Nitride semiconductor device and substrate thereof, method for forming rare earth element added nitride layer, and red light emitting device and method for manufacturing same

By using the GaN layer with the rare earth element Eu as the base treatment layer on the tilted substrate, the risk of macroscopic steps and mixed crystallization is solved, and high-quality nitride semiconductor layer growth is achieved to meet the needs of high-performance semiconductor devices.

CN112640123BActive Publication Date: 2024-10-01THE RITSUMEIKAN TRUST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980055915.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-02-22
Filing Date
2019-08-30
Publication Date
2024-10-01
Estimated Expiration
2039-08-30

AI Technical Summary

Technical Problem

When using an off-angle tilted substrate to form a nitride semiconductor layer, there are macroscopic steps that cause the device characteristics to fail to meet the design requirements, and the addition of In poses the risk of mixed crystallization and lattice strain, making it difficult to achieve high-quality semiconductor devices.

Method used

By setting a GaN layer with the rare earth element Eu on the tilted substrate as a base treatment layer, the surfactant effect of Eu is used to prevent the generation of macro steps, and the added concentration and concentration of Eu are controlled by the organic metal vapor phase epitaxy method (OMVPE method). thickness, ensuring surface planarization, thereby reducing crystal defect density.

Benefits of technology

It achieves the growth of high-quality nitride semiconductor layers without the need for continuous addition, avoids the generation of macroscopic steps, and stably provides performance suitable for light-emitting, high-frequency and high-output power devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112640123B_ABST
    Figure CN112640123B_ABST
Patent Text Reader

Abstract

The present invention provides a manufacturing technology for a nitride semiconductor layer. When a nitride semiconductor layer is formed on an angle-inclined substrate to manufacture a semiconductor device, there is no risk of mixed crystal formation with GaN to cause lattice strain and crystal defects. In addition, a material that does not require continuous addition is used to prevent the occurrence of macroscopic steps, thereby stably supplying high-quality semiconductor devices. A nitride semiconductor device is a nitride semiconductor device formed by arranging a nitride semiconductor layer on a substrate, the substrate being an angle-inclined substrate, a rare earth element added nitride layer to which a rare earth element is added as a base treatment layer is provided on the substrate, and a nitride semiconductor layer is provided on the rare earth element added nitride layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nitride semiconductor device and a substrate thereof, a method for forming a rare earth element added nitride layer, and a red light emitting device and a method for manufacturing the same. Background Art

[0002] In recent years, light-emitting diodes (LEDs) and laser diodes (LDs) have been widely used. For example, LEDs are used in various display devices, backlights of liquid crystal displays, such as mobile phones, and white lighting. On the other hand, LDs are used as light sources for blue-ray discs, for recording and playing high-definition videos, optical communications, CDs, DVDs, etc.

[0003] In addition, the use of high-frequency devices such as MMIC (monolithic microwave integrated circuit) and HEMT (High Electron Mobility Transistor) for mobile phones, power transistors for inverters related to automobiles, and high-output power devices such as Schottky barrier diodes (SBD) have recently expanded.

[0004] Semiconductor elements constituting these devices are generally manufactured by forming a nitride semiconductor layer such as gallium nitride (GaN), aluminum nitride (AlN), or indium nitride (InN) on a substrate such as sapphire.

[0005] As a method for forming a nitride semiconductor layer on a substrate, a method of growing a nitride semiconductor layer on the (0001) (c-plane) of the substrate is generally used. However, in this method, piezoelectric polarization sometimes occurs due to strain generated during film formation, resulting in a problem that the device characteristics cannot be obtained as originally expected. That is, with the occurrence of piezoelectric polarization, an internal electric field is generated in the nitride semiconductor layer, and the wave functions of electrons and holes are separated, thereby reducing the probability of radiative recombination in the nitride semiconductor layer, and sometimes the expected device characteristics cannot be achieved.

[0006] Therefore, research is being conducted on the use of a substrate having a surface slightly tilted relative to the c-plane (angle-tilted substrate), using the slightly tilted surface as the film-forming surface, and growing the film in an orientation slightly tilted a few degrees from the

[0001] direction along the crystal axis, so that the nitride semiconductor layer can achieve multiple advantages such as reducing the crystal defect density and improving the luminous efficiency, thereby achieving improved device characteristics (for example, Patent Document 1).

[0007] Figure 8 is a diagram illustrating the crystal growth using the off-angle tilted substrate, Ga Figure 8As shown in the large circle on the right side of the lower section of , GaN crystals grow by adsorption along the central part of the c-plane adjacent to each other at a distance c. Figure 8 As shown in the center of the lower section, the c-plane is tilted by only an angle θ. As a result, Figure 8 As shown in the upper part of , the step height (the thickness of the Ga-N monolayer) in the off-angle tilted substrate becomes (c / 2), and the platform width (the width over which Ga atoms can diffuse) becomes (c / 2tanθ).

[0008] However, in the case of this method, it is clear that if the off-angle is increased excessively in order to achieve the goal of reducing the crystal defect density, dramatically improving the luminous efficiency, etc., the platform width will be sharply narrowed, resulting in huge macroscopic steps accompanied by a step aggregation mechanism. This will cause a new problem in the manufacture of nitride semiconductor light-emitting devices and electronic devices, in which device characteristics that meet the design cannot be obtained.

[0009] Fig. 9 is a diagram specifically showing the relationship between the deflection angle and the platform width, with the vertical axis being the platform width and the horizontal axis being the deflection angle θ. Fig. 9 It can be seen that the terrace width is inversely correlated with the size of the off-angle. Just by changing the off-angle θ from 0.15° to 1°, the terrace width is sharply narrowed from 99.0nm to 14.9nm. Moreover, if the terrace width is narrowed too much, step aggregation occurs, resulting in the formation of macroscopic steps with large step heights.

[0010] If such a macroscopic step appears, the difference in the introduction efficiency caused by the atomic species (such as Ga) near the step will produce a strong composition distribution in the crystal when making a mixed crystal (such as AlGaN), which will have a great impact on the device characteristics when making a nanostructure that requires control at a scale of several nanometers, such as a quantum well structure. In particular, in the field of light-emitting devices, strict control of the emission wavelength becomes difficult, and there are many issues in practical application.

[0011] Furthermore, even if the surface of the substrate is smoothed by grinding or etching, macroscopic steps will reappear if a nitride semiconductor layer is formed thereon, and thus device characteristics that meet the design cannot be obtained.

[0012] Therefore, it is believed that in order to produce high-quality, high-performance nitride semiconductor light-emitting devices and electronic devices according to design, crystal growth technology that maintains a flat surface without macroscopic steps is indispensable. For example, a technology of adding indium (In) to nitride has been proposed (non-patent document 1).

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: Japanese Patent Application Publication No. 2004-335635

[0016] Non-patent literature

[0017] Non-patent document 1: CK Shu et al., "Isoelectronic In-doping effect in GaN films grown by metalorganic chemical vapor deposition", Appl. Phys. Lett. 73, 641 (1998) Summary of the invention

[0018] Problem that the invention aims to solve

[0019] However, various problems are known to exist with the addition of In. For example, the addition of In has the risk of forming a mixed crystal with GaN to form InGaN, and the formation of InGaN has the risk of causing lattice strain and crystal defects, so strict flow control is required. In addition, continuous addition of In is required to remove macroscopic steps.

[0020] Therefore, the object of the present invention is to provide a manufacturing technology for a nitride semiconductor layer. When a nitride semiconductor layer is formed on an angle-tilted substrate to manufacture a semiconductor device, there is no risk of inter-crystallization with GaN to cause lattice strain and crystal defects like In. In addition, materials that do not require continuous addition are used to prevent the generation of macroscopic steps, thereby being able to stably supply high-quality semiconductor devices.

[0021] Means used to solve problems

[0022] The inventors have successfully led the world in the production of red light-emitting diodes using a GaN layer to which Eu, one of the rare earth elements, is added (Eu-added GaN layer) as a light-emitting layer, and have achieved an unattainable level of organic metal vapor phase epitaxy (OMVPE) of the Eu-added GaN layer controlled at the atomic level.

[0023] The inventors learned in this process that the surface of the Eu-added GaN layer was flattened and found that Eu had a surfactant effect. Therefore, when a nitride semiconductor thin film is formed on an angle-tilted substrate to make a semiconductor device, when a Eu-added GaN layer is provided on the angle-tilted substrate as a base treatment layer, it is believed that the surfactant effect of Eu may be exerted to prevent the occurrence of macroscopic steps during the growth of the nitride semiconductor layer, and various experiments and studies have been conducted.

[0024] The results show that even at a low Eu addition concentration of less than 1at%, the macroscopic steps on the surface of the off-angle tilted substrate are drastically reduced when the Eu-doped GaN layer is grown, and even if a GaN layer without Eu addition is grown on the Eu-doped GaN layer with a thickness exceeding 5μm, no macroscopic steps are produced, and a flat surface is formed at the atomic level, maintaining the surface flattening effect brought about by Eu addition, resulting in such academically significant results.

[0025] The mechanism that causes the phenomenon of preventing the formation of macroscopic steps by adding Eu is still under investigation, but it is speculated that the addition of In promotes the diffusion of Ga atoms and achieves smoothing, while Eu hinders the diffusion of Ga and prevents the formation of macroscopic steps, thereby exerting an excellent surfactant effect and smoothing the surface of the Eu-added GaN layer and the GaN layer without Eu added formed thereon.

[0026] Furthermore, the addition of Eu at the low addition concentration of 1 at% or less mentioned above is different from the addition of In and does not require continuous addition. In addition, Eu at the low addition concentration does not form a mixed crystal with GaN to form InGaN like In, but is added in a manner that partially replaces Ga in GaN, so there is no risk of crystal defects and no strict flow control is required.

[0027] This eliminates the need for strict flow control and continuous addition in the actual manufacture of nitride semiconductor devices, and is of great significance.

[0028] Furthermore, in the present invention, by providing a Eu-doped GaN layer as a base treatment layer, the occurrence of macroscopic steps can be prevented, thereby stably supplying nitride semiconductor devices that are suitable not only for light-emitting devices but also for high-frequency devices and high-output power devices.

[0029] Furthermore, further experiments and studies were conducted on the preferred concentration of Eu added and the preferred thickness of the Eu added GaN layer, and it was found that the preferred concentration of Eu added in the Eu added GaN layer is 0.001 to 10 at%, and the preferred thickness of the Eu added GaN layer is 0.1 nm or more. It should be noted that there is no particular upper limit for the thickness of the Eu added GaN layer, but if the saturation of the surface smoothing caused by the surfactant effect of Eu is taken into consideration, it is believed that a sufficient effect can be obtained with a thickness of about 2 μm.

[0030] It should be noted that, in the above description, GaN is cited as a nitride and Eu is cited as an additive element, but the inventors further conducted experiments and studies and found that as nitrides, even so-called GaN-based nitrides such as AlN and InN other than GaN (including mixed crystals of InGaN, AlGaN, etc.) have chemical properties that are basically the same as those of GaN, and therefore can also be used. In addition, it is known that the additive element is not limited to Eu, and if it is a rare earth element that collectively refers to Sc, Y, and lanthanide elements from La to Lu that have basically the same chemical properties, then under the same conditions as Eu, the same excellent surfactant effect can be exerted.

[0031] In addition, the results of the research on the substrate show that, as a substrate, in addition to sapphire, even if SiC or Si is used, by providing a rare earth element added nitride layer such as Eu added nitride layer, the same surfactant effect can be obtained. SiC has high thermal conductivity and excellent heat release, so it is suitable for manufacturing high-power devices. In addition, Si is cheap and can easily obtain large sizes, so it is suitable for making nitride semiconductor devices at a low price. In addition, it is also preferred to use a nitride semiconductor comprising GaN, InN, AlN, or any two or more of these mixed crystals.

[0032] The inventions described in claims 1 to 7 are inventions based on the above findings. The invention described in claim 1 is a nitride semiconductor device.

[0033] It is a nitride semiconductor device composed of a nitride semiconductor layer provided on a substrate.

[0034] The above-mentioned substrate is an angle-inclined substrate.

[0035] On the substrate, a rare earth element added nitride layer to which a rare earth element is added is provided as a base treatment layer for suppressing the generation of macro steps and flattening the surface.

[0036] A nitride semiconductor layer is provided on the rare earth element added nitride layer.

[0037] Furthermore, the invention described in claim 2 relates to the nitride semiconductor device described in claim 1, characterized in that:

[0038] The rare earth element added nitride layer is a layer in which the rare earth element is added to GaN, InN, AlN, or a mixed crystal of any two or more of these.

[0039] Furthermore, the invention described in claim 3 relates to the nitride semiconductor device described in claim 1 or claim 2, characterized in that:

[0040] The rare earth element added concentration in the rare earth element added nitride layer is 0.001 to 10 at %.

[0041] Furthermore, the invention described in claim 4 relates to the nitride semiconductor device described in any one of claims 1 to 3, characterized in that:

[0042] The rare earth element added nitride layer has a thickness of 0.1 nm or more.

[0043] In addition, the invention described in claim 5 relates to the nitride semiconductor device described in any one of claims 1 to 4, characterized in that:

[0044] The above-mentioned rare earth element is Eu.

[0045] In addition, the invention described in claim 6 relates to the nitride semiconductor device described in any one of claims 1 to 5, characterized in that:

[0046] The substrate is any one of sapphire, SiC, and Si, or a nitride semiconductor including GaN, InN, AlN, or a mixed crystal of any two or more of these.

[0047] In addition, the invention described in claim 7 relates to the nitride semiconductor device described in any one of claims 1 to 6, characterized in that:

[0048] The nitride semiconductor device is any of a light emitting device, a high frequency device, and a high output power device.

[0049] In the above, a nitride semiconductor device is manufactured by providing a rare earth element added nitride layer as a base treatment layer on an angle-inclined substrate and then providing a rare earth element added nitride semiconductor layer. However, the same effect can be obtained by manufacturing a nitride semiconductor device by prefabricating a substrate having a rare earth element added nitride layer formed on an angle-inclined substrate and providing it to a third party, and then growing a nitride semiconductor layer not added with a rare earth element on the substrate having the rare earth element added nitride layer.

[0050] That is, the invention described in claim 8 is a substrate, characterized in that:

[0051] It is a substrate used in the manufacture of nitride semiconductor devices.

[0052] A rare earth element added nitride layer to which a rare earth element is added is provided on the off-angle inclined substrate as a base treatment layer for suppressing the generation of macro steps and flattening the surface.

[0053] Furthermore, the invention described in claim 9 relates to the substrate described in claim 8, characterized in that:

[0054] The rare earth element added nitride layer is a layer in which the rare earth element is added to GaN, InN, AlN, or a mixed crystal of any two or more of these.

[0055] In addition, the invention described in claim 10 relates to the substrate described in claim 8 or claim 9, characterized in that:

[0056] The rare earth element added concentration in the rare earth element added nitride layer is 0.001 to 10 at %.

[0057] In addition, the invention described in claim 11 relates to a substrate described in any one of claims 8 to 10, characterized in that:

[0058] The rare earth element added nitride layer has a thickness of 0.1 nm or more.

[0059] In addition, the invention described in claim 12 relates to a substrate according to any one of claims 8 to 11, characterized in that:

[0060] The above-mentioned rare earth element is Eu.

[0061] In addition, the invention described in claim 13 relates to a substrate according to any one of claims 8 to 12, characterized in that:

[0062] The above-mentioned off-angle tilted substrate is any one of sapphire, SiC, and Si, or a nitride semiconductor including GaN, InN, AlN, or a mixed crystal of any two or more of these.

[0063] The above-mentioned nitride semiconductor device and the nitride layer added with rare earth elements on the substrate involved in the present invention can be manufactured in the following manner: by utilizing the organic metal vapor phase epitaxy method (OMVPE method), while changing the temperature conditions, and without taking out from the reaction container during the process, a nitride layer without rare earth element addition and a nitride layer with rare earth element addition are formed on the angle-tilted substrate in a series of steps.

[0064] Here, the reason why the rare earth element non-added nitride layer is formed before the rare earth element added nitride layer is that, like sapphire and GaN, the lattice constants in the angle-tilted substrate and the nitride layer are different, and in addition, if the propagation of crystal defects in the angle-tilted substrate is considered, it is preferable to provide the rare earth element non-added nitride layer between the angle-tilted substrate and the rare earth element added nitride layer. Specifically, it is preferable to provide two types of rare earth element non-added nitride layers, namely, a low-temperature grown rare earth element non-added LT (Low Temperature)-nitride layer and a high-temperature grown rare earth element non-added ud (Undoped)-nitride layer.

[0065] By providing the LT-nitride layer, the lattice constants of the off-angle tilted substrate and the nitride layer are matched, which can prevent the occurrence of cracks. In addition, by providing the ud-nitride layer, dislocations as crystal defects can be suppressed, and high-quality nitride crystals can be obtained.

[0066] Specifically, first, as in the past, an LT-nitride layer and an ud-nitride layer are formed on the off-angle tilted substrate as a nitride layer without rare earth element addition, and then the temperature is changed to 900-1100° C. to form a rare earth element added nitride layer on the nitride layer without rare earth element addition.

[0067] At this time, the surface of the rare earth element added nitride layer is flattened by the surfactant effect of the added rare earth element. Therefore, even if a nitride semiconductor layer is provided on the rare earth element added nitride layer as a base treatment layer to manufacture a nitride semiconductor device, no macroscopic steps will be generated, and a nitride semiconductor device with excellent device characteristics can be stably supplied.

[0068] Furthermore, for the formation of nitride layers to which rare earth elements are not added (LT-nitride layers, ud-nitride layers), nitride layers to which rare earth elements are added, and further the formation of nitride semiconductor layers, when growing each nitride layer, it can be carried out by only setting whether to change the temperature conditions and whether to add rare earth elements. Therefore, it can be carried out in a series of steps without taking out from the reaction vessel.

[0069] It should be noted that, among the above, the process may be performed until the formation of a rare earth element added nitride layer in advance, and then a nitride semiconductor layer may be formed using the nitride semiconductor layer as a substrate, thereby manufacturing a nitride semiconductor device.

[0070] The inventions described in technical solutions 14 to 17 are inventions based on the above findings. The invention described in technical solution 14 is a method for forming a rare earth element added nitride layer, characterized in that:

[0071] A method for forming a rare earth element added nitride layer by forming a rare earth element added nitride layer on an off-angle inclined substrate, comprising:

[0072] forming a nitride layer to which rare earth elements are not added on the above-mentioned off-angle tilted substrate; and

[0073] a step of forming a rare earth element added nitride layer on the rare earth element non-added nitride layer as a base treatment layer for suppressing the generation of macro steps and flattening the surface,

[0074] The above steps are carried out through a series of forming steps without taking out the reaction vessel by using an organometallic vapor phase epitaxy method, and

[0075] The formation of the rare earth element added nitride layer is performed at a temperature of 900 to 1100°C.

[0076] Furthermore, the invention described in technical solution 15 is a substrate, characterized in that:

[0077] It is formed by sequentially stacking a nitride layer without rare earth element addition and a nitride layer with rare earth element addition on an off-angle inclined substrate. The above-mentioned nitride layer with rare earth element addition serves as a base treatment layer for suppressing the generation of macro steps and flattening the surface.

[0078] In addition, the invention described in claim 16 is a method for manufacturing a nitride semiconductor device.

[0079] A nitride semiconductor layer is formed on the rare earth element added nitride layer formed by the method for forming a rare earth element added nitride layer described in Technical Solution 14 to manufacture a nitride semiconductor device.

[0080] In addition, the invention described in claim 17 is a nitride semiconductor device, characterized in that:

[0081] It is formed by sequentially stacking a nitride layer without rare earth element addition, a nitride layer with rare earth element addition, and a nitride semiconductor layer on an off-angle inclined substrate. The above-mentioned nitride layer with rare earth element addition serves as a base treatment layer to suppress the generation of macro steps and flatten the surface.

[0082] As described above, the present inventors have succeeded in leading the world in manufacturing red light-emitting diodes using Eu-doped GaN layers as active layers (light-emitting layers), but there is an increasing desire for further improvement in the light-emitting intensity thereof.

[0083] In the process of studying how to further improve the luminous intensity in such red light-emitting diodes, the inventors believed that in light-emitting devices that utilize the light emission of rare earth ions, such as red light-emitting diodes with Eu-doped GaN layers as active layers, high-concentration doping of rare earth elements directly contributes to the increase in luminous intensity. Therefore, crystal growth technology that can add rare earth elements at high concentrations is indispensable, and specific research was conducted.

[0084] The results show that in the thin film growth of nitride semiconductors, when the crystal axis is tilted several degrees from the

[0001] direction, that is, when an off-angle tilted substrate is used to carry out crystal growth of a Eu-doped GaN layer as an active layer, a strong step flow growth mechanism can be obtained, thereby enabling high-concentration doping of Eu.

[0085] Specifically, it was found that when a Eu-added GaN layer is grown on a slightly inclined surface of an off-angle tilted substrate, a powerful step flow growth mechanism is induced, which promotes step flow growth on the entire surface. Therefore, even at a Eu / Ga flow ratio (Eu / Ga ratio) exceeding 2.4%, which is considered to be the optimal growth condition for the growth of a Eu-added GaN layer on a coaxial substrate, Eu is efficiently introduced into the active layer, and the Eu-added GaN layer continues to grow while maintaining the quality (high crystallinity) of the GaN film, thereby obtaining extremely excellent luminescence intensity.

[0086] That is, in the growth of Eu-added GaN layer on the conventional coaxial substrate, as the concentration of Eu addition increases, a unique hillock structure is generated on the surface, which easily becomes a rough growth surface, resulting in a reduction in crystal quality and an obstruction to the improvement of luminous intensity. In addition, under high current injection, that is, high excitation state, the luminous intensity is saturated, resulting in the occurrence of the so-called efficiency drop phenomenon. Therefore, in the past, in the formation of Eu-added GaN layer, 2.4% was considered to be the optimal growth condition for the Eu / Ga ratio. However, in the present invention, as described above, by increasing the Eu / Ga ratio on the off-angle tilted substrate to grow the Eu-added GaN layer, the formation of the hillock structure accompanying the Eu addition is suppressed, and a Eu-added GaN layer into which Eu is introduced at a high concentration is formed, thereby obtaining extremely excellent luminous intensity.

[0087] Regarding the luminescence intensity, when O is co-added together with Eu, the fluctuation of the local structure around Eu in the active layer is greatly reduced, the luminescence spectrum (PL spectrum) is sharpened, and the luminescence intensity is further improved. Therefore, the Eu-added GaN layer is preferably set as a Eu and O co-added GaN layer.

[0088] Furthermore, such a red light-emitting device can be made using an angle-inclined substrate that has been subjected to the above-mentioned base treatment in advance, but since the base treatment layer is also a Eu-added GaN layer, it is preferred to directly form the Eu-added GaN layer on the angle-inclined substrate. That is, the Eu-added GaN layer formed initially functions as a base treatment layer of the angle-inclined substrate, and the Eu-added GaN layer formed thereon functions as an active layer. Therefore, in an environment where the base treatment is performed, the base treatment and the formation of the active layer can be performed in the form of a series of processes, and a more efficient active layer can be formed. In addition, effective utilization of Eu can be achieved, so a high material gain can be obtained.

[0089] It should be noted that such a significant improvement in luminescence intensity can be obtained even when Pr is used instead of Eu as the added rare earth element. In this case, the Pr-added GaN layer can also be directly formed on the angle-tilted substrate, but it is preferred to form the Pr-added GaN layer as the active layer on the angle-tilted substrate that has been subjected to a base treatment in advance.

[0090] The inventions described in technical solutions 18 to 22 are inventions based on the above findings. The invention described in technical solution 18 is a red light emitting device, characterized in that:

[0091] As the active layer, a rare earth element added nitride layer is formed in which Eu or Pr is added as a rare earth element to GaN, InN, AlN or a mixed crystal of any two or more of these.

[0092] The above-mentioned active layer is formed on the substrate described in any one of Technical Solutions 8 to Technical Solutions 13.

[0093] Furthermore, the invention described in technical solution 19 is a red light emitting device, characterized in that:

[0094] A rare earth element added nitride layer in which Eu as a rare earth element is added to GaN, InN, AlN or a mixed crystal of any two or more of these is formed on the off-angle tilted substrate as a base treatment layer for suppressing the generation of macro steps and flattening the surface.

[0095] In addition, the invention described in Technical Solution 20 relates to the red light-emitting device described in Technical Solution 18 or Technical Solution 19, characterized in that:

[0096] The rare earth element added nitride layer is a rare earth element added nitride layer to which oxygen is co-doped.

[0097] In addition, the invention described in technical solution 21 is a method for manufacturing a red light-emitting device, characterized in that:

[0098] The method for manufacturing the red light emitting device according to technical solution 19 is

[0099] On the off-angle tilted substrate, a rare earth element added nitride layer to which Eu is added is formed by using an organic metal vapor phase epitaxy method.

[0100] Effects of the Invention

[0101] According to the present invention, when a nitride semiconductor layer is formed on an angle-tilted substrate to manufacture a semiconductor device, there is no risk of inter-crystallization with GaN to cause lattice strain and crystal defects as in the case of In. In addition, by using materials that do not require continuous addition to prevent the occurrence of macroscopic steps, a manufacturing technology for nitride semiconductor layers that can stably supply high-quality semiconductor devices can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0102] Figure 1 It is a schematic diagram showing the structure of a nitride semiconductor device according to one embodiment of the present invention.

[0103] Figure 2 It is a diagram showing a formation process of a nitride semiconductor device in one embodiment of the present invention.

[0104] Figure 3 In one embodiment of the present invention, the diagram shows the results of in-situ observation of the self-surface reflection intensity of laser light irradiated onto a growing GaN layer, (a) is the observation result in an off-angle tilted substrate, and (b) is the observation result in a coaxial substrate.

[0105] Figure 4 The figures show the results of observing the surface of each Eu-non-added GaN layer after growth by an optical microscope (upper section) and an AFM microscope (lower section) in one embodiment of the present invention, wherein (a) is the observation result in a coaxial substrate, and (b) is the observation result in an off-angle tilted substrate.

[0106] Figure 5 The figures show the results of in-situ observation of the reflection intensity of laser light irradiated onto a growing GaN layer in one embodiment of the present invention, wherein (a) is the result of observation in an off-angle tilted substrate, and (b) is the result of observation in a coaxial substrate.

[0107] Figure 6 The figures show the results of observing the surface of the cover layer using an AFM microscope in one embodiment of the present invention, (a) is the observation result in a coaxial substrate, and (b) is the observation result in an off-angle tilted substrate.

[0108] Figure 7 The figures show the results of observing the surface of a sample having a Eu-doped GaN layer provided on an off-angle tilted substrate using (a) an optical microscope and (b) an AFM microscope in one embodiment of the present invention.

[0109] Figure 8 This is a diagram for explaining crystal growth using a substrate with an off-angle tilt.

[0110] Fig. 9 It is a graph showing the relationship between the deflection angle and the platform width.

[0111] Fig.10 It is a schematic diagram showing the structure of a red light-emitting device having a Eu-added GaN layer.

[0112] Fig.11 This is an optical microscope image of the surface of a Eu and O co-doped GaN layer formed using a coaxial substrate.

[0113] Fig.12 This is a diagram for explaining the difference in the surface state of a Eu and O co-doped GaN layer formed using an off-angle tilted substrate and a coaxial substrate.

[0114] Fig.13 The figures are results of measuring the PL spectra of red light-emitting devices having Eu-doped GaN layers formed on coaxial substrates and off-angle tilted substrates at room temperature, wherein (a) shows the relationship between the PL spectrum intensity (au) and the wavelength (nm) (when He-Cd laser, 5 mW excitation), and (b) shows the relationship between the excitation energy (mW) and the PL integrated intensity (au) at a wavelength of 610 to 650 nm. DETAILED DESCRIPTION

[0115] The present invention is described below by giving specific embodiments and using the accompanying drawings. It should be noted that, in the following, a sapphire substrate is given as an example of an off-angle tilt substrate, GaN is given as an example of a nitride, and Eu is given as an example of a rare earth element, but as mentioned above, the invention is not limited thereto.

[0116] 1. Nitride semiconductor devices

[0117] Figure 1 It is a schematic diagram showing the structure of the nitride semiconductor device involved in this embodiment. Figure 1 In the figure, 10 is a sapphire substrate, 40 is a Eu-added GaN layer (GaN:Eu), and a capping layer 50 is formed on the Eu-added GaN layer 40. It should be noted that the capping layer 50 is a Eu-unadded GaN layer (ud-GaN) that becomes a nitride semiconductor layer.

[0118] In this embodiment, the Eu-added GaN layer 40 to which Eu having an excellent surfactant effect is added is provided as the base treatment layer when forming the capping layer 50. Therefore, the capping layer 50 is grown on the Eu-added GaN layer 40 which prevents the generation of macroscopic steps, and even if the thickness exceeds 5 μn, it can be grown while forming a flat surface at the atomic level. In addition, the effect of crystal growth brought about by using the off-angle tilted substrate, which was originally expected, can be fully exerted, and the device characteristics can be improved.

[0119] As described above, in the present embodiment, the surface flattening effect on the Eu-added nitride layer provided as a base treatment layer is also maintained in the covering layer (nitride semiconductor layer) formed on the upper layer, thereby enabling a stable supply of nitride semiconductor devices that are suitable not only as light-emitting devices but also as high-frequency devices and high-output power devices.

[0120] It should be noted that, in this embodiment, Figure 1 As shown, between the sapphire substrate 10 and the Eu-added GaN layer 40, there are two Eu-unadded GaN layers, namely, the LT-GaN layer 20 grown at a low temperature of about 475°C and the Eu-unadded GaN layer (ud-GaN) 30 grown at a high temperature of about 1180°C. As described above, by providing the LT-GaN layer 20, the lattice constants of the sapphire crystal and the GaN crystal can be matched to prevent the occurrence of cracks. In addition, by providing the ud-GaN layer 30, the influence caused by dislocations as crystal defects can be suppressed, and the occurrence of defects in the Eu-added GaN layer can be controlled.

[0121] 2. Method for forming a nitride semiconductor device

[0122] Next, a method for forming the above-mentioned nitride semiconductor device will be described. Figure 2 is a diagram showing the formation process of the nitride semiconductor device in this embodiment. It should be noted that, Figure 2 In FIG. 1 , the upper section shows the gas supplied as a raw material and the supply rate, and the lower section shows the relationship between the growth temperature (vertical axis) and time (horizontal axis).

[0123] In this embodiment, the OMVPE method is used to form the nitride semiconductor device. In addition, trimethylgallium (TMGa) is used as the Ga raw material, and ammonia (NH3) is used as the N raw material. In addition, n-propyltetramethylcyclopentadienyleuropium (Eu[C5(CH3)4(C3H7)]2:EuCp pm 2).

[0124] And, if Figure 1 As shown, on the sapphire substrate 10, according to Figure 2The process shown in the figure sequentially forms the LT-GaN layer 20, the ud-GaN layer 30, the Eu-doped GaN layer 40, and the cap layer 50. Figure 1 and Figure 2 , give specific instructions.

[0125] (1) Formation of LT-GaN layer 20

[0126] First, a sapphire substrate 10 tilted at an angle of 1° is placed in a reaction vessel adjusted to a pressure of 104 kPa. Then, the temperature in the reaction vessel is set to 475°C, and NH3 gas (223 mmol / min) and TMGa gas (52.1 μmol / min) are supplied into the reaction vessel to form a LT-GaN layer 20 with a thickness of 30 nm on the sapphire substrate 10 at a growth rate of 1.3 μm / h.

[0127] (2) Formation of ud-GaN layer 30

[0128] Next, the temperature in the reaction container was set to 1180°C, and NH3 gas (179 mmol / min) and TMGa gas (102 μmol / min) were supplied into the reaction container to form a ud-GaN layer 30 with a thickness of 2 μm on the LT-GaN layer 20 at a growth rate of 3.2 μm / h.

[0129] (3) Formation of Eu-doped GaN Layer 40

[0130] Next, the temperature in the reaction container was set to 960°C, and NH3 gas (179 mmol / min), TMGa gas (25.6 μmol / min), and EuCp were supplied into the reaction container. pm 2 gas (0.586 μmol / min) was used to form a Eu-added GaN layer 40 having a thickness of 40 nm on the ud-GaN layer 30 at a growth rate of 0.78 μm / h.

[0131] (4) Formation of Covering Layer 50

[0132] Next, the temperature in the reaction container was set to 1180°C again, and NH3 gas (179 mmol / min) and TMGa gas (102 μmol / min) were supplied into the reaction container to form a 5 μm thick covering layer 50 on the Eu-added GaN layer 40 at a growth rate of 3.2 μm / h as a nitride semiconductor device.

[0133] It should be noted that among the above, EuCp with high vapor pressure is used as the raw material of Eu. pm 2. You can also use Eu(C 11 H 19O2)3, Eu[C5(CH3)5]2, Eu[C5(CH3)4H]2, etc.

[0134] 3. Evaluation

[0135] (1) Confirmation of the occurrence of macroscopic steps in the off-angle tilted substrate

[0136] As an evaluation sample, a Eu-free GaN layer with a thickness of 7.6 μm was grown on a sapphire substrate tilted at an off-angle of 1° (off-angle tilted substrate) using the OMVPE method. On the other hand, for comparison, a Eu-free GaN layer with a thickness of 7.6 μm was grown on a non-tilted sapphire substrate (coaxial substrate).

[0137] Furthermore, each growing GaN layer was irradiated with a laser beam having a wavelength of 633 nm, and the reflection intensity from the surface was observed in situ. The results are shown in Figure 3 It should be noted that Figure 3 In the figure, (a) is the observation result in the off-angle tilted substrate, (b) is the observation result in the coaxial substrate, the vertical axis on the left is the reflection intensity (arbitrary unit), the vertical axis on the right is the crystal growth temperature (°C), and the horizontal axis is the crystal growth time (min).

[0138] In the case of coaxial substrates, such as Figure 3 As shown in (b), the overall reflection intensity is high and remains at a certain level even if the crystal growth time becomes longer. Figure 3 As shown in (a), it can be seen that the overall reflection intensity decreases, and as the crystal growth time becomes longer, the reflection intensity further decreases. This is believed to be because the nitride layer is formed on the angle-inclined substrate, so the flatness on the surface of the nitride layer is low, and as the film thickness increases, the flatness further decreases.

[0139] Furthermore, the surface of each Eu-free GaN layer after growth was observed by optical microscopy and AFM microscopy (atomic force microscopy) to evaluate its surface state. Figure 4 It should be noted that Figure 4 In the figure, the upper part shows the observation results based on an optical microscope, and the lower part shows the observation results based on an AFM microscope. The left side shows the observation results in (a) a coaxial substrate, and the right side shows (b) an off-angle tilted substrate.

[0140] like Figure 4 As shown, in the case of the coaxial substrate, no macroscopic steps were observed and the surface was flat. In contrast, in the case of the off-angle tilted substrate, huge macroscopic steps were observed due to step aggregation, a wavy structure was generated on the surface, and the flatness was impaired.

[0141] (2) Evaluation of Flatness on Eu-free GaN Layer

[0142] Next, as evaluation samples, a 30nm thick LT-GaN layer, a 2μm thick ud-GaN layer, a 40nm thick Eu-doped GaN layer, and a 5μm thick cap layer (ud-GaN layer) were grown on the same substrates (off-angle tilted substrate and coaxial substrate) as above. On the other hand, for comparison, ud-GaN layers were grown on each substrate until the total thickness became the same.

[0143] Furthermore, similarly to the above, the reflection intensity of each layer during growth was observed in situ, and the surface of each GaN layer at the top after growth was observed with an AFM microscope and an optical microscope to evaluate the surface state.

[0144] Figure 5 The observation results of reflection intensity are shown in FIG. Figure 5 In the figure, the upper part shows the observation results in (a) an off-angle tilted substrate, the lower part shows the observation results in (b) a coaxial substrate, the left side shows the observation results in all steps, and the right side shows the observation results in the growth of the cap layer. In addition, the solid line shows the observation results in the sample with Eu-doped GaN layer, and the dotted line shows the observation results in the sample with only ud-GaN layer.

[0145] In the case of coaxial substrates, such as Figure 5 As shown in (b), the reflection intensity of the sample with Eu-doped GaN layer does not change much from the reflection intensity of the sample with only ud-GaN layer, and remains at a certain level even if the crystal growth time is prolonged. Figure 5 As shown in (a), by providing the Eu-doped GaN layer, the reflection intensity is greatly improved compared to the sample with only the ud-GaN layer. This result shows that when forming the cap layer, the growth of the Eu-doped GaN layer has a great influence on the improvement of the flatness.

[0146] Figure 6 , the results of observing the surface of the cover layer by AFM microscope are shown. It should be noted that, here, the observation results of the sample with Eu-doped GaN layer are shown, (a) is the observation result of the coaxial substrate, and (b) is the observation result of the off-angle tilted substrate.

[0147] Depend on Figure 6 It is understood that by providing the Eu-doped GaN layer on the off-angle tilted substrate, the surface state is comparable to that of the coaxial substrate.

[0148] Figure 7 , the results of observing the surface of a sample having a Eu-added GaN layer provided on an off-angle tilted substrate using (a) an optical microscope and (b) an AFM microscope are shown.

[0149] Depend on Figure 7 It can be seen that by providing the Eu-doped GaN layer, the surface of the cap layer is smoothed, and its surface roughness RMS becomes very small at 0.15nm. This result shows that the addition of Eu prevents the occurrence of macroscopic steps and forms a GaN layer with a flat surface at the atomic level, showing the excellent surfactant effect of Eu.

[0150] It should be noted that, in the above, an example of growing a Eu-added GaN layer on an off-angle tilted substrate and providing a covering layer thereon is given to illustrate its surfactant effect. The Eu-added GaN layer and the ud-GaN layer can also be stacked multiple times in pairs, thereby achieving further smoothing of the surface state.

[0151] 4. Application to semiconductor devices

[0152] As described above, in this embodiment, by providing a Eu-doped GaN layer on an angle-tilted substrate, a substrate with low defect density can be provided. Therefore, compared with the past, blue and green LEDs with high luminous efficiency can be realized by leaps and bounds. In addition, since a low dislocation density is achieved on an angle-tilted substrate, a device with less leakage current can be realized, and a highly reliable nitride power device can be manufactured.

[0153] 5. Red light emitting device

[0154] Next, the red light-emitting device according to this embodiment will be described in detail.

[0155] (1) Problems with the prior art

[0156] First, problems in the growth of a conventional Eu-added GaN layer on a coaxial substrate will be described. Specifically, why the optimum growth condition for the Eu-added GaN layer is considered to be a Eu / Ga ratio of 2.4% will be described.

[0157] First, as evaluation samples, red light-emitting devices were fabricated in which a Eu and O co-doped GaN layer was formed on a coaxial substrate with the Eu / Ga ratio changed to 2.4%, 3.5%, and 7.1%.

[0158] Specifically, initially, a non-additive GaN layer (LT-GaN layer and ud-GaN layer) with a thickness of about several μm is grown on a coaxial sapphire substrate, and then TMGa is introduced as a Ga raw material, NH3 is introduced as a N raw material, and EuCp bubbled with a carrier gas (supplied together with oxygen) is introduced as a Eu raw material at a predetermined Eu / Ga ratio. pm2. A 300nm thick Eu and O co-doped GaN layer is grown. Finally, a 10nm thick ud-GaN layer is grown to complete the production of three red light-emitting devices (refer to Fig.10 ).

[0159] Fig.11 Figure 1 is an optical microscope image of the surface of the Eu and O co-doped GaN layer formed in the three evaluation samples obtained. Fig.11 It is found that in the case of the coaxial sapphire substrate, as the Eu / Ga ratio increases to 2.4%, 3.5%, and 7.1%, the surface flatness is lost, and in particular, when the ratio changes from 3.5% to 7.1%, the crystal growth surface is rapidly deteriorated.

[0160] And, in Fig.12 The upper part, Fig.11 The surface state of the Eu and O co-doped GaN layer obtained in the two cases of Eu / Ga ratio of 3.5% and 7.1% is shown by increasing the magnification of the optical microscope. Fig.12 It is found that when a Eu and O co-doped GaN layer is formed on a coaxial substrate, the active layer grows spirally, so that as the Eu / Ga ratio increases, a large number of spiral hillocks are formed, causing surface roughness.

[0161] in addition, Fig.13 The results of measuring the PL spectrum of the Eu-doped GaN layer formed on the coaxial substrate at room temperature are shown in FIG. Fig.13 In the figure, (a) shows the relationship between PL spectrum intensity (au) and wavelength (nm) (when He-Cd laser, 5 mW excitation), and (b) shows the relationship between excitation energy (mW) and PL integrated intensity (au) at wavelengths of 610 to 650 nm.

[0162] Depend on Fig.13 (a) It can be seen that in the case of a coaxial substrate, as the Eu / Ga ratio increases, the 5 D0→ 7 The luminescence peak of F2 rises. However, on the other hand, Fig.13 As shown in (b), under strong excitation, even if the Eu / Ga ratio is increased, the saturation phenomenon of luminescence is enhanced, and when the Eu / Ga ratio is 7.1%, the luminescence intensity is slightly reduced compared with the case of 3.5%.

[0163] Therefore, considering the surface state of the Eu-added GaN layer, the best growth condition for growing a Eu-added GaN layer on a coaxial substrate has been a Eu / Ga ratio of 2.4%, and further increasing the Eu / Ga ratio is considered to be problematic.

[0164] (2) Eu-doped GaN layer formed on an off-angle tilted substrate

[0165] Next, as this embodiment, the surface state and light emission intensity in the case where a Eu-doped GaN layer is formed on an off-angle tilted substrate will be described.

[0166] The present inventors focused on the fact that a strong step flow growth mechanism can be obtained when crystal growth is carried out along the crystal axis slightly tilted by several degrees from the

[0001] direction in the thin film growth of a nitride semiconductor as described above, and formed a Eu-doped GaN layer on an off-angle tilted substrate.

[0167] Specifically, two types of red light-emitting devices with Eu / Ga ratios of 3.5% and 7.1% were fabricated on a slightly tilted (0001) sapphire substrate having an off-angle of 2° along the m-axis direction, similarly to the above-mentioned coaxial substrate.

[0168] exist Fig.12 The lower part of the figure shows the surface state of the obtained Eu and O co-doped GaN layer. Fig.12 It can be seen that in the case of an off-angle tilted substrate, the growth of the active layer is performed by step flow growth rather than spiral growth, thereby suppressing the formation of spiral hillocks. Even if the Eu / Ga ratio becomes higher, the active layer grows while maintaining high crystallinity.

[0169] in addition, Fig.13 The PL spectrum measurement results of the Eu-doped GaN layer formed on the off-angle tilted substrate with a Eu / Ga ratio of 3.5% are also shown. Fig.13 (a) It can be seen that in the case of the off-angle tilted substrate, even if the Eu / Ga ratio is set to 3.5%, a strong luminescence intensity that cannot be obtained with the coaxial substrate is obtained. Fig.13 (b) It can be seen that the saturation phenomenon of light emission is suppressed, and the light emission intensity is improved by 2.04 times compared with the conventional coaxial substrate (Eu / Ga ratio 2.4%).

[0170] It was confirmed that such an improvement in luminescence intensity is due to the fact that, even with the same Eu / Ga ratio, the incorporation of Eu into the active layer is improved, and the Eu concentration in the Eu-added GaN layer becomes higher. Therefore, by forming a Eu-added GaN layer on an off-angle tilted substrate, a Eu-added GaN layer with a high Eu concentration can be formed, which is expected to be a method for achieving an improvement in luminescence intensity.

[0171] (3) Practicality of the red light-emitting device according to this embodiment

[0172] As described above, in the red light-emitting device involved in this embodiment, a Eu-doped GaN layer with a high Eu concentration can be formed on an angle-inclined substrate, which can directly contribute to the realization of a strong luminous intensity, so that a high-efficiency red light-emitting device can be produced, and by applying it to a semiconductor LED in the visible light region developed with GaN-based materials as the center, a high-brightness light-emitting diode can be realized. In addition, in the development of laser diodes with a rare earth-doped semiconductor layer including a red light-emitting layer as an active layer, which has attracted much attention in recent years, high material gain can be achieved by adding a high concentration of rare earth elements such as Eu.

[0173] As mentioned above, although this invention is demonstrated based on embodiment, this invention is not limited to said embodiment. Various changes can be added to said embodiment within the range which is the same as this invention and is equivalent.

[0174] Description of Reference Numerals

[0175] 10 Sapphire substrate

[0176] 20 LT-GaN layer

[0177] 30 ud-GaN layer

[0178] 40 Eu added GaN layer

[0179] 50 Overlay

[0180] Distance between cc surfaces

[0181] θ deflection angle

Claims

1. A nitride semiconductor device, characterized in that: A nitride semiconductor device is formed by providing a nitride semiconductor layer on a substrate. The substrate is an off-angle inclined substrate, wherein the off-angle inclined substrate is a substrate having a surface slightly inclined relative to the c-plane, On the substrate, a rare earth element added nitride layer is provided as a base treatment layer for suppressing the generation of macro steps and flattening the surface, wherein the rare earth element is Eu or Pr. A nitride semiconductor layer is provided on the rare earth element added nitride layer. The rare earth element added nitride layer is a layer in which the rare earth element is added to GaN, InN, AlN, or a mixed crystal of any two or more of these.

2. The nitride semiconductor device according to claim 1, wherein: The rare earth element added concentration in the rare earth element added nitride layer is 0.001 at % to 10 at %.

3. The nitride semiconductor device according to claim 1, wherein: The rare earth element added nitride layer has a thickness of 0.1 nm or more.

4. The nitride semiconductor device according to claim 1, wherein: The rare earth element is Eu.

5. The nitride semiconductor device according to claim 1, wherein: The substrate is any one of sapphire, SiC, and Si, or a nitride semiconductor including GaN, InN, AlN, or a mixed crystal of any two or more of these.

6. The nitride semiconductor device according to claim 1, wherein: The nitride semiconductor device is any one of a light emitting device, a high frequency device, and a high output power device.

7. A substrate used in manufacturing a nitride semiconductor device, characterized in that: A rare earth element added nitride layer to which a rare earth element is added is provided on an angle-inclined substrate as a base treatment layer to suppress the generation of macro steps and flatten the surface, wherein the angle-inclined substrate is a substrate having a surface slightly inclined relative to a c-plane, and the rare earth element is Eu or Pr, The rare earth element added nitride layer is a layer in which the rare earth element is added to GaN, InN, AlN, or a mixed crystal of any two or more of these.

8. The substrate according to claim 7, characterized in that The rare earth element added concentration in the rare earth element added nitride layer is 0.001 at % to 10 at %.

9. The substrate according to claim 7, characterized in that The rare earth element added nitride layer has a thickness of 0.1 nm or more.

10. The substrate according to claim 7, characterized in that The rare earth element is Eu.

11. The substrate according to claim 7, characterized in that The off-angle tilted substrate is any one of sapphire, SiC, and Si, or a nitride semiconductor including GaN, InN, AlN, or a mixed crystal of any two or more of these.

12. A method for forming a rare earth element added nitride layer, characterized in that: The invention relates to a method for forming a rare earth element added nitride layer on an off-angle tilted substrate, wherein the off-angle tilted substrate is a substrate having a surface slightly tilted relative to a c-plane, the rare earth element is Eu or Pr, and the rare earth element added nitride layer is a layer in which the rare earth element is added to GaN, InN, AlN, or a mixed crystal of any two or more of these. The method has: forming a nitride layer without rare earth element addition on the off-angle tilted substrate; and forming a rare earth element added nitride layer on the rare earth element non-added nitride layer as a base treatment layer for suppressing the generation of macro steps and flattening the surface, The above steps are carried out through a series of forming steps by an organometallic vapor phase epitaxy method without taking out the reaction vessel. The rare earth element added nitride layer is formed at a temperature of 900°C to 1100°C.

13. A substrate used in manufacturing a nitride semiconductor device, characterized in that: It is formed by sequentially stacking a nitride layer without rare earth element addition and a nitride layer with rare earth element addition on an off-angle tilted substrate, wherein the nitride layer with rare earth element addition serves as a base treatment layer for suppressing the generation of macro steps and flattening the surface, the off-angle tilted substrate is a substrate having a surface slightly tilted relative to the c-plane, the rare earth element is Eu or Pr, and the nitride layer with rare earth element addition is a layer in which the rare earth element is added to a mixed crystal of GaN, InN, AlN, or any two or more of these.

14. A method for manufacturing a nitride semiconductor device, A nitride semiconductor layer is formed on the rare earth element added nitride layer formed by the method for forming a rare earth element added nitride layer according to claim 12, thereby manufacturing a nitride semiconductor device.

15. A nitride semiconductor device, characterized in that: It is formed by sequentially stacking a nitride layer without rare earth element addition, a nitride layer with rare earth element addition, and a nitride semiconductor layer on an off-angle tilted substrate, wherein the rare earth element added nitride layer serves as a base treatment layer for suppressing the generation of macro steps and flattening the surface, the off-angle tilted substrate is a substrate having a surface slightly tilted relative to the c-plane, the rare earth element is Eu or Pr, and the rare earth element added nitride layer is a layer in which the rare earth element is added to a mixed crystal of GaN, InN, AlN, or any two or more of these.

16. A red light emitting device, characterized in that: As an active layer, a rare earth element added nitride layer is formed in which Eu or Pr as a rare earth element is added to GaN, InN, AlN or a mixed crystal of any two or more of these. The active layer is formed on the substrate according to any one of claims 7 to 11.

17. A red light emitting device, characterized in that: A rare earth element added nitride layer is formed on the angle-tilted substrate, in which Eu is added as a rare earth element to GaN, InN, AlN or a mixed crystal of any two or more of these, as a base treatment layer to suppress the formation of macro steps and flatten the surface. The angle-tilted substrate is a substrate having a surface slightly inclined relative to the c-plane.

18. The red light emitting device according to claim 16 or claim 17, characterized in that: The rare earth element added nitride layer is a rare earth element added nitride layer to which oxygen is co-added.

19. A method for manufacturing a red light emitting device, characterized in that: The method for manufacturing a red light emitting device according to claim 17, On the off-angle tilted substrate, a rare earth element added nitride layer to which Eu is added is formed by using an organic metal vapor phase epitaxy method.