Adhesive tape for dicing and method for producing semiconductor chip

By using an addition-reactive silicone-based adhesive and a cross-linking agent in the adhesive tape for cutting, and using a photosensitive platinum catalyst to promote the cross-linking reaction, the problem of insufficient adhesion and residual glue residue on the semiconductor chip is solved, and the chip is realized Stable picking and efficient production.

CN112602172BActive Publication Date: 2024-10-15MAXELL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980055642.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-03
Filing Date
2019-08-30
Publication Date
2024-10-15
Estimated Expiration
2039-08-30

AI Technical Summary

Technical Problem

When using adhesive tape for dicing in the prior art, the composition of the adhesive layer results in insufficient adhesion of the semiconductor chip, making it easy to fly, and residual adhesive remains during peeling, affecting the quality of the chip.

Method used

An adhesive layer containing an addition-reactive silicone-based adhesive and a cross-linking agent is used, and a photosensitive platinum catalyst is used to promote the cross-linking reaction, improve the cohesion of the adhesive, reduce the tack force, ensure good pick-up properties of semiconductor chips and reduce residue Glue is generated.

Benefits of technology

It achieves stable pasting and good pickup of semiconductor chips during the cutting process, reduces the generation of residual glue, and improves chip quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112602172B_ABST
    Figure CN112602172B_ABST
Patent Text Reader

Abstract

A dicing adhesive tape comprises a substrate and a silicone adhesive layer laminated on the substrate, and is used when a semiconductor material having a plurality of semiconductor elements coated with a coating material is divided into a plurality of semiconductor chips. The silicone adhesive layer has an addition reaction type silicone adhesive as a main agent, and contains a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type silicone adhesive. The mass ratio of the silicone material to the silicone resin is in the range of 35 / 65 to 50 / 50, and the content ratio of the silicone material having an olefin group in the total mass of the silicone material and the silicone resin is in the range of 35 mass % or more and 50 mass % or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a dicing adhesive tape used for dicing a semiconductor material as a semiconductor chip material, and a method for manufacturing a semiconductor chip using the dicing adhesive tape. Background Art

[0002] Conventionally, as a dicing adhesive tape for producing a semiconductor chip having an LED (Light Emitting Diode) or the like, an adhesive tape having an adhesive layer composed of an acrylic resin is known (see Patent Document 1).

[0003] Furthermore, as a dicing adhesive tape for producing a semiconductor chip having an LED or the like, an adhesive tape having an adhesive layer composed of a silicone-based resin is known (see Patent Documents 2 and 3).

[0004] Furthermore, as a method for producing semiconductor chips using a dicing tape, there is known a method in which an adhesive tape is attached to the substrate side of a semiconductor element substrate having a plurality of semiconductor elements formed thereon, and the semiconductor element substrate is cut by a dicing machine (see Patent Document 4).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2013-38408

[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-050216

[0009] Patent Document 3: Japanese Patent Application Publication No. 2016-122812

[0010] Patent Document 4: Japanese Patent Application Publication No. 2005-93503 Summary of the invention

[0011] Problems to be solved by the invention

[0012] In addition, in recent years, as a method for producing semiconductor chips that are singulated by dicing, the following technology has been proposed: a technology in which an adhesive tape is attached to a semiconductor material formed by coating a plurality of semiconductor elements with a coating material such as a sealing resin or a phosphor and then dicing the semiconductor material; a technology corresponding to the so-called wafer-level CSP (chip-scale packaging) process.

[0013] In this way, when the adhesive tape is attached to the semiconductor material formed by coating the semiconductor element with the coating material, the adhesive strength may be insufficient due to the composition of the adhesive layer in the adhesive tape, the raw material of the coating material, etc., and the semiconductor chips separated by dicing may fly away. In addition, if the ball viscosity and adhesive strength of the adhesive layer are designed to be high in order to suppress the scattering of the semiconductor chips, when the obtained semiconductor chips are peeled off from the adhesive tape, the adhesive may remain on the semiconductor chips in an attached state, which is called residual adhesive.

[0014] The object of the present invention is to provide an adhesive tape for dicing which has good adhesion and tackiness to a semiconductor material having a plurality of semiconductor elements covered with a covering material and which suppresses residual adhesive on the semiconductor chip when the semiconductor chip singulated by dicing is peeled off, and a method for manufacturing a semiconductor chip using the adhesive tape.

[0015] Methods for solving problems

[0016] Based on such a purpose, the inventors of the present invention have conducted in-depth research on the adhesive layer of the adhesive tape for cutting, and found that if the adhesive layer is configured to have a photosensitive platinum (Pt) catalyst added to a specific adhesive comprising at least an addition reaction type silicone adhesive and a cross-linking agent for the addition reaction type silicone adhesive, then it can have good adhesion to a semiconductor material having multiple semiconductor elements coated with a coating material, and residual adhesive on the semiconductor chip can be suppressed when the semiconductor chip singulated by cutting is peeled off, thereby completing the present invention.

[0017] That is, it was found that: by setting the adhesive layer of the dicing adhesive tape to the above-mentioned structure, when the semiconductor material having a plurality of semiconductor elements coated with a coating material is divided into a plurality of semiconductor chips, the semiconductor chips that are singulated during dicing can be suppressed from scattering due to good viscosity and adhesion. In addition, on the other hand, when the semiconductor chips that are singulated by dicing are peeled off from the dicing adhesive tape, the photosensitive platinum (Pt) catalyst in the adhesive can be activated by irradiating the adhesive layer with light such as ultraviolet rays, thereby promoting the cross-linking reaction of the addition reaction type silicone adhesive and the cross-linking agent for the addition reaction type silicone adhesive, and the cohesive force of the adhesive becomes larger than that before light irradiation. As a result, the viscosity of the adhesive layer is appropriately reduced, and the failure mode in the further holding force test is "interface peeling" or "not falling" in the holding force test. It was found that the pickup property of the semiconductor chip from the dicing adhesive tape becomes good, and the residual adhesive on the semiconductor chip can be suppressed.

[0018] The dicing adhesive tape of the present invention is a dicing adhesive tape characterized in that it is a dicing adhesive tape comprising a substrate and a silicone adhesive layer laminated on the substrate, and is used when a semiconductor material having a plurality of semiconductor elements covered with a covering material is divided into a plurality of semiconductor chips, the silicone adhesive layer having an addition reaction type silicone adhesive as a main agent, and containing a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type silicone adhesive, the mass ratio (Gw) / (Rw) of the total mass (Gw) of the silicone material (G) contained in the silicone adhesive layer to the total mass (Rw) of the silicone resin (R) is in the range of 35 / 65 to 50 / 50, the content ratio of the silicone material (G1) having an alkenyl group in the total mass of the silicone material (G) and the silicone resin (R) is in the range of 35 mass % or more and 50 mass % or less, and ... The adhesion characteristics of Z0237 (2009) satisfy all of the following conditions (a) to (c).

[0019] (a) The adhesive force to the BA-SUS test plate before light irradiation is 2.4 N / 10 mm or more and 5.5 N / 10 mm or less.

[0020] (b) Regarding the value of the ball number in the inclined ball viscosity test (inclination angle 30°, temperature 23°C, relative humidity 50% RH), when the value of the ball number before light irradiation is set to BN0 and the value of the ball number after light irradiation is set to BN1, the relationship is BN0>BN1.

[0021] (c) In the holding strength test after light irradiation (temperature 40°C, relative humidity 33% RH, standing time 5000 minutes), the failure phenomenon when dropped means that the interface between the above-mentioned silicone-based adhesive layer and the BA-SUS test plate is peeled off, or the adhesive does not fall in the holding strength test.

[0022] Here, the dicing adhesive tape may be characterized in that the dicing adhesive tape is used by being attached to the semiconductor material in which the plurality of semiconductor elements are sealed with the covering material made of silicone resin from the covering material side.

[0023] In addition, from another viewpoint, the dicing adhesive tape of the present invention is a dicing adhesive tape characterized in that it is a dicing adhesive tape comprising a substrate and a silicone adhesive layer laminated on the substrate, and is used when a semiconductor material having a plurality of semiconductor elements coated with a coating material is divided into a plurality of semiconductor chips, wherein the silicone adhesive layer is mainly composed of a mixture of an addition reaction type silicone adhesive and a peroxide curing type silicone adhesive, and contains a photosensitive platinum (Pt) catalyst. The present invention relates to a silicone adhesive layer comprising a silicone material (G) and a cross-linking agent for the addition reaction type silicone adhesive, wherein the mass ratio (Gw) / (Rw) of the total mass (Gw) of the silicone material (G) contained in the silicone adhesive layer to the total mass (Rw) of the silicone resin (R) is in the range of 40 / 60 to 56 / 44, the content ratio of the silicone material (G1) having an alkenyl group in the total mass of the silicone material (G) and the silicone resin (R) is in the range of 14 mass % to 42 mass %, and all of the following conditions (a) to (c) are satisfied in terms of adhesive properties according to JIS Z 0237 (2009).

[0024] (a) The adhesive force to the BA-SUS test plate before light irradiation is 2.4 N / 10 mm or more and 5.5 N / 10 mm or less.

[0025] (b) Regarding the value of the ball number in the inclined ball viscosity test (inclination angle 30°, temperature 23°C, relative humidity 50% RH), when the value of the ball number before light irradiation is set to BN0 and the value of the ball number after light irradiation is set to BN1, the relationship is BN0>BN1.

[0026] (c) In the holding strength test after light irradiation (temperature 40°C, relative humidity 33% RH, standing time 5000 minutes), the failure phenomenon when dropped means that the interface between the above-mentioned silicone-based adhesive layer and the BA-SUS test plate is peeled off, or the adhesive does not fall in the holding strength test.

[0027] Here, the dicing adhesive tape may be characterized in that the dicing adhesive tape is used by being attached to the semiconductor material in which the plurality of semiconductor elements are sealed with the covering material made of silicone resin from the covering material side.

[0028] The silicone-based adhesive layer may further include an initiator composed of a peroxide.

[0029] In addition, from another point of view, the manufacturing method of the semiconductor chip of the present invention is a manufacturing method of the following semiconductor chip, which includes the following steps: a pasting step, for a semiconductor element substrate on which a plurality of the above-mentioned semiconductor elements sealed with a sealing resin composed of a silicone resin is formed on the substrate, the above-mentioned dicing adhesive tape is pasted from the sealing resin side; a cutting step, for cutting the above-mentioned semiconductor element substrate to which the above-mentioned dicing adhesive tape is pasted into a plurality of semiconductor chips; an irradiation step, for irradiating the above-mentioned dicing adhesive tape of the above-mentioned semiconductor element substrate with light; and a peeling step, for peeling the above-mentioned dicing adhesive tape from the above-mentioned plurality of semiconductor chips.

[0030] Effects of the Invention

[0031] According to the present invention, there can be provided an adhesive tape for dicing and a method for manufacturing a semiconductor chip using the same. The adhesive tape for dicing has good adhesion and tackiness to a semiconductor material formed by coating a plurality of semiconductor elements with a coating material before light irradiation, and has good pickup properties for the semiconductor chip when the semiconductor chip separated into pieces by dicing is peeled off after light irradiation, and also suppresses residual adhesive on the semiconductor chip. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] [ Figure 1 ] is a diagram showing an example of the structure of a dicing adhesive tape applicable to the present embodiment.

[0033] [ Figure 2 ](a) to (e) are diagrams showing a method for manufacturing a semiconductor chip using the adhesive tape of the present embodiment.

[0034] [ Figure 3 ] is a schematic diagram showing the relationship between the crosslinking density of the addition reaction type silicone-based adhesive in the adhesive layer and the result of the holding force test of the adhesive tape (drop time). DETAILED DESCRIPTION

[0035] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0036] [Composition of adhesive tape]

[0037] Figure 1 The present invention is a diagram showing an example of the structure of a dicing adhesive tape 1 (hereinafter referred to as adhesive tape 1) applicable to the present embodiment. The adhesive tape 1 of the present embodiment is used for dicing semiconductor materials as raw materials of semiconductor chips in the manufacturing process of semiconductor chips having semiconductor elements such as LEDs (light emitting diodes) and power semiconductors.

[0038] like Figure 1As shown, the adhesive tape 1 has a structure in which an adhesive layer 3 as an example of a silicone-based adhesive layer is laminated on a base material 2 .

[0039] It should be noted that, although not shown in the figure, the adhesive tape 1 may also include an anchor coat layer for improving the adhesion between the substrate 2 and the adhesive layer 3 as required. In addition, the surface of the substrate 2 (the surface opposite to the surface facing the adhesive layer 3) may be subjected to surface treatment. Furthermore, the surface of the adhesive layer 3 (the surface opposite to the surface facing the substrate 2) may also be provided with a release liner.

[0040] <Base material>

[0041] The substrate 2 of this embodiment is made of a material that can transmit ultraviolet light or the like. There is no particular limitation on the material of the substrate 2 as long as it can transmit ultraviolet light or the like, and for example, plastics that can transmit ultraviolet light or the like can be used. It should be noted that, here, the fact that ultraviolet light or the like can be transmitted does not mean that the transmittance of ultraviolet light or the like is 100%, but that light can be transmitted to a degree that can at least promote the addition reaction of the addition reaction type silicone adhesive and the crosslinking agent in the adhesive layer 3 using the photosensitive platinum (Pt) catalyst described later.

[0042] As the material of the substrate 2, specifically, resin films such as polyethylene terephthalate, polyethylene naphthalate, polyphenylene sulfide, biaxially stretched polypropylene, aliphatic polyimide (transparent polyimide), polycycloolefin, fluorine resin, and polyolefin resin can be used. In addition, for example, a composite film obtained by laminating polyethylene terephthalate and a polyolefin resin film, a composite film obtained by further laminating these composite films with a resin film, and a resin film made into multiple layers by coextrusion can also be used for the substrate 2 according to the application.

[0043] Among them, as the substrate 2, it is preferable to use a material containing polyethylene terephthalate as a main component.

[0044] <Adhesive layer>

[0045] The adhesive layer 3 of the present embodiment includes a curable silicone adhesive. Specifically, the adhesive layer 3 includes an addition reaction type silicone adhesive as the curable silicone adhesive. In addition, the adhesive layer 3 may also include a peroxide curable silicone adhesive as the curable silicone adhesive in addition to the addition reaction type silicone adhesive. Usually, the addition reaction type silicone adhesive and the peroxide curable silicone adhesive both include an organic silicone material (G) composed of an organic polysiloxane and an organic silicone resin (R) composed of an organic polysiloxane.

[0046] Hereinafter, the adhesive layer 3 including an addition reaction type silicone adhesive as a curable silicone adhesive is described in detail, with the adhesive layer 3 including an addition reaction type silicone adhesive and a peroxide curable silicone adhesive as a curable silicone adhesive being described as a second embodiment.

[0047] <Adhesive layer of the first aspect>

[0048] The adhesive layer 3 of the first embodiment includes an addition reaction type silicone adhesive and a cross-linking agent as an example of a curing agent for cross-linking the addition reaction type silicone adhesive. In addition, the adhesive layer 3 of the first embodiment includes a photosensitive platinum (Pt) catalyst that promotes the reaction between the addition reaction type silicone adhesive and the cross-linking agent by irradiation with light such as ultraviolet rays. It should be noted that the adhesive layer 3 of the first embodiment does not contain a peroxide curing type silicone adhesive.

[0049] Furthermore, the adhesive layer 3 of the first embodiment may contain other additives such as a reinforcing filler, a cohesive force improving agent, and a coloring agent as necessary.

[0050] (Addition reaction type silicone adhesive)

[0051] The addition reaction type silicone adhesive may be any conventionally known adhesive, but is generally an adhesive comprising an organic silicone material (G1) composed of an organopolysiloxane such as polydimethylsiloxane containing at least two alkenyl groups bonded to silicon atoms per molecule on average, and an organic silicone resin (R1) composed of an organopolysiloxane such as polydimethylsiloxane. Here, the organic silicone resin (R1) composed of an organopolysiloxane such as polydimethylsiloxane does not contain an alkenyl group bonded to silicon atoms.

[0052] Hereinafter, the silicone material (G1) composed of an organopolysiloxane such as polydimethylsiloxane having an average of at least two alkenyl groups bonded to silicon atoms per molecule and the silicone resin (R1) composed of an organopolysiloxane such as polydimethylsiloxane contained in the addition reaction type silicone adhesive are described in further detail.

[0053] It should be noted that in the following description, the organic silicone material (G1) composed of an organic polysiloxane such as polydimethylsiloxane containing at least two alkenyl groups bonded to silicon atoms in one molecule on average is sometimes expressed as an organic silicone material (G1) composed of an organic polysiloxane such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms, or is simply expressed as an organic silicone material (G1) having alkenyl groups.

[0054] [Silicone material (G1) composed of organopolysiloxane such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms]

[0055] The silicone material (G1) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms in this embodiment is not particularly limited as long as it is an organopolysiloxane used in addition reaction type silicone adhesives, that is, an organopolysiloxane containing at least 2 alkenyl groups bonded to silicon atoms in an average of 1 molecule. As the molecular structure of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms, for example, a linear structure in which the main chain portion is composed of diorganosiloxane repeating units, a structure in which a part of the molecular structure contains branched chains, a branched structure, or a cyclic structure can be listed. Among them, from the perspective of mechanical strength and physical properties of the adhesive after irradiation with ultraviolet light, etc., a linear structure is preferred.

[0056] The organic silicone material (G1) composed of an organopolysiloxane containing alkenyl groups bonded to silicon atoms may be in an oily state or a raw gel state, and is preferably in a raw gel state.

[0057] In the case of an oily state, the viscosity of the organic silicone material (G1) composed of an organic polysiloxane is preferably 1,000 mPa·s or more at 25° C. If the viscosity is less than 1,000 mPa·s, the adhesive before and after light irradiation may not exhibit the desired adhesive properties, and the adhesion between the adhesive layer 3 and the substrate 2 may deteriorate.

[0058] In the case of a raw gel, the viscosity of the organopolysiloxane (G1) when dissolved in toluene at a concentration of 30% by mass is preferably 100,000 mPa·s or less at 25° C. If the viscosity exceeds 100,000 mPa·s, stirring may become difficult during preparation of the adhesive composition.

[0059] In addition, the said viscosity can be measured using the BM type rotational viscometer.

[0060] Examples of the organosilicone material (G1) composed of an organopolysiloxane containing an alkenyl group bonded to a silicon atom include, but are not limited to, those represented by the following general formula (1) or (2).

[0061] [Chemistry 1]

[0062] R 1 (3-a) X a SiO-(R 1 XSiO) m -(R 1 2SiO) n -SiR 1 (3-a) X a General formula (1)

[0063] [Chemistry 2]

[0064] R 1 2(OH)SiO-(R 1 XSiO) m+2 -(R 1 2SiO) n -SiR 1 2(OH) General formula (2)

[0065] Here, in the above general formula (1) and general formula (2), R 1 They are independently monovalent hydrocarbon groups without an aliphatic unsaturated bond, and X is an organic group containing an alkenyl group. a is an integer of 0 to 3, m is an integer of 0 or greater, and n is an integer of 100 or greater, but a and m are not simultaneously 0. m+n is a value when the viscosity of the organopolysiloxane at 25°C is 1,000 mPa·s or greater.

[0066] As R 1 , preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 7 carbon atoms, without an aliphatic unsaturated bond. Examples thereof include alkyl groups such as methyl, ethyl, propyl, and butyl; cycloalkyl groups such as cyclohexyl; and aryl groups such as phenyl and tolyl, and methyl or phenyl is particularly preferred.

[0067] As X, an organic group containing an alkenyl group having 2 to 10 carbon atoms is preferred. For example, vinyl, allyl, hexenyl, octenyl, acryloyl propyl, acryloyl methyl, methacryloyl propyl, acryloyloxy propyl, acryloyloxymethyl, methacryloyloxypropyl, methacryloyloxymethyl, cyclohexenylethyl, and vinyloxypropyl can be listed. Among them, lower alkenyl groups such as vinyl and allyl are preferred, and vinyl is particularly preferred from an industrial point of view. The bonding position of the alkenyl group is not particularly limited, and can be a molecular chain terminal, a molecular chain side chain, or both a molecular chain terminal and a molecular chain side chain.

[0068] The number of the alkenyl groups mentioned above varies within an appropriate range depending on the content of the silicone resin (R1) composed of organopolysiloxanes such as polydimethylsiloxane contained in the addition reaction type silicone adhesive, the amount of crosslinking agent added, and other added components, so it cannot be generalized. For example, relative to 100 organic groups of the organopolysiloxane, it is usually preferably in the range of 0.1 to 3.0. And, within the range of this ratio, the molecular weight is adjusted in a manner to achieve the above-mentioned viscosity range, preferably in a manner that the number of the alkenyl groups in one molecule of the organopolysiloxane is at least 2 on average. If the number of the alkenyl groups mentioned above is less than 0.1 relative to 100 organic groups of the organopolysiloxane, when the adhesive tape 1 is irradiated with light, the adhesive is not easy to cure and the cohesive force is difficult to improve. In this case, the desired reduction in adhesive force and the failure mode in the holding force test cannot be obtained, and when the obtained semiconductor chips etc. are peeled off from the adhesive tape 1 after the adhesive tape 1 is used for cutting semiconductor element substrates etc., there is a risk that the pick-up property of the individualized semiconductor chips will deteriorate, and there is a risk that residual adhesive will be easily generated on the semiconductor chips etc. On the other hand, if the number of the alkenyl groups exceeds 3.0 with respect to 100 organic groups of the organopolysiloxane, in the case where a release liner treated with a fluoroalkyl-modified silicone is provided in the adhesive tape 1, the release force of the release liner with respect to the adhesive layer 3 may become large.

[0069] [Silicone resin (R1) composed of organopolysiloxane such as polydimethylsiloxane]

[0070] The organic silicone resin (R1) composed of an organic polysiloxane such as polydimethylsiloxane in this embodiment has R 2 3SiO 0.5 The organopolysiloxane having an organopolysiloxane unit (M unit) and an SiO2 unit (Q unit) is called a so-called MQ resin. The organosilicone resin (R1) composed of an organopolysiloxane such as polydimethylsiloxane basically has no alkenyl group in the molecule, and a conventionally known resin can be used. 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and examples of the above R 1 The above-mentioned organopolysiloxane preferably has R 2 3SiO 0.5 The R is contained in a manner such that the molar ratio of the unit / SiO2 unit is in the range of 0.5 or more and 1.7 or less. 2 3SiO 0.5 unit and SiO2 unit. If R 2 3SiO 0.5 The molar ratio of SiO2 unit / SiO2 unit is less than 0.5, and the adhesive force and tackiness of the obtained adhesive layer 3 may be reduced. 2 3SiO 0.5Unit / SiO2 unit's molar ratio exceeds 1.7, then the adhesive force and the holding power of the obtained adhesive layer 3 are sometimes reduced.It should be noted that the above-mentioned organopolysiloxane may also have an OH group.In this case, relative to the gross mass of the above-mentioned organopolysiloxane, the content of the OH group is preferably below 4.0 mass %.If the OH group exceeds the above-mentioned upper limit, then the curability of the adhesive may be reduced.

[0071] In the present embodiment, in order to set the adhesive force of the adhesive tape 1 to be 2.4 N / 10 mm or more and 5.5 N / 10 mm or less, the silicone resin (R2) composed of an organopolysiloxane such as polydimethylsiloxane is preferably an MQ resin. However, the silicone resin (R2) composed of an organopolysiloxane such as polydimethylsiloxane may contain R as an impurity when synthesizing the MQ resin. 2 SiO 1.5 Unit (T unit) and / or R 2 SiO unit (D unit).

[0072] The above-mentioned silicone rubber material (G1) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms and silicone resin (R1) composed of organopolysiloxanes such as polydimethylsiloxane can also be used by simply mixing. In addition, as the silicone rubber material (G1) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms, in the case of containing the organopolysiloxane represented by the above-mentioned general formula (2), as long as the characteristics of the present invention are not impaired, the silicone rubber material (G1) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms and silicone resin (R1) composed of organopolysiloxanes such as polydimethylsiloxane can also be used in the form of a (partial) condensation reaction product obtained by preliminarily reacting the silicone rubber material (G1) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms and the silicone resin (R1) composed of organopolysiloxanes such as polydimethylsiloxane.

[0073] (Mass ratio (Gw) / (Rw) of the total mass (Gw) of the silicone material (G) contained in the adhesive layer of the first embodiment to the total mass (Rw) of the silicone resin (R), and the content ratio of the silicone material (G1) having an alkenyl group in the total mass of the silicone material (G) and the silicone resin (R))

[0074] In the silicone adhesive constituting the adhesive layer 3 of the first embodiment, the total mass (Gw) of the silicone material (G) is consistent with the mass (G1w) of the silicone material (G1) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms in the addition reaction type silicone adhesive. Similarly, in the silicone adhesive constituting the adhesive layer 3 of the first embodiment, the total mass (Rw) of the silicone resin (R) is consistent with the mass (R1w) of the silicone resin (R1) composed of organopolysiloxanes such as polydimethylsiloxane in the addition reaction type silicone adhesive.

[0075] The mass ratio (Gw) / (Rw) (=(G1w) / (R1w)) of the total mass (Gw) of the silicone rubber material (G) to the total mass (Rw) of the silicone resin (R) contained in the adhesive layer 3 of the first embodiment is preferably in the range of 35 / 65 to 50 / 50.

[0076] In this case, the content ratio of the organic silicone material (G1) having an alkenyl group in the total mass of the organic silicone material (G) and the silicone resin (R) {(G1w) / ((Gw)+(Rw))}×100 is of course also preferably in the range of 35 mass % or more and 50 mass % or less as described above.

[0077] If the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) contained in the adhesive layer 3 of the first mode to the total mass (Rw) of the organic silicone resin (R), and the content ratio of the organic silicone material (G1) having an olefin group in the total mass of the organic silicone material (G) and the organic silicone resin (R) are less than the lower limit of the above range, the adhesive is difficult to cure and the cohesive force is difficult to improve when the adhesive tape 1 is irradiated with light. In this case, the desired reduction in adhesive force and the failure mode in the holding force test cannot be obtained. After the adhesive tape 1 is used for cutting a semiconductor element substrate, when the obtained semiconductor chip is peeled off from the adhesive tape 1, there is a risk that the pickup of the singulated semiconductor chip will deteriorate, and there is a risk that residual adhesive will easily form on the semiconductor chip.

[0078] On the other hand, if the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) contained in the adhesive layer 3 of the first mode to the total mass (Rw) of the organic silicone resin (R), and the content ratio of the organic silicone material (G1) having an olefin group in the total mass of the organic silicone material (G) and the organic silicone resin (R) exceed the upper limit of the above range, the adhesive layer 3 becomes too soft due to the organic silicone material (G) component in the uncured state of the adhesive before irradiation with light. In this case, when cutting a semiconductor element substrate, etc., the vibration of the cutting is easily transmitted to the adhesive layer 3, and the amplitude becomes large, for example, there is a risk that the semiconductor element substrate will shift from the reference position. And, accompanied by this, there is a risk of generating fragments (fragments) on the singulated semiconductor chip, and there is a risk of size deviation of each single semiconductor chip.

[0079] In contrast, by setting the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) contained in the adhesive layer 3 of the first mode to the total mass (Rw) of the organic silicone resin (R), and the content ratio of the organic silicone material (G1) having an olefin group in the total mass of the organic silicone material (G) and the organic silicone resin (R) to the above range, the following effects can be achieved. That is, in the stage before irradiation with light such as ultraviolet rays, the adhesive layer 3 in the uncured state can be given appropriate adhesion and viscosity that will not cause the semiconductor chips, etc., that are cut pieces, to fly away during cutting. On the other hand, after light irradiation, the cohesive force is improved by curing the adhesive layer 3, so that the desired adhesion reduction and failure mode in the holding force test can be obtained. As a result, after the adhesive tape 1 is used for cutting of a semiconductor element substrate, etc., good pickup when the obtained semiconductor chips, etc. are peeled off from the adhesive tape 1 can be achieved, and residual adhesive on the semiconductor chips, etc. can be suppressed.

[0080] In addition, as the addition reaction type silicone adhesive of the present invention, commercially available addition reaction type silicone adhesives can also be used. Specifically, for example, KR3700, KR3701, X-40-3237-1, X-40-3240, X-40-3291-1, X-40-3229, X-40-3270, X-40-3306 (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd., TSR1512, TSR1516, XR37-B9204 (all trade names) manufactured by Momentive Advanced Materials Co., Ltd. is a type to which a platinum (Pt)-based catalyst and a cross-linking agent described later are not added, such as SD4580, SD4584, SD4585, SD4560, SD4564, SD4565, SD4570, SD4574, SD4575, SD4600PFC, SD4593, and DC7651ADHESIVE (all trade names) manufactured by Dow Corning Toray Corporation.

[0081] (Crosslinking agent)

[0082] The crosslinking agent is used to crosslink the alkenyl groups contained in the addition reaction type silicone adhesive. As the crosslinking agent, an organopolysiloxane having at least two, preferably three or more hydrogen atoms (SiH) bonded to silicon atoms in one molecule (organohydrogenpolysiloxane) is used.

[0083] Examples of the molecular structure of the organohydrogenpolysiloxane used as the crosslinking agent include a linear structure, a partially branched linear structure, a branched chain structure, and a network structure. The viscosity of the organohydrogenpolysiloxane at 25° C. is preferably in the range of 1 to 5,000 mPa·s.

[0084] In addition, the said viscosity can be measured using the BM type rotational viscometer.

[0085] Conventionally known organohydrogenpolysiloxanes can be used as the crosslinking agent. For example, examples of the organohydrogenpolysiloxane include those represented by the following general formula (3) or (4), but are not limited thereto.

[0086] [Chemistry 3]

[0087] H b R 3 (3-b) SiO-(HR 3 SiO) p -(R 3 2SiO) q -SiR 3 (3-b) H b (Formula 3)

[0088] [Chemistry 4]

[0089]

[0090] Here, in the general formula (3) and the general formula (4), R 3 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, b is 0 or 1, p and q are integers and are values ​​such that the viscosity of the organohydrogenpolysiloxane at 25°C is 1 to 5,000 mPa·s. r is an integer greater than 2, s is an integer greater than 0, and r+s≧3, preferably 8≧r+s≧3. The organohydrogenpolysiloxane may be a mixture of two or more.

[0091] R 3 It is a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 7 carbon atoms. Examples thereof include alkyl groups such as methyl, ethyl, propyl, and butyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl and tolyl; and alkenyl groups such as vinyl and allyl. Methyl or phenyl is particularly preferred.

[0092] The content of the organohydrogenpolysiloxane used as a cross-linking agent in the adhesive layer 3 of the first embodiment is preferably an amount that makes the total amount of hydrogen atoms (SiH) bonded to silicon atoms in the organohydrogenpolysiloxane be in the range of 0.15 mol equivalent or more and 15.0 mol equivalent or less relative to the total amount of alkenyl groups in the organic silicone material (G1) composed of an organopolysiloxane such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms, and more preferably in the range of 1.0 mol equivalent or more and 10.0 mol equivalent or less.

[0093] When the content of the organohydrogenpolysiloxane is less than the above lower limit, the adhesive is not easily cured and the cohesive force is not easily improved when the adhesive tape 1 is irradiated with light. In this case, the desired reduction in adhesive force and the failure mode in the holding force test cannot be obtained, and when the adhesive tape 1 is used for dicing a semiconductor element substrate, etc. and the obtained semiconductor chips, etc. are peeled off from the adhesive tape 1, there is a risk that the pickup properties of the singulated semiconductor chips will deteriorate, and there is a risk that residual adhesive will easily form on the semiconductor chips, etc.

[0094] On the other hand, when the content of the organohydrogenpolysiloxane exceeds the above upper limit, there is a risk that the unreacted organohydrogenpolysiloxane may contaminate the semiconductor chip. In addition, the hydrogen atoms (SiH) bonded to silicon atoms in the unreacted organohydrogenpolysiloxane react with oxygen and moisture in the air to change into SiOH, and the adhesive force of the adhesive layer 3 to the adherend increases, and there is a risk that the pickup property of the semiconductor chip after singulation may deteriorate.

[0095] As described above, the content of the crosslinking agent in the adhesive layer 3 of the first embodiment can be adjusted so that the total amount of hydrogen atoms (SiH) bonded to silicon atoms in the organohydrogenpolysiloxane is within the above-mentioned range relative to the total amount of alkenyl groups in the organic silicone material (G1) composed of an organic polysiloxane such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms.

[0096] The content of the cross-linking agent that satisfies this range varies depending on the number of hydrogen atoms (SiH) bonded to silicon atoms in the cross-linking agent. For example, the cross-linking agent can be added in a range of not less than 0.2 parts by mass and not more than 20.0 parts by mass based on solid content per 100 parts by mass of the addition reaction type silicone-based adhesive.

[0097] By setting the content of the crosslinking agent to the above range relative to the addition reaction type silicone adhesive, when the semiconductor chip is peeled off from the dicing adhesive tape, the photosensitive platinum (Pt) catalyst in the silicone adhesive can be activated by irradiating the adhesive layer 3 with light such as ultraviolet rays, promoting the crosslinking reaction between the addition reaction type silicone adhesive and the crosslinking agent for the addition reaction type silicone adhesive, and the cohesive force of the adhesive becomes greater than before the light irradiation. As a result, the adhesive force of the adhesive layer 3 is appropriately reduced, and good pickup can be achieved when the semiconductor chip is peeled off from the adhesive tape 1, and residual adhesive on the semiconductor chip can be suppressed.

[0098] The crosslinking agent is not particularly limited as long as it is a crosslinking agent used as an addition reaction type silicone adhesive, that is, an organopolysiloxane (organohydrogenpolysiloxane) having at least two hydrogen atoms (SiH) bonded to silicon atoms in one molecule. Specifically, examples thereof include X-92-122 (trade name) manufactured by Shin-Etsu Chemical Co., Ltd. and BY24-741 (trade name) manufactured by Dow Corning Toray Co., Ltd.

[0099] (Photosensitive platinum (Pt) catalyst)

[0100] The photosensitive platinum (Pt) catalyst is used to promote curing caused by the addition reaction (hydrosilylation) of the addition reaction type silicone adhesive and the crosslinking agent constituting the adhesive layer 3 by irradiation with light such as ultraviolet rays. The wavelength of light that can be used to promote curing caused by the addition reaction of the addition reaction type silicone adhesive and the crosslinking agent is preferably in the range of 240 nm to 400 nm.

[0101] As the photosensitive platinum (Pt) catalyst, a photoactive cyclopentadienyl platinum (IV) compound is preferably used in view of good photosensitivity and reaction rate.

[0102] The photoactive cyclopentadienyl platinum (IV) compound is not particularly limited, and examples thereof include (cyclopentadienyl)dimethyltrimethylsilylmethylplatinum, (cyclopentadienyl)diethyltrimethylsilylmethylplatinum, (cyclopentadienyl)dipropyltrimethylsilylmethylplatinum, (cyclopentadienyl)diisopropyltrimethylsilylmethylplatinum, (cyclopentadienyl)diallyltrimethylsilylmethylplatinum, (cyclopentadienyl)dibenzyltrimethylsilylmethylplatinum, (cyclopentadienyl)dimethyltriethylsilylmethylplatinum, Alkyl methyl platinum, (cyclopentadienyl) dimethyl tripropyl silyl methyl platinum, (cyclopentadienyl) dimethyl triisopropyl silyl methyl platinum, (cyclopentadienyl) dimethyl triphenyl silyl methyl platinum, (cyclopentadienyl) dimethyl dimethyl phenyl silyl methyl platinum, (cyclopentadienyl) dimethyl methyl diphenyl silyl methyl platinum, (cyclopentadienyl) dimethyl dimethyl (trimethylsiloxy) silyl methyl platinum, (cyclopentadienyl) dimethyl dimethyl (dimethylvinylsiloxy) silyl alkyl methylplatinum, [(1'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [(2'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-methyl-3-(1'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-methyl-3-(2'-naphthyl)cyclopentadienyl]trimethylsilylmethylplatinum, [(4'-biphenyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-(4'-biphenyl)-3-methylcyclopentadienyl]trimethylsilyl Methylplatinum, [(9'-phenanthrenyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-methyl-3-(9'-phenanthrenyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-(2'-anthryl)-3-methylcyclopentadienyl]trimethylsilylmethylplatinum, [(2'-anthryl)cyclopentadienyl]trimethylsilylmethylplatinum, [(1'-pyrenyl)cyclopentadienyl]trimethylsilylmethylplatinum, [1-methyl-3-(1'-pyrenyl)cyclopentadienyl]trimethylsilylmethylplatinum, and the like.

[0103] The cyclopentadienyl ring in the above compounds may be substituted with methyl, chlorine, fluorine, trimethylsilyl, triethylsilyl, dimethylphenylsilyl, methyldiphenylsilyl, triphenylsilyl, phenyl, fluorophenyl, chlorophenyl, methoxy, naphthyl, biphenyl, anthracenyl, pyrene, 2-benzoylnaphthalene, thioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, anthraquinone, 1-chloroanthraquinone, acetophenone, benzophenone, 9,10-dimethylanthracene, 9,10-dichloroanthracene, and a cyclopentadienyl ring substituted with one or more groups selected from these groups.

[0104] In the above compounds, the cyclopentadienyl ring may be substituted by an η5-fluorenyl group.

[0105] The cyclopentadienyl ring in the above-mentioned compound is preferably an unsubstituted cyclopentadienyl ring, a cyclopentadienyl ring substituted with one or more aromatic organic groups, a cyclopentadienyl ring substituted with one or more aliphatic organic groups, or a cyclopentadienyl ring substituted with one or more aromatic organic groups and one or more aliphatic organic groups. In addition, the organic group that may be substituted with the cyclopentadienyl ring is preferably a naphthyl, a biphenylyl, an anthracenyl, a phenanthrenyl, and a pyrenyl.

[0106] The content of the photosensitive platinum (Pt) catalyst in the adhesive layer 3 of the first embodiment is not particularly limited as long as it can promote the addition reaction of the addition reaction type silicone adhesive and the crosslinking agent by irradiation with light such as ultraviolet rays. The content of the photosensitive platinum (Pt) catalyst in the adhesive layer 3 of the first embodiment is preferably set to a range of 0.1 mass parts or more and 3.0 mass parts or less in terms of solid content relative to 100 mass parts of the solid content of the addition reaction type silicone adhesive.

[0107] (Cohesion enhancing agent)

[0108] The cohesion enhancer is used as needed to enhance the cohesion of the adhesive layer 3. The cohesion enhancer is not particularly limited, and for example, a multifunctional thiol is used. As the cohesion enhancer composed of a multifunctional thiol, for example, KARENZ (registered trademark) MT-PE1 and KARENZ MT-NR1 manufactured by Showa Denko K.K. can be cited.

[0109] However, since addition reaction type silicone adhesives are incompatible with multifunctional thiols, in order to use multifunctional thiols as cohesion improving agents, a compatibilizing agent for addition reaction type silicone adhesives and multifunctional thiols must be used. The compatibilizing agent is not particularly limited, and examples thereof include KBM-802 and KBM-803 (both trade names) manufactured by Shin-Etsu Chemical Co., Ltd., which are silane coupling agents having a mercapto group, and SH6062 (trade name) manufactured by Dow Corning Toray Co., Ltd.

[0110] When a cohesion enhancer is used in the adhesive layer 3, the amount of the cohesion enhancer added is preferably in the range of 6 parts by mass or less in terms of solid content relative to 100 parts by mass of the solid content of the addition reaction type silicone adhesive. When the amount of the cohesion enhancer added exceeds 6 parts by mass in terms of solid content relative to 100 parts by mass of the solid content of the addition reaction type silicone adhesive, the addition reaction type silicone adhesive and the multifunctional thiol as the cohesion enhancer may phase separate even if a compatibilizing agent is added.

[0111] (Reinforcement filler)

[0112] The reinforcing filler is used as needed to improve the strength of the adhesive layer 3. The reinforcing filler is not particularly limited, and examples thereof include AEROSIL (registered trademark) 130, AEROSIL 200, and AEROSIL 300 manufactured by AEROSIL Co., Ltd. of Japan, REOLOSIL (registered trademark) QS-102 and REOLOSIL QS-30 manufactured by Tokuyama Co., Ltd., CARPLEX (registered trademark) 80 manufactured by DSL. Japan Co., Ltd., and Hi-Sil (registered trademark) -233-D manufactured by PPG.

[0113] <Adhesive layer of the second embodiment>

[0114] The adhesive layer 3 of the second embodiment includes a peroxide-curable silicone adhesive in addition to the addition reaction type silicone adhesive, crosslinking agent and photosensitive platinum (Pt) catalyst contained in the adhesive layer 3 of the first embodiment. In addition, the adhesive layer 3 of the second embodiment may also include an initiator for starting the polymerization reaction of the peroxide-curable silicone adhesive. Furthermore, the adhesive layer 3 of the second embodiment may also include other additives such as reinforcing fillers, cohesion enhancers, colorants, etc. as needed, similarly to the adhesive layer 3 of the first embodiment.

[0115] (Peroxide-curable silicone adhesive)

[0116] The peroxide-curable silicone adhesive may be a conventionally known material, and is generally an adhesive comprising an organic silicone material (G2) composed of an organic polysiloxane such as polydimethylsiloxane and an organic silicone resin (R2) composed of an organic polysiloxane such as polydimethylsiloxane. It should be noted that the organic silicone material (G2) composed of an organic polysiloxane contained in the peroxide-curable silicone adhesive is different from the organic silicone material (G1) contained in the addition reaction type silicone adhesive, and generally does not contain an alkenyl group bonded to a silicon atom.

[0117] Hereinafter, the silicone material (G2) composed of organopolysiloxane such as polydimethylsiloxane not containing alkenyl groups bonded to silicon atoms and the silicone resin (R2) composed of organopolysiloxane such as polydimethylsiloxane contained in the peroxide-curable silicone adhesive will be described in further detail.

[0118] In the following description, the silicone material (G2) composed of an organopolysiloxane such as polydimethylsiloxane not containing an alkenyl group bonded to a silicon atom may be simply referred to as the silicone material (G2) composed of an organopolysiloxane such as polydimethylsiloxane.

[0119] [Silicone material (G2) composed of organopolysiloxane such as polydimethylsiloxane containing no alkenyl group bonded to silicon atoms]

[0120] The organic silicone material (G2) composed of an organic polysiloxane such as polydimethylsiloxane in this embodiment is not particularly limited as long as it is a material used in a peroxide-curable organic silicone adhesive, that is, a material that does not contain an olefin group bonded to a silicon atom. Examples of the molecular structure of such an organic polysiloxane include a linear structure in which the main chain portion is composed of diorganosiloxane repeating units, a structure in which a part of the molecular structure includes a branched chain, a branched structure, or a cyclic structure.

[0121] The organic silicone material (G2) composed of an organopolysiloxane such as polydimethylsiloxane which does not contain an alkenyl group bonded to a silicon atom may be in an oily state or a raw gel state, and is preferably in a raw gel state.

[0122] In the case of an oily state, the viscosity of the organic silicone material (G2) composed of an organic polysiloxane is preferably 1,000 mPa·s or more at 25° C. When the viscosity is less than 1,000 mPa·s, the adhesive before and after light irradiation may not exhibit the desired adhesive properties, and the adhesion between the adhesive layer 3 and the substrate 2 may deteriorate.

[0123] In the case of a raw gel, the viscosity of the organopolysiloxane (G2) when dissolved in toluene at a concentration of 30% by mass is preferably 100,000 mPa·s or less at 25° C. If the viscosity exceeds 100,000 mPa·s, stirring may become difficult when preparing the adhesive composition.

[0124] In addition, the said viscosity can be measured using the BM type rotational viscometer.

[0125] Examples of the organic silicone material (G2) composed of an organopolysiloxane such as polydimethylsiloxane that does not contain an alkenyl group bonded to a silicon atom include, but are not limited to, those represented by the following general formula (5) or (6).

[0126] [Chemistry 5]

[0127] R 4 3SiO-(R 4 2SiO) t -SiR 4 3 General formula (5)

[0128] [Chemistry 6]

[0129] R 4 2(OH)SiO-(R 4 2SiO) t -SiR 4 2(OH) General formula (6)

[0130] Here, in the above general formula (5) and general formula (6), R 4 Each of them is independently a monovalent hydrocarbon group having no aliphatic unsaturated bond, t is an integer of 100 or more, and is a value that makes the viscosity of the diorganopolysiloxane at 25° C. 1,000 mPa·s or more.

[0131] As R 4 , preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 7 carbon atoms, without an aliphatic unsaturated bond. Examples thereof include alkyl groups such as methyl, ethyl, propyl, and butyl; cycloalkyl groups such as cyclohexyl; and aryl groups such as phenyl and tolyl, and methyl is particularly preferred.

[0132] [Silicone resin (R2) composed of organopolysiloxane such as polydimethylsiloxane]

[0133] The silicone resin (R2) composed of an organopolysiloxane such as polydimethylsiloxane in this embodiment can be the same silicone resin as the silicone resin (R1) composed of an organopolysiloxane such as polydimethylsiloxane used in the above-mentioned addition reaction type silicone adhesive. 2 3SiO 0.5 The organopolysiloxane containing an organopolysiloxane unit (M unit) and an SiO2 unit (Q unit) is called a so-called MQ resin. The organosilicone resin (R1) composed of an organopolysiloxane such as polydimethylsiloxane basically has no alkenyl group in the molecule, and a conventionally known one can be used. 2 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and examples of the above R 1 The above-mentioned organopolysiloxane is preferably in the form of a monovalent hydrocarbon group with R 2 3SiO 0.5 The R is contained in a manner that the molar ratio of the unit / SiO2 unit is in the range of 0.5 or more and 1.7 or less. 2 3SiO 0.5 unit and SiO2 unit. 2 3SiO 0.5 When the molar ratio of R unit / SiO2 unit is less than 0.5, the adhesive force and tackiness of the obtained adhesive layer 3 may be reduced. 2 3SiO 0.5 Unit / SiO2 unit molar ratio exceeds 1.7, then the adhesive force and the holding power of the obtained adhesive layer 3 are sometimes reduced.It should be noted that the above-mentioned organopolysiloxane may also have an OH group.In this case, relative to the gross mass of the above-mentioned organopolysiloxane, the content of the OH group is preferably below 4.0 mass %.If the OH group exceeds the above-mentioned upper limit, the curability of the adhesive may be reduced.

[0134] In this embodiment, in order to set the adhesive force of the adhesive tape 1 to be greater than 2.4 N / 10 mm and less than 5.5 N / 10 mm, the organic silicone resin (R2) composed of an organic polysiloxane such as polydimethylsiloxane is preferably an MQ resin. However, the organic silicone resin (R2) composed of an organic polysiloxane such as polydimethylsiloxane may contain R as an impurity when synthesizing the MQ resin. 2 SiO 1.5 Unit (T unit) and / or R 2 SiO unit (D unit).

[0135] The above-mentioned silicone rubber material (G2) composed of organopolysiloxanes such as polydimethylsiloxanes not containing alkenyl groups bonded to silicon atoms and silicone resin (R2) composed of organopolysiloxanes such as polydimethylsiloxanes can also be simply mixed and used. In addition, as the silicone rubber material (G2) composed of organopolysiloxanes such as polydimethylsiloxanes not containing alkenyl groups bonded to silicon atoms, in the case of containing the organopolysiloxane represented by the above-mentioned general formula (6), as long as the characteristics of the present invention are not impaired, the silicone rubber material (G2) composed of organopolysiloxanes such as polydimethylsiloxanes not containing alkenyl groups bonded to silicon atoms and silicone resin (R2) composed of organopolysiloxanes such as polydimethylsiloxanes can also be used in the form of a (partial) condensation reaction product obtained by preliminarily reacting the silicone rubber material (G2) composed of organopolysiloxanes such as polydimethylsiloxanes and the organopolysiloxanes such as polydimethylsiloxanes.

[0136] (Mass ratio (Gw) / (Rw) of the total mass (Gw) of the silicone material (G) contained in the adhesive layer of the second embodiment to the total mass (Rw) of the silicone resin (R), and the content ratio of the silicone material (G1) having an alkenyl group in the total mass of the silicone material (G) and the silicone resin (R))

[0137] As described above, the silicone adhesive constituting the adhesive layer 3 of the second embodiment includes an addition reaction type silicone adhesive and a peroxide curing type silicone adhesive. Therefore, in the silicone adhesive constituting the adhesive layer 3 of the second embodiment, the total mass (Gw) of the silicone material (G) is the mass (G1w) of the silicone material (G1) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms in the addition reaction type silicone adhesive and the mass (G2w) of the silicone material (G2) composed of organopolysiloxanes such as polydimethylsiloxane containing alkenyl groups bonded to silicon atoms in the peroxide curing type silicone adhesive. In addition, in the silicone adhesive constituting the adhesive layer 3 of the second mode, the total mass (Rw) of the silicone resin (R) is the total mass (R1w) of the silicone resin (R1) composed of organic polysiloxanes such as polydimethylsiloxane in the addition reaction type silicone adhesive and the mass (R2w) of the silicone resin (R2) composed of organic polysiloxanes such as polydimethylsiloxane in the peroxide curing type silicone adhesive.

[0138] The mass ratio (Gw) / (Rw) (=(G1w+G2w) / (R1w+R2w)) of the total mass (Gw) of the silicone material (G) contained in the adhesive layer 3 of the second embodiment to the total mass (Rw) of the silicone resin (R) is preferably in the range of 40 / 60 to 56 / 44.

[0139] In this case, the content ratio of the organic silicone material (G1) having an alkenyl group in the total mass of the organic silicone material (G) and the silicone resin (R) {(G1w) / ((Gw)+(Rw))}×100 is preferably in the range of 14 mass % or more and 42 mass % or less.

[0140] If the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) to the total mass (Rw) of the organic silicone resin (R) contained in the adhesive layer 3 of the second embodiment is less than the lower limit of the above range, the adhesive force and the viscous force of the adhesive layer 3 may be reduced. In this case, when the adhesive tape 1 is used for cutting the semiconductor element substrate, fluorescent substrate, etc. described later, the semiconductor chips, etc., which are cut pieces, may fly.

[0141] On the other hand, if the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) contained in the adhesive layer 3 of the second mode to the total mass (Rw) of the organic silicone resin (R) exceeds the upper limit of the above range, then when the mass of the organic silicone material (G1) in the addition reaction type organic silicone adhesive is particularly large, the adhesive layer 3 becomes too soft due to the organic silicone material (G) component in the uncured state of the adhesive before irradiation with light. In this case, when cutting the semiconductor element substrate, etc., the vibration of the cutting is easily transmitted to the adhesive layer 3 and the amplitude becomes large, for example, there is a risk that the semiconductor element substrate will shift from the reference position. And with this, there is a risk of broken pieces (fragments) on the singulated semiconductor chip, and there is a risk of size deviation of each single semiconductor chip.

[0142] In addition, when the mass of the silicone rubber material (G2) in the peroxide-curable silicone adhesive is particularly high, the curing of the peroxide-curable silicone adhesive by the initiator is easy to proceed, and the adhesive force and tackiness of the adhesive layer 3 may be reduced. In this case, when the adhesive tape 1 is used for cutting semiconductor element substrates, fluorescent substrates, etc. described later, semiconductor chips, etc., which are cut pieces, may fly away.

[0143] If the content ratio of the organic silicone material (G1) having an alkenyl group in the adhesive layer 3 of the second mode in the total mass of the organic silicone material (G) and the silicone resin (R) is less than the lower limit of the above range, the adhesive is not easy to cure and the cohesive force is not easy to increase when the adhesive tape 1 is irradiated with light. In this case, the desired adhesive force reduction and the failure mode in the holding force test cannot be obtained. After the adhesive tape 1 is used for cutting a semiconductor element substrate, when the obtained semiconductor chip is peeled off from the adhesive tape 1, there is a risk that the pickup property of the singulated semiconductor chip will deteriorate, and there is a risk that residual adhesive will be easily generated on the semiconductor chip.

[0144] On the other hand, if the content ratio of the organic silicone material (G1) having alkenyl groups in the adhesive layer 3 of the second mode in the total mass of the organic silicone material (G) and the silicone resin (R) exceeds the upper limit of the above range, the adhesive layer 3 becomes too soft due to the organic silicone material (G) component when the adhesive is not cured before irradiation with light. In this case, when cutting the semiconductor element substrate, etc., the vibration of the cutting is easily transmitted to the adhesive layer 3 and the amplitude becomes larger, for example, there is a risk that the semiconductor element substrate will shift from the reference position. Moreover, there is a risk of generating fragments (chips) on the singulated semiconductor chip, and there is a risk of size deviation on each single semiconductor chip.

[0145] Regarding the content of the peroxide-curable silicone adhesive in the adhesive layer 3 of the second embodiment, when mixed with the addition reaction type silicone adhesive, the ratio of the silicone material (G2) to the silicone resin (R2) of the peroxide-curable silicone adhesive can be considered and adjusted in such a way that the mass ratio (Gw) / (Rw) of the total mass (Gw) of the silicone material (G) contained in the adhesive layer of the second embodiment to the total mass (Rw) of the silicone resin (R) and the content ratio of the silicone material (G1) having an olefin group in the total mass of the silicone material (G) and the silicone resin (R) are within the above-mentioned range.

[0146] By setting the content of the peroxide silicone adhesive in the adhesive layer 3 of the second embodiment to the above range, when the adhesive tape 1 is used for dicing semiconductor element substrates, fluorescent substrates, etc., it is possible to suppress scattering of semiconductor chips as cut pieces and residual adhesive when peeling the adhesive tape 1.

[0147] In addition, as the peroxide-curable silicone adhesive of the present invention, commercially available peroxide-curable silicone adhesives may also be used. Specifically, for example, KR100 and KR101-10 (all trade names) manufactured by Shin-Etsu Chemical Co., Ltd., YR3340, YR3286, PSA610-SM, and XR37-B6722 (all trade names) manufactured by Momentive Advanced Materials Co., Ltd., and SH4280, SH4282, SE4200, BY24-717, BY24-715, and Q2-7735 (all trade names) manufactured by Dow Corning Toray Co., Ltd. may be cited.

[0148] (Initiator)

[0149] As the initiator, a peroxide, more specifically an organic peroxide, can be used. There are no particular restrictions on the organic peroxide used as the initiator, and examples thereof include benzoyl peroxide, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,1′-di-tert-butylperoxy-3,3,5-trimethylenecyclohexane, and 1,3-di-(tert-butylperoxy)-diisopropylbenzene. Commercially available products include NYPER K40 manufactured by NOF Corporation.

[0150] The content of the initiator in the adhesive layer 3 of the second mode is preferably 10 parts by mass or less in terms of solid content relative to 100 parts by mass of the solid content of the peroxide-curable silicone adhesive. In the case where the content of the initiator in the adhesive layer 3 of the second mode exceeds 10 parts by mass in terms of solid content relative to 100 parts by mass of the solid content of the peroxide-curable silicone adhesive, the curing reaction of the peroxide-curable silicone adhesive in the adhesive layer 3 sometimes proceeds excessively. In this case, the adhesive layer 3 becomes hard, and the adhesive force of the adhesive tape 1 is easily reduced. Moreover, when the adhesive tape 1 is used for cutting semiconductor element substrates, etc., when the semiconductor element substrates, etc. are cut, the semiconductor chips, etc., which are cut pieces, may be easily peeled off from the adhesive tape 1 and scattered.

[0151] <Thickness>

[0152] The thickness of the adhesive layer 3 is preferably in the range of 10 μm or more and 100 μm or less, and more preferably in the range of 20 μm or more and 40 μm or less. When the thickness of the adhesive layer 3 is less than 10 μm, the adhesive force of the adhesive tape 1 is easily reduced due to the thinning of the thickness of the silicone adhesive contained in the adhesive layer 3. On the other hand, when the thickness of the adhesive layer 3 is thicker than 100 μm, cohesion failure of the adhesive layer 3 may easily occur. Moreover, after the adhesive tape 1 is used for cutting of semiconductor element substrates, etc., when the obtained semiconductor chips, etc. are peeled off from the adhesive tape 1, there is a risk that residual adhesive is easily generated on the semiconductor chips, etc. In addition, when cutting semiconductor element substrates, etc., the vibration of the cutting is easily transmitted to the adhesive layer 3 and the amplitude becomes larger, for example, there is a risk that the semiconductor element substrate is offset from the reference position. Moreover, along with this, there is a risk of fragments (fragments) on the singulated semiconductor chips, and there is a risk of size deviation on each single semiconductor chip.

[0153] <Adhesion coating>

[0154] As described above, in the adhesive tape 1 of the present embodiment, an adhesion-promoting coating matching the type of the substrate 2 may be provided between the substrate 2 and the adhesive layer 3, or a surface treatment such as a corona treatment may be performed, depending on the manufacturing conditions of the adhesive tape 1, the use conditions of the manufactured adhesive tape 1, etc. Thus, the adhesion between the substrate 2 and the adhesive layer 3 can be improved.

[0155] <Surface treatment>

[0156] The surface of the substrate 2 (the surface on the opposite side to the surface of the adhesive layer 3) may also be subjected to a surface treatment such as a peeling improvement treatment. The treatment agent used for the surface treatment of the substrate 2 is not particularly limited, and for example, non-silicone peeling treatment agents such as long-chain alkyl vinyl monomer polymers, fluoroalkyl vinyl monomer polymers, polyvinyl alcohol urethanes, and aminoalkyd resins may be used. As such non-silicone peeling treatment agents, for example, PEELOIL 1050 and PEELOIL 1200 manufactured by Ichibansha Oil Industry Co., Ltd. may be cited.

[0157] <Release liner>

[0158] In addition, a release liner may be provided on the surface of the adhesive layer 3 (the surface opposite to the surface facing the substrate 2) as required. As the release liner, a release liner may be used which is a release liner on a film such as paper, polyethylene, polypropylene, polyethylene terephthalate, etc., to which a release treatment for improving the release property from the silicone-based adhesive contained in the adhesive layer 3 is applied. The material used in the release treatment of the release liner is not particularly limited, and for example, materials such as fluoroalkyl-modified silicone, long-chain alkyl vinyl monomer polymer, and aminoalkyd resin may be used.

[0159] <Adhesive tape thickness>

[0160] The thickness of the entire adhesive tape 1 having the above-described configuration is preferably in the range of 20 μm or more and 200 μm or less.

[0161] When the thickness of the adhesive tape 1 is less than 20 μm, when the adhesive tape 1 is used for dicing a semiconductor element substrate or the like, it may be difficult to peel the formed semiconductor chip or the like from the adhesive tape 1 .

[0162] On the other hand, when the thickness of the adhesive tape 1 exceeds 200 μm, it is difficult for the adhesive tape 1 to follow the unevenness formed on the adhesive surface of the semiconductor element substrate when the adhesive tape 1 is attached to the semiconductor element substrate. In this case, the bonding area between the adhesive tape 1 and the semiconductor element substrate becomes small, and the semiconductor chips may be easily scattered during dicing.

[0163] [Manufacturing method of adhesive tape]

[0164] Next, a method for producing the adhesive tape 1 of the present embodiment will be described. It should be noted that the method for producing the adhesive tape 1 described below is an example, and the method for producing the adhesive tape 1 is not limited thereto.

[0165] Here, the first embodiment of the adhesive tape 1 in which the adhesive layer 3 contains an addition reaction type silicone adhesive as a curable silicone adhesive and the second embodiment of the adhesive tape 1 in which the adhesive layer 3 contains an addition reaction type silicone adhesive and a peroxide curable silicone adhesive as curable silicone adhesive can be manufactured by the same manufacturing method.

[0166] When manufacturing the adhesive tape 1, first, a curable silicone adhesive and other components such as a crosslinking agent are dissolved in a general organic solvent such as toluene or ethyl acetate to obtain an adhesive solution. Next, the adhesive solution is applied to the surface of the substrate 2 that has been subjected to surface treatment and an adhesion-promoting coating as required, using a notch wheel coater or the like, in a manner to a predetermined thickness.

[0167] Next, the base material 2 coated with the adhesive solution is heated at a temperature of 60° C. to 160° C. for several minutes to several tens of minutes to dry and cure the adhesive solution, thereby forming an adhesive layer 3 .

[0168] Through the above process, we can obtain Figure 1 The adhesive tape 1 shown in the figure has an adhesive layer 3 laminated on a substrate 2 .

[0169] [How to use adhesive tape]

[0170] The adhesive tape 1 of the present embodiment is used for cutting semiconductor materials, which are raw materials of semiconductor chips, in the manufacturing process of semiconductor chips having semiconductor elements such as LEDs (Light Emitting Diodes) and power semiconductors.

[0171] Specifically, the adhesive tape 1 is used to cut a semiconductor element substrate on which a plurality of semiconductor elements such as LED elements and power semiconductor elements are formed on a substrate made of resin, ceramic, etc. to obtain individual semiconductor chips. Here, for a semiconductor element substrate on which a plurality of semiconductor elements are formed on a substrate, a sealing resin as an example of a covering material is sometimes provided in a manner of covering the semiconductor elements in order to protect the semiconductor elements from the influence of the external environment such as temperature and humidity.

[0172] The adhesive tape 1 of the present embodiment can be more preferably used for dicing a semiconductor element substrate provided with a sealing resin, in particular.

[0173] As a method for obtaining a plurality of semiconductor chips by cutting a semiconductor element substrate provided with a sealing resin, for example, the following method is conventionally known.

[0174] First, a dicing adhesive tape is attached to the substrate side of the semiconductor element substrate, and the semiconductor element substrate is cut from the side where the semiconductor element is formed using a dicing machine, etc. Then, each semiconductor chip formed by cutting is peeled off from the adhesive tape, thereby obtaining a plurality of semiconductor chips.

[0175] However, when the semiconductor element substrate is cut by sticking the dicing tape from the substrate side of the semiconductor element substrate, there are problems such as so-called edge collapse (ダレ) occurring on the cut surface (substrate side of the semiconductor chip) or the cut surface becoming rough.

[0176] Therefore, in recent years, in order to solve such a problem, the following method has been proposed, namely, to a semiconductor element substrate, a dicing adhesive tape is affixed from the side where the semiconductor element is formed, that is, the sealing resin side that seals the semiconductor element, rather than from the substrate side, and the semiconductor element substrate is cut.

[0177] Here, as a sealing resin for semiconductor elements such as LEDs and power semiconductors, epoxy resins with excellent electrical properties and heat resistance have been used in the past. However, epoxy resins have the following problems: they are prone to discoloration when used for high-output LEDs and power semiconductors, when used for short-wavelength LEDs, or due to the use environment of the semiconductor chip.

[0178] In contrast, silicone resins are used more often in recent years as sealing resins for semiconductor elements such as LEDs and power semiconductors because they are less likely to discolor due to heat or light than epoxy resins. More specifically, silicone resins containing either or both of methyl and phenyl groups as functional groups, i.e., methyl-containing silicone resins, phenyl-containing silicone resins, and silicone resins containing both methyl and phenyl groups, are used more often.

[0179] By using a silicone resin as a sealing resin for a semiconductor element, discoloration of the sealing resin due to heat or light can be suppressed.

[0180] In addition, the light transmittance of silicone resin is as high as 88% or more (wavelength 400-800nm) and the refractive index is as high as 1.41 or more. Therefore, when the semiconductor element is an LED, by using silicone resin as a sealing resin, the light emitted by the LED can be effectively extracted to the outside of the package. Among the above-mentioned silicone resins, by using silicone resins containing phenyl, the efficiency of emitted light can be further improved compared with the case of using silicone resins containing methyl.

[0181] The methyl group-containing silicone resin is not particularly limited, and examples thereof include KER-2300, KER-2460, KER-2500N, KER-2600, KER-2700, KER-2900, and X-32-2528 manufactured by Shin-Etsu Chemical Co., Ltd., IVS4312, IVS4312, XE14-C2042, IVS4542, IVS4546, IVS4622, IVS4632, IVS4742, IVS4752, IVSG3445, IVSG0810, IVSG5778, XE13-C2479, and IVSM4500 manufactured by Dow Corning Toray Corporation, and OE-6351, OE-6336, and OE-6301 manufactured by Momentive Advanced Materials Co., Ltd.

[0182] The silicone resin containing a methyl group and a phenyl group is not particularly limited, and examples thereof include KER-6075, KER-6150, and KER-6020 manufactured by Shin-Etsu Chemical Co., Ltd.

[0183] The phenyl group-containing silicone resin is not particularly limited, and examples thereof include KER-6110, KER-6000, KER-6200, ASP-1111, ASP-1060, ASP-1120, and ASP-1050P manufactured by Shin-Etsu Chemical Co., Ltd., XE14-C2508 manufactured by Momentive High-Tech Materials Co., Ltd., and OE-6520, OE-6550, OE-6631, OE-6636, OE-6635, and OE-6630 manufactured by Dow Corning Toray Corporation.

[0184] Conventionally, as a dicing adhesive tape for cutting semiconductor elements, an adhesive tape having an adhesive layer composed of, for example, an acrylic resin-based adhesive has been used.

[0185] However, if such a conventional adhesive tape is adhered to the side of the semiconductor element substrate where the semiconductor element is formed (sealing resin side) and the semiconductor element substrate is cut, if, for example, the adhesion between the sealing resin and the adhesive tape is insufficient, problems such as semiconductor chips flying apart may occur during cutting.

[0186] In particular, the above-mentioned silicone resin has a property of high demoulding properties compared with epoxy resins and the like that have been used as sealing resins in the past. Therefore, for semiconductor element substrates using silicone resin as sealing resin, when an adhesive tape whose adhesive layer is composed of an acrylic resin-based adhesive is attached, the adhesive force between the silicone resin as sealing resin and the adhesive tape is likely to decrease. As a result, when cutting the semiconductor element substrate, it is more likely to cause problems such as the scattering of semiconductor chips.

[0187] In contrast, in the adhesive tape 1 of the present embodiment, as described above, the adhesive layer 3 includes a silicone adhesive formed by mixing an organic silicone material (G) and an organic silicone resin (R) at an appropriate ratio, so that when cutting a semiconductor element substrate, even when the adhesive tape is used from the sealing resin side composed of the organic silicone resin, the adhesive force and the adhesive force with the sealing resin of the semiconductor element substrate can be well maintained. In addition, compared with conventional adhesive tapes, the generation of semiconductor chips flying when cutting a semiconductor element substrate can be suppressed.

[0188] On the other hand, the adhesive layer 3 contains the above-mentioned silicone adhesive as well as a photosensitive platinum (Pt) catalyst and a cross-linking agent, so that by irradiating light such as ultraviolet rays, the photosensitive platinum (Pt) catalyst in the silicone adhesive can be activated, promoting the cross-linking reaction between the addition reaction type silicone adhesive and the cross-linking agent for the addition reaction type silicone adhesive, and the cohesive force of the adhesive becomes greater than before light irradiation. As a result, the viscosity of the adhesive layer 3 is appropriately reduced, and the failure mode in the further holding force test is "interface peeling" or "no falling" in the holding force test. As a result, good pickup when peeling the semiconductor chip from the adhesive tape 1 can be achieved, and residual adhesive on the semiconductor chip can be suppressed.

[0189] Hereinafter, a method of using the adhesive tape 1 of the present embodiment and a method of manufacturing a semiconductor chip using the adhesive tape 1 of the present embodiment will be described in detail. Figure 2 (a) to (e) are views showing a method for manufacturing a semiconductor chip using the adhesive tape 1 of the present embodiment.

[0190] It should be noted that, here, the case of manufacturing a semiconductor chip having an LED element as a semiconductor element using the adhesive tape 1 is cited as an example for description. In addition, the method described below is an example of a method for using the adhesive tape 1 and a method for manufacturing a semiconductor chip using the adhesive tape 1, but is not limited to the following method.

[0191] In this embodiment, first, a plurality of semiconductor elements 102 are mounted on a substrate 101 made of, for example, a resin material, ceramics, etc., to produce a semiconductor element substrate 100. It should be noted that the semiconductor element 102 is, for example, an LED element, which is not shown in the figure, but is formed by stacking a plurality of semiconductor layers including, for example, a light-emitting layer that emits light when electricity is applied, and an electrode is formed on the upper portion.

[0192] Next, the plurality of semiconductor elements formed on the substrate 101 of the semiconductor element substrate 100 are sealed with a sealing resin 103 made of a silicone resin (sealing step). It should be noted that, in this example, the plurality of semiconductor elements 102 are sealed together with the sealing resin 103, but each semiconductor element 102 may be sealed separately with the sealing resin 103.

[0193] Then, if Figure 2 As shown in (a), the adhesive tape 1 and the semiconductor element substrate 100 are attached to each other so that the adhesive layer 3 of the adhesive tape 1 faces the sealing resin 103 of the semiconductor element substrate 100 (attaching step).

[0194] Then, if Figure 2 As shown in (b) and (c), the semiconductor element substrate 100 is cut along the predetermined cutting line X by a dicing machine or the like while the adhesive tape 1 is attached to the semiconductor element substrate 100 (cutting process). In this example, the semiconductor element substrate 100 to which the adhesive tape 1 is attached is cut from the substrate 101 side. Figure 2 As shown in (c), in this example, so-called full cutting is performed in which the semiconductor element substrate 100 is completely cut in the thickness direction.

[0195] Then, if Figure 2 As shown in (d), the adhesive tape 1 attached to the semiconductor element substrate 100 is irradiated with ultraviolet light from the substrate 2 side (ultraviolet light irradiation step). As described above, the substrate 2 is made of a material that can transmit ultraviolet light. Therefore, by irradiating the adhesive tape 1 with ultraviolet light from the substrate 2 side, the ultraviolet light passes through the substrate 2 and irradiates the adhesive layer 3.

[0196] In the adhesive tape 1 of the present embodiment, since the adhesive layer 3 has a photosensitive platinum (Pt) catalyst, the addition reaction of the addition reaction type silicone adhesive and the crosslinking agent in the adhesive layer 3 can be promoted by irradiating the adhesive layer 3 with ultraviolet rays. As a result, the crosslinking density, that is, the cohesive force in the adhesive layer 3 increases compared to before the ultraviolet irradiation, and the adhesive force of the adhesive layer 3 decreases.

[0197] Next, the semiconductor chip 200 formed by cutting the semiconductor element substrate 100 is peeled off (picked up) from the adhesive tape 1, so that Figure 2 As shown in (e), the individualized semiconductor chips 200 can be obtained (peeling step).

[0198] As described above, in the adhesive tape 1 of the present embodiment, the adhesive layer 3 comprises a silicone adhesive formed by mixing an organic silicone material (G) and an organic silicone resin (R) in an appropriate ratio. Thus, when the adhesive tape 1 is used for dicing, the adhesive force and viscous force between the adhesive tape 1 and the semiconductor element substrate 100 can be well maintained.

[0199] In recent years, silicone resins with high mold release properties are often used as sealing resins 103 for sealing semiconductor elements 102. In contrast, the adhesive tape 1 of this embodiment has the above-described structure and thus has good adhesion and tack to the sealing resins 103 made of silicone resins.

[0200] As a result, when the adhesive tape 1 of the present embodiment is used for dicing the semiconductor element substrate 100 , it is possible to suppress the scattering of the semiconductor chips 200 .

[0201] Furthermore, the silicone-based adhesive contained in the adhesive layer 3 of the adhesive tape 1 of the present embodiment has good adhesion to the sealing resin 103 as described above, and has a property of high mold releasability.

[0202] Furthermore, the adhesive tape 1 of the present embodiment includes, for example, a photosensitive platinum (Pt) catalyst that promotes the addition reaction of the addition reaction type silicone adhesive and the crosslinking agent by irradiation with light such as ultraviolet rays. Moreover, by irradiating the adhesive layer 3 with light through the substrate 2 after the cutting process and before the stripping process, the addition reaction of the addition reaction type silicone adhesive and the crosslinking agent in the adhesive layer 3 can be promoted, the cohesive force can be increased, and the viscosity of the adhesive layer 3 can be reduced. As a result, in the stripping process, when the semiconductor chip 200 obtained by cutting the semiconductor element substrate 100 is stripped (picked up) from the adhesive tape 1, the generation of so-called residual adhesive of the adhesive attached to the semiconductor chip 200 can be suppressed. In addition, good pick-up performance when the semiconductor chip 200 is stripped from the adhesive tape 1 can be achieved.

[0203] It should be noted that the above description is about a method of attaching the adhesive tape 1 from the sealing resin side and dicing a semiconductor element substrate having a plurality of semiconductor elements formed thereon to obtain individual semiconductor chips. However, the use of the adhesive tape 1 of this embodiment is not limited thereto.

[0204] The adhesive tape 1 of this embodiment can also be used, for example, in the manufacture of chip-level packaged LEDs to cut a semiconductor material formed by coating a plurality of LED elements with a phosphor as an example of a coating material to obtain individual chip-level packaged LEDs. It should be noted that the so-called phosphor is a member in which a fluorescent material is dispersed in a resin material, ceramic, or the like.

[0205] In recent years, with the miniaturization of chip-scale packaged LEDs, there is a tendency for the chip-scale packaged LEDs that have been singulated to be easily scattered during dicing. In contrast, by using the adhesive tape 1 of the present embodiment having the above-mentioned structure, the adhesion between the phosphor and the adhesive layer 3 can be well maintained, and the scattering of the chip-scale packaged LEDs that have been singulated can be suppressed.

[0206] Furthermore, after dicing, the adhesive layer 3 is irradiated with ultraviolet rays to reduce the adhesive force, thereby facilitating the peeling of the individual chip-scale package LEDs from the adhesive tape 1 and suppressing the generation of adhesive residue on the peeled chip-scale package LEDs.

[0207] Example

[0208] Next, the present invention will be described in more detail using Examples and Comparative Examples. It should be noted that the present invention is not limited to the following Examples.

[0209] The present inventors prepared adhesive tapes 1 by making the components of the adhesive layer 3, the thickness of each layer, etc. different for the first embodiment in which the adhesive layer 3 includes an addition reaction type silicone adhesive as a curable silicone adhesive and the second embodiment in which the adhesive layer 3 includes an addition reaction type silicone adhesive and a peroxide curable silicone adhesive as a curable silicone adhesive, and evaluated the prepared adhesive tapes 1. It should be noted that in the following examples, Examples 1 to 8 correspond to the first embodiment, and Examples 9 to 15 correspond to the second embodiment.

[0210] Hereinafter, each example and each comparative example will be described in detail.

[0211] 1. Production of adhesive tape 1

[0212] (Example 1)

[0213] Toluene, 166.67 parts by mass of an addition reaction type silicone adhesive composed of an organopolysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule (SD4584 (trade name) manufactured by Dow Corning Toray Co., Ltd., a crosslinking agent-free type, solid content concentration 60% by mass), and 3.30 parts by mass of a crosslinking agent composed of an organopolysiloxane having a hydrosilyl group in the molecule (BY24-741 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content concentration 20% by mass) were mixed and stirred. Next, 5.33 parts by mass of a solution of a photosensitive platinum (Pt) catalyst (trimethyl (methylcyclopentadienyl) platinum (IV) manufactured by Sigma Aldrich Japan Co., Ltd.) diluted with toluene to a solid content concentration of 15% by mass was added, mixed and stirred, and the adhesive solution of the first embodiment was prepared.

[0214] Next, the adhesive solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 120° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.

[0215] (Example 2)

[0216] In the preparation of the adhesive solution of the first method, an addition reaction type silicone adhesive composed of an organic polysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule (SD4584 (trade name) manufactured by Dow Corning Toray Co., Ltd., a cross-linking agent-free type, solid content concentration 60% by mass) is used, and the thickness of the adhesive layer 3 after drying is set to 30 μm. Except for this, the same operation as in Example 1 is performed to obtain an adhesive tape 1 with a total thickness of 68 μm after drying.

[0217] (Example 3)

[0218] An adhesive tape 1 having a total thickness of 22 μm after drying was obtained in the same manner as in Example 2 except that a PET film having a thickness of 12 μm was used as the substrate 2 and the thickness of the adhesive layer 3 after drying was 10 μm.

[0219] (Example 4)

[0220] In the preparation of the adhesive solution of the first method, an addition reaction type silicone adhesive composed of an organic polysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule (SD4585 (trade name) manufactured by Dow Corning Toray Co., Ltd., a cross-linking agent-free type, solid content concentration 60% by mass) is used, as the substrate 2, a PET film with a thickness of 50 μm is used, and the thickness of the adhesive layer 3 after drying is set to 40 μm. Except for this, the same operation as in Example 1 is carried out to obtain an adhesive tape 1 with a total thickness of 90 μm after drying.

[0221] (Example 5)

[0222] In the preparation of the adhesive solution of the first mode, the same operation as in Example 1 was carried out except that the addition amount of the crosslinking agent (BY24-741 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content concentration 20% by mass) was set to 1.65 parts by mass, to obtain an adhesive tape 1 having a total thickness of 58 μm after drying.

[0223] (Example 6)

[0224] In the preparation of the first mode of the adhesive solution, the same operation as in Example 1 was carried out except that the addition amount of the crosslinking agent (BY24-741 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content concentration 20% by mass) was set to 8.25 parts by mass, to obtain an adhesive tape 1 having a total thickness of 58 μm after drying.

[0225] (Example 7)

[0226] In the preparation of the adhesive solution of the first method, the addition amount of a solution of a photosensitive platinum (Pt) catalyst (trimethyl(methylcyclopentadienyl)platinum(IV) manufactured by Sigma Aldrich Japan Co., Ltd.) diluted with toluene to a solid content concentration of 15% by mass was set to 2.00 parts by mass. Except for this, the same operation as in Example 1 was performed to obtain an adhesive tape 1 with a total thickness of 58 μm after drying.

[0227] (Example 8)

[0228] In the preparation of the adhesive solution of the first method, the addition amount of a solution of a photosensitive platinum (Pt) catalyst (trimethyl(methylcyclopentadienyl)platinum(IV) manufactured by Sigma Aldrich Japan Co., Ltd.) diluted with toluene to a solid content concentration of 15% by mass was set to 20.00 parts by mass. Except for this, the same operation as in Example 1 was performed to obtain an adhesive tape 1 with a total thickness of 58 μm after drying.

[0229] (Example 9)

[0230] Toluene, 166.67 parts by mass of an addition reaction type silicone adhesive composed of an organopolysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule (SD4584 (trade name) manufactured by Dow Corning Toray Co., Ltd., a crosslinking agent-free type, solid content concentration 60% by mass), and 3.30 parts by mass of a crosslinking agent composed of an organopolysiloxane having a hydrosilyl group in the molecule (BY24-741 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content concentration 20% by mass) were mixed and stirred. Next, 5.33 parts by mass of a solution of a photosensitive platinum (Pt) catalyst (trimethyl (methylcyclopentadienyl) platinum (IV) manufactured by Sigma Aldrich Japan Co., Ltd.) diluted with toluene to a solid content concentration of 15% by mass was added, mixed and stirred, and an addition reaction type silicone adhesive solution was prepared.

[0231] On the other hand, toluene, 166.67 parts by mass of a peroxide-curable silicone adhesive composed of an organopolysiloxane (SH4280 (trade name) manufactured by Dow Corning Toray Corporation, with a solid content concentration of 60% by mass), and 5.00 parts by mass of an initiator composed of methyl benzoyl peroxide (NYPER K40 (trade name) manufactured by NOF Corporation, with a solid content concentration of 40% by mass) were mixed and stirred to prepare a peroxide-curable silicone adhesive solution.

[0232] Next, the obtained addition reaction type silicone adhesive solution and peroxide curing type silicone adhesive solution are mixed and stirred to prepare the adhesive solution of the second embodiment. It should be noted that the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted so that 100 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0233] Next, the adhesive solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.

[0234] (Example 10)

[0235] In the preparation of the adhesive solution of the second method, the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted in a manner such that 63.70 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive. Except for this, the same operation as in Example 9 is performed to obtain an adhesive tape 1 with a total thickness of 58 μm after drying.

[0236] (Example 11)

[0237] In the preparation of the adhesive solution of the second method, the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted in a manner such that 150 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive. Except for this, the same operation as in Example 9 is performed to obtain an adhesive tape 1 with a total thickness of 58 μm after drying.

[0238] (Example 12)

[0239] In the preparation of the addition reaction type silicone adhesive solution of the second mode of adhesive solution, as an addition reaction type silicone adhesive composed of an organic polysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule, SD4580 (trade name) manufactured by Dow Corning Toray Corporation without added crosslinking agent (solid content concentration 60 mass %) is used. Except for this, the same operation as in Example 9 is carried out to obtain an adhesive tape 1 with a total thickness of 58 μm after drying.

[0240] (Example 13)

[0241] In the preparation of the addition reaction type silicone adhesive solution of the second mode of adhesive solution, as an addition reaction type silicone adhesive composed of an organic polysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule, SD4586 (trade name) manufactured by Dow Corning Toray Co., Ltd. without added crosslinking agent (solid content concentration 60 mass %) is used. Except for this, the same operation as in Example 9 is carried out to obtain an adhesive tape 1 with a total thickness of 58 μm after drying.

[0242] (Example 14)

[0243] Toluene, 166.67 parts by mass of an addition reaction type silicone adhesive composed of an organopolysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule (SD4585 (trade name) manufactured by Dow Corning Toray Co., Ltd., a crosslinking agent-free type, solid content concentration 60% by mass), and 3.30 parts by mass of a crosslinking agent composed of an organopolysiloxane having a hydrosilyl group in the molecule (BY24-741 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content concentration 20% by mass) were mixed and stirred. Next, 5.33 parts by mass of a solution of a photosensitive platinum (Pt) catalyst (trimethyl (methylcyclopentadienyl) platinum (IV) manufactured by Sigma Aldrich Japan Co., Ltd.) diluted with toluene to a solid content concentration of 15% by mass was added, mixed and stirred, and an addition reaction type silicone adhesive solution was prepared.

[0244] Meanwhile, toluene and 166.67 parts by mass of a peroxide-curable silicone adhesive composed of an organopolysiloxane (BY24-717 (trade name), manufactured by Dow Corning Toray Corporation, solid content concentration 60% by mass) were mixed and stirred to prepare a peroxide-curable silicone adhesive solution.

[0245] Next, the obtained addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution are mixed and stirred to prepare the adhesive solution of the second embodiment. It should be noted that the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted so that 20 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0246] Next, the adhesive solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.

[0247] (Example 15)

[0248] First, in the same manner as the adhesive solution of the first embodiment of Example 4, an addition reaction type silicone-based adhesive solution was prepared.

[0249] On the other hand, toluene, 250.00 parts by mass of a peroxide-curable silicone adhesive composed of an organopolysiloxane (SE4200 (trade name) manufactured by Dow Corning Toray Corporation, with a solid content concentration of 40% by mass), and 5.00 parts by mass of an initiator composed of methyl benzoyl peroxide (NYPER K40 (trade name) manufactured by NOF Corporation, with a solid content concentration of 40% by mass) were mixed and stirred to prepare a peroxide-curable silicone adhesive solution.

[0250] Next, the obtained addition reaction type silicone adhesive solution and peroxide curing type silicone adhesive solution are mixed and stirred to prepare the adhesive solution of the second embodiment. It should be noted that the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted so that 150 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0251] Next, the adhesive solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 125 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 145 μm after drying was obtained.

[0252] (Comparative Example 1)

[0253] An adhesive tape 1 having a total thickness of 73 μm after drying was obtained in the same manner as in Example 1, except that 6 parts by mass of a platinum metal catalyst (NC-25 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content 25% by mass) was used instead of a solution of a photosensitive platinum (Pt) catalyst (trimethyl(methylcyclopentadienyl)platinum(IV) manufactured by Sigma Aldrich Japan Co., Ltd.), and the thickness of the adhesive layer 3 after drying was set to 35 μm.

[0254] (Comparative Example 2)

[0255] To the adhesive solution of Example 1, 10.00 parts by mass of YF3897 (trade name), a linear polysiloxane having silanol groups at both ends and a solid content of 100% by mass, manufactured by Momentive High-Tech Materials Co., Ltd., was further added as a silicone resin (R3) used in an addition reaction-type silicone-based adhesive, and the thickness of the adhesive layer 3 after drying was set to 30 μm. Except for this, the same operation as in Example 1 was performed to obtain an adhesive tape 1 with a total thickness of 68 μm after drying.

[0256] (Comparative Example 3)

[0257] As an addition reaction type silicone adhesive composed of an organic polysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule, SD4586 (trade name) manufactured by Dow Corning Toray Corporation without added crosslinking agent (solid content concentration 60% by mass) was used, and the thickness of the adhesive layer 3 after drying was set to 40 μm. Except for this, the same operation as in Example 1 was carried out to obtain an adhesive tape 1 with a total thickness of 78 μm after drying.

[0258] (Comparative Example 4)

[0259] Toluene, 166.67 parts by mass of an addition reaction type silicone adhesive composed of an organopolysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule (SD4584 (trade name) manufactured by Dow Corning Toray Co., Ltd., a crosslinking agent-free type, solid content concentration 60% by mass), and 3.30 parts by mass of a crosslinking agent composed of an organopolysiloxane having a hydrosilyl group in the molecule (BY24-741 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content concentration 20% by mass) were mixed and stirred. Next, 6.00 parts by mass of a platinum metal catalyst (NC-25 (trade name) manufactured by Dow Corning Toray Co., Ltd., solid content 25% by mass) were added, mixed and stirred, and an addition reaction type silicone adhesive solution was prepared.

[0260] On the other hand, a peroxide-curable silicone-based adhesive solution was prepared in the same manner as in Example 9.

[0261] Next, the obtained addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution are mixed and stirred to prepare an adhesive mixed solution. It should be noted that the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted so that 50 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0262] Next, the adhesive mixed solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 30 μm after drying. Thus, an adhesive tape 1 having a total thickness of 68 μm after drying was obtained.

[0263] (Comparative Example 5)

[0264] First, in the same manner as the adhesive solution of the first embodiment of Example 2, an addition reaction type silicone-based adhesive solution was prepared.

[0265] On the other hand, toluene, 166.67 parts by mass of a peroxide-curable silicone adhesive composed of an organopolysiloxane (BY241-717 (trade name) manufactured by Dow Corning Toray Corporation, with a solid content concentration of 60% by mass), and 5.00 parts by mass of an initiator composed of methyl benzoyl peroxide (NYPER K40 (trade name) manufactured by NOF Corporation, with a solid content concentration of 40% by mass) were mixed and stirred to prepare a peroxide-curable silicone adhesive solution.

[0266] Next, the obtained addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution are mixed and stirred to prepare an adhesive mixed solution. It should be noted that the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted so that 100 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0267] Next, the adhesive mixed solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.

[0268] (Comparative Example 6)

[0269] First, as an addition reaction type silicone adhesive composed of an organic polysiloxane having a vinylsilyl group as an alkenyl group bonded to a silicon atom in the molecule, SD4587 (trade name) manufactured by Dow Corning Toray Corporation without adding a crosslinking agent (solid content concentration of 60% by mass) was used. Except for this, the addition reaction type silicone adhesive was prepared in the same manner as in Example 1.

[0270] On the other hand, a peroxide-curable silicone-based adhesive solution was prepared in the same manner as in Example 15.

[0271] Next, the obtained addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution are mixed and stirred to prepare an adhesive mixed solution. It should be noted that the mixing ratio of the addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution is adjusted so that 100 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0272] Next, the adhesive mixed solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.

[0273] (Comparative Example 7)

[0274] First, in the same manner as in Comparative Example 2, an addition reaction type silicone-based adhesive solution was prepared.

[0275] On the other hand, a peroxide-curable silicone-based adhesive solution was prepared in the same manner as in Comparative Example 5.

[0276] Next, the obtained addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution are mixed and stirred to prepare an adhesive mixed solution. It should be noted that the mixing ratio of the addition reaction type silicone adhesive and the peroxide curing type silicone adhesive is adjusted so that 150 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0277] Next, the adhesive mixed solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.

[0278] (Comparative Example 8)

[0279] First, in the same manner as in Example 13, an addition reaction type silicone-based adhesive solution was prepared.

[0280] On the other hand, a peroxide-curable silicone-based adhesive solution was prepared in the same manner as in Comparative Example 6.

[0281] Next, the obtained addition reaction type silicone adhesive solution and the peroxide curing type silicone adhesive solution are mixed and stirred to prepare an adhesive mixed solution. It should be noted that the mixing ratio of the addition reaction type silicone adhesive and the peroxide curing type silicone adhesive is adjusted so that 30 parts by mass (solid content) of the peroxide curing type silicone adhesive is contained relative to 100 parts by mass (solid content) of the addition reaction type silicone adhesive.

[0282] Next, the adhesive mixed solution was applied to a substrate 2 made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then heated at 160° C. for 3 minutes to form an adhesive layer 3 having a thickness of 20 μm after drying. Thus, an adhesive tape 1 having a total thickness of 58 μm after drying was obtained.

[0283] The contents of the components of the adhesive layer 3 and the thickness of each layer in Examples 1 to 15 and Comparative Examples 1 to 8 are shown in Tables 1 to 3. In Tables 1 to 3, the words "organic silicone material" and "organic silicone resin" are abbreviated as "material" and "resin", respectively.

[0284] [Table 1]

[0285]

[0286] [Table 2]

[0287]

[0288]

[0289] [Table 3]

[0290] 2. Evaluation Method

[0291] Next, the evaluation method of the adhesive tape 1 will be described.

[0292] (1) Adhesion test

[0293] The adhesive tapes 1 prepared in Examples 1 to 15 and Comparative Examples 1 to 8 were subjected to an adhesion test to BA-SUS (peel adhesion test) according to the method described in the adhesive tape / adhesive sheet test method (JIS Z 0237 (2009)).

[0294] Specifically, the adhesive tape 1 was attached to a stainless steel plate (SUS304) with a surface roughness (Ra) of 50±25 nm after bright annealing (BA), and a roller with a mass of 2000 g was reciprocated once at a speed of 5 mm / s for pressure bonding. Then, after leaving it for 20 to 40 minutes, it was peeled off at a speed of 5 mm / s in a direction 180° to the stainless steel plate using a tensile testing machine, and the adhesion to the polished SUS plate was measured.

[0295] The adhesive strength test was also performed on the adhesive tape 1 before ultraviolet irradiation. In addition, as a result of the adhesive strength test, if the fixing force of the adhesive tape 1 when used for cutting semiconductor materials is considered, it is preferably 2.4 N / 10 mm or more and 5.5 N / 10 mm or less.

[0296] (2) Ball viscosity test

[0297] (2-1) Determination of initial ball viscosity

[0298] The adhesive tapes 1 prepared in Examples 1 to 15 and Comparative Examples 1 to 8 were subjected to a ball tack test in accordance with the method described in the adhesive tape / adhesive sheet test method (JIS Z 0237 (2009)).

[0299] (2-2) Determination of ball viscosity after UV irradiation

[0300] The adhesive layer 3 of each adhesive tape 1 prepared in Examples 1 to 15 and Comparative Examples 1 to 8 was bonded to a fluorine-based release film (SS1A manufactured by NIPPA Co., Ltd., thickness 75 μm). Then, ultraviolet rays were irradiated from the substrate 2 side of the adhesive tape 1, and after being left at a temperature of 23° C. and a humidity of 50±5% RH for 20 to 40 minutes, a ball adhesion test was performed in the same manner as the initial ball adhesion test according to the method described in the adhesive tape / adhesive sheet test method (JIS Z0237 (2009)).

[0301] Regarding ultraviolet irradiation, a high-pressure mercury lamp was used and the wavelength was adjusted to 365 nm so that the cumulative light intensity was 1200 mJ / cm 2 It should be noted that the accumulated light intensity was set to 3000 mJ / cm 2 The ball viscosity was also measured in the same manner, but no difference was observed when the cumulative light intensity was set to 1200 mJ / cm 2 Therefore, the accumulated light intensity is set to 1200mJ / cm2 Make an evaluation.

[0302] As a result of the ball tack test, if the pickup properties of semiconductor chips or the like separated by dicing are taken into consideration, the ball tack (ball number) after UV irradiation is preferably lower than the initial ball tack (ball number).

[0303] (3) Holding force test

[0304] (3-1) Determination of initial holding force

[0305] The adhesive tapes 1 prepared in Examples 1 to 15 and Comparative Examples 1 to 8 were subjected to a holding force test in accordance with the method described in the adhesive tape / adhesive sheet test method (JIS Z 0237 (2009)).

[0306] Specifically, it is pasted on a stainless steel plate (SUS304) polished with water-resistant abrasive paper, and maintained at a temperature of 40°C and a humidity of 33% RH with a predetermined weight installed, and the time elapsed from the adhesive tape 1 peeling off from the stainless steel plate to falling off (falling time (minutes)) is measured. Furthermore, the failure mode of the adhesive tape 1 when it is peeled off from the stainless steel plate is observed (whether the failure mode between the adhesive layer 3 and the stainless steel plate is interface peeling or cohesive failure). It should be noted that the measurement of the falling time in the holding force test is carried out until 5000 minutes. In addition, as the results of the holding force test shown in Tables 4 to 6 described later, the falling time (minutes) and the failure mode of the adhesive tape 1 are shown. In addition, the situation where the adhesive tape 1 is not peeled off (falling off) until 5000 minutes is expressed as "holding".

[0307] (3-2) Determination of retention strength after UV irradiation

[0308] The adhesive tape 1 was irradiated with ultraviolet rays in the same manner as described in the measurement of ball tack after UV irradiation, and after leaving it to stand, a holding force test was performed in the same manner as the initial holding force test.

[0309] (3-3) Relationship between holding force and failure mode

[0310] Here, the relationship between the holding force of the adhesive tape 1 and the failure mode will be described. Figure 3 It is a schematic diagram showing the relationship between the crosslinking density of the addition reaction type silicone-based adhesive in the adhesive layer 3 and the result (drop time) of the holding force test of the adhesive tape 1 .

[0311] like Figure 3As shown, in the adhesive tape 1, as the crosslinking density of the addition reaction type silicone adhesive in the adhesive layer 3 increases, the failure mode of the adhesive tape 1 relative to the stainless steel plate in the holding power test changes from [cohesive failure of the adhesive layer 3 (falling)] → [holding (not falling)] → [interface peeling (falling) between the adhesive layer 3 and the stainless steel plate].

[0312] In addition, if Figure 3 As shown, in the region where the failure mode of the adhesive tape 1 is cohesive failure, the holding force (drop time) of the adhesive tape 1 increases as the crosslinking density of the addition reaction type silicone-based adhesive in the adhesive layer 3 increases.

[0313] On the other hand, Figure 3 As shown in the figure, in the region where the failure mode of the adhesive tape 1 is interfacial peeling, the holding force (falling time) of the adhesive tape 1 decreases as the crosslinking density of the addition reaction type silicone adhesive in the adhesive layer 3 increases. This is presumably because as the crosslinking density of the addition reaction type silicone adhesive increases, the cohesive force of the adhesive layer 3 increases, and the adhesive force of the adhesive tape 1 decreases, and as a result, the adhesive tape 1 easily peels off from the stainless steel plate and falls.

[0314] As a result of the holding power test, it is preferred that the failure mode after at least UV irradiation is holding or interface peeling, more preferably at least the failure mode after UV irradiation is interface peeling, and further preferably the failure modes at the initial stage (before UV irradiation) and after UV irradiation are both interface peeling. In addition, when the failure modes at the initial stage (before UV irradiation) and after UV irradiation are both interface peeling, it is preferred that the holding power (falling time) after UV irradiation is lower than the initial stage (before UV irradiation).

[0315] In this case, after the adhesive tape 1 is used for dicing a semiconductor device substrate, when the obtained semiconductor chip is peeled from the adhesive tape 1, UV is irradiated on the adhesive tape 1, so that residual adhesive is less likely to be generated on the semiconductor chip.

[0316] (4) Test on residual silicone resin

[0317] The adhesive tapes 1 prepared in Examples 1 to 15 and Comparative Examples 1 to 8 were subjected to a residual adhesive test on the silicone resin.

[0318] First, agent A and agent B of a methyl-containing silicone resin (KER-2500N (trade name) manufactured by Shin-Etsu Chemical Co., Ltd.) as a silicone resin for LED devices were mixed at a mixing ratio of 1:1 to prepare a mixed solution. The mixed solution was applied to a stainless steel plate and heated at 100°C for 1 hour and further at 150°C for 2 hours to cure, thereby preparing a silicone test piece A.

[0319] Similarly, agent A and agent B of a phenyl-containing silicone resin (KER-6110 (trade name) manufactured by Shin-Etsu Chemical Co., Ltd.) as a silicone resin for LED devices were mixed at a mixing ratio of 3:7 to prepare a mixed solution. The mixed solution was applied to a stainless steel plate and heated at 100°C for 2 hours and further at 150°C for 5 hours to cure, thereby preparing a silicone test piece B.

[0320] Next, the adhesive layer 3 of the adhesive tape 1 was attached to the silicone test pieces A and B, respectively, and a roller with a mass of 2000 g was reciprocated once at a speed of 5 mm / s for crimping. Next, the adhesive tape 1 was irradiated with ultraviolet rays from the substrate 2 side in the same manner as described in the measurement of ball adhesion after UV irradiation, and then placed in an environment of temperature 40°C and humidity 90% RH for 120 hours. Then, the adhesive tape 1 was peeled off at a speed of 800 mm / s to 1200 mm / s at room temperature in a direction of 90° to the silicone test pieces A and B, and the residual adhesive on the silicone test pieces A and B was confirmed by visual inspection.

[0321] (5) Test on epoxy resin residual glue

[0322] The adhesive tapes 1 prepared in Examples 1 to 15 and Comparative Examples 1 to 8 were subjected to a residual adhesive test on epoxy resin.

[0323] For an epoxy test piece consisting of an epoxy resin plate (NL-EG-23 (trade name) manufactured by Nikko Chemical Co., Ltd.) obtained by impregnating epoxy resin in a glass cloth substrate, the adhesive layer 3 of the adhesive tape 1 was pasted, and a roller with a mass of 2000 g was reciprocated once at a speed of 5 mm / s for crimping. Then, the adhesive tape 1 was irradiated with ultraviolet rays from the substrate 2 side in the same manner as the conditions described in the measurement of ball adhesion after UV irradiation, and then placed in an environment of temperature 40°C and humidity 90% RH for 120 hours. Then, at room temperature, the adhesive tape 1 was peeled off at a speed of 800 mm / s to 1200 mm / s in a direction of 90° to the epoxy test piece, and the residual adhesive on the epoxy test piece was confirmed by visual inspection.

[0324] The silicone resin residual adhesive test and the epoxy resin residual adhesive test were evaluated according to the following criteria: An evaluation of A or B was considered acceptable.

[0325] A: No residual adhesive within 100% of the test piece per unit area

[0326] B: Residual adhesive is observed within a range of less than 2% per unit area of ​​the test piece

[0327] C: Residual adhesive is observed in the range of 2% or more and less than 5% per unit area of ​​the test piece

[0328] D: Glue residue is observed in an area of ​​5% or more per unit area of ​​the test piece, or glue residue is observed at the edge of the test piece.

[0329] (6) Cutting test

[0330] A cutting test was performed on the adhesive tapes 1 produced in Examples 1 to 15 and Comparative Examples 1 to 8.

[0331] Specifically, first, a molding epoxy resin (CEL-400ZHF40-W75G (trade name) manufactured by Hitachi Chemical Co., Ltd.) was charged into a mold and sealed at a pressure of 50 kgf / cm 2 (491N / cm 2 ), the sealing material was heat cured under the conditions of a thickness of 0.3 mm and a heating temperature of 150° C.×300 seconds to produce a circular plate-shaped (diameter 200 mm (8 inches)) cut test piece.

[0332] In addition, the adhesive layer 3 of the adhesive tape 1 was pasted on the cutting ring, and the part that oozed out from the ring was cut off, and then further pasted on a fluorine-based release film (SS1A (trade name) manufactured by NIPPA Co., Ltd., thickness 75 μm). Then, a roller with a mass of 2000 g was reciprocated to press the adhesive tape 1 and the ring part. Then, the fluorine-based release film was peeled off, and the cut test piece was pasted on the adhesive layer in the center of the ring and pressed.

[0333] Furthermore, the dicing test piece was cut into 10 mm × 10 mm chips together with the adhesive tape 1 using a dicing device (A-WD-100A (trade name)) manufactured by Tokyo Seimitsu Co., Ltd. and a dicing blade manufactured by Disco Co., Ltd. At this time, the number of scattered chips was measured to evaluate the fixing force in the dicing test.

[0334] Next, the adhesive tape 1 attached to the chip singulated into 10 mm × 10 mm pieces was irradiated with ultraviolet light under the same conditions as described in the measurement of ball tack after UV irradiation. Then, the singulated chips were picked up from the adhesive tape 1, and the presence of residual adhesive on the chips was visually confirmed to evaluate the residual adhesive in the dicing test. In addition, the number of chips that failed to be picked up was measured to evaluate the pick-up performance in the dicing test.

[0335] The fixing force in the cutting test was evaluated according to the following criteria: An evaluation of A or B was considered acceptable.

[0336] A: The number of scattered chips is 0 out of 100.

[0337] B: The number of scattered chips is 1 in 100

[0338] C: The number of scattered chips is 2 out of 100

[0339] D: The number of scattered chips is 3 or more in 100

[0340] The residual adhesive in the cutting test was evaluated according to the following criteria. An evaluation of A was considered acceptable.

[0341] A: No residual glue was observed on the chip

[0342] D: Residual adhesive is observed on the chip, or adhesive wire drawing is observed on the side of the chip

[0343] The pick-up property in the cutting test was evaluated according to the following criteria: An evaluation of A or B was considered acceptable.

[0344] A: The number of chips that failed to be picked up is 0 out of 100.

[0345] B: The number of chips that failed to be picked up is 1 in 100

[0346] C: The number of chips that failed to be picked up is 2 out of 100

[0347] D: The number of chips that failed to be picked up is 3 or more out of 100

[0348] 3. Test results

[0349] Tables 4 to 6 show the evaluation results of the adhesive tapes 1 of Examples 1 to 15 and Comparative Examples 1 to 8.

[0350] [Table 4]

[0351]

[0352] [Table 5]

[0353]

[0354] [Table 6]

[0355]

[0356] As shown in Tables 4 to 6, it was confirmed that in the adhesive tapes 1 of Examples 1 to 8 corresponding to the first mode in which the adhesive layer 3 is mainly composed of an addition reaction type silicone adhesive and contains a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type silicone adhesive, and in the adhesive tapes 1 of Examples 9 to 15 corresponding to the second mode in which the adhesive layer 3 is mainly composed of a mixture of an addition reaction type silicone adhesive and a peroxide curing type silicone adhesive and contains a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type silicone adhesive, satisfactory results were obtained in the adhesion test, ball adhesion test, holding force test, silicone resin residual adhesive test, epoxy resin residual adhesive test, and cutting test (fixing force, residual adhesive and pickup properties).

[0357] Thus, it was confirmed that the adhesive tapes 1 of Examples 1 to 8 corresponding to the first mode in which the adhesive layer 3 has an addition reaction type silicone adhesive as the main agent and contains a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type silicone adhesive, and the adhesive tapes 1 of Examples 9 to 15 corresponding to the second mode in which the adhesive layer 3 has a mixture of an addition reaction type silicone adhesive and a peroxide curing type silicone adhesive as the main agent and contains a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type silicone adhesive, are useful as adhesive tapes for cutting semiconductor materials, more specifically, as adhesive tapes for cutting that are adhered from the sealing resin side of a semiconductor element substrate and used for cutting.

[0358] In contrast, it was confirmed that in Comparison Examples 1 to 3 in which the adhesive layer 3 did not satisfy the conditions of the adhesive layer 3 of the first mode, and Comparison Examples 4 to 8 in which the adhesive layer 3 did not satisfy the conditions of the adhesive layer 3 of the second mode, all test results were worse than those of Examples 1 to 15 in the silicone resin residual adhesive test, the epoxy resin residual adhesive test, and the cutting test (fixing force, residual adhesive, and pickup properties).

[0359] Specifically, in the adhesive tape 1 of Comparative Example 1 in which the adhesive layer 3 of the first mode does not contain a photosensitive platinum (Pt) catalyst, although a conventional platinum (Pt) catalyst is contained, no change is observed in the results of the ball adhesion test and the holding force test before and after UV irradiation, and the improvement of the cohesive force is insufficient, so a large amount of residual adhesive is observed in the silicone resin residual adhesive test and the epoxy resin residual adhesive test. In addition, in the cutting test, the pick-up property of the chip of the cut test piece is poor, and residual adhesive is observed on the chip.

[0360] In addition, the adhesive tape 1 of Comparative Example 4 in which the adhesive layer 3 of the second embodiment does not contain a photosensitive platinum (Pt) catalyst also exhibited the same results as those of Comparative Example 1.

[0361] Furthermore, in the adhesive tape 1 of Comparative Example 2, in which the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) to the total mass (Rw) of the organic silicone resin (R) and the content ratio of the organic silicone material (G1) having an olefin group in the total mass of the organic silicone material (G) and the organic silicone resin (R) are respectively less than the lower limit of the adhesive layer 3 of the first mode, the adhesion is high, the changes in the results of the ball adhesion test and the retention test before and after UV irradiation are small, and the cohesion improvement is slightly insufficient. Therefore, in the test of residual adhesive on the organic silicone resin and the test of residual adhesive on the epoxy resin, a large amount of residual adhesive was observed. In addition, in the cutting test, the pick-up property of the chip of the cut test piece was poor, and residual adhesive was also observed on the surface of the chip.

[0362] Furthermore, in the adhesive tape 1 of Comparative Example 3, in which the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) to the total mass (Rw) of the organic silicone resin (R) and the content ratio of the organic silicone material (G1) having an olefin group in the total mass of the organic silicone material (G) and the organic silicone resin (R) respectively exceed the upper limit value of the adhesive layer 3 of the first mode, although the results of the ball viscosity test and the retention test changed before and after UV irradiation, the cohesion was improved, but the adhesion was low. Therefore, in the cutting test, the fixing force of the cut test piece was low, and a large number of chips were observed to be scattered. It should be noted that no residual glue was observed in the test of residual glue on the organic silicone resin and the test of residual glue on the epoxy resin. In addition, in the cutting test, no residual glue was observed for the chips that did not scatter.

[0363] Furthermore, it can be seen that in the adhesive tape 1 of Comparative Example 5, in which the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) to the total mass (Rw) of the organic silicone resin (R) is less than the lower limit of the adhesive layer 3 of the second mode, although the results of the ball viscosity test and the retention test changed slightly before and after UV irradiation, and the cohesion was improved, it cannot be said to be sufficient. In the cutting test, the pick-up property of the chip of the cut test piece was slightly poor. It should be noted that in the test of residual glue on the organic silicone resin and the test of residual glue on the epoxy resin, the residual glue was observed to a small extent, and in the cutting test, no residual glue was observed for the chips that could be picked up.

[0364] Furthermore, in the adhesive tape 1 of Comparative Example 6, in which the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) to the total mass (Rw) of the organic silicone resin (R) exceeds the upper limit value of the adhesive layer 3 of the second mode, although the results of the ball viscosity test and the retention test changed before and after UV irradiation, the cohesion was improved, but the adhesion was low, so in the cutting test, the fixing force of the cutting test piece was low, and a large number of chips were observed to fly. It should be noted that no residual glue was observed in the test of residual glue on the organic silicone resin and the test of residual glue on the epoxy resin. In addition, in the cutting test, no residual glue was observed for the chips that did not fly.

[0365] Furthermore, in the adhesive tape 1 of Comparative Example 7, in which the mass ratio (Gw) / (Rw) of the total mass (Gw) of the organic silicone material (G) to the total mass (Rw) of the organic silicone resin (R) exceeds the upper limit of the adhesive layer 3 of the second mode, and the content ratio of the organic silicone material (G1) having an olefin group in the total mass of the organic silicone material (G) and the organic silicone resin (R) is less than the lower limit of the adhesive layer 3 of the second mode, the adhesive force is high due to the effect of the curing of the peroxide-curing organic silicone adhesive, and the results of the ball adhesion test and the holding force test before and after UV irradiation change little, and the further improvement of the cohesive force is slightly insufficient. Therefore, in the test of the residual adhesive of the organic silicone resin and the test of the residual adhesive of the epoxy resin, a large amount of residual adhesive was observed. In addition, in the cutting test, the pick-up property of the chip of the cut test piece was poor, and residual adhesive was also observed on the surface of the chip.

[0366] Furthermore, in the adhesive tape 1 of Comparative Example 8 in which the content ratio of the organic silicone material (G1) having an alkenyl group in the total mass of the organic silicone material (G) and the organic silicone resin (R) exceeds the upper limit value of the adhesive layer 3 of the second mode, although the results of the ball viscosity test and the retention test changed before and after UV irradiation, the cohesion was improved, but the adhesion was low. Therefore, in the cutting test, the fixing force of the cut test piece was low, and a large number of chips were observed to fly. It should be noted that no residual glue was observed in the test of residual glue on the organic silicone resin and the test of residual glue on the epoxy resin. In addition, in the cutting test, no residual glue was observed for the chips that did not fly.

[0367] Explanation of symbols

[0368] 1: Adhesive tape, 2: Base material, 3: Adhesive layer, 100: Semiconductor element substrate, 101: Substrate, 102: Semiconductor element, 103: Sealing resin, 200: Semiconductor chip.

Claims

1. An adhesive tape for cutting, characterized in that: The adhesive comprises a substrate and a silicone adhesive layer laminated on the substrate, and is used when dividing a semiconductor material having a plurality of semiconductor elements covered with a covering material into a plurality of semiconductor chips. The organic silicon adhesive layer has an addition reaction type organic silicon adhesive as a main agent, and contains a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type organic silicon adhesive. The mass ratio Gw / Rw of the total mass Gw of the organic silicone material G contained in the organic silicone adhesive layer to the total mass Rw of the organic silicone resin R is in the range of 35 / 65 to 50 / 50, and the content ratio of the organic silicone material G1 having an alkenyl group in the total mass of the organic silicone material G and the organic silicone resin R is in the range of 35 mass % or more and 50 mass % or less, The dicing adhesive tape satisfies all of the following conditions (a) to (c) in terms of adhesive properties according to JIS Z 0237:2009: (a) The adhesion to the BA-SUS test plate before light irradiation is 2.4 N / 10 mm or more and 5.5 N / 10 mm or less, (b) Regarding the ball number value in the inclined ball viscosity test at an inclination angle of 30°, a temperature of 23°C, and a relative humidity of 50% RH, when the ball number value before light irradiation is set to BN0 and the ball number value after light irradiation is set to BN1, the relationship of BN0>BN1 is established. (c) In the holding strength test after light irradiation at a temperature of 40°C, a relative humidity of 33% RH, and a standing time of 5000 minutes, the failure phenomenon when dropped means that the interface between the silicone-based adhesive layer and the BA-SUS test plate is peeled off, or the adhesive does not drop in the holding strength test.

2. The dicing adhesive tape according to claim 1, characterized in that: The semiconductor material in which the plurality of semiconductor elements are sealed with the covering material made of silicone resin is pasted from the covering material side for use.

3. An adhesive tape for cutting, characterized in that: The adhesive comprises a substrate and a silicone adhesive layer laminated on the substrate, and is used when dividing a semiconductor material having a plurality of semiconductor elements covered with a covering material into a plurality of semiconductor chips. The silicone adhesive layer is mainly composed of a mixture of an addition reaction type silicone adhesive and a peroxide curing type silicone adhesive, and contains a photosensitive platinum (Pt) catalyst and a cross-linking agent for the addition reaction type silicone adhesive. The mass ratio Gw / Rw of the total mass Gw of the organic silicone material G contained in the organic silicone adhesive layer to the total mass Rw of the organic silicone resin R is in the range of 40 / 60 to 56 / 44, and the content ratio of the organic silicone material G1 having an alkenyl group in the total mass of the organic silicone material G and the organic silicone resin R is in the range of 14 mass % or more and 42 mass % or less, The dicing adhesive tape satisfies all of the following conditions (a) to (c) in terms of adhesive properties according to JIS Z 0237:2009: (a) The adhesion to the BA-SUS test plate before light irradiation is 2.4 N / 10 mm or more and 5.5 N / 10 mm or less, (b) Regarding the ball number value in the inclined ball viscosity test at an inclination angle of 30°, a temperature of 23°C, and a relative humidity of 50% RH, when the ball number value before light irradiation is set to BN0 and the ball number value after light irradiation is set to BN1, the relationship of BN0>BN1 is established. (c) In the holding strength test after light irradiation at a temperature of 40°C, a relative humidity of 33% RH, and a standing time of 5000 minutes, the failure phenomenon when dropped means that the interface between the silicone-based adhesive layer and the BA-SUS test plate is peeled off, or the adhesive does not drop in the holding strength test.

4. The adhesive tape for dicing according to claim 3, characterized in that: The semiconductor material in which the plurality of semiconductor elements are sealed with the covering material made of silicone resin is pasted from the covering material side for use.

5. The adhesive tape for dicing according to claim 3 or 4, characterized in that: The silicone-based adhesive layer further includes an initiator composed of a peroxide.

6. A method for manufacturing a semiconductor chip, comprising the following steps: A pasting step of pasting the dicing adhesive tape according to any one of claims 1 to 5 from the side of the sealing resin to a semiconductor element substrate having a plurality of semiconductor elements sealed with a sealing resin composed of a silicone resin formed on the substrate; A cutting step of cutting the semiconductor element substrate to which the dicing tape is attached into a plurality of semiconductor chips; an irradiation step of irradiating light to the dicing adhesive tape of the semiconductor element substrate; as well as The peeling step is to peel the dicing adhesive tape from the plurality of semiconductor chips.