Multifunctional dual alloy catalyst for hydrogen production from bio-oil steam reforming and its application

Preparation by the equal volume impregnation method of Ni-Mg/CaFe2O4 dual alloy catalysts has been solved, and the existing catalyst precious metals are expensive and poor sintering resistance is achieved, high hydrogen yield and good water-gas transformation reaction activity is achieved, and it is suitable for bio-oil water vapor Reconstruction of hydrogen production process.

CN112264023BActive Publication Date: 2024-11-12ENERGY RES INST OF SHANDONG ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011369726.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-11-12
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

The existing bio-oil water vapor reforming hydrogen production catalysts have problems such as expensive precious metal components, poor sintering resistance, low water vapor transformation reaction activity, and increasing the cost of subsequent purification of H2 by-products of CO and CH4.

Method used

Ni-Mg/CaFe2O4 dual alloy catalyst was prepared by equal volume impregnation method. Ni is the main active component, Mg is the co-active component, CaFe2O4 is the support, and the Ca/Fe molar ratio is 1:2 to form NiFe2O4, NiMgO2 and Ca2Fe2O5 solid solution improves the catalyst's resistance to carbon deposit and water-gas transformation reaction activity.

Benefits of technology

It has achieved high hydrogen yield, resistance to carbon deposits, low cost, good CO and CH4 conversion performance, strong catalyst stability, suitable for the hydrogen production process of bio-oil water vapor reforming, significantly improving the water-gas transformation reaction activity and hydrogen yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DEST_PATH_IMAGE002
    Figure DEST_PATH_IMAGE002
Patent Text Reader

Abstract

A multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil and its application, with nickel as the main active component, magnesium as the auxiliary active component, and CaFe2O4 oxygen carrier as the carrier, is prepared to have strong catalytic activity, high hydrogen yield, carbon deposition resistance and high water-gas shift reaction activity. The CaFe2O4 oxygen carrier is prepared as a carrier, and nickel ions and magnesium ions are loaded by a step-by-step equal volume impregnation method, which effectively improves the stability of the catalyst and the nickel dispersion. After calcination and reduction, the catalyst produces a Ni-Mg and Ni-Fe dual alloy, which enhances the catalyst's anti-coking ability and wear resistance. Compared with ordinary carriers, the CaFe2O4 carrier has a high oxygen loading rate and strong interaction with the active component, which can effectively alleviate the problem of catalyst carbon deposition and achieve good CO conversion performance. Under the optimal reaction conditions, the hydrogen yield of the Ni-Mg / CaFe2O4 catalytic reaction is as high as 95%, CO conversion is complete, and the hydrogen purification cost is reduced, which has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a catalyst, in particular to a multifunctional double alloy catalyst for hydrogen production by bio-oil steam reforming and application thereof. Background Art

[0002] As a clean fuel, hydrogen has attracted widespread attention in recent years due to its application in hydrogen fuel cell electric vehicles. At the same time, hydrogen is also an important chemical raw material, mainly used in ammonia synthesis, petroleum refining, and the synthesis of methanol and other fine chemicals. At present, hydrogen mainly comes from fossil fuels and is produced through processes such as catalytic reforming of natural gas, catalytic cracking of petroleum, and gasification of coal. As an important component of renewable energy, biomass has the characteristics of large reserves, renewable, carbon neutral and environmentally friendly, and is considered to be an ideal raw material for hydrogen production. Biomass hydrogen production is divided into biological method and thermochemical conversion method. Although biological hydrogen production has broad prospects, it is still in laboratory research; there are many ways to produce hydrogen by biomass thermochemical conversion, mainly including gasification hydrogen production, thermal cracking hydrogen production, and bio-oil steam reforming hydrogen production. Bio-oil steam reforming hydrogen production refers to the process in which bio-oil produces hydrogen through the combined action of water vapor and catalyst under high temperature conditions. Compared with other biomass thermochemical conversion methods, bio-oil steam reforming hydrogen production significantly improves the hydrogen production efficiency, among which the catalyst components, structure and preparation method can affect the raw material conversion rate, hydrogen yield and selectivity. Bio-oil steam reforming hydrogen production catalysts are mainly composed of precious metal components, such as Rh, Ru, Pt, Pd and Ir, and have been widely used in bio-oil steam reforming hydrogen production reactions. There are a large number of vacancies on the surface of precious metals, which are easy to adsorb reactants, enhance their activation ability, have high catalytic activity, are resistant to sintering and carbon deposition, and show good catalytic performance for water gas shift reactions. However, precious metals are expensive and not suitable for large-scale applications.

[0003] CN 106807387 B discloses a bifunctional catalyst for absorption-enhanced bio-oil steam reforming hydrogen production and a preparation method thereof, wherein Ni is used as an active component and Co, CeO are used as auxiliary agents by using a gel sol method and an impregnation method. 2 , MgO, K 2 O, the carrier is ZrO 2 or Al 2 O 3 The catalyst of the composite of CO and CaO has a hydrogen yield of more than 85% and a hydrogen purity of more than 95%, but the maintenance time is short, only 30 minutes, and it fails to effectively improve the activity of the water gas shift reaction. 4 , increase the subsequent purification H 2 cost. Summary of the invention

[0004] The purpose of the present invention is to provide a multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil, namely Ni-Mg / CaFe, which has simple preparation process, low price, high hydrogen production yield, high water-gas shift reaction activity and resistance to carbon deposition. 2 O 4 Dual alloy catalyst.

[0005] The technical scheme of the present invention is: a multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil, characterized in that Ni is the main active component, Mg is the auxiliary active component; the carrier is CaFe 2 O 4 Oxygen carrier: Ni-Mg / CaFe 2 O 4 The active components and their mass percentages in the catalyst are: Ni: 5%~15%, Mg: 5%~15%, and the mass percentage of the carrier is: 70~90%.

[0006] The specific characteristics of the present invention are that firstly, CaFe is obtained by an equal volume impregnation method. 2 O 4 Oxygen carrier, and then impregnate Ni in equal volumes 2+ ,Mg 2+ Prepared. Ni-Mg / CaFe 2 O 4 The preparation steps are as follows:

[0007] (1) CaFe 2 O 4 The preparation of oxygen carrier includes the following steps: firstly, determine the saturated water absorption rate of CaO, weigh a certain mass of CaO and a certain mass of Fe(NO 3 ) 3 9H 2 O. Then, a certain concentration of Fe(NO 3 ) 3 9H 2 O solution, Fe(NO 3 ) 3 9H 2 O solution is immersed in CaO in equal volumes; the mixture is stirred evenly, ultrasonically treated for 30 minutes, allowed to stand for 2-12 hours, dried in an oven at 100-150°C for 12-24 hours, and then calcined in a muffle furnace at 600-1000°C for 2-5 hours. The calcined sample is placed in air to cool to room temperature, and then ground into a powder of >100 mesh to obtain CaFe 2 O 4 Oxygen carrier.

[0008] (2) Introduction of the main active component Ni: First determine the CaFe2 O 4 Saturated water absorption rate, according to the mass percentage of Ni component, weigh a certain mass of Ni(NO 3 ) 2 6H 2 O. Secondly, based on CaFe 2 O 4 Saturated water absorption rate configures a certain concentration of Ni(NO 3 ) 2 6H 2 O solution, Ni(NO 3 ) 2 6H 2 O solution was immersed in an equal volume of CaFe 2 O 4 ; Mix and stir evenly, treat with ultrasound for 30 minutes, let stand for 2-12 hours, dry in an oven at 100-150℃ for 12-24 hours, then calcine in a muffle furnace at 600-1000℃ for 2-5 hours, cool the calcined sample in air to room temperature, and grind to >100 mesh Ni / CaFe 2 O 4 Powdered.

[0009] (3) Introduction of auxiliary active component Mg: First determine Ni / CaFe 2 O 4 Saturated water absorption rate, according to the mass percentage of Mg component, weigh a certain mass of Mg(NO 3 ) 2 6H 2 O. Secondly, based on Ni / CaFe 2 O 4 Saturated water absorption rate configures a certain concentration of Mg(NO 3 ) 2 6H 2 O solution, Mg(NO 3 ) 2 6H 2 O solution was immersed in an equal volume of Ni / CaFe 2 O 4 ; Mix and stir evenly, treat with ultrasound for 30 minutes, let stand for 2-12 hours, dry in an oven at 100-150°C for 12-24 hours, and then calcine in a muffle furnace at 600-1000°C for 2-5 hours. Cool the calcined sample to room temperature in air, grind and sieve to 30-40 mesh particles to obtain the active components and their mass percentages: Ni: 5%-15%, Mg: 5%-15%, CaFe 2 O 4 The mass percentage of oxygen carrier is: 70~90% Ni-Mg / CaFe 2 O 4catalyst.

[0010] The application of the multifunctional dual alloy catalyst for hydrogen production by bio-oil steam reforming of the present invention is characterized in that a dual alloy catalyst is applied to hydrogen production by bio-oil steam catalytic reforming.

[0011] The specific features of this scheme are as follows: the application process conditions are: reaction temperature is 600~800℃, water-carbon ratio is 2.5~10, liquid hourly space velocity is 1.67~5.01h -1 .

[0012] The beneficial effects of the present invention are: based on the CaFe with high O and Fe content and easy to interact strongly with the additive 2 O 4 The oxygen carrier is a carrier and has a certain catalytic ability and water-gas shift reaction activity; Ni-based catalysts have good activity, are cheap and easy to obtain, Fe has good water-gas shift activity, and Mg is conducive to H 2 Based on the adsorption of O and the promotion of -OH transfer to enhance coke gasification, a step-by-step equal volume impregnation method was used to prepare Ni as the active component, Mg as the auxiliary active component, and CaFe 2 O 4 The carrier has good activity, strong stability, resistance to carbon deposition, high hydrogen yield, and promotes the conversion of CO to CH 4 Bi-alloy catalyst for efficient conversion of bio-oil steam catalytic reforming to hydrogen production. 2 O 4 Ni-Mg / CaFe 2 O 4 Catalyst: In order to improve the catalyst's ability to resist carbon deposition and stability, CaFe was prepared using a molar ratio of Ca / Fe = 1:2 with a dominant Fe molar amount. 2 O 4 Solid solution; During the preparation process, Ni and CaFe 2 O 4 The Fe components in the solution interact strongly at high temperatures to form NiFe 2 O 4 , CaFe 2 O 4 Converted to Ca 2 Fe 2 O 5 After the second impregnation and calcination, the Ni-Mg components interact strongly to form NiMgO 2 Therefore, Ni-Mg / CaFe 2 O 4 The catalyst also contains NiFe 2 O 4 、NiMgO 2 With Ca2 Fe 2 O 5 Three metal oxide solid solutions, O, Fe content is high. After characterization and experimental verification, it is known that the reduced Ni-Mg / CaFe 2 O 4 Produce Ni-Fe and Ni-Mg alloys, and Ca 2 Fe 2 O 5 The synergistic effect of Ni and Mg is remarkable. 2 O 4 Oxygen carriers have good application value and research potential for hydrogen production from bio-oil steam catalytic reforming. Ni-Mg, Ni-Fe and Ca-Fe components work together to promote efficient reactions, increase hydrogen yield and gas production, reduce carbon deposits on the catalyst after the reaction, and maintain long-term catalytic activity. At 600°C, S / C=5, LHSV=3.34h -1 Under these conditions, the hydrogen yield is high, the catalyst carbon deposition is low, the water gas shift reaction and methane steam reforming reaction activity are excellent, and CO and CH 4 , the gas produced is only H 2 With CO 2 , which is convenient for gas purification and separation. Therefore, the catalyst has good application prospects. At the same time, the preparation process is simple, the price is low, the hydrogen yield is high, the carbon deposition resistance is good, and the CO and CH 4 Conversion performance, the interaction between the three solid solutions of Ni-Fe, Ni-Mg and Ca-Fe is obvious, which promotes the positive hydrogen production of steam reforming reaction and the steam reforming of various gas by-products, thereby greatly improving the hydrogen yield. The catalyst has strong stability and strong resistance to carbon deposition, and has bright application prospects.

[0013] The catalyst of the present invention is convenient for preparing the supported CaFe 2 O 4 Oxygen carrier is the landing point, with Ni as the main active component and Mg as the auxiliary active component. After impregnation, calcination and reduction, strong interaction occurs between Ni-Mg-Fe-Ca to form Ni-Fe alloy, Ni-Mg alloy and Ca 2 Fe 2 O 5 Oxygen carrier, a Ni-Mg / CaFe catalyst was prepared to improve the activity of water-gas shift reaction and realize the conversion and absorption of CO; the hydrogen yield was high and the catalyst had strong in-situ carbon removal ability; the stability was strong and it was applied to the hydrogen production process of bio-oil steam reforming. 2 O 4 Double alloy catalyst. The catalyst described in the present invention is based on CaFe with high O and Fe content and easy to interact strongly with the additive. 2 O4 The oxygen carrier is the carrier, Ni and Mg are the main active component and auxiliary active component respectively. 2 O 4 The Fe components in the solution interact strongly at high temperatures to form NiFe 2 O 4 , CaFe 2 O 4 Converted to Ca 2 Fe 2 O 5 ; After the second impregnation, the Ni-Mg components interact strongly to form NiMgO 2 The calcined catalyst is reduced to produce Ni-Fe alloy, Ni-Mg alloy, Ca 2 Fe 2 O 5 The three cooperate with each other to improve the activity of water-gas shift reaction, and the catalyst has less carbon deposition and strong stability. After a long time of catalytic reaction, it maintains high activity and no H removal has been detected. 2 With CO 2 The advantages include gaseous products. DETAILED DESCRIPTION

[0014] In order to better understand the present invention, examples are given to illustrate:

[0015] Example 1: Preparation of a multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil, specifically Ni-Mg / CaFe 2 O 4 Catalyst preparation: 20 g Ni-Mg / CaFe 2 O 4 The steps include:

[0016] (1) Preparation of 20g of composite calcium iron oxygen carrier CaFe 2 O 4 First, determine that the saturated water absorption rate of CaO is about 0.3 g / mL, and weigh 5.19 g CaO and 74.81 g Fe(NO 3 ) 3 9H 2 O, and then prepare 4.32 g / mL Fe(NO 3 ) 3 9H 2 O solution 17.3 mL, Fe(NO 3 ) 3 9H 2O solution was immersed in CaO in equal volumes; the mixture was stirred evenly, ultrasonically treated for 30 minutes, allowed to stand for 12 hours, dried in an oven at 120°C for 12 hours, and then calcined in a muffle furnace at 800°C for 4 hours. The calcined sample was placed in air to cool to room temperature, and then ground into a powder of >100 mesh to obtain CaFe 2 O 4 Oxygen carrier.

[0017] (2) Introduction of the main active component Ni: First determine the CaFe 2 O 4 The saturated water absorption rate is about 1g / mL, and 16gCaFe 2 O 4 Oxygen carrier, followed by CaFe 2 O 4 Saturated water absorption Weigh 15.04g Ni(NO 3 ) 2 6H 2 O to prepare 0.94 g / mL Ni(NO 3 ) 2 6H 2 O solution 16mL, Ni(NO 3 ) 2 6H 2 O solution was immersed in an equal volume of CaFe 2 O 4 ; Mix and stir evenly, ultrasonically treat for 30 minutes, stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground to >100 mesh Ni / CaFe 2 O 4 Powdered.

[0018] (3) Introduction of auxiliary active component Mg: First determine Ni / CaFe 2 O 4 The saturated water absorption rate is about 2g / mL, and 19gNi / CaFe 2 O 4 , followed by Ni / CaFe 2 O 4 Saturated water absorption Weigh 10.67g Mg(NO 3 ) 2 6H 2 O to prepare 1.12 g / mL Mg (NO 3 ) 2 6H 2 O solution 9.5 mL, Mg(NO 3 ) 2 6H 2O solution was immersed in an equal volume of Ni / CaFe 2 O 4 ; Mix and stir evenly, treat with ultrasound for 30 minutes, let stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground and sieved into 30-40 mesh particles, and the active components and their mass percentages are: Ni: 15%, Mg: 5%; the carrier and its mass percentage are: CaFe 2 O 4 :80% Ni-Mg / CaFe 2 O 4 catalyst.

[0019] Example 2: A Ca 2 Fe 2 O 5 Catalyst preparation: 20 g Ca 2 Fe 2 O 5 The steps include:

[0020] First, determine that the saturated water absorption rate of CaO is about 0.3g / mL, and weigh 8.24g of CaO. Then, based on the saturated water absorption rate of CaO, weigh 54.19g of Fe(NO 3 ) 3 9H 2 O prepared 1.97 g / mL Fe(NO 3 ) 3 9H 2 O solution 27.47 mL, Fe(NO 3 ) 3 9H 2 O solution was impregnated into CaO in equal volumes; the mixture was stirred evenly, ultrasonically treated for 30 min, allowed to stand for 12 h, dried in an oven at 120 °C for 12 h, and then calcined in a muffle furnace at 800 °C for 4 h. The calcined sample was placed in air to cool to room temperature, and then ground and sieved into 30-40 mesh particles to obtain CaO with a molar ratio of Ca / Fe = 1:1. 2 Fe 2 O 5 .

[0021] Example 3: A Ni / CaFe 2 O 4 Catalyst preparation: 20 g Ni / CaFe 2 O 4 The steps include:

[0022] (1) Preparation of 20g of composite calcium iron oxygen carrier CaFe 2 O4 First, determine that the saturated water absorption rate of CaO is about 0.3g / mL, and weigh 5.19gCaO. Then, based on the saturated water absorption rate of CaO, weigh 74.81g Fe(NO 3 ) 3 9H 2 O to prepare 4.32 g / mL Fe(NO 3 ) 3 9H 2 O solution 17.3 mL, Fe(NO 3 ) 3 9H 2 O solution was immersed in CaO with a Ca / Fe molar ratio of 1:2; the mixture was stirred evenly, ultrasonicated for 30 min, allowed to stand for 12 h, dried in an oven at 120 °C for 12 h, and then calcined in a muffle furnace at 800 °C for 4 h. The calcined sample was placed in air to cool to room temperature, and then ground into a powder of >100 mesh to obtain CaFe 2 O 4 Oxygen carrier.

[0023] (2) Introduction of the main active component Ni: First determine the CaFe 2 O 4 The saturated water absorption rate is about 1g / mL, and 17gCaFe 2 O 4 , followed by CaFe 2 O 4 Saturated water absorption Weigh 15.04g Ni(NO 3 ) 2 6H 2 O was used to prepare 0.88 g / mL Ni(NO 3 ) 2 6H 2 O solution 17mL, Ni(NO 3 ) 2 6H 2 O solution was immersed in an equal volume of CaFe 2 O 4 ; Mix and stir evenly, treat with ultrasound for 30 minutes, let stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground and sieved to 30-40 mesh particles, and the active component and its mass percentage are: Ni, 15%; the carrier and its mass percentage are: CaFe 2 O 4 Oxygen carrier 85% Ni / CaFe 2 O 4 catalyst.

[0024] Example 4: A Ni-Mg / Ca 2 Fe 2 O 5 Catalyst preparation: 20 g Ni-Mg / Ca 2 Fe 2 O 5 The steps include:

[0025] (1) Preparation of 20 g of composite calcium iron oxygen carrier Ca 2 Fe 2 O 5 First, determine that the saturated water absorption rate of CaO is about 0.3g / mL, and weigh 8.24g CaO. Then, based on the saturated water absorption rate of CaO, weigh 54.19g Fe(NO 3 ) 3 9H 2 O prepared 1.97 g / mL Fe(NO 3 ) 3 9H 2 O solution 27.47 mL, Fe(NO 3 ) 3 9H 2 O solution was impregnated into CaO in equal volumes; the mixture was stirred evenly, ultrasonically treated for 30 min, allowed to stand for 12 h, dried in an oven at 120 °C for 12 h, and then calcined in a muffle furnace at 800 °C for 4 h. The calcined sample was placed in air to cool to room temperature, and then ground and sieved into 30-40 mesh particles to obtain CaO with a molar ratio of Ca / Fe = 1:1. 2 Fe 2 O 5 .

[0026] (2) Introduction of the main active component Ni: First determine the Ca 2 Fe 2 O 5 The saturated water absorption rate is about 1g / mL, and 16gCa 2 Fe 2 O 5 , followed by Ca 2 Fe 2 O 5 Saturated water absorption Weigh 15.04g Ni(NO 3 ) 2 6H 2 O to prepare 0.94 g / mL Ni(NO 3 ) 2 6H 2 O solution 16mL, Ni(NO 3 ) 2 6H 2 O solution was immersed in Ca2 Fe 2 O 5 ; Mix and stir evenly, ultrasonically treat for 30 minutes, stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground to >100 mesh Ni / Ca 2 Fe 2 O 5 Powdered.

[0027] (3) Introduction of the auxiliary active component Mg: First determine the Ni / Ca 2 Fe 2 O 5 The saturated water absorption rate is about 2g / mL, and 19gNi / Ca 2 Fe 2 O 5 , followed by Ni / Ca 2 Fe 2 O 5 Saturated water absorption Weigh 10.67g Mg(NO 3 ) 2 6H 2 O to prepare 1.12 g / mL Mg (NO 3 ) 2 6H 2 O solution 9.5 mL, Mg(NO 3 ) 2 6H 2 O solution was immersed in an equal volume of Ni / Ca 2 Fe 2 O 5 ; Mix and stir evenly, treat with ultrasound for 30 minutes, stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground and sieved into 30-40 mesh particles, and the active components and their mass percentages are: Ni: 15%, Mg: 5%; the carrier and its mass percentage are: Ca 2 Fe 2 O 5 :80% Ni-Mg / Ca 2 Fe 2 O 5 catalyst.

[0028] Example 5: A Ni-Mg / Ca 2 Fe 2 O 5 -CaO catalyst preparation, preparation of 20g Ni-Mg / Ca 2 Fe 2 O5 The steps include:

[0029] (1) Preparation of 20 g of composite calcium iron oxygen carrier Ca 2 Fe 2 O 5 -CaO: First, determine that the saturated water absorption rate of CaO is about 0.3g / mL, and weigh 11.2g CaO. Then, based on the saturated water absorption rate of CaO, weigh 40.4g Fe(NO 3 ) 3 9H 2 O prepared 1.08 g / mL Fe(NO 3 ) 3 9H 2 O solution 37.3 mL, Fe(NO 3 ) 3 9H 2 O solution was impregnated into CaO in equal volumes; the mixture was stirred evenly, ultrasonically treated for 30 min, allowed to stand for 12 h, dried in an oven at 120 °C for 12 h, and then calcined in a muffle furnace at 800 °C for 4 h. The calcined sample was placed in air to cool to room temperature, and then ground and sieved into 30-40 mesh particles to obtain CaO with a molar ratio of Ca / Fe=2:1. 2 Fe 2 O 5 -CaO.

[0030] (2) Introduction of the main active component Ni: First determine the Ca 2 Fe 2 O 5 -CaO saturated water absorption rate is about 0.75g / mL, and weigh 16gCa 2 Fe 2 O 5 , followed by Ca 2 Fe 2 O 5 Saturated water absorption Weigh 15.04g Ni(NO 3 ) 2 6H 2 O to prepare 0.71 g / mL Ni(NO 3 ) 2 6H 2 O solution 21.33 mL, Ni(NO 3 ) 2 6H 2 O solution was immersed in Ca 2 Fe 2 O 5; Mix and stir evenly, ultrasonically treat for 30 minutes, stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground to >100 mesh Ni / Ca 2 Fe 2 O 5 -CaO powder.

[0031] (3) Introduction of the auxiliary active component Mg: First determine the Ni / Ca 2 Fe 2 O 5 -CaO saturated water absorption rate is about 2g / mL, and weigh 19gNi / Ca 2 Fe 2 O 5 -CaO, followed by Ni / Ca 2 Fe 2 O 5 -CaO saturated water absorption Weigh 10.67g Mg(NO 3 ) 2 6H 2 O to prepare 1.12 g / mL Mg (NO 3 ) 2 6H 2 O solution 9.5 mL, Mg(NO 3 ) 2 6H 2 O solution was immersed in an equal volume of Ni / Ca 2 Fe 2 O 5 -CaO; mix and stir evenly, treat with ultrasound for 30 minutes, stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground and sieved to 30-40 mesh particles, and the active components and their mass percentages are: Ni: 15%, Mg: 5%; the carrier and its mass percentage are: Ca 2 Fe 2 O 5 -CaO: 80% Ni-Mg / Ca 2 Fe 2 O 5 -CaO catalyst.

[0032] Catalyst evaluation: A fixed bed reactor was used. 3 g of catalyst was placed in a quartz tube with a diameter of 15 mm and heated in 10% H 2 / N 2 The temperature was raised to 800 °C for reduction for 2 h under a (v / v) atmosphere, and then the temperature was lowered to 600 °C and switched to N 2The purge lasted for at least 30 min, and the injection pump was turned on to inject the water-soluble component of the bio-oil with a water-to-carbon ratio of 5 at a liquid hourly space velocity of 3.34 h -1 The reaction lasts for 180 min, and the gas products after the reaction are H 2 , CO 2 , CO, CH 4 The catalysts prepared in the above five embodiments were respectively tested under the same conditions, and the gas yield comparison is shown in Table 1.

[0033] Table 1 is a comparison of the gas yields obtained in the initial stage of bio-oil steam reforming reaction under different catalysts

[0034]

[0035] From the experimental results in Table 1, it can be seen that compared with other catalysts, Ni-Mg / CaFe 2 O 4 Under the action of catalyst, H 2 The yield is the highest, reaching 95%. Due to the good activity of the catalyst in the water-gas shift reaction, CO is absorbed and converted into CO 2 , so CO 2 The high yield also indicates that at this reaction temperature, the Ca 2 Fe 2 O 5 Relatively stable, with little or no decomposition; and no CH 4 Gas. Ca without active metal components 2 Fe 2 O 5 The catalytic activity is limited, H 2 The yield is low, and the methane reforming reaction and water gas shift reaction activity are poor; Ni / CaFe loaded with only Ni 2 O 4 After reduction, the catalyst only generates Ni-Fe alloy, so the catalyst synergy is better than Ni-Mg / CaFe 2 O 4 Weak, H 2 The yield is low, and the water-gas shift reaction activity is also weaker than Ni-Mg / CaFe 2 O 4 For Ni-Mg / Ca 2 Fe 2 O 5 Ni-Mg / Ca 2 Fe 2 O 5 -CaO, after calcination, its CO 2The yield is low, but due to the low molar amount of Fe in the carrier, the NiO and NiMgO produced by calcining the catalyst 2 , Ca 2 Fe 2 O 5 During reduction, NiMgO 2 Reduced to Ni-Mg alloy, NiO and Ca 2 Fe 2 O 5 The Fe components that overflow from the lattice oxygen defect sites interact with each other and can be reduced to obtain Ni-Fe alloy. 2 Fe 2 O 5 , CaFe 2 O 4 , Ca 2 Fe 2 O 5 The Fe component in -CaO is used as the source of Ni-Fe alloy in the catalyst, and the Ca / Fe molar ratio is 1:1, 1:2, and 2:1, respectively, resulting in the reduction of Ni-Mg / Ca 2 Fe 2 O 5 Ni-Mg / Ca 2 Fe 2 O 5 -The amount of Ni-Fe alloy in CaO is less than that of Ni-Mg / CaFe 2 O 4 Therefore, Ni-Fe, Ni-Mg dual alloys and Ca 2 Fe 2 O 5 The synergistic effect is also weaker than that of Ni-Mg / CaFe 2 O 4 Similarly, the water-gas shift reaction activity is higher than that of Ni-Mg-Fe / CaFe 2 O 4 Table 1 shows that Ni-Mg, Ni-Fe, and Ca-Fe oxygen carriers can synergize with each other after reduction, which helps to improve the hydrogen yield and has excellent water gas shift reaction activity.

[0036] Example 6: Preparation of Ni-Mg / CaFe by one-time equal volume impregnation of active components 2 O 4 , prepare 20g Ni-Mg / CaFe 2 O 4 The steps include:

[0037] (1) Preparation of 20g of composite calcium iron oxygen carrier CaFe 2 O 4First, determine that the saturated water absorption rate of CaO is about 0.3g / mL, and weigh 5.19gCaO. Then, based on the saturated water absorption rate of CaO, weigh 74.81g Fe(NO 3 ) 3 9H 2 O to prepare 4.32 g / mL Fe(NO 3 ) 3 9H 2 O solution 17.3 mL, Fe(NO 3 ) 3 9H 2 O solution was immersed in CaO with a Ca / Fe molar ratio of 1:2; the mixture was stirred evenly, ultrasonicated for 30 min, allowed to stand for 12 h, dried in an oven at 120 °C for 12 h, and then calcined in a muffle furnace at 800 °C for 4 h. The calcined sample was placed in air to cool to room temperature, and then ground into a powder of >100 mesh to obtain CaFe 2 O 4 carrier.

[0038] (2) Introduction of active components: First, determine the CaFe 2 O 4 The saturated water absorption rate is about 1g / mL, and 16gCaFe 2 O 4 , followed by CaFe 2 O 4 Saturated water absorption Weigh 15.04g Ni(NO 3 ) 2 6H 2 O to prepare 1.88 g / mL Ni(NO 3 ) 2 6H 2 O solution 8 mL, weigh 10.67 g Mg(NO 3 ) 2 6H 2 O prepared 1.33 g / mL Mg(NO 3 ) 2 6H 2 O solution 8mL, Ni(NO 3 ) 2 6H 2 O solution and Mg(NO 3 ) 2 6H 2 O solution was immersed in an equal volume of CaFe 2 O 4; Mix and stir evenly, ultrasonically treat for 30 minutes, stand for 12 hours, dry in an oven at 120°C for 12 hours, and then calcine in a muffle furnace at 800°C for 4 hours. The calcined sample is placed in the air to cool to room temperature, and then ground to >100 mesh Ni-Mg / CaFe 2 O 4 Powdered.

[0039] The active components and mass percentages of the catalyst prepared in this example are: Ni: 15%, Mg: 5%; the carrier and mass percentages are: CaFe 2 O 4 :80%, wherein the molar ratio of Ca / Fe is 1:2. The difference from Example 1 is that the active components are impregnated by a single equal volume impregnation method. After characterization and verification, it was found that the catalyst contained: NiO, NiFe 2 O 4 , MgO, Ca 2 Fe 2 O 5 , Ni-Mg solid solution has not yet been formed, and only Ni-Fe alloy, Mg and Ca exist after reduction 2 Fe 2 O 5 The reason is that after multiple calcinations, it is easier for the active metal components to interact strongly to form a solid solution. The gas yield was obtained by conducting an experiment under the same conditions as the above example: H 2 :85%,CO 2 :50%, CO:1%, the catalytic effect is obviously worse than that of Example 1.

[0040] Example 7: Preparation of a dual alloy catalyst for hydrogen production by steam reforming of bio-oil, specifically Ni-Mg / CaFe 2 O 4 Preparation of the catalyst: The preparation method of the catalyst in this embodiment is the same as that in Example 1 and will not be repeated here. The difference lies in the mass percentage of the active component Ni. The active components and mass percentage of the catalyst prepared in this embodiment are: Ni: 5%, Mg: 5%; the carrier and mass percentage are: CaFe 2 O 4 : 90%, wherein the molar ratio of Ca / Fe is 1:2. The catalyst evaluation was carried out under the same experimental conditions as in Example 1. The experimental study found that the gas yield in the initial stage of the reaction was: H 2 :80%,CO 2 :20%, CO:5%, CH 4 :1.3%, the reaction activity decreases rapidly with the increase of reaction time.

[0041] Example 8: Preparation of a dual alloy catalyst for hydrogen production by steam reforming of bio-oil, specifically Ni-Mg / CaFe 2 O 4 Preparation of the catalyst: The catalyst preparation method in this embodiment is the same as that in Example 1 and will not be repeated. The catalyst in Example 1 is ground to a mesh size of 30-40, while the catalyst in this embodiment is ground to a mesh size of 60-80. The catalyst particles are smaller in size, which is not conducive to the full contact between the catalyst and the reaction raw materials, and is easy to clog the reaction device, resulting in low catalytic reaction activity. The catalyst was evaluated under the same experimental conditions as in Example 1. The experimental study found that the gas yield at the initial stage of the reaction was: H 2 :60%, CO 2 :40%, CO:10%, CH 4 :5%, the reaction activity decreases rapidly with time.

[0042] Example 9: A Ni-Mg / CaFe 2 O 4 Catalyst preparation: 20 g Ni-Mg / CaFe 2 O 4 The steps include:

[0043] (1) Preparation of 20g of composite calcium iron oxygen carrier CaFe 2 O 4 First, determine that the saturated water absorption rate of CaO is about 0.3g / mL, and weigh 5.19gCaO. Then, based on the saturated water absorption rate of CaO, weigh 74.81g Fe(NO 3 ) 3 9H 2 O to prepare 4.32 g / mL Fe(NO 3 ) 3 9H 2 O solution 17.3 mL, Fe(NO 3 ) 3 9H 2 O solution was immersed in CaO with a Ca / Fe molar ratio of 1:2; the mixture was stirred evenly, ultrasonicated for 30 min, allowed to stand for 12 h, dried in an oven at 120 °C for 12 h, and then calcined in a muffle furnace at 800 °C for 4 h. The calcined sample was placed in air to cool to room temperature, and then ground into a powder of >100 mesh to obtain CaFe 2 O 4 carrier.

[0044] (2) Introduction of active components: 16 g of CaFe prepared in step (1) 2 O 4The mixture was mechanically mixed with 3g>100 mesh Ni powder and 1g>100 mesh Mg powder for 3h, dried at 120℃ for 12h, and then calcined at 800℃ in a muffle furnace for 4h. The calcined sample was ground and sieved to obtain 30~40 mesh Ni-Mg / CaFe 2 O 4 Dual alloy catalyst.

[0045] The composition and mass percentage of the catalyst prepared in this example are consistent with those in Example 1: the active component and mass percentage are: Ni: 15%, Mg: 5%; the carrier and mass percentage are: CaFe 2 O 4 :80%, wherein the molar ratio of Ca / Fe is 1:2. Example 1 adopts the stepwise equal volume impregnation method, while this example adopts the mechanical mixing method. The interaction between the components is weak, which easily causes catalyst deactivation and carbon deposition. The catalyst evaluation was carried out under the same experimental conditions as Example 1. The experimental study found that the gas yield in the initial stage of the reaction was: H 2 :70%, CO 2 :35%, CO:5%, CH 4 :2%, the reaction activity decreases rapidly with the increase of reaction time.

[0046] Embodiment 10:

[0047] In this embodiment, Ni-Mg / CaFe 2 O 4 The catalyst preparation method, reduction temperature and reduction time are the same as those in Example 1 and will not be described in detail. The difference is that the experimental conditions are: water-carbon ratio is 10, reaction temperature is 600°C, liquid hourly space velocity is 3.34h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :82%, CO 2 :52%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0048] Embodiment 11:

[0049] In this embodiment, Ni-Mg / CaFe 2 O 4 The catalyst preparation method, reduction temperature and reduction time are the same as those in Example 1 and will not be described in detail. The difference is that the experimental conditions are a water-carbon ratio of 5, a reaction temperature of 500°C, and a liquid hourly space velocity of 3.34 h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :80%,CO 2 :50%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0050] Embodiment 12:

[0051] In this embodiment, Ni-Mg / CaFe 2 O 4 The catalyst preparation method, reduction temperature and reduction time are the same as those in Example 1 and will not be described in detail. The difference is that the experimental conditions are: water-carbon ratio is 5, reaction temperature is 600°C, liquid hourly space velocity is 1.67h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :85%,CO 2 :59%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0052] Embodiment 13:

[0053] In this embodiment, Ni-Mg / CaFe 2 O 4 The catalyst preparation method, reduction temperature, reduction time, and reaction conditions are the same as those in Example 1 and will not be described in detail. The difference is that the reaction time is 20 h. A high hydrogen yield of 91% is maintained during the reaction for 3 to 5 h, and is stabilized at 86%, indicating that the catalyst has good stability and catalytic activity and has broad application prospects.

[0054] Embodiment 14:

[0055] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The catalyst preparation method, reduction temperature, reduction time, and reaction conditions are the same as those in Example 4 and will not be repeated here. The difference is that the mass percentage of the active component Ni is: the active component and mass percentage: Ni: 5%, Mg: 5%; the carrier and mass percentage are: Ca 2 Fe 2 O 5 : 90%, wherein the molar ratio of Ca / Fe is 1:1. The catalyst evaluation was carried out under the same experimental conditions as in Example 4. The experimental study found that the gas yield in the initial stage of the reaction was: H 2 :75%, CO 2 :30%, CO:6%, CH 4 :1.5%, the reaction activity decreases rapidly with the increase of reaction time.

[0056] Embodiment 15:

[0057] In this example, the catalyst Ni-Mg / Ca 2 Fe 2 O 5The catalyst preparation method, reduction temperature, reduction time, and reaction conditions are the same as those in Example 4 and will not be repeated here. The catalyst in Example 4 was ground to a mesh size of 30-40, but the difference is that the catalyst in this example was ground to a mesh size of 60-80. The catalyst particle size is smaller, which is not conducive to the full contact between the catalyst and the reaction raw materials, and is easy to clog the reaction device, resulting in low catalytic reaction activity. The catalyst was evaluated under the same experimental conditions as in Example 4. The experimental study found that the gas yield in the initial stage of the reaction was: H 2 :60%, CO 2 :45%, CO:10%, CH 4 :5%, the reaction activity decreases rapidly with time.

[0058] Embodiment 16:

[0059] The Ni-Mg / Ca 2 Fe 2 O 5 The catalyst composition and mass percentage are consistent with those in Example 4: active component and mass percentage: Ni: 5%, Mg: 5%; carrier and mass percentage: Ca 2 Fe 2 O 5 : 90%, wherein the molar ratio of Ca / Fe is 1:1. Example 4 adopts the stepwise equal volume impregnation method, while this example adopts the mechanical mixing method. The interaction between the components is weak, which is easy to cause catalyst deactivation and carbon deposition. The catalyst evaluation was carried out under the same experimental conditions as Example 4. The experimental study found that the gas yield in the initial stage of the reaction was: H 2 :78%,CO 2 :45%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0060] Embodiment 17:

[0061] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The catalyst preparation method, reduction temperature, and reduction time are the same as those in Example 4 and will not be repeated here. The difference is that the experimental conditions are a water-carbon ratio of 10, a reaction temperature of 600°C, and a liquid hourly space velocity of 3.34 h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :80%,CO 2 :55%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0062] Embodiment 18:

[0063] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The catalyst preparation method, reduction temperature, and reduction time are the same as those in Example 4 and will not be repeated here. The difference is that the experimental conditions are a water-carbon ratio of 5, a reaction temperature of 500°C, and a liquid hourly space velocity of 3.34 h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :78%,CO 2 :50%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0064] Embodiment 19:

[0065] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The catalyst preparation method, reduction temperature, and reduction time are the same as those in Example 4 and will not be repeated here. The difference is that the experimental conditions are a water-carbon ratio of 5, a reaction temperature of 600°C, and a liquid hourly space velocity of 1.67 h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :83%,CO 2 :55%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0066] Embodiment 20:

[0067] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The catalyst preparation method, reduction temperature, reduction time, and reaction conditions are the same as those in Example 4 and will not be described in detail. The difference is that the reaction time is 20 h. The reaction maintains a hydrogen yield of 83%, indicating that the catalyst has good stability and catalytic activity, but is lower than that of Ni-Mg / CaFe 2 O 4 There is a gap.

[0068] Embodiment 21:

[0069] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The preparation method, reduction temperature and reduction time of the -CaO catalyst are the same as those in Example 5 and will not be repeated here. The difference is that the mass percentage of the active component Ni is: the active component and mass percentage: Ni: 5%, Mg: 5%; the carrier and mass percentage are: Ca 2 Fe 2 O 5-CaO: 90%, wherein the molar ratio of Ca / Fe is 2:1. The catalyst evaluation was carried out under the same experimental conditions as in Example 5. The experimental study found that the gas yield in the initial stage of the reaction was: H 2 :80%,CO 2 :20%, CO:5%, CH 4 :1.3%, the reaction activity decreases rapidly with the increase of reaction time.

[0070] Embodiment 22:

[0071] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The preparation method, reduction temperature and reduction time of the -CaO catalyst are the same as those in Example 5 and will not be repeated here. The catalyst in Example 5 is ground to 30-40 meshes, while the catalyst in this example is ground to 60-80 meshes. The catalyst particles are smaller in size, which is not conducive to the full contact between the catalyst and the reaction raw materials, and is easy to clog the reaction device, resulting in low catalytic reaction activity. The catalyst was evaluated under the same experimental conditions as in Example 5. The experimental study found that the gas yield in the initial stage of the reaction was: H 2 :65%, CO 2 :30%, CO:10%, CH 4 :4%, the reaction activity decreases rapidly with time.

[0072] Example 23: A Ni-Mg / Ca 2 Fe 2 O 5 -CaO catalyst preparation, preparation of 20g Ni-Mg / Ca 2 Fe 2 O 5 -CaO includes the following steps:

[0073] (1) Preparation of 20 g of composite calcium iron oxygen carrier Ca 2 Fe 2 O 5 -CaO: First, determine that the saturated water absorption rate of CaO is about 0.3g / mL, and weigh 11.2g CaO. Then, based on the saturated water absorption rate of CaO, weigh 40.4g Fe(NO 3 ) 3 9H 2 O prepared 1.08 g / mL Fe(NO 3 ) 3 9H 2 O solution 37.3 mL, Fe(NO 3 ) 3 9H 2O solution was impregnated into CaO in equal volumes; the mixture was stirred evenly, ultrasonically treated for 30 min, allowed to stand for 12 h, dried in an oven at 120 °C for 12 h, and then calcined in a muffle furnace at 800 °C for 4 h. The calcined sample was placed in air to cool to room temperature, and then ground and sieved into 30-40 mesh particles to obtain CaO with a molar ratio of Ca / Fe=2:1. 2 Fe 2 O 5 -CaO.

[0074] (2) Introduction of active components: 16 g of Ca prepared in step (1) 2 Fe 2 O 5 -CaO was mechanically mixed with 3g>100 mesh Ni powder and 1g>100 mesh Mg powder for 3h, dried at 120℃ for 12h, and then calcined at 800℃ in a muffle furnace for 4h. The calcined sample was ground and sieved to obtain 30~40 mesh Ni-Mg / Ca 2 Fe 2 O 5 -CaO catalyst.

[0075] The composition and mass percentage of the catalyst prepared in this example are consistent with those in Example 5: the active component and mass percentage are: Ni: 15%, Mg: 5%; the carrier and mass percentage are: Ca 2 Fe 2 O 5 -CaO: 80%, wherein the molar ratio of Ca / Fe is 2: 1. Example 5 adopts the stepwise equal volume impregnation method, while this example adopts the mechanical mixing method, and the interaction between the components is weak, which is easy to cause catalyst deactivation and carbon deposition.

[0076] The catalyst was evaluated under the same experimental conditions as in Example 5. The experimental study found that the gas yield in the initial stage of the reaction was: 2 :80%,CO 2 :35%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0077] Embodiment 24:

[0078] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The preparation method, reduction temperature and reduction time of the -CaO catalyst are the same as those in Example 5 and will not be described in detail. The difference is that the experimental conditions are a water-carbon ratio of 10, a reaction temperature of 600°C, and a liquid hourly space velocity of 3.34 h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :82%, CO2 :35%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0079] Embodiment 25:

[0080] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The preparation method, reduction temperature and reduction time of the -CaO catalyst are the same as those in Example 5 and will not be repeated here. The difference is that the experimental conditions are a water-carbon ratio of 5, a reaction temperature of 500°C, and a liquid hourly space velocity of 3.34 h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :83%,CO 2 :35%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0081] Embodiment 26:

[0082] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The preparation method, reduction temperature and reduction time of the -CaO catalyst are the same as those in Example 5 and will not be described in detail. The difference is that the experimental conditions are a water-carbon ratio of 5, a reaction temperature of 600°C, and a liquid hourly space velocity of 1.67 h -1 , experimental studies have found that the gas yield in the initial stage of the reaction is: H 2 :83%,CO 2 :40%, CO and CH have not been detected 4 , the reaction activity decreases rapidly with the increase of reaction time.

[0083] Embodiment 27:

[0084] In this embodiment, Ni-Mg / Ca 2 Fe 2 O 5 The preparation method, reduction temperature and reduction time of the -CaO catalyst are the same as those in Example 5 and will not be described in detail. The difference is that the reaction time is 20 h. The reaction maintains a hydrogen yield of 82%, indicating that the catalyst has good stability and catalytic activity, but is lower than that of Ni-Mg / CaFe 2 O 4 The activity is significantly lower.

[0085] The above 27 implementation cases show that the hydrogen yield is related to the synergistic effect of the catalyst active components and the molar ratio of Ca / Fe in the Ca-Fe oxygen carrier. When Ca / Fe=1:2, the loaded Ni-Mg component is beneficial to the interaction with CaFe.2 O 4 Under the conditions of multiple calcinations, strong interactions occur to generate NiFe 2 O 4 , NiMgO 2 With Ca 2 Fe 2 O 5 , Ni-Mg / CaFe after reduction 2 O 4 The catalyst mainly contains Ni-Fe, Ni-Mg alloy and Ca 2 Fe 2 O 5 On the contrary, the catalytic activity of the catalyst with a single oxygen carrier or only Ni active component is limited, and the double alloy cannot be generated after the active component is impregnated once and then calcined and reduced. The examples also show that even if the active component is impregnated in equal volumes in steps, for Ca / Fe with a molar ratio of 1:1 and 2:1, the 2 Fe 2 O 5 With Ca 2 Fe 2 O 5 -CaO carrier, due to the relatively small amount of Fe, the activity of Ni-Fe alloy is limited, and the synergistic effect of the dual alloy and the carrier is limited. This is true regardless of the different preparation methods and reaction conditions. The catalyst activity is higher than that of Ni-Mg / CaFe 2 O 4 The activity is obviously worse. The Ni-Mg / CaFe prepared by the present invention 2 O 4 The dual alloy catalyst can significantly improve the hydrogen yield, water-gas shift reaction activity and catalyst carbon deposition resistance. 2 Fe 2 O 5 The mutual cooperation can promote the byproducts of bio-oil modeling, including CO, CH 4 etc.; promote CC and CH cleavage of bio-oil and its model molecules and enhance H 2 O adsorption provides a large number of surface hydroxyl groups for adsorption, greatly increasing the gas production and hydrogen yield. 2 O helps to resist catalyst coking, the water gas shift reaction is highly active, and CO conversion is thorough. It has been verified that 3g of Ni-Mg / CaFe prepared by step-by-step equal volume impregnation method, reduced at 800℃ for 2h, with Ni impregnation mass of 15% and Mg impregnation mass of 5% 2 O 4 Relatively optimal reaction conditions: water-carbon ratio of 5, reaction temperature of 600℃, liquid hourly space velocity of 3.34h -1The reaction time was 20 hours and the catalytic activity was good. 2 O 4 The dual alloy catalyst has a good prospect for application in the catalytic steam reforming of bio-oil to produce hydrogen.

Claims

1. A multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil, characterized in that: The catalyst comprises Ni as a main active component and Mg as an auxiliary active component; the carrier is CaFe2O4 oxygen carrier; the active components and their mass percentages in the catalyst are: Ni: 5%-15%, Mg: 5%-15%, and the mass percentage of CaFe2O4 oxygen carrier is: 70-90%; the catalyst is firstly prepared by an equal volume impregnation method to obtain CaFe2O4 oxygen carrier as a carrier, and then Ni is impregnated with equal volumes of Ni 2+ ,Mg 2+ Ni-Mg / CaFe2O4 was obtained.

2. A method for preparing a multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil, characterized in that: The method comprises the following steps: (1) preparing CaFe2O4 oxygen carrier: firstly determining the saturated water absorption rate of CaO, weighing a certain mass of CaO and a certain mass of Fe(NO3)3·9H2O according to a Ca / Fe molar ratio of 1:2; secondly preparing a Fe(NO3)3·9H2O solution of a certain concentration according to the saturated water absorption rate of CaO, and impregnating an equal volume of the Fe(NO3)3·9H2O solution into CaO; mixing and stirring evenly, ultrasonically treating for 30 minutes, standing for 2-12 hours, drying in an oven at 100-150°C for 12-24 hours, and then calcining in a muffle furnace at 600-1000°C for 2-5 hours, placing the calcined sample in air to cool to room temperature, and then grinding it to a powder of >100 mesh to obtain the CaFe2O4 oxygen carrier; (2) Introduction of the main active component Ni: First, determine the saturated water absorption rate of CaFe2O4, and weigh a certain mass of Ni(NO3)2·6H2O according to the mass percentage of the Ni component; secondly, prepare a Ni(NO3)2·6H2O solution of a certain concentration according to the saturated water absorption rate of CaFe2O4, and impregnate an equal volume of the Ni(NO3)2·6H2O solution into CaFe2O4; mix and stir evenly, treat with ultrasound for 30 minutes, let stand for 2-12 hours, dry in an oven at 100-150°C for 12-24 hours, and then calcine in a muffle furnace at 600-1000°C for 2-5 hours. The calcined sample is placed in air to cool to room temperature, and ground into a powder of >100 mesh to obtain Ni / CaFe2O4; (3) Introduction of auxiliary active component Mg: First, determine the saturated water absorption rate of Ni / CaFe2O4, and weigh a certain mass of Mg(NO3)2·6H2O according to the mass percentage of Mg component; secondly, prepare a certain concentration of Mg(NO3)2·6H2O solution according to the saturated water absorption rate of Ni / CaFe2O4, and impregnate an equal volume of Mg(NO3)2·6H2O solution into Ni / CaFe2O4; mix and stir evenly, treat with ultrasound for 30 min, let stand for 2~12 h, dry in an oven at 100~150℃ for 12~24 h, and then calcine in a muffle furnace at 600~1000℃ for 2~5 h, place the calcined sample in air to cool to room temperature, grind and sieve to 30~40 mesh particles to obtain Ni-Mg / CaFe2O4 catalyst with active component and mass percentage of Ni: 5%~15%, Mg: 5%~15%, and mass percentage of carrier of CaFe2O4: 70~90%.

3. An application of the multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil as claimed in claim 1, characterized in that: The catalyst is used in hydrogen production by catalytic reforming of bio-oil with water vapor.

4. The use of the multifunctional dual alloy catalyst for hydrogen production by steam reforming of bio-oil according to claim 3, characterized in that: The application process conditions are: reaction temperature of 600-800°C, water-carbon ratio of 2.5-10, liquid hourly space velocity of 1.67-5.01h -1 .