, δ is the oxygen deficiency amount, and M contains at least one of Fe, Mn, Co and Ni).

[0021] According to the present invention, a coating layer containing a carbon compound is formed on the surface of the positive electrode active material particles, and an acidic functional group is included in the coating layer, the amount of the acidic functional group in the composite composed of the positive electrode active material and the coating layer is 0.004mmol / g or more and 0.0062mmol / g or less, and the non-aqueous electrolyte contains a polar solvent with a relative dielectric constant of 20 or more, and the coating layer containing a carbon compound can be used to improve the electronic conductivity and improve the wettability of the non-aqueous electrolyte to the positive electrode active material. Thus, the load characteristics of the lithium ion secondary battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a cross-sectional view of a lithium ion secondary battery in one embodiment of the present invention. DETAILED DESCRIPTION

[0023] Hereinafter, embodiments of the present invention will be shown, and features of the present invention will be described in more detail.

[0024] Hereinafter, a lithium ion secondary battery will be described as an example. The lithium ion secondary battery has a structure in which a stacked body formed by alternately stacking a plurality of positive electrodes and negative electrodes with separators interposed therebetween and a non-aqueous electrolyte are accommodated in an outer casing.

[0025] Figure 1 1 is a cross-sectional view of a lithium ion secondary battery 100 in one embodiment of the present invention. The lithium ion secondary battery 100 has a structure in which a stacked body 10 and a non-aqueous electrolyte 14 are accommodated in a laminated case 20, wherein the stacked body 10 is formed by alternately stacking a plurality of positive electrodes 11 and negative electrodes 12 with a separator 13 interposed therebetween. That is, the lithium ion secondary battery 100 includes a positive electrode 11, a negative electrode 12, a separator 13, and a non-aqueous electrolyte 14.

[0026] The laminate case 20 as an exterior body is formed by thermally and press-bonding peripheral edges of a pair of laminate films 20 a and 20 b to each other.

[0027] The nonaqueous electrolyte 14 accommodated in the laminate case 20 contains a polar solvent having a relative dielectric constant of 20 or more. As the nonaqueous electrolyte 14 containing a polar solvent having a relative dielectric constant of 20 or more, for example, a nonaqueous electrolyte solution containing ethylene carbonate having a relative dielectric constant of 90 can be used.

[0028] The positive terminal 16a is led out from one end of the laminate case 20, and the negative terminal 16b is led out from the other end. The plurality of positive electrodes 11 are connected to the positive terminal 16a via the lead 15a. In addition, the plurality of negative electrodes 12 are connected to the negative terminal 16b via the lead 15b.

[0029] The positive electrode 11 has a positive electrode active material capable of inserting and removing lithium ions. More specifically, the positive electrode 11 has a positive electrode composite material layer containing the positive electrode active material and a positive electrode collector. The positive electrode composite material layer is formed on both sides of the positive electrode collector. The positive electrode collector is, for example, a metal foil such as aluminum.

[0030] The positive electrode active material is, for example, Li x M y P z O 4-δ(Among them, 0.5 <x / y<1.5,y / z> 1, δ is the oxygen deficiency, and M contains at least one of Fe, Mn, Co and Ni). As such an olivine-type lithium phosphate compound, for example, lithium iron phosphate (LiFePO4 (also referred to as LFP)) can be used. Among them, a part of the Fe site of LiFePO4 can be replaced by at least one element selected from the group consisting of Mg, Ca, Ti, Cr, Zr, Zn and Nb. In addition, a part of the Li site can be replaced by Na, and a part of the P site can be replaced by Si.

[0031] The positive electrode composite material layer may contain a conductive aid and a binder in addition to the positive electrode active material. The positive electrode active material is preferably contained in the positive electrode composite material layer in a ratio of 50 wt % or more and 99 wt % or less.

[0032] In this embodiment, a coating layer containing a carbon compound is formed on the surface of the positive electrode active material particles constituting the positive electrode active material. The coating layer contains an acidic functional group. In addition, a composite of the positive electrode active material (hereinafter referred to as a composite) is formed by the positive electrode active material and the coating layer.

[0033] However, the entire surface of the positive electrode active material particle does not need to be covered with the coating layer. In addition, the coating layer may contain, for example, carbon having no acidic functional group.

[0034] The composite can be prepared, for example, by heating a mixture obtained by mixing the constituent material of the positive electrode active material and a carbohydrate having a reducing property in an inert atmosphere. In addition, when the mixture is heat-treated, the heat treatment environment, heating temperature, heating time, etc. are adjusted in order to obtain a carbon compound containing an acidic functional group after the heat treatment. As carbohydrates having a reducing property, for example, sugars such as glucose, fructose, sucrose, and dextrin, cellulose, and carbohydrates having reducing functional groups such as aldehyde groups and ketone groups can be used.

[0035] The type of the acidic functional group is not particularly limited, but is preferably at least one selected from the group consisting of a carboxyl group, a hydroxyl group, a carbonyl group, and a quinone group.

[0036] In the present embodiment, the amount of the acidic functional group in the composite composed of the positive electrode active material and the coating layer is greater than 0.004mmol / g and less than 0.0062mmol / g. By constituting the amount of the acidic functional group to meet the above-mentioned necessary conditions, and containing a polar solvent with a relative dielectric constant of greater than 20 in the non-aqueous electrolyte 14, it is possible to take into account both improving the electronic conductivity by including a coating layer of a carbon compound and promoting the insertion and extraction of lithium ions by improving the wettability of the non-aqueous electrolyte 14 to the positive electrode active material. As a result, compared with the existing lithium ion secondary battery that does not have the above-mentioned structure, in the lithium ion secondary battery 100 in the present embodiment, the load characteristics are improved.

[0037] Here, a coating layer composed of carbon containing no acidic functional groups is formed on the surface of the positive electrode active material particles, that is, a coating layer that does not meet the necessary conditions of the present invention is examined. In this case, it can be considered that compared with a structure in which no carbon is attached to the positive electrode active material particles, the electron conductivity is improved by attaching carbon, but since the positive electrode active material particles are covered with carbon containing no acidic functional groups, lithium ions cannot be smoothly embedded and released based on the positive electrode active material.

[0038] However, according to the lithium ion secondary battery 100 in this embodiment, by forming a coating layer containing a carbon compound having an acidic functional group on the surface of the positive electrode active material particles, and making the content of the acidic functional group the above-mentioned amount, and containing a polar solvent with a relative dielectric constant of 20 or more in the non-aqueous electrolyte 14, it is possible to take into account both improving the electronic conductivity and improving the wettability of the non-aqueous electrolyte 14 for the positive electrode active material.

[0039] In addition, the proportion of the coating layer in the composite is preferably 0.1% by weight or more and 5% by weight or less. By making the proportion of the coating layer in the composite be 0.1% by weight or more and 5% by weight or less, an electronic conduction network via the coating layer can be efficiently formed, reducing the lithium diffusion distance inside the positive electrode active material with high resistance, thereby improving the load characteristics of the lithium ion secondary battery 100. In order to further reduce the lithium diffusion distance inside the positive electrode active material and further improve the load characteristics, the proportion of the coating layer in the composite is more preferably 1% by weight or more and 2% by weight or less.

[0040] The specific surface area of ​​the composite is preferably 9.0 m 2 / g or more. By making the specific surface area of ​​the composite 9.0m 2 / g or more, the lithium diffusion distance inside the positive electrode active material can be reduced, and the load characteristics can be improved. In order to further reduce the lithium diffusion distance inside the positive electrode active material and further improve the load characteristics, the specific surface area of ​​the composite is more preferably 10m 2 / g or more and 13m2 / g or less.

[0041] The negative electrode 12 has a negative electrode active material capable of inserting and removing lithium ions. More specifically, the negative electrode 12 has a negative electrode composite material layer containing the negative electrode active material and a negative electrode collector. The negative electrode composite material layer is formed on both sides of the negative electrode collector.

[0042] The type of negative electrode active material is not particularly limited, and for example, carbon compounds such as graphite, hard carbon and soft carbon, lithium titanate or a material having MO x (Wherein, M is at least one element selected from the group consisting of Ti, Si, Sn, Cr, Fe and Mo, and x is a value in the range of 0.9≤x≤2.0.) An alloy-based substance of at least one selected from the group consisting of metal oxides, silicon, silicon oxides, silicon-containing alloys, silicon-containing compounds, tin, tin oxides, tin-containing alloys and tin-containing compounds.

[0043] The negative electrode current collector is, for example, a metal foil such as copper. The negative electrode composite material layer may contain a conductive aid and a binder in addition to the negative electrode active material.

[0044] The separator 13 is interposed between the positive electrode 11 and the negative electrode 12. The separator 13 is not particularly limited, and various separators that can be used for lithium ion secondary batteries can be used. Figure 1 The diaphragm 13 shown has a bag-like shape, but it may also have a sheet-like shape or a meandering shape.

[0045] <Example>

[0046] (Determination of the amount of acidic functional groups)

[0047] As a positive electrode active material, a lithium iron phosphate powder (hereinafter referred to as LFP powder) is prepared in which a coating layer containing a carbon compound having an acidic functional group is formed on the surface of the lithium iron phosphate particles. The average particle size D50 of the lithium iron phosphate particles as a composite having a coating layer formed on the surface is greater than 1 μm and less than 11 μm, and the specific surface area is 10 m 2 / g or more and 12m 2 / g or less.

[0048] The amount of acidic functional groups contained in the coating layer of the prepared LFP powder was measured by back titration. Back titration is a method in which LFP powder is mixed with an alkaline solution of known concentration, and the amount of reacted alkaline solution is determined by titrating the LFP powder and the unreacted alkaline solution with an acidic solution, and the amount of acidic functional groups is determined based on the amount of reacted alkali.

[0049] Specifically, 3 g of LFP powder was weighed in a container, and stabilized for more than 6 hours in a constant temperature and humidity chamber at a temperature of 25°C and a humidity of 50%. Then, 30 ml of a solution was added and sealed. The solution was prepared by mixing pyridine at a ratio of 0.01 mol / L in methyl isobutyl ketone (MIBK) as an alkaline solution, and ultrasonic dispersion was performed for 1 hour using an ultrasonic cleaner. The dispersion was centrifuged, 10 ml of the separated supernatant was diluted with MIBK, and titrated with a MIBK solution containing 0.01 mol / L perchloric acid. Based on the amount of pyridine consumed by the acidic functional groups on the surface of LFP, the amount of acidic functional groups in the composite (acid point amount) and the amount of acidic functional groups in the coating layer (acid point amount) were calculated.

[0050] It should be noted that, based on the amount of lithium iron phosphate when making LFP powder as a composite, the amount of positive electrode active material in the composite and the amount of coating layer in the composite can be calculated in advance. That is, if the amount of acidic functional groups in the composite can be calculated, the amount of acidic functional groups in the coating layer can also be calculated.

[0051] As shown in Table 1 described below, seven types of LFP powders having different amounts of acidic functional groups and carbon compounds in the composite were prepared, and seven types of batteries for evaluating load characteristics were prepared by the method described below.

[0052] (Production of positive electrode)

[0053] Next, in addition to the above-mentioned LFP powder, acetylene black (AB) was prepared as a conductive additive, and polyvinylidene fluoride (PVdF) was prepared as a binder, and they were dispersed in N-methyl-2-pyrrolidone (NMP) at a weight ratio of LFP powder:AB:PVdF of 85:10:5 to prepare a positive electrode slurry.

[0054] The positive electrode slurry was uniformly applied to both sides of a 20 μm thick strip-shaped aluminum foil using a die coater and dried. Then, the slurry was compacted to 2.0 g / cm using a roll press. 3 The density was then cut into 50 mm × 50 mm sizes to produce a positive electrode. The thickness of the positive electrode composite material layer was about 25 μm.

[0055] (Production of negative electrode)

[0056] Next, natural graphite was prepared as a negative electrode active material, and PVdF was prepared as a binder. These were dispersed in N-methyl-2-pyrrolidone (NMP) at a weight ratio of natural graphite:PVdF of 95:5 to prepare a negative electrode slurry.

[0057] The prepared negative electrode slurry was evenly coated on both sides of a 15 μm thick strip-shaped copper foil using a die coater and dried. It should be noted that the coating amount of the negative electrode slurry was adjusted so that the negative electrode capacity was 1.8 times the positive electrode capacity. Then, a roller press was used to compact it to 1.3 g / cm 3 The density was then cut into a size of 52 mm × 52 mm to produce a negative electrode. The thickness of the negative electrode composite material layer was about 25 μm.

[0058] (Preparation of Electrolyte)

[0059] Next, a mixed solvent of ethylene carbonate (EC) with a relative dielectric constant of 90 and ethyl methyl carbonate (EMC) with a relative dielectric constant of 2.8 in a volume ratio of EC:EMC=25:75 was prepared. Then, 1 mol of lithium hexafluorophosphate (LiPF6) was dissolved per liter of the prepared mixed solvent, and vinylene carbonate (VC) was further added to prepare a non-aqueous electrolyte. The amount of vinylene carbonate added was adjusted so that its proportion relative to the entire non-aqueous electrolyte prepared was 1.0 weight %.

[0060] (Battery production)

[0061] A plurality of positive electrodes and negative electrodes prepared by the above method were alternately stacked with separators interposed therebetween to prepare a stacked battery element. A microporous polypropylene film having a thickness of 20 μm was used as the separator.

[0062] Next, the current collecting lead for connecting to the external connection wire is ultrasonically welded to the manufactured battery element. Then, the battery element is housed in a bag-shaped outer casing made of aluminum laminate, which is manufactured by heat-welding three sides. At this time, the current collecting lead protrudes to the outside of the outer casing.

[0063] Finally, 1.6 g of the nonaqueous electrolyte prepared by the above method was injected into the bag-shaped outer body, and then one of the opened sides was closed to seal the bag-shaped outer body, thereby preparing a battery.

[0064] As described above, seven types of batteries shown in Table 1 described below were produced using seven types of LFP powders having different amounts of acidic functional groups in the composite and carbon compounds in the composite.

[0065] (Initial charge and discharge conditions)

[0066] Each of the produced batteries was charged at a constant current of 0.2 CA until the battery voltage reached 3.8 V under a temperature condition of 25° C., and further charged at a constant voltage of 3.8 V for 10 hours.

[0067] Then, the battery was discharged at a constant current of 1 CA at a temperature of 25° C. until the battery voltage reached 2.5V.

[0068] (Aging treatment)

[0069] Each battery was charged at a constant current of 1 CA at 25°C until the battery voltage reached 3.8 V, and then charged at a constant voltage of 3.8 V until the current decayed to 1 / 50 CA. Then, it was aged at 55°C for one week.

[0070] Furthermore, when gas was generated in the outer casing during initial charge and discharge and during aging treatment, a degassing treatment was performed to discharge the gas to the outside of the outer casing.

[0071] (Output characteristics test)

[0072] <Capacity Check>

[0073] Each of the manufactured batteries was charged at a constant current of 1 CA until the battery voltage reached 3.5 V under a temperature condition of 25° C., and further charged at a constant voltage of 3.5 V until the current decayed to 1 / 50 CA.

[0074] Then, the battery was discharged at a constant current of 1 CA at a temperature of 55° C. until the battery voltage reached 2.5 V, and the discharge capacity was determined. The discharge capacity was taken as the battery capacity. The capacity of each battery is shown in Table 1.

[0075] <Load characteristics check>

[0076] Each battery was charged at 25°C until the depth of charge (SOC) reached 50%, and then the DC resistivity was calculated based on the voltage reached when charging at a constant current of 10C for 20 seconds at 0°C. The calculated DC resistivity was then normalized by the total area of ​​the positive electrode as an indicator of load characteristics. For each battery, the DC resistivity (DCR) normalized by the total area of ​​the positive electrode is shown in Table 1.

[0077] [Table 1]

[0078]

[0079] In Table 1, for seven types of batteries having different amounts of acidic functional groups and carbon compounds in the composite, the amount of acidic functional groups in the composite, the amount of carbon compounds in the composite, the direct current resistivity (DCR) of the battery, the resistance evaluation, and the battery capacity are shown. Samples No. 1 to 5 are batteries for evaluation that meet the necessary conditions of the present invention, which are that the amount of acidic functional groups in the composite is greater than 0.004 mmol / g and less than 0.0062 mmol / g. On the other hand, samples No. 6 and 7 marked with * are batteries for comparison that do not meet the necessary conditions of the present invention.

[0080] As shown in Table 1, the DC resistivity of the battery for comparison of sample No. 6, which does not satisfy the requirements of the present invention, is 87 Ωcm 2 The DC resistivity of the battery used for comparison of sample number 7 is 72 Ωcm 2 The DC resistivity of the batteries for evaluation of sample numbers 1 to 5 that satisfy the requirements of the present invention is 68 Ωcm 2 Therefore, the resistance of the evaluation batteries of sample numbers 1 to 5 satisfying the requirements of the present invention was evaluated as "○", and the resistance of the comparative batteries of sample numbers 6 and 7 not satisfying the requirements of the present invention was evaluated as "×".

[0081] That is, a coating layer containing a carbon compound having an acidic functional group is formed on the surface of the positive electrode active material particles, satisfying the necessary condition that the amount of the acidic functional group in the composite is greater than 0.004 mmol / g and less than 0.0062 mmol / g, and a lithium ion secondary battery containing a polar solvent with a relative dielectric constant of greater than 20 in the non-aqueous electrolyte, has a lower DC resistivity and improved load characteristics compared to existing lithium ion secondary batteries that do not satisfy the above-mentioned necessary conditions.

[0082] In addition, although not shown in Table 1, it can be seen that in a battery in which the non-aqueous electrolyte does not contain a solvent with a relative dielectric constant of 20 or more, even when the amount of the acidic functional group in the composite satisfies the necessary condition of being greater than 0.004 mmol / g and less than 0.0062 mmol / g, the wettability of the electrolyte to the positive electrode active material deteriorates and the load characteristics are low.

[0083] That is, by satisfying the following conditions: the amount of the acidic functional group in the composite is greater than 0.004 mmol / g and less than 0.0062 mmol / g, and in addition, the non-aqueous electrolyte contains a polar solvent having a relative dielectric constant of greater than 20, it is possible to improve the electronic conductivity by including a coating layer containing a carbon compound and promote the embedding and de-embedding of lithium ions by improving the wettability of the non-aqueous electrolyte to the positive electrode active material, thereby improving the load characteristics of the lithium ion secondary battery.

[0084] The present invention is not limited to the above-described embodiments, and various applications and modifications are possible within the scope of the present invention.

[0085] In the above-mentioned embodiment, a lithium-ion secondary battery having a structure in which a laminated body formed by alternately stacking a plurality of positive electrodes and negative electrodes across a separator and a non-aqueous electrolyte are contained in an outer casing is used as an example for explanation, but the structure of the lithium-ion secondary battery of the present invention is not limited to the above-mentioned structure. For example, a lithium-ion secondary battery may also be a structure in which a winding body formed by winding a positive electrode and a negative electrode stacked across a separator and a non-aqueous electrolyte are contained in an outer casing. In addition, the outer casing may also be a metal can instead of a laminated shell.

[0086] As a positive electrode active material, the use of an olivine-type lithium phosphate compound is used as an example for explanation, but the positive electrode active material is not limited to an olivine-type lithium phosphate compound. However, when the present invention is applied using an olivine-type lithium phosphate compound as a positive electrode active material, the shortcomings of the olivine-type lithium phosphate compound with high lithium diffusion resistance and low electron conductivity in the particles can be compensated, and the load characteristics can be effectively improved. That is, by attaching a carbon compound to the surface of the olivine-type lithium phosphate compound, the electron conductivity can be improved. At this time, by adopting a structure such as the present invention, it is possible to take into account both improving the electron conductivity and improving the wettability of the non-aqueous electrolyte to the positive electrode active material, thereby effectively improving the load characteristics.

[0087] It should be noted that the amount of the acidic functional group in the composite can be determined not only from the composite used in manufacturing the battery but also from the positive electrode of the manufactured battery. For example, it can be determined by the following method.

[0088] First, the positive electrode composite material layer is peeled off from the positive electrode of the battery to collect the powdered positive electrode powder, and the collected positive electrode powder is added to N-methyl-2-pyrrolidone (NMP) to dissolve and remove the PVdF as a binder. NMP is further added to the powder after the PVdF is removed and centrifuged to separate the conductive additive and the composite, and then the separated composite is used to determine the amount of the acidic functional group. The acidic functional group can be obtained by the above-mentioned back titration method.

[0089] Explanation of symbols

[0090] 10 Laminated body

[0091] 11 Positive electrode

[0092] 12 Negative electrode

[0093] 13 Diaphragm

[0094] 14 Non-aqueous electrolytes

[0095] 20 Laminated Shell

[0096] 100 Lithium-ion secondary battery

Claims

1. A lithium ion secondary battery, characterized in that: have: A positive electrode having a positive electrode active material capable of inserting and extracting lithium ions; A negative electrode having a negative electrode active material capable of inserting and extracting lithium ions; a separator, disposed between the positive electrode and the negative electrode; and A non-aqueous electrolyte comprising a polar solvent having a relative dielectric constant of 20 or more; A coating layer containing a carbon compound is formed on the surface of the positive electrode active material particles constituting the positive electrode active material, and the coating layer contains an acidic functional group. The amount of the acidic functional group in the composite composed of the positive electrode active material and the coating layer is 0.004 mmol / g or more and 0.0062 mmol / g or less, The coating layer accounts for 0.1% by weight or more and 5% by weight or less in the composite.

2. The lithium ion secondary battery according to claim 1, characterized in that: The specific surface area of ​​the composite is 9.0 m 2 / g or above.

3. The lithium ion secondary battery according to claim 1 or 2, characterized in that: The positive electrode active material is composed of the chemical formula Li x M y P z O 4-δ The olivine-type lithium phosphate compound represented by <x / y<1.5,y / z> 1, δ is the oxygen deficiency amount, and M contains at least one of Fe, Mn, Co and Ni.