Process liquid composition for extreme ultraviolet lithography and pattern forming method using the same

By using a combined liquid of nonionic surfactant and alkaline substance with HLB values ​​of 9 to 16 in the extreme ultraviolet exposure process, the problem of photoresist pattern collapse is solved, and the pattern stability and process margin are significantly improved. , reduces production costs.

CN112272799BActive Publication Date: 2024-11-22YOUNG CHANG CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980038436.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-14
Filing Date
2019-05-22
Publication Date
2024-11-22
Estimated Expiration
2039-05-22

AI Technical Summary

Technical Problem

In semiconductor manufacturing processes, the photoresist pattern is prone to collapse under extreme ultraviolet exposure light sources, resulting in a decrease in process margin, and the existing photoresist performance is difficult to meet the needs of fine pattern formation.

Method used

By studying the HLB value of nonionic surfactants and the types and content of alkaline substances, combined with the use of pure water, a combination of nonionic surfactants with HLB values ​​of 9 to 16 and 0.0001 to 1% alkaline substances was prepared by studying the HLB value of nonionic surfactants with HLB values ​​of 9 to 16 and 0.0001 to 1% alkaline substances with an HLB value of 0.0001 to 1% were prepared. Liquid, used to reduce pattern collapse and improve the development effect of photoresist.

Benefits of technology

It effectively reduces the collapse degree of the photoresist pattern, improves line width roughness and defects, reduces production costs, and improves the uniformity and transparency of the process liquid, significantly improving the stability of the pattern.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002825569470000051
    Figure BDA0002825569470000051
  • Figure BDA0002825569470000061
    Figure BDA0002825569470000061
  • Figure BDA0002825569470000062
    Figure BDA0002825569470000062
Patent Text Reader

Abstract

The present invention relates to a process liquid composition for reducing the collapse of a photoresist pattern including polyhydroxystyrene defined by an extreme ultraviolet light exposure light source and a pattern forming method using the same, wherein the process liquid composition comprises: 0.0001 to 1 weight % of a nonionic surfactant having an HLB value of 9 to 16; 0.0001 to 1 weight % of an alkaline substance selected from the group consisting of tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide or a mixture thereof; and 98 to 99.9998 weight % of water. The present invention has the effect of reducing the collapse of a photoresist pattern including polyhydroxystyrene defined by an extreme ultraviolet light exposure light source.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a process liquid composition for reducing the collapse of a photoresist pattern including polyhydroxystyrene and used in an extreme ultraviolet light exposure light source in a semiconductor manufacturing process, and a pattern forming method using the composition. Background Art

[0002] In the process of manufacturing semiconductors, in order to form finer patterns, a light source with a smaller wavelength band is required. At present, photolithography technology using extreme ultraviolet (EUV, extreme ultra violet, wavelength of 13.5nm) light source is widely used, and it can achieve finer patterns. However, since the etching resistance of photoresists used for extreme ultraviolet light has not been improved, photoresist patterns with large aspect ratios are still required, so pattern collapse is prone to occur during development, resulting in a significant reduction in process margin in the manufacturing process.

[0003] Therefore, it is necessary to develop a technology for improving the collapse that occurs during fine pattern formation. Although the best way to improve the degree of pattern collapse is to improve the performance of the photoresist, the fact that it is currently difficult to newly develop a photoresist that satisfies all performances cannot be ignored.

[0004] While there remains a need to develop new and superior photoresists, efforts are being made to improve the degree of pattern collapse by other methods. Summary of the invention

[0005] Problem to be solved

[0006] The object of the present invention is to provide a method and a process liquid composition for improving pattern collapse occurring in photoresist development in a fine pattern process using extreme ultraviolet light.

[0007] Another object of the present invention is to provide a method for forming a photoresist pattern having excellent quality using the process liquid composition as described above.

[0008] Solutions to the problem

[0009] In the present invention, a process liquid composition for reducing the collapse of a photoresist pattern including polyhydroxystyrene defined by an extreme ultraviolet light exposure light source is developed, with an eye on the type, content and HLB value of a nonionic surfactant, an eye on the type and content of an alkaline substance, and an eye on the content of pure water, and as a result of continuous research and experiments, the problem of the present invention is solved.

[0010] Various surfactants have been used in aqueous type washing liquids used in the development process, but in the present invention, various studies were conducted with an eye on the HLB (Hydrophilic-Lipohilic Balance) value, and as a result, an effective washing liquid was prepared using a nonionic surfactant with an HLB value of 9 to 16.

[0011] A representative method for distinguishing the characteristics between nonionic surfactants includes HLB value. The range of HLB value is distinguished from 0 to 20. The closer the HLB value is to 0, the stronger the hydrophobicity (lipophilicity) of the nonionic surfactant is, and the closer the HLB value is to 20, the stronger the hydrophilicity of the nonionic surfactant is.

[0012] When a nonionic surfactant that tends to be hydrophobic is used in a water-based cleaning liquid that mainly uses ultrapure water, it is possible to induce hydrophobicity of the photoresist wall surface, thereby inducing a reduction in the melting and collapse of the pattern. However, the tendency of nonionic surfactants to aggregate with each other becomes stronger, resulting in uneven physical properties of the cleaning liquid, so there is a concern that defects may occur during use due to the aggregated nonionic surfactants.

[0013] In the present invention, it was confirmed that the smaller the HLB value of the nonionic surfactant, the more significant the effect of improving pattern collapse. However, when excessive nonionic surfactants are used or the HLB value is below 8, it was confirmed that the surfactants aggregated with each other in the aqueous type washing liquid mainly using ultrapure water.

[0014] On the contrary, when a nonionic surfactant tending to be hydrophilic is used, it can be uniformly dispersed in a water-based cleaning liquid mainly using ultrapure water without aggregation to prepare a cleaning liquid with uniform physical properties, and after exposure and development, the surfactant is adsorbed on a part of the hydrophilized photoresist wall surface to reduce the capillary force, thereby improving pattern collapse. However, when a surfactant with excessive hydrophilicity is used, there is a concern that it may cause the photoresist pattern to melt, and may eventually cause pattern collapse.

[0015] In the present invention, various studies and experiments have been conducted, and it has been confirmed that the ability to reduce pattern collapse is insufficient when the HLB value of the nonionic surfactant is 17 or more.

[0016] As a representative developer used in most photolithography processes, tetramethylammonium hydroxide is diluted with pure water to a certain concentration. In most processes, 2.38% by weight of tetramethylammonium hydroxide is mixed with 97.62% by weight of water. In the extreme ultraviolet photolithography process, tetramethylammonium hydroxide is also diluted with pure water and used as a developer.

[0017] In the present invention, it was confirmed that pattern collapse occurs when washing is continuously performed with pure water alone after development in an EUV lithography process.

[0018] Furthermore, it was confirmed that pattern collapse also occurs in the EUV lithography process when a cleaning solution including tetramethylammonium hydroxide in pure water is used continuously after development, or when a cleaning solution including tetramethylammonium hydroxide in pure water is used continuously after washing with pure water alone.

[0019] Based on this result, it can be inferred that in the case of a cleaning solution including tetramethylammonium hydroxide in pure water, a fine pattern exposed by extreme ultraviolet light is weakened and the pattern collapses due to a large or uneven capillary force.

[0020] In the present invention, in order to improve the pattern collapse exposed by extreme ultraviolet light and additionally improve the LWR (Line Width Roughness) and defects of the photoresist pattern required in the extreme ultraviolet light process, it is recognized that the necessity of exploring the force given to the pattern exposed by extreme ultraviolet light by an alkaline substance that is relatively weaker than tetramethylammonium hydroxide is necessary, and research and experiments on this are continuously conducted.

[0021] In the present invention, it was confirmed that when tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide, which are alkaline substances excluding tetramethylammonium hydroxide, are used, LWR and defects are improved without causing pattern collapse.

[0022] Accordingly, as a first preferred embodiment of the present invention, a cleaning solution is provided for reducing the degree of pattern collapse occurring during photoresist development, comprising: 0.0001 to 1 weight % of an alkaline substance selected from the group consisting of tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide or a mixture thereof; 0.0001 to 1 weight % of a nonionic surfactant having an HLB value of 9 to 16; and 98 to 99.9998 weight % of water.

[0023] The surfactant in the above embodiment may be a nonionic surfactant.

[0024] The nonionic surfactant in the above embodiment may be selected from the group consisting of polyoxyethylene alkyl ether, polyoxypropylene alkyl ether, polyoxyethylene oxypropylene alkyl ether or a mixture thereof.

[0025] The HLB value of the polyoxyethylene alkyl ether, polyoxypropylene alkyl ether, and polyoxyethylene oxypropylene alkyl ether in the above embodiment may be 9 to 16.

[0026] In addition, the present invention also provides a method for forming a photoresist pattern, comprising the following steps: (a) coating a photoresist on a semiconductor substrate to form a film; (b) exposing the photoresist film and then developing it to form a pattern; and (c) washing the photoresist pattern using the photolithography process liquid composition.

[0027] The cause of the pattern collapse is believed to be the capillary force generated between the patterns when the patterns are washed with pure water after development. However, it was confirmed that the pattern collapse cannot be completely improved simply by reducing the capillary force.

[0028] When an inappropriate surfactant is used excessively for the purpose of reducing the surface tension of the cleaning solution in order to reduce the capillary force, it may induce melting of the pattern and further induce pattern collapse.

[0029] In order to improve pattern collapse, it is very important to select a surfactant that reduces the surface tension of the washing solution while preventing the melting of the photoresist pattern.

[0030] The cleaning liquid of the present invention has an excellent effect on photoresists using an extreme ultraviolet light source, and in particular has a particularly effective effect of reducing the degree of pattern collapse that occurs during the development of photoresists whose main component resin is polyhydroxystyrene.

[0031] Effects of the Invention

[0032] The process liquid composition for lithography of the present invention is helpful for forming a photoresist pattern including polyhydroxystyrene defined by an extreme ultraviolet light exposure light source. In particular, by adding a simple process, the effect of pattern collapse that is difficult to achieve with a single photoresist can be reduced, thereby saving production costs.

[0033] Best Mode for Carrying Out the Invention

[0034] Hereinafter, the present invention will be described in more detail.

[0035] The invention relates to a process liquid for reducing the degree of pattern collapse occurring in the development of a photoresist, comprising: 0.0001 to 1 weight percent of an alkaline substance, wherein the alkaline substance is selected from the group consisting of tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide or a mixture thereof; 0.0001 to 1 weight percent of a nonionic surfactant having an HLB (Hydrophile-Lipophile Balance) value of 9 to 16; and 98 to 99.9998 weight percent of water.

[0036] Hereinafter, preferred examples and comparative examples of the present invention will be described. However, the following examples are merely preferred examples of the present invention, and the present invention is not limited to the following examples. DETAILED DESCRIPTION

[0037] Examples and Comparative Examples

[0038] [Example 1]

[0039] A process liquid for improving the collapse degree of a photoresist pattern is prepared by the following method. The process liquid includes 0.01 wt % of polyoxyethylene alkyl ether having an HLB value of 9 and 0.01 wt % of tetrabutylammonium hydroxide.

[0040] 0.01 wt % of polyoxyethylene alkyl ether with an HLB value of 9 and 0.01 wt % of tetrabutylammonium hydroxide were added to 99.98 wt % of distilled water, stirred for 5 hours, and then passed through a 0.01 μm filter to remove fine solid impurities, thereby preparing a process liquid for improving the degree of collapse of a photoresist pattern.

[0041] [Example 2 to Example 20]

[0042] According to the compositions described in Tables 1 to 5, process liquids for improving the degree of collapse of a photoresist pattern similar to Example 1 were prepared.

[0043] [Comparative Example 1]

[0044] Pure water (distilled water) generally used as a final process liquid in a development process in a semiconductor device manufacturing process is prepared.

[0045] [Comparative Example 2 to Comparative Example 9]

[0046] For comparison with the examples, process liquids were prepared according to the compositions described in Tables 1 to 5 in the same manner as in Example 1.

[0047]

Table 1

[0048]

[0049]

[0050]

Table 2

[0051]

[0052]

[0053]

Table 3

[0054]

[0055]

Table 4

[0056]

[0057]

Table 5

[0058]

[0059] Experimental examples and comparative experimental examples

[0060] The process liquid composition prepared in Examples 1 to 20 and Comparative Examples 1 to 9 is used to wash the pattern formed by the steps of forming a film by coating a photoresist on a semiconductor substrate; and forming a pattern by developing after exposing the photoresist film. Then, the degree of pattern collapse and the ratio of defect reduction are measured for the silicon wafer with the pattern. The results are shown in Table 6 as Experimental Examples 1 to 20 and Comparative Experimental Examples 1 to 9.

[0061] (1) Confirmation of prevention of pattern collapse

[0062] After the exposure energy and focus were separated, the number of blocks without pattern collapse among all 89 blocks was measured using a critical dimension scanning electron microscope (CD-SEM, Hitachi).

[0063] (2) Defect ratio

[0064] For the photoresist patterns cleaned with respective cleaning liquid reagents, the number of defects (A) was measured using a surface defect observation device (product of KLA Tcncor) and expressed as a percentage (%) of the number of defects (B) when cleaning was performed only with pure water, that is, expressed as (A / B)×100.

[0065] The number of defects after treatment with pure water alone is taken as 100% as the benchmark, and the degree of reduction or increase compared to 100% of the number of defects when treated with pure water alone is expressed as a percentage as the defect number ratio (reduction ratio or increase ratio). The lower the value, the better.

[0066] (3) Transparency

[0067] The transparency of the prepared washing liquid was confirmed visually and indicated as transparent or opaque.

[0068]

Table 6

[0069]

[0070]

[0071] Experimental Examples 1 to 8 were compared with Comparative Experimental Examples 1 to 3. As a result, it was confirmed that when the HLB value of the surfactant was 9 to 16, the number of blocks without pattern collapse increased, the number of defects decreased, and all were transparent. In particular, it was confirmed that when the HLB value was 9 to 13, a more excellent effect was achieved.

[0072] Experimental Examples 2, 9 to 12 were compared with Comparative Experimental Examples 4 and 5. As a result, it was confirmed that when the content of the surfactant was 0.0001 to 1 wt %, the number of blocks without pattern collapse increased, the number of defects decreased, and all were transparent.

[0073] Experimental Examples 2, 13 to 16 were compared with Comparative Experimental Examples 6 and 7. As a result, it was confirmed that when the content of the alkaline substance was 0.0001 to 1 wt %, the number of blocks without pattern collapse increased, the number of defects decreased, and all were transparent.

[0074] Experimental Examples 2, 17, and 18 were compared with Comparative Experimental Example 1. As a result, it was confirmed that when the surfactant was polyoxyethylene alkyl ether, polyoxypropylene alkyl ether, or polyoxyethylene oxypropylene alkyl ether, the number of blocks without pattern collapse increased, the number of defects decreased, and all were transparent. In particular, when the surfactant was polyoxyethylene alkyl ether, a more excellent effect was confirmed.

[0075] Experimental Examples 2, 19, and 20 were compared with Comparative Experimental Examples 8 and 9. As a result, it was confirmed that when the alkaline substance was tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide, the number of blocks without pattern collapse increased, the number of defects decreased, and all were transparent. In particular, when the alkaline substance was tetrabutylammonium hydroxide, a more excellent effect was confirmed.

[0076] On the other hand, the pattern collapse evaluation results of Example 2 confirmed that the number of blocks without pattern collapse was 77, which showed a very excellent effect.

[0077] In contrast, the pattern collapse evaluation results of Comparative Example 1 showed that the number of blocks where pattern collapse did not occur was 46, indicating an unfavorable effect.

[0078] Above, specific parts of the content of the present invention are described in detail, so for those skilled in the art, these specific technologies are only preferred embodiments, and it is self-evident that the scope of the present invention is not limited thereto. Therefore, the essential scope of the present invention will be limited by the attached claims and their equivalents.

Claims

1. A cleaning process liquid composition for reducing the collapse of a photoresist pattern comprising polyhydroxystyrene defined by an extreme ultraviolet exposure light source, characterized in that The process liquid composition consists of: 0.0001 to 1% by weight of a nonionic surfactant having an HLB value of 9 to 13, wherein the nonionic surfactant is a polyoxyethylene alkyl ether; 0.0001 to 1% by weight of an alkaline substance, wherein the alkaline substance is tetrabutylammonium hydroxide; and 98 to 99.9998% by weight of water.

2. A method for forming a photoresist pattern, comprising the following steps: (a) coating a photoresist on a semiconductor substrate to form a film; (b) exposing the photoresist film and then developing it to form a pattern; and (c) cleaning the photoresist pattern using the cleaning process liquid composition according to claim 1.

3. The method for forming a photoresist pattern according to claim 2, wherein: The exposure light source is extreme ultraviolet light.