Solid oxide fuel cell and method for manufacturing the same

By using a laminated structure of metal support and ceramic mixed layer in solid oxide fuel cells, the durability problem of the battery under high temperature and mechanical impact is solved, and more stable battery performance is achieved.

CN112447982BActive Publication Date: 2024-11-15TAIYO YUDEN KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202010884982.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-30
Filing Date
2020-08-28
Publication Date
2024-11-15
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

Solid oxide fuel cells are prone to interlayer peeling under high temperature and mechanical impact, and are difficult to withstand thermal shock and vibration. The prior art is difficult to effectively solve the durability problem of ceramic batteries.

Method used

A mixed layer composed of a metal support layer and a ceramic material is fired in a high-temperature reduction atmosphere through a laminated structure to form a mixed layer of metal and ceramic material, thereby enhancing the adhesion and durability of the electrode framework.

Benefits of technology

It effectively suppresses the interlayer peeling between the support and the anode, improves the durability and stability of the fuel cell, and ensures performance under high temperature and mechanical impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112447982B_ABST
    Figure CN112447982B_ABST
Patent Text Reader

Abstract

The present invention provides a solid oxide fuel cell capable of suppressing interlayer delamination and a method for manufacturing the same. The solid oxide fuel cell is characterized in that it includes: a support layer with a metal as a main component; an anode supported by the support; and a mixed layer provided between the support and the anode, wherein the anode has an electrode skeleton composed of a ceramic material, the ceramic material includes a first oxide with electron conductivity and a second oxide with oxygen ion conductivity, and the mixed layer has a structure in which a metal material and a ceramic material are mixed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid oxide fuel cell and a method for manufacturing the same. Background Art

[0002] A solid oxide fuel cell includes a solid oxide electrolyte layer having oxygen ion conductivity, an anode and a cathode. In the anode, oxygen ions from the cathode through the solid oxide electrolyte layer react with hydrogen contained in the fuel gas. This reaction generates electricity.

[0003] In the commonly used metal ceramic electrode of Ni and ion-conducting oxide, when fuel starvation occurs, Ni may be locally oxidized to NiO, causing the single cell to rupture due to volume expansion. Therefore, anodes that do not use Ni in the electrode skeleton are also being developed.

[0004] For example, the following fuel electrode (anode) is disclosed, which has a first oxide (electron conductive oxide) with electron conductivity and a second oxide (ion conductive oxide) with ion conductivity as an electrode skeleton, and a composite catalyst is introduced into the electrode skeleton by an impregnation method, wherein the first oxide is composed of a titanate perovskite-type oxide, the second oxide is composed of CeO2 doped with Gd2O3 or Sm2O3, and the composite catalyst dispersedly carries a metal catalyst such as Ni (electrode catalyst metal) and contains a third oxide with ion conductivity (for example, refer to patent documents 1 to 3).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-55946

[0008] Patent Document 2: Japanese Patent Application Publication No. 2012-33418

[0009] Patent Document 3: Japanese Patent Application No. 2009-541955 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] In the above-mentioned anode, the electrode skeleton is a sintered body of an ion conductive oxide and an electron conductive oxide, and does not undergo a volume change in a high-temperature reducing atmosphere, thereby avoiding electrode destruction. Moreover, in the composite catalyst introduced by the impregnation method, the metal catalyst is supported and fixed by the oxide, and the aggregation of the metal catalyst is suppressed.

[0012] However, the entire material of the single cell including the support is composed of ceramics, and therefore, it is usually fired in an atmospheric atmosphere. Even if the rupture of the single cell caused by the volume expansion of Ni oxidation is prevented by dispersively supporting the metal catalyst on the electrode skeleton composed of the electron conductive oxide and the ion conductive oxide, it is difficult to solve the fundamental problem that the ceramic solid oxide fuel cell cannot withstand thermal shock and mechanical shock. On the other hand, the metal-supported single cell that can withstand vibration and shock and can withstand rapid temperature rise and fall is fired in a strong reducing atmosphere. When the perovskite-type titanate oxide is fired in a reducing atmosphere, the perovskite-type titanate oxide has poor adhesion to the metal support layer, and interlayer peeling may occur.

[0013] Means for solving technical problems

[0014] The solid oxide fuel cell of the present invention is characterized in that it includes: a support layer with metal as the main component; an anode supported by the support; and a mixed layer arranged between the support and the anode, the anode having an electrode skeleton composed of a ceramic material, the ceramic material containing a first oxide with electron conductivity and a second oxide with oxygen ion conductivity, and the mixed layer having a structure in which a metal material and a ceramic material are mixed.

[0015] The manufacturing method of the solid oxide fuel cell of the present invention is characterized in that it includes: a step of preparing a stacked body, in which a support body raw sheet, a mixed layer raw sheet and an anode raw sheet are stacked, the support body raw sheet contains metal material powder, the mixed layer raw sheet contains metal material powder and ceramic material powder, and the anode raw sheet contains ceramic material powder; and a step of firing the stacked body to form a support body from the support body raw sheet, a mixed layer from the mixed layer raw sheet, and an electrode skeleton composed of the ceramic material from the anode raw sheet. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a schematic cross-sectional view showing the stacked structure of a fuel cell.

[0017] Figure 2 It is an enlarged cross-sectional view showing details of the support, the mixed layer, and the anode.

[0018] Figure 3 This is a diagram showing the flow of a method for manufacturing a fuel cell.

[0019] Figure 4 It is a figure which shows the manufacturing conditions and results of Examples 1-10 and Comparative Examples 1 and 2.

[0020] Description of Reference Numerals

[0021] 10...support body, 20...mixed layer, 21...metal material, 22...ceramic material, 30...anode, 31...first oxide, 32...second oxide, 33...third oxide, 34...catalyst metal, 40...electrolyte layer, 50...reaction prevention layer, 60...cathode, 100...fuel cell. DETAILED DESCRIPTION

[0022] Hereinafter, embodiments will be described with reference to the drawings.

[0023] Figure 1 is a schematic cross-sectional view showing the stacked structure of the solid oxide fuel cell 100. Figure 1 As shown, as an example, the fuel cell 100 has a structure in which a mixed layer 20, an anode 30, an electrolyte layer 40, a reaction prevention layer 50, and a cathode 60 are sequentially stacked on a support 10. A plurality of fuel cells 100 can be stacked to form a fuel cell stack.

[0024] The electrolyte layer 40 is a gas-impermeable dense layer with a solid oxide having oxygen ion conductivity as the main component. Preferably, the electrolyte layer 40 has scandium oxide-yttria-stabilized zirconia (ScYSZ) and the like as the main component. When the concentration of Y2O3+Sc2O3 is between 6 mol% and 15 mol%, the oxygen ion conductivity is the highest, so it is preferred to use a material of this composition. The thickness of the electrolyte layer 40 is preferably less than 20 μm, more preferably less than 10 μm. The thinner the electrolyte layer, the better, but in order to prevent gas leakage on both sides of the electrolyte layer during manufacturing, the thickness is preferably greater than 1 μm.

[0025] The cathode 60 is an electrode having an electrode activity as a cathode, and has electron conductivity and oxygen ion conductivity. For example, the cathode 60 is LSC (lanthanum strontium cobaltate) or the like having electron conductivity and oxygen ion conductivity. LSC is LaCoO3 doped with Sr (strontium).

[0026] The reaction prevention layer 50 is mainly composed of a component that prevents the reaction between the electrolyte layer 40 and the cathode 60. For example, the reaction prevention layer 50 is mainly composed of GDC (Gd-doped cerium oxide) in which Gd (gadolinium) is doped in CeO2. As an example, when the electrolyte layer 40 contains ScYSZ and the cathode 60 contains LSC, the reaction prevention layer 50 prevents the following reaction.

[0027] Sr+ZrO2→SrZrO3

[0028] La+ZrO3→La2Zr2O7

[0029] Figure 21 is an enlarged cross-sectional view showing details of the support 10, the mixed layer 20 and the anode 30. Figure 2 As shown, the support 10 is a member having gas permeability and capable of supporting the mixed layer 20, the anode 30, the electrolyte layer 40, the reaction prevention layer 50, and the cathode 60. The support 10 is a porous metal body, for example, a porous body of Fe-Cr alloy.

[0030] The anode 30 is an electrode having electrode activity as an anode, and has an electrode skeleton of a ceramic material. The electrode skeleton does not contain a metal component. With this structure, when fired in a high-temperature reducing atmosphere, it is possible to suppress the reduction of the porosity of the anode caused by the coarsening of the metal component. In addition, it is possible to suppress the formation of an alloy with the metal component of the support 10, and suppress the reduction of the catalyst function.

[0031] The electrode skeleton of the anode 30 preferably has electron conductivity and oxygen ion conductivity. The anode 30 preferably contains a first oxide 31 as an electron conductive material. As the first oxide 31, for example, a perovskite oxide represented by a composition formula of ABO3 can be used, wherein the A position is at least one selected from Ca, Sr, Ba and La, and the B position is at least one selected from Ti and Cr. The molar ratio of the A position to the B position can be such that the molar ratio of the B position ≥ the molar ratio of the A position. Specifically, as the first oxide 31, LaCrO3-based materials, LaTiO3-based materials, etc. can be used.

[0032] In addition, the electrode skeleton of the anode 30 preferably contains a second oxide 32 as an oxygen ion conductive material. The second oxide 32 is ScYSZ or the like. For example, it is preferred to use ScYSZ having a composition range of 5 mol% to 16 mol% of scandium oxide (Sc2O3) and 1 mol% to 3 mol% of yttrium oxide (Y2O3). ScYSZ in which the total amount of scandium oxide and yttrium oxide added is 6 mol% to 15 mol% is further preferred. This is because within this composition range, the oxygen ion conductivity is the highest. The oxygen ion conductive material is, for example, a material having an oxygen ion migration number of 99% or more. As the second oxide 32, GDC or the like can be used. Figure 2 In the example of FIG. 1 , as the second oxide 32 , the same solid oxide as that contained in the electrolyte layer 40 is used.

[0033] like Figure 2As shown, in the anode 30, for example, the first oxide 31 and the second oxide 32 form an electrode skeleton. A plurality of voids are formed by the electrode skeleton. A catalyst is carried on the surface of the electrode skeleton in the void portion. Therefore, in the electrode skeleton formed continuously in space, a plurality of catalysts are arranged in a spatially dispersed manner. As the catalyst, a composite catalyst is preferably used. For example, as a composite catalyst, a third oxide 33 having oxygen ion conductivity and a catalyst metal 34 are preferably carried on the surface of the electrode skeleton. As the third oxide 33, for example, BaCe doped with Y can be used. 1-x Zr x O3 (BCZY, x = 0 to 1), SrCe doped with Y 1-x Zr x O3 (SCZY, x = 0 ~ 1), LaScO3 doped with Sr (LSS), GDC, etc. As the catalyst metal 34, Ni, etc. can be used. The third oxide 33 can have the same composition as the second oxide 32, or it can have a composition different from the second oxide 32. The metal that acts as the catalyst metal 34 can be in the form of a compound when no power is generated. For example, Ni can be in the form of NiO (nickel oxide). These compounds are reduced by the reducing fuel gas supplied to the anode 30 during power generation and become in the form of a metal that acts as an anode catalyst.

[0034] The mixed layer 20 contains a metal material 21 and a ceramic material 22. In the mixed layer 20, the metal material 21 and the ceramic material 22 are randomly mixed. Therefore, the structure is not formed in which a layer of the metal material 21 and a layer of the ceramic material 22 are stacked. A plurality of voids are also formed in the mixed layer 20. The metal material 21 is not particularly limited as long as it is a metal. Figure 2 In the example of , as the metal material 21, the same metal material as the support 10 is used. As the ceramic material 22, the first oxide 31, the second oxide 32, etc. can be used. For example, as the ceramic material 22, ScYSZ, GDC, LaTiO3-based materials, LaCrO3-based materials, etc. can be used. LaTiO3-based materials and LaCrO3-based materials have high electronic conductivity, and therefore, the ohmic resistance in the mixed layer 20 can be reduced.

[0035] The fuel cell 100 generates electricity through the following actions. An oxidant gas containing oxygen, such as air, is supplied to the cathode 60. In the cathode 60, the oxygen reaching the cathode 60 reacts with electrons supplied from an external circuit to become oxygen ions. The oxygen ions are conducted in the electrolyte layer 40 and migrate to the anode 30 side. On the other hand, a hydrogen-containing fuel gas, such as hydrogen gas and reformed gas, is supplied to the support 10. The fuel gas reaches the anode 30 via the support 10 and the mixing layer 20. The hydrogen reaching the anode 30 releases electrons in the anode 30 and reacts with oxygen ions conducted in the electrolyte layer 40 from the cathode 60 side to become water (H2O). The released electrons are taken out to the outside by the external circuit. The electrons taken out to the outside are supplied to the cathode 60 after performing electrical work. Electricity is generated through the above-mentioned actions.

[0036] In the above-mentioned power generation reaction, the catalyst metal 34 functions as a catalyst in the reaction between hydrogen and oxygen ions. The first oxide 31 is responsible for conducting electrons obtained by the reaction between hydrogen and oxygen ions. The second oxide 32 is responsible for conducting oxygen ions from the electrolyte layer 40 to the anode 30.

[0037] In the fuel cell 100 of the present embodiment, the support body 10 is mainly composed of metal, and the electrode skeleton of the anode 30 is composed of ceramic. In such a structure, when the support body 10 and the anode 30 are fired in a manner in which they are in contact, interlayer peeling may occur between the support body 10 and the anode 30 due to the difference in material properties between the metal and the ceramic. In particular, the ceramic fired in a strong reducing atmosphere has poor adhesion to the metal. In the fuel cell 100 of the present embodiment, a mixed layer 20 is provided between the support body 10 and the anode 30. The mixed layer 20 contains a metal material 21 and a ceramic material 22, and therefore has both the material properties of the metal and the material properties of the ceramic. Therefore, the mixed layer 20 has high adhesion with the support body 10, and has high adhesion with the anode 30. According to the above, interlayer peeling between the support body 10 and the anode 30 can be suppressed.

[0038] When the area ratio of the metal material 21 in the mixed layer 20 is too low, the adhesion between the support 10 and the mixed layer 20 may not be sufficiently obtained. Therefore, it is preferable to set a lower limit for the area ratio of the metal material 21 in the mixed layer 20. On the other hand, when the area ratio of the ceramic material 22 in the mixed layer 20 is too low, the adhesion between the mixed layer 20 and the anode 30 may not be sufficiently obtained. Therefore, it is preferable to set a lower limit for the area ratio of the ceramic material 22 in the mixed layer 20. For example, it is preferable that in the mixed layer 20, the area ratio between the metal material 21 and the ceramic material 22 is 1:9 to 9:1. For example, the area ratio of the metal material 21 excluding the voids in the mixed layer 20 {metal material area / (metal material area+ceramic material area)} is preferably 10% or more, more preferably 25% or more, and further preferably 40% or more. The area ratio of the ceramic material 22 excluding the voids in the mixed layer 20 is preferably 10% or more, more preferably 25% or more, and further preferably 40% or more.

[0039] When the mixed layer 20 is too thin, sufficient adhesion between the support 10 and the anode 30 may not be obtained. Therefore, it is preferable to set a lower limit for the thickness of the mixed layer 20. For example, the mixed layer 20 preferably has a thickness of 1 μm or more, more preferably 3 μm or more, and further preferably 4 μm or more.

[0040] In addition, in the fuel cell 100 of the present embodiment, the third oxide 33 is carried on the electrode skeleton of the anode 30. With this structure, the electrode skeleton can be first formed by firing, and then the third oxide 33 is impregnated and fired at a low temperature. Therefore, even if the second oxide 32 and the third oxide 33 do not have the same composition, the reaction between the oxides can be suppressed. Therefore, as the third oxide 33, the degree of freedom of selecting an oxide suitable for the composite catalyst becomes larger.

[0041] In addition, it is preferred that the relationship of the porosity in the support 10 > the porosity in the mixed layer 20 > the porosity in the anode 30 is established among the porosity in the support 10, the porosity in the mixed layer 20, and the porosity in the anode 30. By establishing this relationship, sufficient gas permeability can be obtained in the support 10. By having a relatively low porosity, the anode 30 can maintain gas permeability and obtain high electron conductivity and high oxygen ion conductivity. In the mixed layer 20, gas permeability can be obtained, and a contact area with the support 10 can be obtained to obtain close adhesion with the support 10. The porosity is a number calculated by the ratio of the estimated area of ​​the voids to the overall area based on the SEM image of the sample cross section.

[0042] Next, a method for manufacturing the fuel cell 100 will be described. Figure 3 It is a diagram showing the flow of a method for manufacturing the fuel cell 100 .

[0043] (Process for producing support material)

[0044] As a material for a support body, metal powder (for example, with a particle size of 10 μm to 100 μm), a plasticizer (for example, adjusted to 1 wt% to 6 wt% in order to adjust the adhesion of the sheet), a solvent (toluene, 2-propanol (IPA), 1-butanol, pine alcohol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% corresponding to the viscosity), a vanishing material (organic matter), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The material for a support body is used as a material for forming the support body 10. The volume ratio of the organic component (vanishing material, binder solid component, plasticizer) to the metal powder is, for example, in the range of 1:1 to 20:1, and the amount of the organic component is adjusted according to the porosity.

[0045] (Process for producing mixed layer material)

[0046] As materials for the mixed layer, ceramic material powder (e.g., with a particle size of 100 nm to 10 μm) as a raw material of the ceramic material 22, small-particle metal material powder (e.g., with a particle size of 1 μm to 10 μm) as a raw material of the metal material 21, a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% according to the viscosity), a plasticizer (e.g., adjusted to 1 wt% to 6 wt% in order to adjust the adhesion of the sheet), a vanishing material (organic matter) and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic component (vanishing material, binder solid component, plasticizer) to the metal powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic component is adjusted according to the porosity. The pore size of the void can be controlled by adjusting the particle size of the vanishing material. The ceramic material powder may contain an electron conductive material powder and an oxide ion conductive material powder. In this case, the volume ratio of the electron conductive material powder to the oxide ion conductive material powder is preferably in the range of 1:9 to 9:1, for example. Even if electrolyte materials such as ScYSZ and GDC are used instead of the electron conductive material, it is possible to produce a single cell without interface peeling. However, from the viewpoint of reducing ohmic resistance, it is preferred to mix the electron conductive material with the metal powder.

[0047] (Process for producing anode material)

[0048] As the material for the anode, a ceramic material powder constituting the electrode skeleton, a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20wt% to 30wt% according to the viscosity), a plasticizer (for example, adjusted to 1wt% to 6wt% in order to adjust the adhesion of the sheet), a vanishing material (organic matter) and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. As the ceramic material powder constituting the electrode skeleton, an electron conductive material powder (for example, with a particle size of 100nm to 10μm) as a raw material of the first oxide 31, an oxygen ion conductive material powder (for example, with a particle size of 100nm to 10μm) as a raw material of the second oxide 32, etc. can be used. The volume ratio of the organic component (vanishing material, binder solid component, plasticizer) to the electron conductive material powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic component is adjusted according to the porosity. The pore size of the void can be controlled by adjusting the particle size of the vanishing material. The volume ratio of the electron conductive material powder to the oxygen ion conductive material powder is, for example, in the range of 3:7 to 7:3.

[0049] (Process for producing electrolyte layer material)

[0050] As a material for the electrolyte layer, an oxygen ion conductive material powder (e.g., ScYSZ, YSZ, GDC, etc., with a particle size of 10nm to 1000nm), a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20wt% to 30wt% according to the viscosity), a plasticizer (e.g., adjusted to 1wt% to 6wt% in order to adjust the adhesion of the sheet), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic component (binder solid component, plasticizer) to the oxygen ion conductive material powder is, for example, in the range of 6:4 to 3:4.

[0051] (Process for producing cathode material)

[0052] As a cathode material, powder of lanthanum strontium cobaltate (LSC: LaSrCoO3), solvent (toluene, 2-propanol (IPA), 1-butanol, pine alcohol, butyl acetate, ethanol, etc., 20wt% to 30wt% according to the viscosity), plasticizer (for example, adjusted to 1wt% to 6wt% in order to adjust the adhesion of the sheet) and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic component (binder solid component, plasticizer) to the LSC powder is, for example, in the range of 6:4 to 1:4.

[0053] (Firing process)

[0054] First, a support sheet is prepared by coating a support material on a PET (polyethylene terephthalate) film. A mixed layer sheet is prepared by coating a mixed layer material on another PET film. An anode sheet is prepared by coating an anode material on another PET film. An electrolyte layer sheet is prepared by coating an electrolyte layer material on another PET film. For example, a plurality of support sheets, a mixed layer sheet, an anode sheet, and an electrolyte layer sheet are sequentially stacked, cut into a predetermined size, and placed under an oxygen partial pressure of 10 -20 The sintering is performed in a reducing atmosphere at atm or less at a temperature range of about 1100° C. to 1300° C. Thus, a half cell including the support 10 , the mixed layer 20 , the electrode skeleton of the anode 30 , and the electrolyte layer 40 can be obtained.

[0055] (Impregnation process)

[0056] Next, the raw materials of the third oxide 33 and the catalyst metal 34 are impregnated into the electrode skeleton of the anode 30. For example, nitrates or chlorides of Zr, Y, Sc, Ce, Gd, and Ni are dissolved in water or alcohols (ethanol, 2-propanol, methanol, etc.), so that when fired at a predetermined temperature in a reducing atmosphere, Gd-doped cerium oxide or Sc, Y-doped zirconium oxide and Ni are generated, a half-cell is impregnated with the obtained nitrate or chloride solution, and the half-cell is dried, and the heat treatment is repeated as many times as required.

[0057] (Reaction prevention layer forming step)

[0058] As the reaction prevention layer 50, for example, a Ce layer having a thickness of 1 μm can be formed by PVD. 0.8 G 0.2 O 2-x .

[0059] (Cathode Formation Step)

[0060] Next, the cathode material is applied onto the reaction prevention layer 50 by screen printing or the like, and then dried. Thereafter, the cathode is sintered by heat treatment. Through the above steps, the fuel cell 100 can be manufactured.

[0061] According to the manufacturing method of this embodiment, the mixed layer material contains a metal material and a ceramic material, so the mixed layer 20 after firing contains a metal material 21 and a ceramic material 22. Therefore, the mixed layer 20 has both the material properties of the metal and the material properties of the ceramic. Therefore, the interlayer delamination between the support 10 and the anode 30 can be suppressed.

[0062] In addition, it is preferable to adjust the amount of the disappearing material in the support material, the mixed layer material, and the anode material so that the relationship of the porosity in the support 10 > the porosity in the mixed layer 20 > the porosity in the anode 30 is established. By establishing this relationship, sufficient gas permeability can be obtained in the support 10. The anode 30 becomes dense and high oxygen ion conductivity can be obtained. In the mixed layer 20, gas permeability can be obtained, and the contact area with the support 10 can be obtained to obtain close adhesion with the support 10.

[0063] In addition, in the manufacturing method of the present embodiment, the electrode skeleton can be first formed by firing, and then impregnated with the composite catalyst and fired at a low temperature (e.g., below 850° C.). Therefore, even if the second oxide 32 and the third oxide 33 do not have the same composition, the reaction between the oxides can be suppressed. Therefore, as the third oxide 33, the degree of freedom in selecting an oxide suitable for the composite catalyst becomes large.

[0064] [Example]

[0065] According to the manufacturing method of the above-described embodiment, the fuel cell 100 is manufactured.

[0066] (Example 1)

[0067] ScYSZ was used as the electrolyte layer 40. The first oxide 31 of the anode 30 was made of a LaTiO3-based material, and the second oxide 32 was made of ScYSZ. The third oxide was made of ScYSZ, and the catalyst metal 34 was made of Ni. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 was made of a LaTiO3-based material. The metal material 21 of the mixed layer 20 was made of SUS (stainless steel). The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 1:1:1. The stacked single cell was placed under an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0068] (Example 2)

[0069] ScYSZ was used as the electrolyte layer 40. The first oxide 31 of the anode 30 was made of a LaCrO3-based material, and the second oxide 32 was made of SYSZ. The third oxide was made of ScYSZ, and the catalyst metal 34 was made of Ni. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 was made of a LaCrO3-based material. The metal material 21 of the mixed layer 20 was made of SUS. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 1:1:1. The stacked single cell was placed under an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0070] (Example 3)

[0071] ScYSZ was used as the electrolyte layer 40. The first oxide 31 of the anode 30 was made of a LaCrO3-based material, and the second oxide 32 was made of ScYSZ. The third oxide was made of GDC, and the catalyst metal 34 was made of Ni. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 was made of a LaCrO3-based material. The metal material 21 of the mixed layer 20 was made of SUS. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 1:1:1. The stacked single cell was subjected to an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0072] (Example 4)

[0073] GDC was used as the electrolyte layer 40. The first oxide 31 of the anode 30 was made of a LaCrO3-based material, and the second oxide 32 was made of GDC. The third oxide was made of ScYSZ, and the catalyst metal 34 was made of Ni. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 was made of a LaCrO3-based material. The metal material 21 of the mixed layer 20 was made of SUS. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 1:1:1. The stacked single cell was placed under an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0074] (Example 5)

[0075] ScYSZ was used as the electrolyte layer 40. The first oxide 31 of the anode 30 used a LaCrO3-based material, and the second oxide 32 used ScYSZ. The third oxide 33 was not used, and Ni was used as the catalyst metal 34. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 used a LaCrO3-based material. The metal material 21 of the mixed layer 20 used SUS. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 1:1:1. The stacked single cell was subjected to an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0076] (Example 6)

[0077] ScYSZ was used as the electrolyte layer 40. LaCrO3-based materials were used as the first oxide 31 of the anode 30, and ScYSZ was used as the second oxide 32. GDC was used as the third oxide, and Ni was used as the catalyst metal 34. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. ScYSZ was used as the ceramic material 22 of the mixed layer 20. SUS was used as the metal material 21 of the mixed layer 20. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 1:1:1. The stacked single cell was placed under an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0078] (Example 7)

[0079] ScYSZ was used as the electrolyte layer 40. The first oxide 31 of the anode 30 was made of a LaTiO3-based material, and the second oxide 32 was made of ScYSZ. The third oxide was made of ScYSZ, and the catalyst metal 34 was made of Ni. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 was made of a LaTiO3-based material. The metal material 21 of the mixed layer 20 was made of SUS. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 1:6:3. The stacked single cell was placed under an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0080] (Example 8)

[0081] ScYSZ was used as the electrolyte layer 40. The first oxide 31 of the anode 30 was made of a LaTiO3-based material, and the second oxide 32 was made of ScYSZ. The third oxide was made of ScYSZ, and the catalyst metal 34 was made of Ni. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 was made of a LaTiO3-based material. The metal material 21 of the mixed layer 20 was made of SUS. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 6:1:3. The stacked single cell was placed under an oxygen partial pressure of 10 -20 The sintering was performed in a reducing atmosphere of atm. Alternatively, the composite catalyst was impregnated and then sintered at a temperature of 850°C or less in an air atmosphere.

[0082] (Example 9)

[0083] ScYSZ was used as the electrolyte layer 40. The first oxide 31 of the anode 30 was made of a LaTiO3-based material, and the second oxide 32 was made of ScYSZ. The third oxide was made of ScYSZ, and the catalyst metal 34 was made of Ni. The electrode skeleton was formed by the first oxide 31 and the second oxide 32. The ceramic material 22 of the mixed layer 20 was made of a LaTiO3-based material. The metal material 21 of the mixed layer 20 was made of SUS. The area ratio of the ceramic material 22, the metal material 21, and the voids in the mixed layer 20 estimated from the SEM image of the sample cross section was 4.5:4.5:1. The stacked single cell was placed under an oxygen partial pressure of 10 -20 The calcination was performed in a reducing atmosphere of atm or less. Alternatively, the calcination was performed in an air atmosphere at a temperature of 850° C. or less after impregnation with the composite catalyst.

[0084] (Comparative Example 1)

[0085] No mixed layer 20 was provided. Other conditions were the same as those in Example 2. The stacked single cells were heated to 10 -20 The firing was carried out in a reducing atmosphere below atm.

[0086] (Comparative Example 2)

[0087] In the anode 30, the electrode skeleton is formed by Ni and ScYSZ. The mixed layer 20 is not provided. In addition, the third oxide 33 and the catalyst metal 34 are not provided. The other conditions are the same as those in Example 1. The stacked single cell is subjected to an oxygen partial pressure of 10 -20 The firing was carried out in a reducing atmosphere below atm.

[0088] The production conditions of Examples 1 to 9 and Comparative Examples 1 and 2 are shown in Figure 4 .

[0089] (Interlayer peeling)

[0090] The presence or absence of interlayer delamination in Examples 1 to 9 and Comparative Examples 1 and 2 was confirmed. In Examples 1 to 9, no interlayer delamination was confirmed. This is considered to be because the mixed layer 20 has a structure in which the metal material 21 and the ceramic material 22 are mixed. In Comparative Example 1, interlayer delamination was confirmed. This is considered to be because the mixed layer 20 is not provided. In addition, no interlayer delamination was confirmed in Comparative Example 2. This is considered to be because Ni as a metal is used in the electrode skeleton of the anode, so the anode plays the role of a mixed layer.

[0091] (Power generation evaluation)

[0092] By measuring the impedance of the fuel cells of Examples 1 to 9 and Comparative Examples 1 and 2, the resistance values ​​were separated and the ohmic resistance of the entire fuel cell and the reaction resistance of the anode 30 were measured. In Comparative Example 2, the ohmic resistance was 0.63 Ω·cm 2 The reaction resistance of the anode is 0.97Ω·cm 2 . The result of observing the cross section of the single cell is that because it was fired in a high-temperature reducing atmosphere, Ni was sintered into large particles of several μm. In addition, the metal powder of the support body formed an alloy in the part that contacted Ni, which can be considered to reduce the catalyst performance. Based on the above, it can be considered that both the ohmic resistance and the reaction resistance have increased significantly. Therefore, in Comparative Example 2, although it was confirmed that there was no interlayer peeling, the power generation performance was greatly reduced. In Comparative Example 1, interlayer peeling occurred, so the power generation performance could not be evaluated.

[0093] In Example 1, the ohmic resistance is 0.25Ωcm 2 , the reaction resistance in the anode 30 is 0.27Ωcm 2 In Example 2, the ohmic resistance is 0.25Ωcm 2 , the reaction resistance in the anode 30 is 0.28Ωcm 2 In Example 3, the ohmic resistance is 0.24Ωcm 2 , the reaction resistance in the anode 30 is 0.27Ωcm 2 In Example 4, the ohmic resistance is 0.2Ωcm 2 , the reaction resistance in the anode 30 is 0.21Ωcm 2 In Example 5, the ohmic resistance is 0.5Ωcm 2 , the reaction resistance in the anode 30 is 1.1Ωcm 2 In Example 6, the ohmic resistance is 0.31Ωcm2 , the reaction resistance in the anode 30 is 0.28Ωcm 2 In Example 7, the ohmic resistance is 0.25Ωcm 2 , the reaction resistance in the anode 30 is 0.27Ωcm 2 In Example 8, the ohmic resistance is 0.25Ω·cm 2 , the reaction resistance in the anode 30 is 0.27Ω·cm 2 In Example 9, the ohmic resistance is 0.25Ωcm 2 , the reaction resistance in the anode 30 is 0.82Ω·cm 2 .

[0094] The results of Examples 1 to 9 show that the ohmic resistance is improved by including the first oxide 31 having electron conductivity in the electrode skeleton of the anode 30. The results of Examples 2 to 6 show that as a result of firing in a reducing atmosphere, LaCrO3 is not decomposed into CrO3, and an anode 30 equivalent to that when a LaTiO3-based material is used can be produced. The results of Examples 1 to 4 and 6 to 9 show that the anode reaction resistance is improved by including the third oxide having oxygen ion conductivity in the composite catalyst.

[0095] Furthermore, from the results of Example 3, it is considered that even when ScYSZ is used for the electrode skeleton of the anode 30, the reaction between ScYSZ and GDC can be suppressed by lowering the firing temperature after impregnation.

[0096] The results of Example 4 show that both the ohmic resistance and the anode reaction resistance are the lowest. This is believed to be due to the following reasons: the ion conductivity of GDC is high; and the electrode reaction resistance caused by the electron conductivity in the reducing atmosphere is reduced.

[0097] In addition, as can be seen from the comparison between Example 3 and Example 6, by using a ceramic having electron conductivity in the mixed layer 20 , the ohmic resistance can be further reduced.

[0098] The results of Example 9 show that when the area ratio of the voids in the mixed layer 20 exceeds 10%, the anode reaction resistance decreases.

[0099] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to these specific embodiments, and various modifications and changes can be made within the scope of the gist of the present invention described in the claims.

Claims

1. A solid oxide fuel cell, characterized in that: include: A support body with metal as the main component; an anode supported by the support; and A mixed layer disposed between the support and the anode, The anode has an electrode skeleton composed of a ceramic material, wherein the ceramic material includes a first oxide having electron conductivity and a second oxide having oxygen ion conductivity. The mixed layer has a structure formed by mixing metal material and ceramic material. The first oxide is LaTiO3, The ceramic material of the mixed layer is LaTiO3.

2. The solid oxide fuel cell according to claim 1, wherein: The ceramic material of the mixed layer has electronic conductivity.

3. The solid oxide fuel cell according to claim 1 or 2, characterized in that: The porosity of the mixed layer is 10% or more.

4. The solid oxide fuel cell according to claim 1 or 2, characterized in that: In the mixed layer, an area ratio of the metal material to the ceramic material is 1:9 to 9:

1.

5. The solid oxide fuel cell according to claim 1 or 2, characterized in that: The mixed layer has a thickness of 1 μm or more.

6. The solid oxide fuel cell according to claim 1 or 2, characterized in that: The porosity of the support, the mixed layer, and the anode has a relationship of porosity in the support > porosity in the mixed layer > porosity in the anode.

7. The solid oxide fuel cell according to claim 1 or 2, characterized in that: The anode includes a catalyst supported on the electrode skeleton.

8. The solid oxide fuel cell according to claim 7, wherein: The catalyst includes a catalyst metal and a third oxide having oxygen ion conductivity.

9. A method for manufacturing a solid oxide fuel cell, characterized in that: include: A step of preparing a laminated body in which a support green sheet, a mixed layer green sheet, and an anode green sheet are stacked, the support green sheet containing metal material powder, the mixed layer green sheet containing metal material powder and ceramic material powder, the anode green sheet containing ceramic material powder, the ceramic material of the anode green sheet containing a first oxide having electron conductivity and a second oxide having oxygen ion conductivity; and The step of firing the laminated body to form a support body from the support body green sheet, a mixed layer from the mixed layer green sheet, and an electrode skeleton composed of the ceramic material from the anode green sheet, The first oxide is LaTiO3, The ceramic material of the mixed layer green sheet is LaTiO3.

10. The method for manufacturing a solid oxide fuel cell according to claim 9, wherein: A catalyst is introduced into the electrode skeleton by an impregnation method, and the catalyst is fired.

Citation Information

Patent Citations

  • Solid oxide fuel cell and method for manufacturing the same

    JP2012033418A

  • Solid-oxide fuel cell

    CN103765647A

  • Power generation cell for solid oxide fuel cell

    JP2012074307A

  • Metal-supported solid oxide fuel cell