Application and preparation method of a lithium battery pole piece nano-organic silicon cross-linked sphere micropowder coating process in lithium battery manufacturing

By coating nano-silicon crosslinked ball micro powder on the surface of the electrode sheet of the lithium battery, the short circuit and explosion problems caused by the melting and shrinking of the separator at high temperatures of the lithium-ion battery is solved, and higher safety and heat resistance are achieved, and lowered cost.

CN112542609BActive Publication Date: 2024-12-06JIANGXIMOQUANNEW MATERIALSCO LID
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011570373.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-26
Publication Date
2024-12-06
Estimated Expiration
2040-12-26

AI Technical Summary

Technical Problem

The existing lithium-ion battery separators are prone to melt and shrink at high temperatures, resulting in short circuits, explosions and fires. The existing coating performance modification has failed to fundamentally solve this problem.

Method used

The surface of the lithium battery electrode sheet is uniformly coated with nano-silicon cross-linked ball micropowder coating, using its high heat resistance and hydrophobic properties to replace traditional separators, absorb electrolyte to conduct lithium ions, and make a separator-free lithium ion battery.

Benefits of technology

The short circuit and explosion problems caused by diaphragm shrinkage caused by high battery temperature are completely solved, which improves the safety and heat resistance of the battery, and reduces material and production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium-ion battery preparation, and specifically discloses a lithium battery pole piece nano-organosilicon cross-linked spherical powder coating process for use in lithium battery manufacturing and a method for making the coating, wherein the coating comprises an adhesive and closely arranged nano-organosilicon cross-linked spherical powder. The present invention innovatively uses a gas-heat spraying method to uniformly coat the surface of the lithium-ion battery pole piece with a silicone cross-linked spherical powder coating to replace the lithium battery diaphragm to isolate the positive and negative pole pieces, and uses the gaps between nano-organosilicon cross-linked spherical powder particles to absorb electrolyte and conduct lithium ions, thereby manufacturing a diaphragm-free lithium-ion battery, which completely solves the safety problem of battery short circuit, fire and explosion caused by diaphragm shrinkage due to high battery temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion battery preparation, and specifically relates to an application and a preparation method of a lithium battery pole piece nano-organic silicon cross-linked spherical micropowder coating process in lithium battery manufacturing. Background Art

[0002] Lithium-ion batteries are currently widely used in many fields such as mobile phones, computers and electric vehicles due to their many advantages such as high voltage, large specific energy, wide operating temperature range, high specific power, stable discharge and long storage time. As one of the key materials of lithium-ion batteries, the diaphragm is used to isolate the positive and negative electrodes, prevent short circuits and allow lithium ions to pass freely in the electrolyte. The commercial diaphragms are polyolefin diaphragms, including high-density polyethylene (HDPE) and polypropylene (PP) diaphragms. These two diaphragms have low melting points of 130°C and 165°C respectively. In the case of overheating of the battery, these two diaphragms are prone to melt shrinkage, causing short circuits between the positive and negative electrodes, resulting in serious safety accidents of battery explosion and fire. In order to improve the thermal stability of the diaphragm, a large number of literature and patents provide ceramic coating, PVDF coating, PMMA coating and silicone powder coating diaphragm technology. The thermal stability of the diaphragm is improved by coating a ceramic layer, PVDF, PMMA and silicone powder coating on the surface of the polyolefin diaphragm. These coated diaphragms can also well solve the safety performance of polyolefin diaphragms, and are therefore widely used in high-voltage and high-power lithium batteries.

[0003] However, these coating modifications can only treat the symptoms and not the root cause, and cannot fundamentally change the low melting point and thermal melt shrinkage characteristics of polyolefin separators. When the battery temperature exceeds the heat resistance limit of these modified separators, safety accidents such as separator shrinkage, battery short circuit, and explosion and fire may also occur. Summary of the invention

[0004] The present invention provides a lithium battery pole piece nano-organosilicon cross-linked spherical micropowder coating process for use in lithium battery manufacturing and a production method. The technical idea adopted by the present invention is to uniformly coat the surface of the lithium ion battery pole piece with an air-heat spraying method to replace the lithium battery diaphragm to isolate the positive and negative pole pieces, and use the gaps between the nano-organosilicon cross-linked spherical micropowder particles to absorb the electrolyte and conduct lithium ions. In this way, a diaphragm-free lithium ion battery is produced, which completely solves the safety problem of battery short circuit, fire and explosion caused by diaphragm shrinkage due to high battery temperature.

[0005] To achieve the above object, the present invention provides the following technical solution: an application and preparation method of a lithium battery pole piece nano-organic silicon cross-linked spherical powder coating process in lithium battery manufacturing, characterized in that it includes the following operating steps:

[0006] Step (1) Granulation: An alkoxysilane (such as methyltrimethoxysilane, phenyltrimethoxysilane) or an alkoxysilane and an oxysilane containing epoxy, amino, methacryloxy, mercapto or vinyl reactive groups are gradually added dropwise into an alkaline aqueous solution. The alkaline aqueous solution is a potassium hydroxide or sodium hydroxide aqueous solution of a certain concentration. An organic amine such as ethylenediamine, diethylamine, triethylamine or ammonia water may also be used. The mass ratio of methyltrimethoxysilane or its partial hydrolysis polycondensate to the alkaline aqueous solution should be controlled at 0 to 15:100. The pH value of the mixed reaction solution is maintained at 10 to 13. The temperature is generally between 15°C and 80°C. The stirring speed is 150 to 180 rpm / min. The reaction time including the feeding time is 0.5 to 12 h. The microparticles obtained by the polycondensation are filtered, washed, dried and crushed to obtain micron-sized spherical silicone resin powder.

[0007] Step (2) slurry preparation: add 0.5-3% by mass of an alkyl anionic surfactant to 30-80% by mass of deionized water, mix and stir evenly, then add 30-60% by mass of spherical silicone resin powder to mix and stir evenly, mix and stir for 0.5-2h under vacuum conditions, then add 3-10% by mass of a water-soluble resin binder and 1-5% by mass of a thickener, and then mix and stir for 2-3h under vacuum conditions to prepare a water-based nano-organosilicon cross-linked ball coating slurry.

[0008] Step (3) coating: the rolled positive and negative electrode sheets of the battery are placed on a coating machine equipped with an automatic retracting device, a spraying device, a high-temperature tunnel oven or a dry gas tunnel oven, and a laser thickness gauge, and the prepared nano-organosilicon cross-linked ball slurry is transported to a special heated spray die head through a CNC metering pump of the coating machine spraying device, the die head temperature is between 40°C and 80°C, and the slurry is evenly and continuously coated on one side of the rolled positive or negative electrode sheet, and then transported to a high-temperature tunnel oven or a dry gas tunnel oven at a temperature of 40°C to 120°C for drying through the automatic retracting device, and then the other side of the electrode sheet is coated in this way to obtain a positive or negative electrode sheet with one or both sides coated.

[0009] Step (4) making a battery: the coated electrode in the above step (3) is further subjected to the steps of sheet making, winding or lamination, assembly, and electrolyte injection to finally obtain a diaphragm-free lithium-ion battery.

[0010] The composition of the positive electrode slurry layer and the negative electrode slurry layer in the present invention, as well as the above-mentioned production details, are well known in the art and will not be described in detail in the present invention.

[0011] Preferably, in step (1), the nano-organic silicon cross-linked sphere is a particle having a three-dimensional cross-linked network molecular structure, which is a kind of solid powder with true spherical shape and uniform particle size distribution, and its chemical structure is a cured resin obtained by dense cross-linking of infusible trifunctional components, including polysilsesquioxane (PSSQ), polyphenylsilsesquioxane (PPSQ) and polymethylsilsesquioxane (PMSQ); and polysilsesquioxane containing epoxy, amino, methacryloxy, mercapto, and vinyl reactive groups.

[0012] Preferably, in step (1), the spherical silicone resin powder is prepared by a hydrolysis / polymerization method, using alkoxysilane (such as methyltrimethoxysilane, phenyltrimethoxysilane) as a raw material, and is prepared by hydrolysis and polycondensation; or by using alkoxysilane and oxysilane containing reactive groups such as epoxy, amino, methacryloxy, mercapto, vinyl, etc., and is prepared by hydrolysis and polycondensation.

[0013] Preferably, in step (1), the particle size of the organosilicon cross-linked sphere particles is 200 to 8000 nanometers.

[0014] Preferably, in step (2), the water-soluble resin is one or more of water-based polyacrylic resin, water-based maleic anhydride-modified polyacrylic resin, water-based polyurethane resin, water-based polystyrene resin and water-based epoxy resin.

[0015] Preferably, in step (2), the dispersant is one or more of aminoorganosilane, carboxylorganosilane, polyol, phenylsulfonate, alkyl quaternary ammonium salt, alkyl quaternary phosphonium salt and their derivatives.

[0016] Preferably, in step (2), the thickener is one or more of CMC, sodium alginate, terpineol, polyvinyl alcohol, guar gum, polyacrylic acid or polyurethane.

[0017] Preferably, in step (2), the vacuum stirring time is 0.5 to 7 hours, and the stirring speed is 100 to 500 rpm / mi.

[0018] Preferably, in step (3), the lithium battery pole pieces are rolled positive and negative battery pole pieces, and the positive or negative pole pieces are coated on one or both sides, and the coating thickness is 1-40 μm.

[0019] Preferably, in step (3), the coating machine is equipped with an automatic retracting and releasing device, a spraying device, a high-temperature tunnel oven or a dry gas tunnel oven, and a laser thickness gauge; the spraying device includes a storage tank, a CNC metering pump, and a special spray die; the special heated air spray die has a die temperature between 40°C and 80°C; the tunnel oven is a horizontal or arch bridge oven with an air electric heating system, or an air wheel dehumidification and drying system, and an air duct circulation system, and the tunnel oven is a multi-section tunnel oven with a length not limited to 6-36 meters; the heating temperature of the tunnel oven is between 40°C and 120°C.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. In the present invention, a layer of nano-organic silicon cross-linked spherical powder is coated on the surface of the positive electrode or negative electrode of the lithium battery to replace the diaphragm, and then assembled into a battery. The glass transition temperature of organic silicon is as high as 450°C, and it has high heat resistance, which completely solves the safety problem of battery short circuit, fire and explosion caused by diaphragm shrinkage due to high battery temperature;

[0022] 2. In the present invention, since the coating thickness is less than the thickness of the existing diaphragm, and the nano-organic silicon cross-linked spherical powder has a light specific gravity and a volume density between 0.4 and 0.7, the weight utilization rate and space utilization rate inside the lithium-ion battery cell are further improved, thereby improving the weight energy density and volume energy density of the lithium-ion battery, and achieving lightweight lithium batteries.

[0023] 3. In the present invention, nano-organic silicon cross-linked spherical powder is used as a single coating powder. The hydrophobic properties of the spherical silicone resin powder and the smooth particle surface reduce the moisture content of the electrode and the adsorption amount of redundant electrolyte, thereby reducing the material and production costs of the battery.

[0024] 4. In the present invention, nano-organic silicon cross-linked spherical powder is used as a single coating powder. The spherical silicone resin powder has excellent weather resistance, solvent resistance, acid and alkali resistance, and a stable chemical system structure, thereby improving the stability of the chemical system of the lithium-ion battery. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] The present invention provides the following technical solution: an application and preparation method of a lithium battery pole piece nano-organic silicon cross-linked spherical micropowder coating process in lithium battery manufacturing, comprising the following operating steps:

[0028] Step (1) Granulation: 50 kg of methyltrimethoxysilane (Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd., purity ≥ 99%) was gradually added dropwise to 500 kg of NaOH (Shanghai Debang Chemical Co., Ltd., analytical grade) aqueous solution (pH 12.5, temperature 40°C), with a stirring speed of 180 rpm / min, a dropping speed of 100 g / min, and a dropping time of about 30 min. The mixture was then cooled to 25°C to 30°C for 4 to 5 h, and 18 kg of acetic acid (Changzhou Qidi Chemical Co., Ltd., analytical grade) was added for neutralization and filtration. The mixture was washed once with methanol (Nantong Runzhou Chemical Co., Ltd., industrial grade), washed three times with deionized water (homemade), and filtered to obtain a white solid powder. The mixture was dried in a vacuum oven at 80°C for 2 h to obtain about 25 kg of spherical silicone resin micropowder with an average particle size of 800 nanometers, and a CV (%) value of about 20%.

[0029] Step (2) slurry preparation: 25 kg of the spherical silicone resin powder prepared in step (1) is added to 35 kg of deionized water and mixed and stirred evenly. At the same time, 800 g of oxalic acid-hexanediol polyester polyphosphoric acid is added. After mixing and stirring for 0.5-2 h under vacuum conditions, 360 g of an acrylic copolymer water-based adhesive (GR-401, Hunan Gaorui Power Materials Co., Ltd.) and 500 g of a thickener are added. The mixture is then mixed and stirred for 2-3 h under vacuum conditions to prepare a water-based nano-organic silicone cross-linked ball coating slurry.

[0030] Step (3) coating: a rolled negative electrode sheet (negative electrode material is B&T GSN) with a width of 300 mm is first coated and dried on one side of the sheet on a CNC air spray coating machine, with a coating thickness of 8 μm. Then, the other side of the sheet is coated and dried, with a coating thickness of 8 μm, to obtain a double-sided nano-organic silicon cross-linked spherical micropowder coated negative electrode sheet.

[0031] Step (4) making a battery: using 4.35V high-energy lithium cobalt oxide (LCO-983 from Peking University) as the positive electrode material to prepare a positive electrode sheet, slitting, sheeting and winding the prepared double-sided organosilicon cross-linked ball micropowder coated negative electrode sheet and positive electrode sheet, adding an electrolyte with a molar concentration of lithium hexafluorophosphate of 1.2 (Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd.) to make a 18650-3000mAh steel shell cylindrical lithium ion battery, and placing the fully charged battery in a test box, and at a rapid heating rate, after reaching a temperature of 150°C ± 2°C, keep the battery in the test box for 2 hours (30 minutes as stipulated in the national standard GB / T18287-2000 "General Specification for Ion Batteries for Honeycombs"), and the battery does not catch fire or explode.

[0032] Example 2

[0033] The present invention provides the following technical solutions:

[0034] Step (1) Granulation: 50 kg of methyltrimethoxysilane (Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd., purity ≥ 99%) was gradually added dropwise to 400 kg of NaOH (Shanghai Debang Chemical Co., Ltd., analytical grade) aqueous solution (pH 12.5, temperature 40°C), with a stirring speed of 180 rpm / min, a dropping speed of 100 g / min, and a dropping time of about 30 min. The mixture was then cooled to 25°C to 30°C for 4 to 5 h, and 18 kg of acetic acid (Changzhou Qidi Chemical Co., Ltd., analytical grade) was added for neutralization and filtration. The mixture was washed once with methanol (Nantong Runzhou Chemical Co., Ltd., industrial grade), washed three times with deionized water (self-made), and filtered to obtain a white solid powder. The mixture was dried in a vacuum oven at 80°C for 2 h to obtain about 25 kg of spherical silicone resin micropowder with an average particle size of 800 nanometers, and a CV (%) value of about 20%.

[0035] Step (2) slurry preparation: 25 kg of the spherical silicone resin powder prepared in step (1) is added to 35 kg of deionized water and mixed and stirred evenly. At the same time, 800 g of oxalic acid-hexanediol polyester polyphosphoric acid is added. After mixing and stirring for 0.5-2 h under vacuum conditions, 360 g of an acrylic copolymer water-based adhesive (GR-401, Hunan Gaorui Power Materials Co., Ltd.) and 500 g of a thickener are added. The mixture is then mixed and stirred for 2-3 h under vacuum conditions to prepare a water-based nano-organic silicone cross-linked ball coating slurry.

[0036] Step (3) coating: a rolled positive electrode sheet with a width of 300 mm (the positive electrode material is Peking University LCO-983 high-energy lithium cobalt oxide) is first coated and dried on one side of the electrode sheet on a CNC air spray coating machine, with a coating thickness of 8 μm, and then the other side of the electrode sheet is coated and dried, with a coating thickness of 8 μm, to obtain a double-sided nano-organic silicon cross-linked spherical micropowder coated positive electrode sheet.

[0037] Step (4) making a battery: using BTR GSN artificial graphite as the negative electrode material to prepare a negative electrode sheet, slitting, sheeting and winding the prepared double-sided organosilicon cross-linked spherical micropowder coated positive electrode sheet and negative electrode sheet, adding an electrolyte with a molar concentration of lithium hexafluorophosphate of 1.2 (Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd.) to make a 18650-3000mAh steel shell cylindrical lithium ion battery, and placing the fully charged battery in a test box, and at a rapid heating rate, after reaching a temperature of 150°C ± 2°C, keep the battery in the test box for 2 hours (30 minutes as stipulated in the national standard GB / T18287-2000 "General Specification for Ion Batteries for Honeycombs"), and the battery does not catch fire or explode.

[0038] Example 3

[0039] The present invention provides the following technical solutions:

[0040] Step (1) Granulation: 50 kg of methyltrimethoxysilane (Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd., purity ≥ 99%) was gradually added dropwise to 500 kg of NaOH (Shanghai Debang Chemical Co., Ltd., analytical grade) aqueous solution (pH 12.5, temperature 40°C), with a stirring speed of 180 rpm / min, a dropping speed of 100 g / min, and a dropping time of about 30 min. The mixture was then cooled to 25°C to 30°C for 4 to 5 h, and 18 kg of acetic acid (Changzhou Qidi Chemical Co., Ltd., analytical grade) was added for neutralization and filtration. The mixture was washed once with methanol (Nantong Runzhou Chemical Co., Ltd., industrial grade), washed three times with deionized water (homemade), and filtered to obtain a white solid powder. The mixture was dried in a vacuum oven at 80°C for 2 h to obtain about 25 kg of spherical silicone resin micropowder with an average particle size of 800 nanometers, and a CV (%) value of about 20%.

[0041] Step (2) slurry preparation: 25 kg of the spherical silicone resin powder prepared in step (1) is added to 30 kg of deionized water and mixed and stirred evenly. At the same time, 800 g of oxalic acid-hexanediol polyester polyphosphoric acid is added. After mixing and stirring for 0.5-2 h under vacuum conditions, 360 g of an acrylic copolymer water-based adhesive (GR-401, Hunan Gaorui Power Materials Co., Ltd.) and 500 g of a thickener are added. The mixture is then mixed and stirred for 2-3 h under vacuum conditions to prepare a water-based nano-organic silicone cross-linked ball coating slurry.

[0042] Step (3) coating: the first step is to coat and dry one side of a 300 mm wide negative electrode roll (the negative electrode material is BYD GSN) on a CNC air spray coating machine, with a coating thickness of 8 μm, to obtain a single-sided nano-silicon cross-linked spherical micropowder coated negative electrode sheet; the second step is to coat and dry one side of a 300 mm wide positive electrode roll (the positive electrode material is Peking University Pioneer LCO-983 high-energy lithium cobalt oxide) on a CNC air spray coating machine, with a coating thickness of 8 μm, to obtain a single-sided nano-silicon cross-linked spherical micropowder coated positive electrode sheet.

[0043] Step (4) making a battery: the prepared single-sided organosilicon cross-linked spherical micropowder coated negative electrode sheet and the single-sided nano-organosilicon cross-linked spherical micropowder coated positive electrode sheet are slit, sheet-formed, and wound, and an electrolyte with a molar concentration of lithium hexafluorophosphate of 1.2 (Zhangjiagang Guotai Huarong Chemical New Materials Co., Ltd.) is added to make a 18650-3000mAh steel shell cylindrical lithium ion battery, and the fully charged battery is placed in a test box, and after the temperature reaches 150°C±2°C at a rapid heating rate, the battery is kept in the test box for 2 hours (30 minutes as specified in the national standard GB / T18287-2000 "General Specification for Ion Batteries for Honeycombs"), and the battery does not catch fire or explode.

[0044] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are included in the protection scope of the present invention.

Claims

1. A method for applying a lithium battery pole piece nano-organic silicon cross-linked sphere micropowder coating process in lithium battery manufacturing, characterized in that: The steps include: Step (1) granulation: methyltrimethoxysilane is gradually added dropwise into an alkaline aqueous solution, wherein the alkaline aqueous solution is a certain concentration of potassium hydroxide or sodium hydroxide aqueous solution, or ethylenediamine, diethylamine, triethylamine organic amine or ammonia water, the mass ratio of methyltrimethoxysilane or its partial hydrolysis polycondensate to the alkaline aqueous solution is controlled to be 0 to 15:100, the pH value of the mixed reaction liquid is maintained at 10 to 13, the temperature is between 15° C. and 80° C., the stirring speed is 150 to 180 rpm / min, the reaction time including the feeding time is 0.5 to 12 h, and the microparticles obtained by polycondensation are filtered, washed, dried, and crushed to obtain nano-scale spherical silicone resin powder; Step (2) slurrying: adding 0.5-3% by weight of an alkyl anionic surfactant dispersant to 30-80% by weight of deionized water, mixing and stirring evenly, then adding 30-60% by weight of spherical silicone resin powder to the mixture, mixing and stirring evenly under vacuum conditions for 0.5-2 hours, then adding 3-10% by weight of a water-soluble resin binder and 1-5% by weight of a thickener, and then mixing and stirring under vacuum conditions for 2-3 hours to prepare a water-based nano-organosilicon cross-linked ball coating slurry; Step (3) coating: placing the rolled positive and negative electrode sheets of the battery on a coating machine equipped with an automatic retracting device, a spraying device, a high-temperature tunnel oven or a dry gas tunnel oven, and a laser thickness gauge, and conveying the prepared nano-organosilicon cross-linked ball coating slurry to a special heated spraying die head through a CNC metering pump of the coating machine spraying device, the die head temperature being between 40°C and 80°C, and coating the rolled positive or negative electrode sheet uniformly and continuously on one side, and then conveying the rolled positive or negative electrode sheet to a high-temperature tunnel oven or a dry gas tunnel oven at a temperature of 80°C to 110°C for drying through the automatic retracting device, and then coating the other side of the electrode sheet in this way to obtain a double-sided coated positive or negative electrode sheet; Step (4) making a battery: the coated electrode in the above step (3) is further subjected to the steps of sheet making, winding or laminating, assembling, and injecting electrolyte to finally obtain a diaphragm-free lithium-ion battery. In the step (1), the nano-organic silicon cross-linked sphere is a particle having a three-dimensional cross-linked network molecular structure, which is a kind of solid powder with true spherical shape and uniform particle size distribution. Its chemical structure is a cured resin obtained by dense cross-linking of infusible trifunctional components, including polysilsesquioxane (PSSQ), polyphenylsilsesquioxane (PPSQ) and polymethylsilsesquioxane (PMSQ), as well as polysilsesquioxane containing epoxy, amino, methacryloxy, mercapto, and vinyl reactive groups; In the step (1), the particle size of the organosilicon cross-linked sphere particles is 200 to 8000 nanometers; In the step (2), the dispersant is one or more of aminoorganosilane, carboxylorganosilane, polyol, phenylsulfonate, alkyl quaternary ammonium salt, alkyl quaternary phosphonium salt and their derivatives. In the step (2), the thickener is one or more of CMC, sodium alginate, terpineol, polyvinyl alcohol, guar gum, polyacrylic acid or polyurethane. In step (3), the spraying device includes a storage tank, a CNC metering pump, and a special spray die head; the special heated spray die head is an air die head; the tunnel oven is a horizontal or arch bridge oven with an air heating system, or an air wheel dehumidification and drying system, and an air duct circulation system; the tunnel oven is a multi-section tunnel oven with a length of 6-36 meters; the heating temperature of the tunnel oven is between 40°C and 120°C, In the step (3), the positive electrode or negative electrode plate is coated on both sides, and the thickness of the coating is 1-40 μm.

2. The method for applying the lithium battery pole piece nano-organic silicon cross-linked sphere micropowder coating process in lithium battery manufacturing according to claim 1 is characterized in that: In the step (1), the spherical silicone resin powder is prepared by a hydrolysis / polymerization method, using methyltrimethoxysilane as a raw material, and is obtained by hydrolysis and polycondensation; or by using methyltrimethoxysilane and an oxysilane containing epoxy, amino, methacryloxy, mercapto, or vinyl reactive groups, and is obtained by hydrolysis and polycondensation.

3. The method for applying the lithium battery pole piece nano-organic silicon cross-linked sphere micropowder coating process in lithium battery manufacturing according to claim 1 is characterized in that: In the step (2), the water-soluble resin is one or more of water-based polyacrylic resin, water-based maleic anhydride-modified polyacrylic resin, water-based polyurethane resin, water-based polystyrene resin and water-based epoxy resin.