A processing method for a network filter housing and a product thereof

Through the stamping mold single-use terminal pins and bending structure, combined with the design of inner and outer connecting rods, the problems of complex processing of electronic component shells and insolid welding in the prior art are solved, and efficient processing and welding are achieved The effect improves the adhesion and conductivity of the product.

CN112828192BActive Publication Date: 2024-11-05DONGGUAN FUHANG ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110027294.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-09
Publication Date
2024-11-05
Estimated Expiration
2041-01-09

AI Technical Summary

Technical Problem

The existing electronic component shell with metal terminals has complex processing technology, low efficiency, and lack of inner connecting rod structure, resulting in unsolid welding, prone to oxidation and dummy welding, affecting the adhesion and conductivity of the product.

Method used

Using a processing method of network filter housing, the terminal pins and bending structure are formed by stamping molds at one time, and the inner connecting rod and the outer connecting rod are connected to simplify the process and improve product quality. The outer connecting rod is cut off after electroplating to prevent Oxidize and design tin-crawling bevels during welding to improve welding firmness.

Benefits of technology

The process has been greatly simplified, the processing efficiency and product quality have been improved, the firmness and conductivity of welding have been ensured, the occurrence of false welding has been prevented, and the safety performance of the product has been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112828192B_ABST
    Figure CN112828192B_ABST
Patent Text Reader

Abstract

The present invention discloses a processing method for a network filter housing, comprising the following steps: (1) stamping and bending the terminal pins into one piece; (2) injection molding a plastic shell: forming a plurality of plastic shells by injection molding on a symmetrically arranged semi-finished product, and forming an outer terminal pin group and an inner terminal pin group on the plastic shell, wherein the outer terminal pin group is connected to an outer connecting rod, and the inner terminal pin group is connected to an inner connecting rod; (3) bending and cutting the outer connecting rod into one piece: stamping and bending the outer terminal pin group at the same time, and forming a second bending portion and a third bending portion on each outer terminal pin respectively; cutting the outer connecting rod along an outer pre-cut groove; (4) electroplating: electroplating the surface of the outer terminal pin group and the inner terminal pin group to form a metal protective layer; (5) obtaining a finished product: breaking the inner connecting rod along an inner pre-cut groove, and separating the inner connecting rod from the plastic shell, and obtaining a plurality of network filter housings with metal terminal pins. The present invention also discloses a product obtained by implementing the above processing method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an electronic component and a processing method thereof, in particular to a processing method of a network filter housing and a product thereof. Background Art

[0002] In the existing processing technology of electronic component housings with metal terminal pins, there are mainly the following two shortcomings:

[0003] (1) Terminal pin forming and terminal pin bending require at least two sets of molds and at least two processes to complete, which is complex and inefficient;

[0004] (2) There is no inner connecting rod structure. After the injection molding is completed, the terminal pins are bent. Then the outer connecting rod is used to connect the terminal pins on each shell for conductive electroplating and electroplating protective layer. After electroplating, the outer connecting rod is cut. The position where the outer connecting rod is cut is not electroplated with a protective layer, which will expose the copper. Over time, it will be oxidized. When the client solders, it will not be able to weld, affecting the electrical connection. The product has low adhesion on the PCB board and is not firm.

[0005] (3) The misaligned pins include a strip portion and a plurality of terminal pins formed on one side of the strip, wherein the plurality of terminal pins are arranged in a row, and a certain gap is maintained between adjacent terminal pins. The prior art terminal pins are too narrow in spacing, which easily leads to soldering during soldering, resulting in poor appearance and function. At the same time, the too narrow spacing increases the difficulty of enameled wire sorting and reduces work efficiency. Summary of the invention

[0006] In view of the above-mentioned shortcomings, an object of the present invention is to provide a method for processing a network filter housing, which can greatly simplify the process and improve the processing efficiency and product quality.

[0007] The purpose of the present invention is also to provide a network filter housing processed by the above-mentioned processing method, which has a reasonable structural design, which is not only conducive to the smooth and rapid subsequent winding and improves work efficiency; but also, when it is subsequently soldered to a PCB board, it can smoothly crawl tin to wrap the welding end, improve the welding firmness, prevent the occurrence of cold solder joints, ensure good conductivity, and improve product safety performance.

[0008] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:

[0009] A method for processing a network filter housing, characterized in that it comprises the following steps:

[0010] (1) Terminal pins are stamped and bent into one piece:

[0011] (1.1) Punching inner pre-cut grooves: Punching out several inner pre-cut grooves on the sheet;

[0012] (1.2) Stamping terminal pins: a plurality of terminal pins are respectively stamped out on the sheet corresponding to each inner pre-cut groove position to obtain an array terminal pin group corresponding to the plurality of inner pre-cut grooves, and an inner connecting rod and an outer connecting rod are formed on both sides of the sheet to connect the array terminal pin group together;

[0013] (1.3) Punching external pre-cut grooves: Punching a plurality of external pre-cut grooves on the side of the array terminal pin group close to the external connecting rod, and forming an external pre-cut groove on each terminal pin of the terminal pin group;

[0014] (1.4) Stamping and bending: stamping and bending the array terminal pin group at the same time, and forming a first bending portion on each terminal pin, and the first bending portion is formed between the inner pre-cut groove and the outer pre-cut groove to form a semi-finished product;

[0015] (2) Injection molding plastic shell: The semi-finished products are symmetrically arranged in pairs, and a plurality of plastic shells are formed by injection molding on the symmetrically arranged semi-finished products, and each plastic shell is formed on the first bending portion of the two groups of terminal pin groups on the two symmetrically arranged semi-finished products, and an outer terminal pin group and an inner terminal pin group are formed on the plastic shell, the outer terminal pin group is connected to the outer connecting rod, and the inner terminal pin group is connected to the inner connecting rod;

[0016] (3) Bending and cutting the external connecting rod to form an integrated body: the external terminal pin group is simultaneously stamped and bent, and a second bending portion and a third bending portion are formed on each external terminal pin, and the second bending portion and the third bending portion are formed between the first bending portion and the external pre-cut groove; at the same time, the external connecting rod is cut off along the external pre-cut groove;

[0017] (4) electroplating: electroplating the surfaces of the outer terminal pin group and the inner terminal pin group so that metal protective layers are formed on the outer surfaces of the outer terminal pin group and the inner terminal pin group respectively;

[0018] (5) Remove the inner connecting rod to obtain the finished product: Place the whole into the jig track and position it well, break off the inner connecting rod along the inner pre-cut groove, and separate the inner connecting rod from the inner terminal pin group on the plastic shell to obtain several network filter shells with metal terminal pins.

[0019] As a further improvement of the present invention, in the step (1.1): a number of corresponding pre-cut half grooves are punched out on the upper and lower surfaces of the sheet respectively, and each two corresponding pre-cut half grooves on the upper and lower surfaces of the sheet form an inner pre-cut groove.

[0020] As a further improvement of the present invention, the step (1.2) comprises the following steps:

[0021] (1.2.1) First, punch out a number of inner terminal pins on the sheet corresponding to each inner pre-cut groove position;

[0022] (1.2.2) A number of outer terminal pins corresponding to and connected to the inner terminal pins are then punched out on the sheet to form an array terminal pin group.

[0023] As a further improvement of the present invention, in the step (1.2.1), when punching out a plurality of inner terminal pins, a wire hanging groove is formed on both sides of the plurality of inner terminal pins close to the inner pre-cut groove.

[0024] As a further improvement of the present invention, in the step (1.3), a tin climbing slope is formed on the inner side of the outer pre-cut groove away from the outer connecting rod.

[0025] As a further improvement of the present invention, in the step (4), metal nickel or metal tin is electroplated on the surface of the outer terminal pin group and the inner terminal pin group.

[0026] As a further improvement of the present invention, a baking step is further included between step (2) and step (3), wherein the baking step is performed at a temperature of 135° C. to 145° C. for 2 h to 3 h.

[0027] As a further improvement of the present invention, after the baking step, a burr treatment step is performed: the baked semi-finished product is placed in the track of the sandblasting machine, the conveyor belt is opened and the sandblasting gun head is adjusted to align with the burr portion of the semi-finished product to be treated; the air pressure switch of the sandblasting gun head is turned on, and the air pressure is adjusted to 25-35KG; the sand suction machine is turned on, and then the conveyor belt and the sandblasting air pressure are turned on to perform sandblasting to remove the burrs.

[0028] The network filter housing processed by implementing the above method is characterized in that it includes a plastic shell and two groups of terminal pin groups arranged on opposite sides of the plastic shell, wherein the terminal pin group is composed of a plurality of terminal pins arranged in parallel, each terminal pin is mainly composed of an outer terminal pin and an inner terminal pin connected as one body, and a first bending portion embedded in the plastic shell is formed between the outer terminal pin and the inner terminal pin, a second bending portion and a third bending portion are formed on the outer terminal pin and located on the outside of the plastic shell; and an offset pin is formed on the first bending portion.

[0029] As a further improvement of the present invention, a welding end is formed at the end of the pin of the external terminal, and a tin climbing slope is formed on the welding end.

[0030] As a further improvement of the present invention, wire hanging grooves are respectively formed on two opposite sides of the inner terminal pins.

[0031] As a further improvement of the present invention, a cutting groove is formed on the lower end surface of the plastic shell corresponding to the positions of the two groups of terminal pins, and the cutting groove is located between the outer terminal pins and the inner terminal pins.

[0032] As a further improvement of the present invention, a wire management groove is formed on the inner side surface of the plastic shell at positions corresponding to the inner terminal pins.

[0033] As a further improvement of the present invention, half of a retaining wall is formed at both ends of the plastic shell.

[0034] The beneficial effects of the present invention are:

[0035] (1) The processing method of the network filter housing of the present invention can form the terminal pins and the bending structure at one time through a set of stamping dies and a single process, which greatly simplifies the process and improves the processing efficiency.

[0036] (2) The array terminal pin group is connected together by forming an inner connecting rod and an outer connecting rod, so that the array terminal pin group can be processed simultaneously in various processes, thereby improving processing efficiency and product quality. Specifically, the connecting function of the outer connecting rod connects several terminal pins of the terminal pin group together, so that the plastic shell can be injection molded on two relatively arranged groups of terminal pins; the connecting function of the inner connecting rod can improve the strength and firmness of the terminal pins in the entire semi-finished product, and prevent the terminal pins from being bent and deformed; and the function of the inner connecting rod is to connect several terminal pins on the outer shell, conduct electricity to several terminal pins through the inner connection, and electroplate the metal plating protective layer around the terminal pins.

[0037] (3) Placing the electroplating process after the terminal pin bending and outer connecting rod cutting processes can not only ensure that the protective layer is plated on the surface of the terminal pin, but also prevent the electroplating protective layer from being damaged, thereby ensuring the quality of the entire product and facilitating the subsequent customer to firmly solder the terminal pin of the product on the PCB board.

[0038] (4) The network filter housing of the present invention has a reasonable structural design, which is not only conducive to the smooth and rapid subsequent winding and improves work efficiency; but also, when it is subsequently soldered to the PCB board, it can smoothly crawl tin to wrap the welding end, improve the welding firmness, prevent the occurrence of cold solder joints, ensure good conductivity, and improve product safety performance.

[0039] The above is an overview of the technical solution of the invention. The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 is a flow chart of the present invention;

[0041] Figure 2 This is a schematic diagram of the structure of step (1.1) of the present invention;

[0042] Figure 3 This is a schematic diagram of the structure of step (1.2.1) of the present invention;

[0043] Figure 4 This is a schematic diagram of the structure of step (1.2.2) of the present invention;

[0044] Figure 5 This is a schematic diagram of the structure of step (1.3) of the present invention;

[0045] Figure 6 This is a schematic diagram of the structure of step (1.4) of the present invention;

[0046] Figure 7 This is a schematic diagram of the structure of step (2) of the present invention;

[0047] Figure 8 This is a schematic diagram of the structure of step (3) of the present invention;

[0048] Fig. 9 It is a front structural schematic diagram of the network filter housing in the present invention;

[0049] Fig.10 It is a schematic diagram of the back structure of the network filter housing in the present invention. DETAILED DESCRIPTION

[0050] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings and preferred embodiments.

[0051] Please refer to Figure 1 The embodiment of the present invention provides a method for processing a network filter housing, comprising the following steps:

[0052] (1) Terminal pins are stamped and bent into one piece:

[0053] (1.1) Punching inner pre-cut grooves: Punch out several inner pre-cut grooves 11 on the sheet 1. The sheet 1 can be made of copper sheet, such as Figure 2 As shown;

[0054] (1.2) Stamping terminal pins: A plurality of terminal pins 120 are respectively stamped out on the sheet 1 corresponding to each inner pre-cut groove 11 to obtain an array terminal pin group 12 corresponding to the plurality of inner pre-cut grooves 11, and an inner connecting rod 13 and an outer connecting rod 14 are formed on both sides of the sheet 1 to connect the array terminal pin group 12 together. Figure 3 and Figure 4 As shown;

[0055] (1.3) Punching external pre-cut grooves: A plurality of external pre-cut grooves 15 are punched out on the array terminal pin group 12 near the outer connecting rod 14, and an external pre-cut groove 15 is formed on each terminal pin 120 of the terminal pin group 12. Figure 5 As shown;

[0056] (1.4) Stamping and bending: The array terminal pin group 12 is simultaneously stamped and bent, specifically 90°, and a first bending portion 16 is formed on each terminal pin 120, and the first bending portion 16 is formed between the inner pre-cut groove 11 and the outer pre-cut groove 15, forming a semi-finished product, such as Figure 6 As shown;

[0057] (2) Injection molding plastic shell: The semi-finished products 10 are symmetrically arranged in pairs, and a plurality of plastic shells 2 are formed by injection molding on the symmetrically arranged semi-finished products 10, and each plastic shell 2 is formed on the first bending portion 16 of the two groups of terminal pin groups 12 on the two symmetrically arranged semi-finished products 10, and an outer terminal pin group 121 and an inner terminal pin group 122 are formed on the plastic shell 2, the outer terminal pin group 121 is connected to the outer connecting rod 14, and the inner terminal pin group 122 is connected to the inner connecting rod 13, such as Figure 7 As shown;

[0058] (3) Bending and cutting the outer connecting rod to form an integrated body: The outer terminal pin group 121 is simultaneously stamped and bent, and a second bending portion 17 and a third bending portion 18 are formed on each outer terminal pin, and the second bending portion 17 and the third bending portion 18 are formed between the first bending portion 16 and the outer pre-cut groove 15; at the same time, the outer connecting rod 14 is cut off along the outer pre-cut groove 15, such as Figure 8 As shown;

[0059] (4) Electroplating: Electroplating is performed on the surfaces of the outer terminal pin group 121 and the inner terminal pin group 122 so that metal protective layers are formed on the outer surfaces of the outer terminal pin group 121 and the inner terminal pin group 122 respectively; specifically, metal nickel or metal tin is electroplated on the surfaces of the outer terminal pin group 121 and the inner terminal pin group 122.

[0060] (5) Remove the inner connecting rod to obtain the finished product: Place the whole into the jig track and position it well. Break off the inner connecting rod along the inner pre-cut groove. The inner connecting rod is separated from the inner terminal pin group on the plastic shell to obtain several network filter shells with metal terminal pins, such as Fig. 9 As shown;

[0061] (6) Full inspection: The appearance of the plastic shell and terminal pins of the network filter housing are inspected simultaneously. After the full inspection, several network filter housings are pushed into the blister tube for packaging through the jig track to protect the terminal pins and prevent them from being skewed or deformed.

[0062] In this embodiment, before performing step (1), a trimming step is first performed to trim the two side edges of the sheet 1 (i.e., the edges of the subsequent inner connecting rod 13 and the outer connecting rod 14) to ensure smooth feeding of the sheet 1 during stamping, flatness of the sheet 1, and precise dimensions of the ends of the inner connecting rod 13 and the outer connecting rod 14, so that in the subsequent manufacturing process, the terminal pins can be placed in the injection mold and the sealing glue can be precisely positioned.

[0063] This embodiment adopts a double lower mold turntable injection molding machine to perform the injection molding process, and the injection molding efficiency is high.

[0064] In step (1) of this embodiment, after the sheet 1 is placed in a set of stamping dies, the array terminal pin group 12 and the bending structure can be formed after it comes out, that is, the terminal pins and the bending structure can be formed at one time in one process, which greatly simplifies the process and improves the processing efficiency.

[0065] In the step (1.1): a number of corresponding pre-cut half grooves are punched out on the upper and lower surfaces of the sheet 1, and each two corresponding pre-cut half grooves on the upper and lower surfaces of the sheet form an inner pre-cut groove 11. After the terminal pin 120 is subsequently formed, the terminal pin 120 can have pre-cut half grooves on both sides, so that the inner connecting rod 13 can be quickly broken off later.

[0066] The step (1.2) comprises the following steps:

[0067] (1.2.1) First, a plurality of inner terminal pins 1201 are punched out on the sheet 1 corresponding to each inner pre-cut groove 11, such as Figure 3 As shown;

[0068] (1.2.2) A plurality of external terminal pins 1202 are punched out on the sheet 1 to be connected one-to-one with the internal terminal pins 1201, so as to form an array terminal pin group 12, such as Figure 4 shown.

[0069] After forming the array terminal pin group 12 in step (1.2), the array terminal pin group 12 is connected together by the inner connecting rod 13 and the outer connecting rod 14, so that the array terminal pin group 12 can be processed simultaneously in the subsequent processes, thereby improving the processing efficiency and product quality. Specifically, the connecting function of the outer connecting rod 14 connects the plurality of terminal pins 120 of the terminal pin group 12 together, so that the plastic shell can be injection molded on the two relatively arranged groups of terminal pin groups 12; the connecting function of the inner connecting rod 13 can improve the strength and firmness of the terminal pins 120 in the entire semi-finished product, and prevent the terminal pins 120 from being bent and deformed.

[0070] In the step (1.2.1), when punching out a plurality of inner terminal pins 1201, a wire hanging groove 19 is formed on both sides of the plurality of inner terminal pins 1201 near the inner pre-cut groove 11, such as Figure 3 shown.

[0071] In step (1.3) of this embodiment, the outer pre-cut groove is punched out to facilitate the subsequent cutting of the outer connecting rod 14 from the terminal pin group 12.

[0072] At the same time, in the step (1.3), a tin climbing slope 12022 is formed on the inner side of the outer pre-cut groove 15 away from the outer connecting rod 14, such as Figure 7 After the outer connecting rod 14 is cut off, the tin climbing slope 12022 will be exposed at the end of the terminal pin 120. When the client subsequently solders the board, the solder can easily climb the tin climbing slope 12022, thereby improving the solder adhesion.

[0073] Between step (2) and step (3), a baking step is also included, wherein the product is baked at a temperature of 135° C.-145° C. for 2 h-3 h to release the internal stress of the product.

[0074] After the baking step, the burr treatment step is performed: put the baked semi-finished product into the track of the sandblasting machine, open the conveyor belt and adjust the sandblasting gun head to align it with the part of the semi-finished product where the burrs need to be treated; turn on the air pressure switch of the sandblasting gun head and adjust the air pressure to 25-35KG; turn on the sand suction machine, then turn on the conveyor belt and the sandblasting air pressure, and perform sandblasting to remove the burrs.

[0075] In this embodiment, if Figures 6 to 8 As shown, after 10 sets of terminal pin groups 12 are formed on a sheet 1 at one time, 10 plastic shells are formed on two identical sheets 1, which can greatly improve the processing efficiency. After step (5), 10 finished products can be obtained at one time. Of course, the number of finished products formed at one time can be increased or decreased according to specific needs.

[0076] The processing method of the network filter housing of this embodiment can form the terminal pins and the bending structure in one process at one time through a set of stamping dies, which greatly simplifies the process and improves the processing efficiency. At the same time, the array terminal pin group 12 is connected together by forming the inner connecting rod 13 and the outer connecting rod 14, which is convenient for the subsequent simultaneous processing of the array terminal pin group 12, thereby improving the processing efficiency and product quality. Specifically, the connecting function of the outer connecting rod 14 connects several terminal pins 120 of the terminal pin group 12 together, which is convenient for the subsequent injection molding of the plastic shell on the two relatively arranged groups of terminal pin groups 12; the connecting function of the inner connecting rod 13 can improve the strength and firmness of the terminal pins 120 in the entire semi-finished product, and prevent the terminal pins 120 from being bent and deformed. At the same time, placing the electroplating process after the terminal pin bending and the outer connecting rod cutting process can not only ensure that the protective layer is electroplated on the surface of the terminal pin, but also that the electroplating protective layer will not be damaged, thereby ensuring the quality of the entire product, and facilitating the subsequent client to firmly solder the terminal pins of the product on the PCB board.

[0077] The embodiment of the present invention also provides a network filter housing processed by the above method, such as Fig. 9 and Fig.10As shown, it includes a plastic shell 2 and two groups of terminal pin groups 12 arranged on opposite sides of the plastic shell 2, wherein the terminal pin group 12 is composed of a plurality of terminal pins 120 arranged in parallel, each terminal pin 120 is mainly composed of an outer terminal pin 1202 and an inner terminal pin 1201 connected as one body, and a first bending portion 16 embedded in the plastic shell 2 is formed between the outer terminal pin 1202 and the inner terminal pin 1201, and a second bending portion 17 and a third bending portion 18 are formed on the outer terminal pin 1202 and located on the outside of the plastic shell 2.

[0078] In this embodiment, a wire hanging groove 19 is formed on the two opposite sides of the inner terminal pin 1201. At the same time, a wire cutting groove 21 is formed on the lower end surface of the plastic shell 2 corresponding to the positions of the two groups of terminal pins 12, and the wire cutting groove 21 is located between the outer terminal pin 1202 and the inner terminal pin 1201. Because the inner cavity of the plastic shell 2 of the product needs to be arranged with a magnetic core, the magnetic core is wound with enameled wire, and the enameled wire is to be wound in the wire hanging groove 19 of the inner terminal pin 1201. After the enameled wire is wound several times, it is fixed on the inner terminal pin 1201. The wire ends left by the enameled wire wound around each inner terminal pin 1201 are cut off with a blade along the wire cutting groove 21. The setting of the wire cutting groove 21 is conducive to smooth wire cutting, accurate positioning, and improved work efficiency.

[0079] In this embodiment, a welding end 12021 is formed at the end of the external terminal pin 1202, and a tin climbing slope 12022 is formed on the welding end 12021. The welding end 2021 is provided at the end of the external terminal pin 1202, and the tin climbing slope 12022 is formed on the welding end 12021, so that the welding foot of the obtained network filter housing is a welding end of a wedge-shaped structure, so that the housing welding foot is easy to solder when it is soldered to the PCB board, which is conducive to tin climbing along the slope of the wedge-shaped structure (i.e., the tin climbing slope 12022) to wrap the welding end 12021, thereby improving the welding firmness, preventing the occurrence of cold solder joints, ensuring good conductivity, and improving product safety performance.

[0080] In this embodiment, a staggered pin 161 is formed on the first bending portion 16. Figure 5 As shown. The setting of the offset pin 161 is conducive to having sufficient pin spacing space for winding the network filter housing when winding, so as to improve the winding efficiency. At the same time, the setting of the offset pin 161 can prevent the phenomenon of soldering between the two terminal pins when the terminal pins of the network filter housing are soldered, thereby effectively preventing the phenomenon of short circuit.

[0081] In this embodiment, a wire management groove 22 is formed on the inner side surface of the plastic shell 2 at a position corresponding to the inner terminal pins 1201 .

[0082] The arrangement of the cable management slot 22 has the following three advantages:

[0083] (1) It is beneficial for the enameled wire to be wound along the wire management groove 22 and fixed on the wire hanging groove 19 of the inner terminal pin 1201, thereby improving the winding efficiency;

[0084] (2) It is beneficial to isolate the enameled wire from the enameled wire on the previous inner terminal pin 1201 to prevent short circuit;

[0085] (3) It is helpful to shorten the distance between the enameled wire and the inner terminal pin 1201. If the enameled wire is far away from the winding position of the inner terminal pin 1201, the white wire is too long during soldering, which may cause the enameled wire to short-circuit or break.

[0086] At the same time, half retaining walls 23 are formed at both ends of the plastic shell 2. The purpose of setting the half retaining walls 23 is to leave enough space for the terminal pins on the edge of the shell, so as to facilitate the winding of the four terminal pins on the edge and improve the winding efficiency.

[0087] In this embodiment, the upper surface of the plastic shell 2 is a textured surface, which is conducive to clear surface printing; the surrounding side surfaces are smooth; the inner side surface of the lower surface is a textured surface, which is conducive to placing the magnetic core into the inner cavity and fixing it more firmly by gluing.

[0088] At the same time, the front corner and the back corner are formed on the plastic shell 2, which plays a role in positioning in the subsequent processes.

[0089] The network filter housing of the present invention has a reasonable structural design, which is not only conducive to the smooth and rapid subsequent winding and improves work efficiency; but also, when it is subsequently welded to a PCB board, it can smoothly crawl tin to wrap the welding end, improve the welding firmness, prevent the occurrence of cold solder joints, ensure good conductivity, and improve product safety performance.

[0090] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, other structures obtained by adopting the same or similar technical features as the above-mentioned embodiments of the present invention are within the protection scope of the present invention.

Claims

1. A method for processing a network filter housing, characterized in that: The following steps are involved: (1) Terminal pins are stamped and bent into one piece: (1.1) Punching inner pre-cut grooves: Punching out several inner pre-cut grooves on the sheet; (1.2) Stamping terminal pins: A plurality of terminal pins are respectively stamped out on the sheet corresponding to each inner pre-cut groove position to obtain an array terminal pin group corresponding to the plurality of inner pre-cut grooves, and an inner connecting rod and an outer connecting rod are formed on both sides of the sheet to connect the array terminal pin group together; (1.3) Punching external pre-cut grooves: A plurality of external pre-cut grooves are punched out on the side of the array terminal pin group close to the external connecting rod, and one external pre-cut groove is formed on each terminal pin of the terminal pin group; (1.4) Stamping and bending: stamping and bending the array terminal pin group at the same time, and forming a first bending portion on each terminal pin, and the first bending portion is formed between the inner pre-cut groove and the outer pre-cut groove to form a semi-finished product; (2) Injection molding plastic shell: The semi-finished products are symmetrically arranged in pairs, and a plurality of plastic shells are formed by injection molding on the symmetrically arranged semi-finished products, and each plastic shell is formed on the first bending portion of the two groups of terminal pin groups on the two symmetrically arranged semi-finished products, and an outer terminal pin group and an inner terminal pin group are formed on the plastic shell, the outer terminal pin group is connected to the outer connecting rod, and the inner terminal pin group is connected to the inner connecting rod; (3) Bending and cutting the external connecting rod to form an integrated body: the external terminal pin group is simultaneously stamped and bent, and a second bending portion and a third bending portion are formed on each external terminal pin, and the second bending portion and the third bending portion are formed between the first bending portion and the external pre-cut groove; at the same time, the external connecting rod is cut off along the external pre-cut groove; (4) Electroplating: Electroplating is performed on the surface of the outer terminal pin group and the inner terminal pin group so that a metal protective layer is formed on the outer surface of the outer terminal pin group and the inner terminal pin group respectively; (5) Remove the inner connecting rod to obtain the finished product: Place the whole into the jig track and position it well, break off the inner connecting rod along the inner pre-cut groove, and separate the inner connecting rod from the inner terminal pin group on the plastic shell to obtain several network filter shells with metal terminal pins.

2. The method for processing a network filter housing according to claim 1, characterized in that: In the step (1.1): a number of corresponding pre-cut half grooves are punched out on the upper and lower surfaces of the sheet respectively, and each two corresponding pre-cut half grooves on the upper and lower surfaces of the sheet form an inner pre-cut groove.

3. The method for processing a network filter housing according to claim 1, characterized in that: The step (1.2) comprises the following steps: (1.2.1) First, punch out a number of inner terminal pins on the sheet corresponding to each inner pre-cut groove position; (1.2.2) A number of outer terminal pins are then punched out on the sheet to be connected one-to-one with the inner terminal pins, forming an array terminal pin group.

4. The method for processing a network filter housing according to claim 3, characterized in that: In the step (1.2.1), when punching out a plurality of inner terminal pins, a wire hanging groove is formed on both sides of the plurality of inner terminal pins near the inner pre-cut groove.

5. The method for processing a network filter housing according to claim 1, characterized in that: In the step (1.3), a tin climbing slope is formed on the inner side of the outer pre-cut groove away from the outer connecting rod.

6. The method for processing a network filter housing according to claim 1, characterized in that: In the step (4), metal nickel or metal tin is electroplated on the surface of the outer terminal pin group and the inner terminal pin group.

7. The method for processing a network filter housing according to claim 1, characterized in that: Between step (2) and step (3), a baking step is also included, wherein the baking step is performed at a temperature of 135° C. to 145° C. for 2 h to 3 h.

8. The method for processing a network filter housing according to claim 7, characterized in that: After the baking step, the burr treatment step is performed: put the baked semi-finished product into the track of the sandblasting machine, open the conveyor belt and adjust the sandblasting gun head to align it with the part of the semi-finished product where the burrs need to be treated; turn on the air pressure switch of the sandblasting gun head and adjust the air pressure to 25-35KG; Turn on the sand suction machine, then turn on the conveyor belt and the sandblasting air pressure, and perform sandblasting to remove burrs.