Semiconductor structure and method for forming the same
By introducing a stacked structure of a diffusion barrier layer and an inversion layer into the semiconductor structure, the doped ions in the drain region are prevented from diffusing into the channel region, the problem of the short channel effect caused by the diffusion of doped ions is solved, and the electrical properties of the semiconductor structure are improved. performance.
Patent Information
- Application Number
- CN201911150860.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-11-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-11-21
AI Technical Summary
When the existing semiconductor structure is in operation, doped ions in the drain region easily diffuse into the channel region below the gate structure, causing the depletion layer in the drain region to expand, causing serious short channel effects and affecting electrical performance.
A diffusion barrier layer is introduced into the semiconductor structure and is located in the drift region between the drain region and the gate structure to block the diffusion of doped ions to the channel region. By forming adjacent well regions, drift regions, gate structures, The specific layout of the source and drain regions uses a stacked structure of diffusion barrier layers and inversion layers to control the migration of doped ions.
It effectively prevents the diffusion of doped ions, prevents the expansion of the depletion layer in the drain region, improves the short channel effect, and improves the electrical performance of the semiconductor structure.
Smart Images

Figure CN112825327B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] In the development of power integrated circuits, the single-chip process developed to integrate power switches and control circuits, especially the lateral double diffusion MOS (LDMOS) process currently used to make monolithic integrated circuits, is a mainstream trend. The LDMOS process is a planar diffusion on the surface of the semiconductor substrate to form a lateral main current path. Since LDMOS is manufactured using a typical IC process, the control circuit and LDMOS can be integrated on a monolithic power IC. The LDMOS process uses reduced surface electric field (RESURE) technology and low thickness epitaxy (BPI) or N-well to achieve the goals of high voltage and low on-resistance.
[0003] The LDMOS device is a field effect transistor device (FET) similar to a conventional field effect transistor (FET) device, both of which include forming a pair of source / drain regions separated by a channel region in a semiconductor substrate, and forming a gate electrode in turn above the channel region. However, the LDMOS device is different from the conventional FET device in that the pair of source / drain regions in the conventional FET device are made symmetrical with the gate electrode, while the drain region in the LDMOS device is farther away from the gate electrode than the source region, and the drain region is simultaneously formed in a doped well (having the same polarity as the drain region) used to separate the channel region and the drain region. Summary of the invention
[0004] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, so as to optimize the electrical performance of the semiconductor structure.
[0005] To solve the above problems, an embodiment of the present invention provides a semiconductor structure, including: a substrate, wherein the substrate has an adjacent well region and a drift region; a gate structure located on the substrate at the junction of the well region and the drift region; a source region located in the well region on one side of the gate structure; a drain region located in the drift region on the other side of the gate structure; and a diffusion barrier layer located in the drift region between the drain region and the gate structure, wherein the diffusion barrier layer is used to prevent doped ions in the drain region from diffusing into the channel region below the gate structure.
[0006] Correspondingly, an embodiment of the present invention also provides a method for forming a semiconductor structure, comprising: providing a substrate, wherein an adjacent well region and a drift region are formed in the substrate; forming a groove in the drift region; forming a diffusion barrier layer in the groove; after forming the diffusion barrier layer, forming a gate structure on the substrate at the junction of the well region and the drift region, the gate structure is located on a side of the diffusion barrier layer close to the well region; forming a source region in the well region on one side of the gate structure, and forming a drain region in the drift region on the other side of the gate structure, the drain region being located on a side of the diffusion barrier layer in the drift region away from the well region.
[0007] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0008] In the semiconductor structure of the embodiment of the present invention, a substrate has adjacent well regions and drift regions, a gate structure is located on the substrate at the junction of the well region and the drift region, a source region is located in the well region on one side of the gate structure, a drain region is located in the drift region on the other side of the gate structure, a diffusion barrier layer is located in the drift region between the drain region and the gate structure, and the diffusion barrier layer is used to block the doped ions in the drain region from diffusing into the channel region below the gate structure; when the semiconductor structure is working, under the action of the diffusion barrier layer, the doped ions in the drain region are not easily diffused into the channel region below the gate structure, which makes it difficult for the depletion layer of the drain region to expand, which is beneficial to improving the short channel effect, thereby improving the electrical performance of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 It is a schematic diagram of the structure of a semiconductor structure;
[0010] Figures 2 to 10 is a schematic structural diagram corresponding to each step in the first embodiment of the method for forming a semiconductor structure of the present invention;
[0011] Fig.11 and Fig.12 It is a schematic structural diagram corresponding to each step in the second embodiment of the method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION
[0012] As can be seen from the background art, the semiconductor structures currently formed still have the problem of poor electrical performance. The reasons for the poor performance of the semiconductor structure are now analyzed in conjunction with a method for forming a semiconductor structure.
[0013] refer to Figure 1 , showing a schematic structural diagram of a semiconductor structure.
[0014] The semiconductor structure shows a design of an LDMOS, and the semiconductor structure includes: a substrate (not shown in the figure) and a fin 10 located on the substrate, wherein the fin 10 has an adjacent well region 11 and a drift region 12; a gate structure 20, spanning the fin 10 at the junction of the well region 11 and the drift region 12, and covering part of the top wall and part of the side wall of the fin 10; a source region 31, located in the well region 11 on one side of the gate structure 20; and a drain region 32, located in the drift region 12 on the other side of the gate structure 20 and isolated from the gate structure 20.
[0015] Taking an N-type lateral double diffused metal oxide semiconductor field effect transistor (NLDMOS) as an example, when the device is working, carriers flow out from the drain region 32, pass through the drift region 12 between the drain region 32 and the gate structure 20, and flow to the channel below the gate structure 20. Usually, the drain region 32 has N-type ions (such as phosphorus ions, arsenic ions or antimony ions) for improving the migration rate of carriers, but the doped ions in the drain region 32 are easy to diffuse into the channel region below the gate structure 20. When the semiconductor structure is working, the depletion layer of the drain region 32 is easy to expand, so that the short channel effect is serious, resulting in poor electrical performance of the semiconductor structure.
[0016] In order to solve the technical problem, an embodiment of the present invention provides a semiconductor structure, including: a substrate, having adjacent well regions and drift regions therein; a gate structure located on the substrate at the junction of the well regions and the drift regions; a source region located in the well region on one side of the gate structure; a drain region located in the drift region on the other side of the gate structure; and a diffusion barrier layer located in the drift region between the drain region and the gate structure, the diffusion barrier layer being used to block doped ions in the drain region from diffusing into the channel region below the gate structure.
[0017] In the semiconductor structure of the embodiment of the present invention, a substrate has adjacent well regions and drift regions, a gate structure is located on the substrate at the junction of the well region and the drift region, a source region is located in the well region on one side of the gate structure, a drain region is located in the drift region on the other side of the gate structure, a diffusion barrier layer is located in the drift region between the drain region and the gate structure, and the diffusion barrier layer is used to block the doped ions in the drain region from diffusing into the channel region below the gate structure; when the semiconductor structure is working, under the action of the diffusion barrier layer, the doped ions in the drain region are not easily diffused into the channel region below the gate structure, which makes it difficult for the depletion layer of the drain region to expand, which is beneficial to improving the short channel effect, thereby improving the electrical performance of the semiconductor structure.
[0018] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and easy to understand, specific embodiments of the embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0019] Figures 2 to 10 , is a schematic structural diagram corresponding to each step in the first embodiment of the method for forming a semiconductor structure according to an embodiment of the present invention. The method for forming a semiconductor structure provided by an embodiment of the present invention will be described in detail below in conjunction with the accompanying drawings.
[0020] refer to Figures 2 to 4 , Figure 3 for Figure 2 The cross-section in the AA direction, Figure 4 is based on Figure 2 A cross-sectional view of a substrate is provided, in which adjacent well regions 101 (such as Figure 3 ) and the drift region 102 (as shown Figure 3 shown).
[0021] The substrate is used to provide a process platform for the subsequent formation of LDMOS.
[0022] In this embodiment, the base includes a substrate 100 and a fin 109 located on the substrate 100 .
[0023] In this embodiment, the semiconductor structure is an LDMOS fin field effect transistor as an example, and the substrate includes a substrate 100 and a fin 109 separated on the substrate 100. In other embodiments, the LDMOS may also be a planar transistor, and the corresponding substrate is a planar substrate.
[0024] In this embodiment, the substrate 100 is a silicon substrate. In other embodiments, the substrate may also be a substrate of other materials such as a germanium substrate, a silicon germanium substrate, a silicon carbide substrate, a gallium arsenide substrate, or an indium gallium substrate, and the substrate may also be a silicon on insulator substrate or a germanium on insulator substrate.
[0025] In this embodiment, the fin 109 is an integral structure with the substrate 100. In other embodiments, the fin may also be a semiconductor layer epitaxially grown on the substrate, so as to achieve the purpose of accurately controlling the initial fin height.
[0026] Therefore, the material of the fin 109 is the same as that of the substrate 100, and the material of the fin 109 is silicon. In other embodiments, the material of the fin may also be a semiconductor material such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the material of the fin may also be different from that of the substrate.
[0027] The drift region 102 contains first-type ions, and the well region 101 contains second-type ions. The first-type ions and the second-type ions have different conductivity types.
[0028] Specifically, the well region 101 and the drift region 102 are formed in the fin 109 and are in contact with each other. The well region 101 serves as a lateral diffusion region to form a channel with a concentration gradient, and the drift region 102 is used to withstand a large partial pressure.
[0029] Specifically, in this embodiment, when the semiconductor structure is used to form NLDMOS, the first type of ions are N-type ions, which include one or more of phosphorus ions, arsenic ions, and antimony ions; the second type of ions are P-type ions, which include one or more of boron ions, gallium ions, and indium ions.
[0030] When the semiconductor structure is used to form PLDMOS, the first type of ions are P type ions, which include one or more of boron ions, gallium ions and indium ions, and the second type of ions are N type ions, which include one or more of phosphorus ions, arsenic ions and antimony ions.
[0031] Specifically, the steps of forming the well region 101 and the drift region 102 include: forming an isolation material layer 112 covering the side walls of the substrate 100 and the fin 109; using a planarization process to remove the isolation material layer 112 above the top of the fin 109; after removing the isolation material layer 112 above the top of the fin 109, forming a first injection mask layer (not shown in the figure), the first injection mask layer exposes the fin 109 to be formed with the drift region 102; doping the fin 109 exposed by the first injection mask layer with first-type ions to form the drift region 102; after forming the drift region 102, forming a second injection mask layer 113 covering the drift region 102 and exposing a partial area of the fin 109, the second injection mask layer 113 exposes the fin 109 to be formed with the well region; doping the fin 109 exposed by the second injection mask layer 113 with second-type ions to form the well region 101.
[0032] In this embodiment, the drift region 102 is formed first, and then the well region 101 is formed. In other embodiments, the well region may be formed first, and then the drift region may be formed.
[0033] In the embodiment of the present invention, the fin portion 109 exposed by the first implantation mask layer is doped with the first type ions by ion implantation to form the drift region 102. Ion implantation has the characteristics of simple operation and low process cost.
[0034] In the embodiment of the present invention, the fin portion 109 exposed by the second implantation mask layer 113 is doped with the second type ions by ion implantation to form the well region 101. Ion implantation has the characteristics of simple operation and low process cost.
[0035] In this embodiment, the first implantation mask layer and the second implantation mask layer 113 are used as implantation masks for forming the well region 101 and the drift region 102 respectively.
[0036] The first injection mask layer and the second injection mask layer 113 are made of materials that can function as masks and are easy to remove, so that damage to other film structures is reduced when the first injection mask layer and the second injection mask layer 113 are removed.
[0037] In this embodiment, the materials of the first injection mask layer and the second injection mask layer 113 are organic materials, such as: BARC (bottom anti-reflective coating) material, ODL (organic dielectric layer) material, spin on carbon (SOC), photoresist, DARC (dielectric anti-reflective coating) material, DUO (Deep UV Light Absorbing Oxide) material or APF (Advanced Patterning Film) material.
[0038] The method for forming a semiconductor structure includes: after forming the well region 101 , removing the second implantation mask layer 113 .
[0039] In the embodiment of the present invention, the isolation material layer 112 covers the sidewalls of the fin 109 and the substrate 100. Therefore, in the process of forming the well region 101 and the drift region 102 by ion implantation, the isolation material layer 112 protects the substrate 100 and the fin 109 from damage.
[0040] like Figure 4 As shown, the method for forming the semiconductor structure further includes: after forming the drift region 102 and the well region 101 , etching back a portion of the thickness of the isolation material layer 112 to form an isolation layer 111 .
[0041] The isolation layer 111 is used to isolate adjacent fins 109 .
[0042] In this embodiment, the material of the isolation layer 111 is silicon oxide. Silicon oxide is a commonly used dielectric material with low cost and high process compatibility, which is conducive to reducing the process difficulty and process cost of forming the isolation layer 111. In addition, the dielectric constant of silicon oxide is small, which is also conducive to improving the subsequent isolation of adjacent devices.
[0043] refer to Figure 5 , a trench 114 is formed in the drift region 102 .
[0044] The trench 114 provides space for the subsequent formation of a diffusion barrier layer.
[0045] In this embodiment, the drift region 102 is etched by a dry etching process to form a groove 114 in the drift region 102. The dry etching process has anisotropic etching characteristics and good etching profile control, which is conducive to making the morphology of the groove 114 meet the process requirements. In addition, the dry etching process is conducive to accurately controlling the depth of the groove 114.
[0046] It should be noted that, in the process of forming the trench 114 in the drift region 102 , the trench 114 is also formed in the well region 101 .
[0047] In this embodiment, the step of forming the groove 114 includes: forming a mask layer 115 on the substrate, the mask layer 115 having an opening 116, the opening 116 exposing the area where the groove is to be formed; etching the drift region 102 and the well region 101 using the mask layer 115 as a mask, and forming the groove 114 in both the drift region 102 and the well region 101.
[0048] Specifically, the mask layer 115 is formed on the drift region 102 and the well region 101 .
[0049] The mask layer 115 is a material that can function as a mask and is easy to remove, so that damage to other film structures is reduced when the mask layer 115 is subsequently removed.
[0050] In the present embodiment, the material of the mask layer 115 is an organic material, for example: BARC (bottom anti-reflective coating) material, ODL (organic dielectric layer) material, spin on carbon (SOC), photoresist, DARC (dielectric anti-reflective coating) material, DUO (Deep UV Light Absorbing Oxide) material or APF (Advanced Patterning Film) material.
[0051] The step of forming the mask layer 115 includes: forming a mask material layer (not shown) covering the substrate; patterning the mask material layer to form an opening 116 in the mask material layer, and the remaining mask material layer serves as the mask layer 115 .
[0052] In this embodiment, the mask material layer is formed by a spin coating process.
[0053] The subsequent semiconductor structure formation process also includes: forming a gate structure on the substrate at the junction of the well region 101 and the drift region 102, the gate structure being located between the trench 114 in the drift region 102 and the trench 114 in the well region 101; after the gate structure is formed, forming a drain region in the drift region 102, the drain region being located on a side of the trench 114 in the drift region 102 away from the well region 101, and forming a source region in the well region 101, the source region being located on a side of the trench 114 in the well region 101 away from the drift region 102.
[0054] It should be noted that the groove 114 should not be too deep or too shallow. Usually the source region and the drain region are formed in the same step, and the bottom of the source region and the bottom of the drain region are at approximately the same height in the fin 109. If the groove 114 is too deep, when the semiconductor structure is working, the path of the current flowing from the drain region through the channel and the source region becomes larger, thereby causing the on-resistance of the semiconductor structure to become larger, and then the on-current becomes smaller, which is not easy to improve the electrical performance of the semiconductor structure. If the groove 114 is too shallow, the first type ions in the drain region may still diffuse from the bottom of the diffusion barrier layer to the channel region below the gate structure, and when the semiconductor structure is working, the depletion layer of the drain region is easy to expand, which is not conducive to improving the short channel effect. And if it is too little below the bottom of the drain region, the stress of the diffusion barrier layer 106 on the source region and the drain region is small, and it is not easy to significantly increase the migration rate of carriers in the channel. In this embodiment, in the step of forming the trench 114 , the bottom of the trench 114 is 10 nanometers to 20 nanometers lower than the bottom of the drain region formed subsequently. Low means that the bottom of the trench 114 is located below the bottom of the drain region.
[0055] It should be noted that, with the extension direction perpendicular to the gate structure as the lateral direction, the lateral dimension of the trench 114 should not be too large or too small. A diffusion barrier layer is subsequently formed in the trench 114. The material of the diffusion barrier layer is a high-stress dielectric material. If the lateral dimension of the diffusion barrier layer is too large, the stress of the top of the diffusion barrier layer 106 on the subsequently formed source region and drain region is too large, which is easy to cause fractures or dislocations in the source region and drain region. On the one hand, it is easy to cause leakage current in the source region and drain region. On the other hand, when the semiconductor structure is working, the fractures or dislocations in the source region and drain region are easy to generate excessive heat, resulting in poor performance of the semiconductor structure. In addition, because the material of the diffusion barrier layer 106 is a dielectric material, the lateral dimension of the diffusion barrier layer 106 is too large, which is easy to cause the on-resistance of the semiconductor structure to increase and the on-current to decrease, and it is not easy to improve the electrical performance of the semiconductor structure. If the lateral dimension of the trench 114 is too small, the first type ions in the source region and drain region are easy to pass through the diffusion barrier layer and diffuse into the channel region. When the semiconductor structure is working, the depletion layers of the source region and the drain region are easily expanded, and it is difficult to improve the short channel effect. In this embodiment, in the step of forming the trench 114, the lateral dimension of the trench 114 is 20 nanometers to 30 nanometers.
[0056] refer to Figure 6 to Figure 7 , a diffusion barrier layer 106 (eg, Figure 7 shown).
[0057] In the embodiment of the present invention, the substrate has adjacent well regions 101 and drift regions 102, and subsequently a gate structure is formed on the substrate at the junction of the well regions 101 and the drift regions 102, and a drain region is formed in the drift region 102, and the drain region is located on the side of the trench 114 in the drift region 102 away from the well region 101. The diffusion barrier layer 106 is located in the drift region 102 between the drain region and the gate structure, and the diffusion barrier layer 106 is used to block the doped ions in the drain region from diffusing into the channel region below the gate structure; when the semiconductor structure is working, under the action of the diffusion barrier layer 106, the doped ions in the drain region are not easy to diffuse into the channel region below the gate structure, which makes it difficult for the depletion layers of the source region and the drain region on both sides of the gate structure to expand, which is conducive to improving the short channel effect, and further improving the electrical performance of the semiconductor structure.
[0058] It should be noted that the diffusion barrier layer 106 is also formed in the trench 114 in the well region 101 . Therefore, the diffusion barrier layer 106 in the well region 101 is used to block the first type ions in the source region from diffusing into the channel region below the gate structure 103 .
[0059] In this embodiment, the material of the diffusion barrier layer 106 includes silicon nitride. Silicon nitride has a high density, which can make it difficult for the first type ions in the drain region to pass through the diffusion barrier layer 106 and diffuse into the channel region. Silicon nitride is a commonly used and low-cost dielectric material in the process, and has high process compatibility, which is conducive to reducing the process difficulty and process cost of forming the diffusion barrier layer 106. In other embodiments, the material of the diffusion barrier layer can also be diamond-like carbon, which has a high density and can also make the first type ions in the drain region diffuse into the channel region.
[0060] It should also be noted that the diffusion barrier layer 106 can also provide stress to the drain region, and can increase the migration rate of carriers in the channel when the semiconductor structure is working.
[0061] In this embodiment, the semiconductor structure is NLDMOS, and the diffusion barrier layer 106 is used to provide tensile stress to the source region and the drain region, and the stretching channel can improve the mobility of electrons. In other embodiments, the semiconductor structure is PLDMOS, and the diffusion barrier layer is used to provide compressive stress to the source region and the drain region, and the compressing channel can improve the mobility of holes.
[0062] In this embodiment, the material of the diffusion barrier layer 106 includes silicon nitride, which is a high-stress material and can provide stress to the drain region, and can increase the migration rate of carriers in the channel when the semiconductor structure is working. In other embodiments, when the material of the diffusion barrier layer is diamond-like carbon, diamond-like carbon is a high-stress material and can also provide stress to the drain region, and can increase the migration rate of carriers in the channel when the semiconductor structure is working.
[0063] The step of forming the diffusion barrier layer 106 includes: forming a diffusion barrier material layer 117 (eg, Figure 6 As shown); a planarization process is used to remove the diffusion barrier material layer 117 above the opening 116; after the planarization process, a portion of the thickness of the diffusion barrier material layer 117 is etched back, and the remaining diffusion barrier material layer 117 located in the trench 114 serves as the diffusion barrier layer 106.
[0064] In this embodiment, a high density plasma chemical vapor deposition process (HDPCVD) is used to form the diffusion barrier material layer 117. The high density plasma chemical vapor deposition process allows the deposition process to be applied to low temperatures (250 degrees Celsius to 450 degrees Celsius). During the process, deposition and etching can be performed simultaneously in the same reaction chamber, and it has better high aspect ratio gap filling capability, good deposited film, strong adhesion to silicon wafers, higher deposition rate, and fewer deposition defects such as voids or pinholes, which is beneficial to improving the density of the diffusion barrier material layer 117, and correspondingly, it is beneficial to improve the stress of the diffusion barrier layer 106 on the channel. In other embodiments, the diffusion barrier material layer can also be formed by an atomic layer deposition process.
[0065] The method for forming a semiconductor structure further includes: after forming the diffusion barrier layer 106 , removing the mask layer 115 .
[0066] In this embodiment, an ashing process is used to remove the mask layer 115 .
[0067] It should be noted that, in conjunction with the reference Figure 6 The method for forming a semiconductor structure further includes: after forming the trench 114 and before forming the diffusion barrier layer 106 in the trench 114, forming an inversion layer 107 on the sidewalls and bottom walls of the trench 114, wherein the inversion layer 107 is doped with second-type ions, and the second-type ions have a different conductivity type from the first-type ions.
[0068] The conductivity type of the second type ions is different from the conductivity type of the first type ions. The inversion layer 107 makes it difficult for the first type ions in the source region and the drain region to diffuse to the surface of the diffusion barrier layer 106. When the semiconductor structure is working, it is difficult for leakage current to exist on the sidewall and the bottom of the diffusion barrier layer 106. In addition, the stacked structure composed of the diffusion barrier layer 106 and the inversion layer 107 makes it difficult for the first type ions in the source region and the drain region to diffuse into the channel region. Therefore, when the semiconductor structure is working, the depletion layer of the source region and the drain region is not easy to expand, which is conducive to improving the short channel effect, and further conducive to improving the electrical performance of the semiconductor structure.
[0069] In this embodiment, the step of forming the inversion layer 107 includes: forming an epitaxial layer (not shown in the figure) in the trench 114 by a selective epitaxial growth (SEG) process, and doping the epitaxial layer with second type ions during the process of forming the epitaxial layer.
[0070] The epitaxial layer formed by the selective epitaxial growth process has high purity, few growth defects and high formation quality. In other embodiments, the epitaxial layer can also be formed by atomic layer deposition process, chemical vapor deposition process or low pressure furnace process.
[0071] In this embodiment, an in-situ self-doping process is used to perform ion doping on the epitaxial layer to form the inversion layer 107. The in-situ self-doping method is helpful to improve the uniformity of the doping ion concentration in the inversion layer 107, thereby improving the quality and performance of the inversion layer 107. In other embodiments, after the epitaxial layer is formed, the epitaxial layer can be ion doped by ion implantation to form the inversion layer.
[0072] Specifically, the material of the epitaxial layer includes silicon carbide, silicon or silicon germanium. In this embodiment, the material of the epitaxial layer includes silicon. The inversion layer 107 is formed by a selective epitaxial growth process, and the material of the fin 109 is silicon, which is conducive to improving the formation quality of the epitaxial layer.
[0073] In this embodiment, the semiconductor structure is NLDMOS, the second type ions are P type ions, and the P type ions include boron ions, gallium ions or indium ions. In other embodiments, the semiconductor structure is PLDMOS, the second type ions are N type ions, and the N type ions include phosphorus ions, arsenic ions or antimony ions.
[0074] It should be noted that the inversion layer 107 is not too thick or too thin. The main material of the inversion layer 107 is silicon, and the density of silicon is lower than that of silicon nitride. If the inversion layer 107 is too thick, the inversion layer 107 will occupy too much space of the diffusion barrier layer 106, resulting in a smaller space for forming the diffusion barrier layer 106, resulting in a weaker blocking ability of the stacked structure composed of the inversion layer 107 and the diffusion barrier layer 106 for the first type ions. Correspondingly, it is also easy to cause the stress of the diffusion barrier layer 106 on the drain region to be insufficient, and it is not easy to increase the migration rate of carriers in the channel. If the inversion layer 107 is too thin, when the first type ions in the source region and the drain region diffuse into the inversion layer 107, the second type ions in the inversion layer 107 are easy to be electrically neutralized with the first type ions, thereby causing the first type ions in the drain region to diffuse on the surface of the diffusion barrier layer 106, resulting in leakage current on the sidewalls and bottom of the diffusion barrier layer 106 in the well region 101. In this embodiment, the thickness of the inversion layer 107 is 5 nanometers to 10 nanometers.
[0075] It should be noted that the method for forming the semiconductor structure further includes: after forming the diffusion barrier layer 106 and before forming the gate structure, performing an annealing process on the diffusion barrier layer 106 .
[0076] The annealing process makes the diffusion barrier layer 106 more dense, and the diffusion barrier layer 106 can provide greater stress to the source region and the drain region formed subsequently.
[0077] In this embodiment, spike annealing is used to anneal the diffusion barrier layer 106. In other embodiments, laser annealing may be used to anneal the diffusion barrier layer.
[0078] refer to Figure 8 After forming the diffusion barrier layer 106 , a gate structure 103 is formed on the substrate at the junction of the well region 101 and the drift region 102 . The gate structure 103 is located on a side of the diffusion barrier layer 106 close to the well region 101 .
[0079] In the substrate, a channel region is formed in the region covered by the gate structure 103. Specifically, in the fin 109, a region covered by the gate structure 103 serves as the channel region.
[0080] In this embodiment, the gate structure 103 is used to control the opening and closing of the LDMOS channel.
[0081] Specifically, the gate structure 103 spans over the fin 109 and covers a portion of the top wall and a portion of the side wall of the fin 109 .
[0082] Since LDMOS is a high voltage device, the gate structure 103 includes: a gate dielectric layer 1031 located on the surface of the fin 109 at the junction of the well region 101 and the drift region 102 ; and a gate layer 1032 located on the gate dielectric layer 1031 .
[0083] In this embodiment, the gate structure 103 is a polysilicon gate structure. Accordingly, the material of the gate dielectric layer 1031 is silicon oxide; and the material of the gate layer 1032 is polysilicon.
[0084] In this embodiment, the semiconductor structure further includes: forming a sidewall spacer 110 on the sidewall of the gate structure 103. During the formation of the semiconductor structure, the sidewall spacer 110 protects the sidewall of the gate structure 103.
[0085] In this embodiment, the material of the spacer 110 includes one or more of silicon nitride, silicon oxynitride, silicon carbide, silicon carbide nitride, boron nitride, silicon boron nitride, and silicon boron nitride carbon.
[0086] refer to Fig. 9 A source region 104 is formed in the well region 101 on one side of the gate structure 103 , and a drain region 105 is formed in the drift region 102 on the other side of the gate structure. The drain region 105 is located on a side of the diffusion barrier layer 106 in the drift region 102 away from the well region 101 .
[0087] When the semiconductor structure is working, the source region 104 and the drain region 105 are used to provide stress for the channel and improve the mobility of carriers in the channel.
[0088] In this embodiment, the conductivity type of the doped ions in the drain region 105 and the source region 104 is the same as the conductivity type of the doped ions in the drift region 102 , which are both first-type ions.
[0089] Specifically, the steps of forming the drain region 105 and the doping region 106 include: forming a blocking layer (not shown in the figure) on the drift region 102 and the well region 101, the blocking layer covering the diffusion barrier layer 106; forming the drain region 105 in the drift region 102 and forming the source region 104 in the well region 101 using the blocking layer as a doping mask.
[0090] The shielding layer serves as a doping mask for forming the source region 104 and the drain region 105 . During the process of doping to form the source region 104 and the drain region 105 , the probability of the diffusion barrier layer 106 being doped is reduced, so that the diffusion barrier layer 106 can better block the first type ions in the source region 104 and the drain region 105 from diffusing into the channel region.
[0091] The shielding layer is a material that can act as a mask and is easy to remove, so that damage to other film layer structures is reduced when the shielding layer is subsequently removed.
[0092] In this embodiment, the material of the shielding layer is an organic material, for example, a BARC material, an ODL material, a SOC material, a photoresist, a DARC material, a DUO material or an APF material.
[0093] The method for forming the semiconductor structure further includes: after forming the source region 104 and the drain region 105 , removing the shielding layer.
[0094] It should be noted that, in this embodiment, the groove 114 (such as Figure 5 In the step shown in FIG. 1 , the bottom of the trench 114 is 10 to 20 nanometers lower than the bottom of the drain region formed subsequently. Therefore, the bottom of the drain region 105 is 10 to 20 nanometers higher than the bottom of the diffusion barrier layer 106.
[0095] refer to Fig.10 After forming the source region 104 and the drain region 105 , a silicide blocking layer 108 is formed on the drift region 102 between the gate structure 103 and the drain region 105 , and the silicide blocking layer 108 extends to the sidewall and a portion of the top of the gate structure 103 near the drain region 105 .
[0096] In the embodiment of the present invention, the source region 104 and the drain region 105 are formed first, and then the silicide barrier layer 108 is formed. In the process of forming the silicide barrier layer 108, the silicide barrier layer 108 can accurately cover the diffusion barrier layer 106 and the partial area of the drain region 105 close to the gate structure 103, so that the metal silicide layer formed subsequently is not easy to contact the diffusion barrier layer 106, thereby avoiding the problem of tip leakage in the semiconductor structure. In addition, the source region 104 and the drain region 105 are formed before the silicide barrier layer 108, so that the source region 104 and the drain region 105 are used for a larger process window, and then the area formed by the source region 104 and the drain region 105 is larger, so that the contact resistance of the semiconductor structure is smaller.
[0097] It should be noted that the silicide blocking layer 108 also extends to a portion of the drain region 105 close to the gate structure 103 .
[0098] The silicide blocking layer 108 is used to prevent the growth of a silicide layer, thereby preventing the silicide layer from forming on the drift region 102 between the gate structure 103 and the drain region 105, avoiding the silicide layer from adversely affecting the formation of a depletion region in the drift region 102, thereby ensuring the withstand voltage performance of the NLDMOS.
[0099] Specifically, the material of the silicide blocking layer 108 includes one or more of silicon oxide, silicon nitride and silicon oxynitride. In this embodiment, the material of the silicide blocking layer 108 is silicon oxide.
[0100] It should also be noted that, in the method for forming the semiconductor structure in this embodiment, the source region 104 and the drain region 105 are formed first, and then the silicide blocking layer 108 is formed.
[0101] In other embodiments, a silicide barrier layer may be formed first, and then the source region and the drain region may be formed. The silicide barrier layer formed first may act as a mask in the subsequent process of forming the source region and the drain region, so that in the process of doping to form the source region and the drain region, the first type ions are shielded by the silicide barrier layer and are not easy to enter the drift region between the gate structure and the drain region, thereby making it difficult for the first type ions to diffuse into the channel region, and when the semiconductor structure is working, the depletion layer of the source region and the drain region is not easy to expand, which is conducive to improving the short channel effect and enhancing the electrical performance of the semiconductor structure.
[0102] refer to Fig.11 and Fig.12 , is a schematic diagram of the structure corresponding to each step in the second embodiment of the method for forming a semiconductor structure according to an embodiment of the present invention. The similarities between this embodiment and the first embodiment are not repeated here. The differences between this embodiment and the first embodiment are:
[0103] refer to Fig.11 The shielding layer (not shown) exposes a portion of the diffusion barrier layer 206 of the drift region 202 away from the gate structure 203. Accordingly, in the process of forming the drain region 205 using the shielding layer as a doping mask, a portion of the diffusion barrier layer 206 of the drift region 202 away from the gate structure 203 forms the drain region 205.
[0104] The drain region 205 will occupy the diffusion barrier layer 206 in part of the drift region 202 and the inversion layer 207 in part of the drift region 202, and the remaining inversion layer 207 is only formed between the diffusion barrier layer 206 and the drift region 202, and the drain region 205 is directly in contact with the diffusion barrier layer 206. The diffusion barrier layer 206 can make the drain region 205 obtain greater stress when blocking the first type ions in the drain region 205 from diffusing into the channel region, which is beneficial to improving the migration rate of carriers in the channel when the semiconductor structure is working.
[0105] In this embodiment, the blocking layer also exposes a partial area of the diffusion barrier layer 206 of the well region 201 away from the gate structure 203. Accordingly, in the process of forming the source region 204 using the blocking layer as a doping mask, a partial area of the diffusion barrier layer 206 of the well region 201 away from the gate structure 203 forms the source region 204.
[0106] The source region 204 will occupy the diffusion barrier layer 206 in part of the well region 201 and the inversion layer 207 in part of the well region 201, and the remaining inversion layer 207 is only formed between the diffusion barrier layer 206 and the well region 201, and the source region 204 is directly in contact with the diffusion barrier layer 206. The source region 204 is directly in contact with the diffusion barrier layer 206, and the diffusion barrier layer 206 can make the source region 204 obtain greater stress when blocking the first type ions of the source region 204 from diffusing into the channel region, which is beneficial to improving the migration rate of carriers in the channel when the semiconductor structure is working.
[0107] refer to Fig.12 After forming the source region 204 and the drain region 205 , a silicide blocking layer 208 is formed on the drift region 202 between the gate structure 203 and the drain region 205 , and the silicide blocking layer 208 extends to the sidewall and a portion of the top of the gate structure 203 near the drain region 205 .
[0108] In the embodiment of the present invention, the source region 204 and the drain region 205 are formed first, and then the silicide barrier layer 208 is formed. In the process of forming the silicide barrier layer 208, the silicide barrier layer 208 can accurately cover the diffusion barrier layer 206 and the partial area of the drain region 205 close to the gate structure 203, so that the metal silicide layer formed subsequently is not easy to contact the diffusion barrier layer 206, thereby avoiding the problem of tip leakage in the semiconductor structure. In addition, the source region 204 and the drain region 205 are formed before the silicide barrier layer 208, so that the source region 204 and the drain region 205 are used for a larger process window, and then the area formed by the source region 204 and the drain region 205 is larger, so that the contact resistance of the semiconductor structure is smaller.
[0109] It should be noted that the silicide blocking layer 208 also extends to a portion of the drain region 205 close to the gate structure 203 .
[0110] The silicide blocking layer 208 is used to prevent the growth of a silicide layer, thereby preventing the silicide layer from forming on the drift region 202 between the gate structure 203 and the drain region 205, avoiding the silicide layer from adversely affecting the formation of a depletion region in the drift region 202, thereby ensuring the withstand voltage performance of the NLDMOS.
[0111] Specifically, the material of the silicide blocking layer 208 includes one or more of silicon oxide, silicon nitride and silicon oxynitride. In this embodiment, the material of the silicide blocking layer 208 is silicon oxide.
[0112] It should also be noted that, in the method for forming the semiconductor structure in this embodiment, the source region 204 and the drain region 205 are formed first, and then the silicide blocking layer 208 is formed.
[0113] In other embodiments, a silicide barrier layer may be formed first, and then the source region and the drain region may be formed. The silicide barrier layer formed first may act as a mask in the subsequent process of forming the source region and the drain region, so that in the process of doping to form the source region and the drain region, the first type ions are shielded by the silicide barrier layer and are not easy to enter the drift region between the gate structure and the drain region, thereby making it difficult for the first type ions to diffuse into the channel region, and when the semiconductor structure is working, the depletion layer of the source region and the drain region is not easy to expand, which is conducive to improving the short channel effect and enhancing the electrical performance of the semiconductor structure.
[0114] Fig.10 The semiconductor structure provided by the embodiment of the present invention will be described in detail below in conjunction with the accompanying drawings.
[0115] refer to Fig.10 The semiconductor structure of this embodiment includes: a substrate, in which adjacent well regions 101 and drift regions 102 are formed; a gate structure 103, located on the substrate at the junction of the well region 101 and the drift region 102; a source region 104, located in the well region 101 on one side of the gate structure 103; a drain region 105, located in the drift region 102 on the other side of the gate structure 103; a diffusion barrier layer 106, located in the drift region 102 between the drain region 105 and the gate structure 103, and the diffusion barrier layer 106 is used to prevent doped ions in the drain region 105 from diffusing into the channel region below the gate structure 103.
[0116] In the semiconductor structure of the embodiment of the present invention, the diffusion barrier layer 106 is located in the drift region 102 between the drain region 105 and the gate structure 103, and the diffusion barrier layer 106 is used to prevent the doped ions in the drain region 105 from diffusing into the channel region below the gate structure 103; when the semiconductor structure is working, under the action of the diffusion barrier layer 106, the doped ions in the drain region 105 are not easy to diffuse into the channel region below the gate structure 103, which makes it difficult for the depletion layer of the drain region 105 to expand, which is beneficial to improving the short channel effect, and further improving the electrical performance of the semiconductor structure.
[0117] In this embodiment, the semiconductor structure is an LDMOS fin field effect transistor as an example, and the substrate includes a substrate 100 and a fin 109 separated on the substrate 100. In other embodiments, the LDMOS may also be a planar transistor, and the corresponding substrate is a planar substrate.
[0118] In this embodiment, the substrate 100 is a silicon substrate. In other embodiments, the substrate may also be a substrate of other materials such as a germanium substrate, a silicon germanium substrate, a silicon carbide substrate, a gallium arsenide substrate, or an indium gallium substrate, and the substrate may also be a silicon on insulator substrate or a germanium on insulator substrate.
[0119] In this embodiment, the fin 109 is an integral structure with the substrate 100. In other embodiments, the fin may also be a semiconductor layer epitaxially grown on the substrate, so as to achieve the purpose of accurately controlling the initial fin height.
[0120] Therefore, the material of the fin 109 is the same as that of the substrate 100, and the material of the fin 109 is silicon. In other embodiments, the material of the fin may also be a semiconductor material such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the material of the fin may also be different from that of the substrate.
[0121] The semiconductor structure further includes an isolation layer (not shown in the figure) located on the substrate 100 where the fin 109 is exposed.
[0122] The isolation layer is used as a shallow trench isolation (STI) structure to isolate adjacent devices.
[0123] In this embodiment, the material of the isolation layer is silicon oxide. Silicon oxide is a commonly used dielectric material with low cost and high process compatibility, which is conducive to reducing the process difficulty and process cost of forming the isolation layer; in addition, the dielectric constant of silicon oxide is small, which is also conducive to improving the effect of the isolation layer for isolating adjacent devices. In other embodiments, the material of the isolation layer can also be other dielectric materials such as silicon nitride or silicon oxynitride.
[0124] In this embodiment, the well region 101 and the drift region 102 are located in the fin 109 and are in contact with each other. The well region 101 serves as a lateral diffusion region to form a channel with a concentration gradient, and the drift region 102 is used to withstand a large partial pressure.
[0125] First-type ions are formed in the drift region 102 , and second-type ions are formed in the well region 101 . The second-type ions have a different conductivity type from the first-type ions.
[0126] Specifically, the semiconductor structure in this embodiment is NLDMOS, the first type of ions are N-type ions, the N-type ions include one or more of phosphorus ions, arsenic ions and antimony ions, and the second type of ions are P-type ions, the P-type ions include one or more of boron ions, gallium ions and indium ions.
[0127] In other embodiments, when the semiconductor structure is PLDMOS, the first type of ions are P type ions, which include one or more of boron ions, gallium ions, and indium ions; the second type of ions are N type ions, which include one or more of phosphorus ions, arsenic ions, and antimony ions.
[0128] In this embodiment, the gate structure 103 is used to control the opening and closing of the LDMOS channel.
[0129] Specifically, the gate structure 103 spans over the fin 109 and covers a portion of the top wall and a portion of the side wall of the fin 109. In the fin 109, the area covered by the gate structure 103 serves as a channel region.
[0130] Since LDMOS is a high voltage device, the gate structure 103 includes: a gate dielectric layer 1031 located on the surface of the fin 109 at the junction of the well region 101 and the drift region 102 ; and a gate layer 1032 located on the gate dielectric layer 1031 .
[0131] In this embodiment, the gate structure 103 is a polysilicon gate structure. Accordingly, the material of the gate dielectric layer 1031 is silicon oxide; and the material of the gate layer 1032 is polysilicon.
[0132] In other embodiments, the gate structure may also be a metal gate structure, and accordingly, the gate dielectric layer is a high-k gate dielectric layer, and the gate layer is a metal gate electrode.
[0133] In this embodiment, the semiconductor structure further includes: a sidewall spacer 110 located on the sidewall of the gate structure 103. The sidewall spacer 110 is used to define the formation area of the source region 104 and is also used to protect the sidewall of the gate structure 103 during the formation of the semiconductor structure.
[0134] In this embodiment, the material of the spacer 110 includes one or more of silicon nitride, silicon oxynitride, silicon carbide, silicon carbide nitride, boron nitride, silicon boron nitride, and silicon boron nitride carbon.
[0135] The semiconductor structure further includes: a source region 104 located in the well region 101 on the other side of the gate structure 103 ; and a drain region 105 located in the drift region 102 on the other side of the gate structure 103 .
[0136] The conductivity type of the doped ions in the drain region 105 and the source region 104 is the same as the conductivity type of the doped ions in the drift region 102 , and accordingly, both the source region 104 and the drain region 105 have first-type ions;
[0137] When the semiconductor structure is working, the source region 104 and the drain region 105 provide stress for the channel, thereby increasing the migration rate of carriers in the channel.
[0138] Specifically, the drain region 105 is located in the drift region 102 on one side of the gate structure 103 ; and the source region 104 is located in the well region 101 on the other side of the gate structure 103 .
[0139] In this embodiment, the semiconductor structure is NLDMOS, and the first type ions in the source region 104 and the drain region 105 are N type ions. In other embodiments, when the semiconductor structure is PLDMOS, the first type ions in the source region and the drain region are P type ions.
[0140] The diffusion barrier layer 106 is located in the drift region 102 between the drain region 105 and the gate structure 103 . The diffusion barrier layer 106 is used to block the first type ions in the drain region 105 from diffusing into the channel region below the gate structure 103 .
[0141] In this embodiment, the material of the diffusion barrier layer 106 includes silicon nitride. Silicon nitride has a high density, which can make it difficult for the first type ions in the drain region 105 to pass through the diffusion barrier layer 106 and diffuse into the channel region. Silicon nitride is a commonly used dielectric material with low cost and has high process compatibility, which is conducive to reducing the process difficulty and process cost of forming the diffusion barrier layer 106. In other embodiments, the material of the diffusion barrier layer can also be diamond-like carbon, which has a high density and can also make the first type ions in the drain region diffuse into the channel region.
[0142] It should also be noted that the diffusion barrier layer 106 can also provide stress to the drain region 105, and can increase the migration rate of carriers in the channel when the semiconductor structure is working.
[0143] In this embodiment, the material of the diffusion barrier layer 106 includes silicon nitride, which is a high-stress material and can provide stress to the drain region 105. When the semiconductor structure is working, the migration rate of carriers in the channel can be increased. In other embodiments, when the material of the diffusion barrier layer is diamond-like carbon, diamond-like carbon is a high-stress material and can also provide stress to the drain region. When the semiconductor structure is working, the migration rate of carriers in the channel can be increased.
[0144] In this embodiment, the semiconductor structure is NLDMOS, and the diffusion barrier layer 106 is used to provide tensile stress to the drain region 105. The stretching channel can improve the mobility of electrons. In other embodiments, the semiconductor structure is PLDMOS, and the diffusion barrier layer is used to provide compression stress to the drain region. The compression channel can improve the mobility of holes.
[0145] It should be noted that the diffusion barrier layer 106 is also located in the well region 101 between the gate structure 103 and the source region 104 .
[0146] The diffusion barrier layer 106 in the well region 101 is used to block the first type ions in the source region 104 from diffusing into the channel region below the gate structure 103 .
[0147] At the same time, the diffusion barrier layer 106 in the well region 101 can also provide stress to the source region 104, and can increase the migration rate of carriers in the channel when the semiconductor structure is working.
[0148] In this embodiment, the bottom end of the diffusion barrier layer 106 is lower than the bottom end of the drain region 105. By making the bottom end of the diffusion barrier layer 106 lower than the bottom end of the drain region 105, the path for the first type ions in the drain region 105 to diffuse from the bottom end of the diffusion barrier layer 106 to the channel region becomes longer, so that the first type ions in the drain region 105 are not easy to diffuse from the bottom end of the diffusion barrier layer 106 to the channel region below the gate structure 103. When the semiconductor structure is working, the depletion layer of the drain region 105 is not easy to expand, which is conducive to improving the short channel effect, and further improving the electrical performance of the semiconductor structure.
[0149] In addition, compared with the case where the bottom of the diffusion barrier layer is higher than or flush with the bottom of the drain region, the bottom of the diffusion barrier layer 106 is lower than the bottom of the drain region 105, which is also beneficial to increase the stress of the diffusion barrier layer 106 on the source region 104 and the drain region 105, thereby improving the migration rate of carriers in the channel.
[0150] It should be noted that the distance from the bottom of the diffusion barrier layer 106 to the bottom of the drain region 105 should not be too small or too large. Usually, the source region 104 and the drain region 105 are formed in the same step, and the bottom of the source region 104 and the bottom of the drain region 105 are at approximately the same height in the fin 109. If the distance is too small, the first type ions in the drain region 105 and the source region 104 may still diffuse from the bottom of the diffusion barrier layer 106 to the channel region below the gate structure 103, and when the semiconductor structure is working, the depletion layer of the drain region 105 and the source region 104 is easy to expand, which is not conducive to improving the short channel effect. If the distance is too small, the stress of the diffusion barrier layer 106 on the source region 104 and the drain region 105 is small, and it is not easy to significantly improve the migration rate of carriers in the channel. If the distance is too large, when the semiconductor structure is working, the path of the current flowing from the drain region 105 through the channel and the source region 104 becomes larger, thereby increasing the on-resistance of the semiconductor structure, and then reducing the on-current, making it difficult to improve the electrical performance of the semiconductor structure. In this embodiment, the bottom of the diffusion barrier layer is 10 nanometers to 20 nanometers lower than the bottom of the drain region.
[0151] It should be noted that, with the extension direction perpendicular to the gate structure 103 as the lateral direction, the lateral dimension of the diffusion barrier layer 106 should not be too large or too small. The material of the diffusion barrier layer 106 is a high-stress material. If the lateral dimension of the diffusion barrier layer 106 is too large, the stress of the top of the diffusion barrier layer 106 on the source region 104 and the drain region 105 is too large, which is easy to cause the source region 104 and the drain region 105 to have a fracture or dislocation. On the one hand, it is easy to cause the source region 104 and the drain region 105 to have a leakage current. On the other hand, when the semiconductor structure is working, the fracture or dislocation in the source region 104 and the drain region 105 is easy to generate too much heat, resulting in poor performance of the semiconductor structure; in addition, because the material of the diffusion barrier layer 106 is a dielectric material, the lateral dimension of the diffusion barrier layer 106 is too large, which is easy to cause the on-resistance of the semiconductor structure to increase and the on-current to decrease, and it is not easy to improve the electrical performance of the semiconductor structure. If the lateral dimension of the diffusion barrier layer 106 is too small, the first type ions in the source region 104 and the drain region 105 are easy to pass through the diffusion barrier layer 106 and diffuse into the channel region. When the semiconductor structure is working, the depletion layer of the source region 104 and the drain region 105 is easy to expand, and it is difficult to improve the short channel effect. In this embodiment, the lateral dimension of the diffusion barrier layer 106 is 20 nanometers to 30 nanometers.
[0152] Continue to refer Fig.10 The semiconductor structure further includes: an inversion layer 107, located between the diffusion barrier layer 106 and the drift region 102 and between the diffusion barrier layer 106 and the drain region 105, and the inversion layer 107 has second-type ions, and the second-type ions have a different conductivity type from the first-type ions.
[0153] The conductivity type of the second type ions is different from the conductivity type of the first type ions. The inversion layer 107 makes it difficult for the first type ions in the drain region 105 to diffuse to the surface of the diffusion barrier layer 106. When the semiconductor structure is working, it is difficult for leakage current to exist on the sidewall and bottom of the diffusion barrier layer 106. In addition, the stacked structure composed of the diffusion barrier layer 106 and the inversion layer 107 makes it difficult for the first type ions in the drain region 105 to diffuse into the channel region. Therefore, when the semiconductor structure is working, the depletion layer of the drain region 105 is not easy to expand, which is conducive to improving the short channel effect, and further conducive to improving the electrical performance of the semiconductor structure.
[0154] It should be noted that the inversion layer 107 is also located in the well region 101 . The inversion layer 107 in the well region 101 is located between the diffusion barrier layer 106 and the well region 101 and between the diffusion barrier layer 106 and the source region 104 .
[0155] Similarly, the inversion layer 107 in the well region 101 makes it difficult for the first type ions in the source region 104 to diffuse to the surface of the diffusion barrier layer 106 in the well region 101, and when the semiconductor structure is working, it is difficult for leakage current to exist on the sidewalls and the bottom of the diffusion barrier layer 106 in the well region 101. In addition, in the well region 101, the stacked structure composed of the diffusion barrier layer 106 and the inversion layer 107 makes it difficult for the first type ions in the source region 104 to diffuse into the channel region. Therefore, when the semiconductor structure is working, the depletion layer of the source region 104 is not easy to expand, which is conducive to improving the short channel effect, and further conducive to improving the electrical performance of the semiconductor structure.
[0156] Specifically, the material of the inversion layer 107 includes silicon carbide, silicon or silicon germanium with second-type ions. In this embodiment, the material of the inversion layer 107 includes silicon with second-type ions. The inversion layer 107 is generally formed by a selective epitaxial growth process, the material of the fin 109 is silicon, and the material of the inversion layer 107 is silicon with second-type ions, which is conducive to improving the formation quality of the inversion layer 107.
[0157] In this embodiment, the semiconductor structure is NLDMOS, the second type ions are P type ions, and the P type ions include boron ions, gallium ions or indium ions. In other embodiments, the semiconductor structure is PLDMOS, the second type ions are N type ions, and the N type ions include phosphorus ions, arsenic ions or antimony ions.
[0158] It should be noted that the inversion layer 107 is not too thick or too thin. The main material of the inversion layer 107 is silicon, and the density of silicon is lower than that of silicon nitride. If the inversion layer 107 is too thick, the inversion layer 107 will occupy too much space of the diffusion barrier layer 106, resulting in a smaller space for forming the diffusion barrier layer 106, resulting in a weaker blocking ability of the stacked structure composed of the inversion layer 107 and the diffusion barrier layer 106 for the first type ions. Correspondingly, it is also easy to cause the stress of the diffusion barrier layer 106 on the drain region 105 to be insufficient, and it is not easy to increase the migration rate of carriers in the channel. If the inversion layer 107 is too thin, when the first type ions in the source region 104 and the drain region 105 diffuse into the inversion layer 107, the second type ions in the inversion layer 107 are easy to be electrically neutralized with the first type ions, thereby causing the first type ions in the drain region 105 to diffuse on the surface of the diffusion barrier layer 106, resulting in leakage current on the sidewalls and bottom of the diffusion barrier layer 106 in the well region 101. In this embodiment, the thickness of the inversion layer 107 is 5 nanometers to 10 nanometers.
[0159] Fig.12 It is a structural schematic diagram of a second embodiment of a semiconductor structure according to an embodiment of the present invention.
[0160] The similarities between this embodiment and the first embodiment are not repeated here. The difference between this embodiment and the first embodiment is that: another schematic diagram of the position of the diffusion barrier layer 206 in the semiconductor structure is shown, the diffusion barrier layer 206 is directly in contact with the drain region 205, and the inversion layer 207 is located between the diffusion barrier layer 206 and the drift region 202.
[0161] In this embodiment, the drain region 205 is directly in contact with the diffusion barrier layer 206. The diffusion barrier layer 206 can enable the drain region 205 to obtain greater stress while blocking the first type ions in the drain region 205 from diffusing into the channel region, which is beneficial to improving the migration rate of carriers in the channel when the semiconductor structure is working.
[0162] It should be noted that the inversion layer 207 is also located in the well region 201 . The inversion layer 207 in the well region 201 is located between the diffusion barrier layer 206 and the well region 201 . The diffusion barrier layer 206 is in direct contact with the source region 204 .
[0163] In this embodiment, the source region 204 is directly in contact with the diffusion barrier layer 206. The diffusion barrier layer 206 can enable the source region 204 to obtain greater stress while blocking the first type ions in the source region 204 from diffusing into the channel region. This is beneficial to improving the migration rate of carriers in the channel when the semiconductor structure is working.
[0164] The semiconductor structure includes a silicide blocking layer 208 located on the drift region 202 between the gate structure 203 and the drain region 205 , and the silicide blocking layer 208 extends to the sidewall and a portion of the top of the gate structure 203 near the drain region 205 .
[0165] It should be noted that the silicide blocking layer 208 also extends to a portion of the drain region 205 close to the gate structure 203 .
[0166] The silicide blocking layer 208 is used to prevent the growth of a silicide layer, thereby preventing the silicide layer from forming on the drift region 202 between the gate structure 203 and the drain region 205, avoiding the silicide layer from adversely affecting the formation of a depletion region in the drift region 202, thereby ensuring the withstand voltage performance of the NLDMOS.
[0167] Specifically, the material of the silicide blocking layer 208 includes one or more of silicon oxide, silicon nitride and silicon oxynitride. In this embodiment, the material of the silicide blocking layer 208 is silicon oxide.
[0168] The semiconductor structure can be formed by the formation method described in the above embodiment, or by other formation methods. For the specific description of the semiconductor structure described in this embodiment, reference can be made to the corresponding description in the above embodiment, and this embodiment will not be repeated here.
[0169] Although the embodiments of the present invention are disclosed above, the embodiments of the present invention are not limited thereto. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the embodiments of the present invention. Therefore, the protection scope of the embodiments of the present invention shall be subject to the scope defined by the claims.
Claims
1. A semiconductor structure, It is characterized in that include: A substrate having a well region and a drift region adjacent to each other; A gate structure, located on the substrate at the junction of the well region and the drift region; a source region, located in the well region on one side of the gate structure; a drain region located in the drift region on the other side of the gate structure; A diffusion barrier layer is located in the drift region between the drain region and the gate structure, and is used to block the doped ions in the drain region from diffusing into the channel region below the gate structure. The diffusion barrier layer is also located in the well region between the gate structure and the source region.
2. The semiconductor structure according to claim 1, It is characterized in that The drift region has a first type of ions; The semiconductor structure further includes an inversion layer located between the diffusion barrier layer and the drift region, or between the diffusion barrier layer and the drift region and between the diffusion barrier layer and the drain region, wherein the inversion layer contains second-type ions having a different conductivity type from the first-type ions.
3. The semiconductor structure according to claim 2, It is characterized in that The thickness of the inversion layer is 5 nanometers to 10 nanometers.
4. The semiconductor structure according to claim 2, It is characterized in that The material of the inversion layer includes silicon carbide, silicon or silicon germanium having the second type ions.
5. The semiconductor structure according to claim 1 or 2, It is characterized in that The bottom of the diffusion barrier layer is 10 nanometers to 20 nanometers lower than the bottom of the drain region.
6. The semiconductor structure according to claim 1 or 2, It is characterized in that Taking the extension direction perpendicular to the gate structure as the lateral direction, the lateral dimension of the diffusion barrier layer is 20 nanometers to 30 nanometers.
7. The semiconductor structure according to claim 1 or 2, It is characterized in that The material of the diffusion barrier layer includes silicon nitride or diamond-like carbon.
8. The semiconductor structure according to claim 1 or 2, It is characterized in that The diffusion barrier layer is in contact with the drain region.
9. A method for forming a semiconductor structure, It is characterized in that include: Providing a substrate, wherein adjacent well regions and drift regions are formed in the substrate; forming a trench in the drift region, wherein during the process of forming the trench in the drift region, the trench is also formed in the well region; forming a diffusion barrier layer in the trench; After forming the diffusion barrier layer, forming a gate structure on the substrate at the junction of the well region and the drift region, the gate structure is located on a side of the diffusion barrier layer close to the well region, and in the step of forming the gate structure, the gate structure is located between the diffusion barrier layer in the drift region and the diffusion barrier layer in the well region; A source region is formed in the well region on one side of the gate structure, and a drain region is formed in the drift region on the other side of the gate structure, wherein the drain region is located on a side of the diffusion barrier layer in the drift region away from the well region; in the step of forming the source region, the source region is located on a side of the diffusion barrier layer in the well region away from the drift region.
10. The method for forming a semiconductor structure according to claim 9, It is characterized in that In the step of forming the drift region, the drift region is doped with first type ions; The method for forming the semiconductor structure also includes: after forming the trench and before forming the diffusion barrier layer in the trench, forming an inversion layer on the sidewalls and bottom walls of the trench, wherein the inversion layer is doped with second type ions, and the second type ions have a different conductivity type from the first type ions.
11. The method for forming a semiconductor structure according to claim 10, It is characterized in that The thickness of the inversion layer is 5 nanometers to 10 nanometers.
12. The method for forming a semiconductor structure according to claim 10, It is characterized in that The step of forming the inversion layer includes: forming an epitaxial layer in the trench by adopting a selective epitaxial growth process, and doping the epitaxial layer with second type ions during the process of forming the epitaxial layer.
13. The method for forming a semiconductor structure according to claim 9 or 10, It is characterized in that In the process of forming the drain region, the drain region is in contact with the diffusion barrier layer.
14. The method for forming a semiconductor structure according to claim 9 or 10, It is characterized in that The step of forming the groove includes: forming a mask layer on the substrate; The substrate is etched using the mask layer as a mask by a dry etching process to form the groove.
15. The method for forming a semiconductor structure according to claim 9 or 10, It is characterized in that In the step of forming the drain region, the bottom of the drain region is 10 nanometers to 20 nanometers higher than the bottom of the diffusion barrier layer.
16. The method for forming a semiconductor structure according to claim 9 or 10, It is characterized in that In the step of forming the groove, the lateral dimension of the groove is 30 nanometers to 50 nanometers, with the direction perpendicular to the extension direction of the groove being the lateral dimension.
17. The method for forming a semiconductor structure according to claim 9 or 10, It is characterized in that The diffusion barrier layer is formed in the trench by using a high density plasma chemical vapor deposition process or an atomic layer deposition process.
18. The method for forming a semiconductor structure according to claim 9 or 10, It is characterized in that The material of the diffusion barrier layer includes silicon nitride or diamond-like carbon.