Positive electrode active material, preparation method thereof and lithium secondary battery containing the same
By controlling the area of plate-like particles on the secondary particle surface and the pH conditions in the co-precipitation reaction in the positive active material, the problem of low thermal stability of the layered material is solved, and a positive active material with high nickel concentration and high output characteristics is achieved. , improving the thermal stability of the battery and the electrolyte decomposition reaction.
Patent Information
- Application Number
- CN201980074470.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-09-16
AI Technical Summary
Existing layered cathode active materials are prone to structural collapse during charging and discharging, and have low thermal stability. The increase in Ni content in the ternary NCM system leads to reduced thermal stability, making it difficult to commercialize.
By controlling the primary particle structure on the surface of the secondary particles, ensuring that the area of the plate-shaped particles on its surface is greater than or equal to 20% to 100%, and adjusting the pH conditions in the co-precipitation reaction to form a positive active material with a high nickel concentration and inhibit electrolysis Liquid side reactions.
The thermal stability of the positive active material is improved, the electrolyte decomposition reaction is reduced, and the thermal stability and nickel concentration of the battery are enhanced, thereby improving the output characteristics of the battery.
Smart Images

Figure CN112997338B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material, a preparation method thereof and a lithium secondary battery comprising the same. Background Art
[0002] In recent years, with the explosive growth in demand for IT mobile devices and small electric drive devices (electric bicycles, small EVs, etc.) and the increasing demand for electric vehicles with a range of more than 400 km, research and development of secondary batteries with high capacity and high energy density are actively carried out worldwide.
[0003] In order to prepare such a high-capacity battery, a high-capacity positive electrode material is required.
[0004] Among existing layered cathode active materials, the one with the highest capacity is LiNiO2 (275 mAh / g), but it is prone to structural collapse during charge and discharge, and has low thermal stability due to oxidation number problems, making it difficult to commercialize in practice.
[0005] In order to solve this problem, the unstable Ni sites must be replaced by other stable transition metals (Co, Mn, etc.). For this purpose, a ternary NCM system substituted with Co and Mn was developed.
[0006] However, for the ternary NCM system, the thermal stability decreases as the Ni content increases. Summary of the invention
[0007] Technical issues
[0008] Therefore, the present inventors have proposed a method for suppressing the decomposition reaction of the electrolyte on the positive electrode surface by controlling the structure of the primary particles on the surface of the layered secondary particles. This can improve the thermal stability of the positive electrode active material.
[0009] Technical Solution
[0010] One embodiment of the present invention provides a positive electrode active material, which is a lithium metal oxide particle in the form of a secondary particle including a primary particle, wherein the surface of the secondary particle includes a plate-like primary particle whose narrow angle between the c-axis of the primary particle and the straight line connecting the virtual point of the center of the primary particle and the center point of the secondary particle is 60° to 90°.
[0011] The surface of the secondary particles refers to the portion of the secondary particles consisting of the outermost primary particles.
[0012] Figure 1 is a schematic diagram of a secondary particle according to one embodiment of the present invention.
[0013] like Figure 1As shown, in order to define the direction of primary particle arrangement, the plate-like primary particles are defined as plate-like particles whose narrow angle is 60° to 90° between the c-axis of the primary particle and the straight line connecting the virtual point at the center of the primary particle and the center point of the secondary particle. More specifically, it can be 70° to 90°.
[0014] In addition, the primary particles whose angle is greater than or equal to 0° and less than 60° are defined as needle-shaped. More specifically, the primary particles whose angle is greater than or equal to 0° and less than or equal to 20° may be needle-shaped.
[0015] Due to the plate-like particles on the surface of the secondary particles, a side reaction with an electrolyte can be suppressed, thereby improving the thermal stability of the positive electrode active material.
[0016] More specifically, the area occupied by the plate-like primary particles may be greater than or equal to 20% by area, more specifically, greater than or equal to 30% by area, relative to 100% by area of a circle defined by a center point of the secondary particle and 50% by radius of the secondary particle.
[0017] Specifically, Figure 2 is a SEM picture of secondary particles according to one embodiment of the present invention.
[0018] like Figure 2 As shown, after setting a circle with the center of the secondary particle as a reference, the area of the plate-like primary particle inside the circle can be calculated.
[0019] At this time, if Figure 2 As shown, the area occupied by the plate-like primary particles may be greater than or equal to 20 area%. In this case, as described above, the side reaction with the electrolyte can be effectively suppressed. It is further preferred that it is greater than or equal to 50 area%, and more preferably greater than or equal to 70 area%. As an upper limit, 100 area% of the total area may be plate-like particles, but in fact, there are some needle-like particles, so there may be less than or equal to 95 area% of plate-like particles.
[0020] The average length of the plate-like primary particles present in the area may be 750 nm to 1.25 μm relative to 100 area % of an area formed by a circle based on a center point of the secondary particle to 50% of the radius of the secondary particle.
[0021] The length of the plate-like primary particles refers to the length of the longest direction of the particles. When the average length of the primary particles satisfies the above range, target battery characteristics can be ensured.
[0022] In addition, the interior of the secondary particle may include a needle-shaped primary particle whose narrow angle between the c-axis of the primary particle and the straight line connecting the virtual point at the center of the primary particle and the center point of the secondary particle is greater than or equal to 0° and less than 60°. More specifically, the needle-shaped primary particle may be 0° to 20°.
[0023] More specifically, the interior of the secondary particle may be a radial structure in which needle-shaped particles are arranged toward the center of the secondary particle.
[0024] This internally oriented structure develops when there is a concentration gradient in which the nickel concentration in the secondary particles decreases from the inside to the surface.
[0025] Even in such a case, the core at the central part of the secondary particle may include a central part having a constant nickel concentration. This can be appropriately controlled by the mixing method of the raw material materials in the precursor preparation step described later.
[0026] More specifically, the nickel content of the metal in the secondary particles may be greater than or equal to 80 mol %. In order to obtain high output characteristics that cannot be obtained in the existing positive electrode active material having a nickel content of less than or equal to 50 mol %, the nickel concentration may be increased.
[0027] In another embodiment of the present invention, a method for preparing a positive electrode active material is provided, which comprises: a step of adding a metal salt aqueous solution to a coprecipitation reactor to obtain a metal precursor; and a step of mixing the metal precursor and a lithium raw material and then calcining to obtain a positive electrode active material. In the step of adding a metal salt aqueous solution to the coprecipitation reactor to obtain a metal precursor, the pH conditions are changed in the range of 1 hour % to 30 hour % at the end time of the reaction, relative to the total reaction time of 100 hour %.
[0028] More specifically, a method for changing the pH at the reaction end time point in the step of obtaining a precursor by a coprecipitation reaction may be provided. In this case, the reaction end time point may refer to 1 hour % to 30 hour % from the last end time in 100 hour % of the total reaction time.
[0029] More specifically, the reaction end time point may refer to 1 hour % to 10 hour % or 1 hour % to 5 hour % from the final end time in 100 hour % of the total reaction time.
[0030] This may affect the formation of the surface plate-like primary particles of the positive electrode active material of one embodiment of the present invention described above, which can be appropriately controlled to meet the desired specifications.
[0031] Specifically, the difference between the reaction start pH and the reaction end pH of the step of adding the metal salt aqueous solution to obtain the metal precursor in the coprecipitation reactor may be 0.1 to 0.8. Two steps including a narrower range are also described.
[0032] More specifically, the pH condition may be adjusted upward by 0.1 to 0.8 within the range of 1 to 30 hours at the end of the reaction relative to the total reaction time of 100 hours. When such a range is satisfied, plate-like particles existing on the surface of the secondary particles may be uniformly formed.
[0033] More specifically, the pH condition can be increased at a rate of 0.0016 pH / min to 0.0133 pH / min, more specifically, at a rate of 0.0066 pH / min to 0.0133 pH / min.
[0034] Such process conditions will be described in more detail in the following examples.
[0035] In another embodiment of the present invention, a lithium secondary battery is provided, which includes: a positive electrode, which includes the positive electrode active material according to one embodiment of the present invention; a negative electrode, which includes the negative electrode active material; and an electrolyte located between the positive electrode and the negative electrode.
[0036] The description of the positive electrode active material is the same as that of the aforementioned embodiment of the present invention, and thus will not be repeated herein.
[0037] The positive active material layer may include a binder and a conductive material.
[0038] The binder plays a role in allowing the positive electrode active material particles to be well bonded to each other and allowing the positive electrode active material to be well bonded to the current collector.
[0039] The conductive material is used to impart conductivity to the electrode, and any conductive material may be used as long as it does not cause chemical changes in the constituted battery.
[0040] The negative electrode includes a current collector and a negative electrode active material layer formed on the current collector, wherein the negative electrode active material layer includes a negative electrode active material.
[0041] As the negative electrode active material, a material capable of reversibly inserting / deinserting lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide may be used.
[0042] As the material capable of reversibly inserting and extracting lithium ions, any carbon-based negative electrode active material generally used as a carbon material in lithium ion secondary batteries can be used, and as a typical example thereof, crystalline carbon, amorphous carbon, or a combination thereof can be used.
[0043] As the alloy of the lithium metal, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.
[0044] Examples of the material capable of lithium doping and dedoping include Si, SiO x (0<x<2), Si-Y alloy (the Y is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements and combinations thereof, but not Si), Sn, SnO2, Sn-Y (the Y is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements and combinations thereof, but not Sn), etc.
[0045] Examples of the transition metal oxide include vanadium oxide, lithium vanadium oxide, etc. The negative electrode active material layer also includes a binder and may further include a conductive material.
[0046] The binder plays a role in allowing negative electrode active material particles to be well bonded to each other and allowing the negative electrode active material to be well bonded to the current collector.
[0047] The conductive material is used to impart conductivity to the electrode, and any conductive material may be used as long as it does not cause chemical changes in the constituted battery.
[0048] As the current collector, a material selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer material coated with a conductive metal, and a combination thereof may be used.
[0049] For the negative electrode and the positive electrode, an active material, a conductive material and a binder are mixed in a solvent to prepare an active material composition, and the composition is coated on a current collector to prepare the negative electrode and the positive electrode. Such an electrode preparation method is well known in the art, so a detailed description is omitted in this specification. As the solvent, N-methylpyrrolidone and the like can be used, but it is not limited thereto.
[0050] The electrolyte includes a nonaqueous organic solvent and a lithium salt.
[0051] The nonaqueous organic solvent functions as a medium through which ions participating in the electrochemical reaction of the battery can migrate.
[0052] The lithium salt is a material that functions as a lithium ion source in a battery when dissolved in an organic solvent, thereby ensuring the basic operation of a lithium secondary battery and promoting the migration of lithium ions between a positive electrode and a negative electrode.
[0053] Depending on the type of lithium secondary battery, a separator may also be present between the positive electrode and the negative electrode. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride or a multilayer film of at least two layers thereof may be used, and of course mixed multilayer films such as polyethylene / polypropylene two-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, polypropylene / polyethylene / polypropylene three-layer separators, etc. may be used.
[0054] For lithium secondary batteries, according to the types of separators and electrolytes used, they can be divided into lithium ion batteries, lithium ion polymer batteries and lithium polymer batteries. According to the shape, they can be divided into cylindrical, prismatic, button-shaped, and pouch-shaped. According to the size, they can be divided into block type and thin film type. The structure and preparation method of these batteries are well known in the field, so they will not be described in detail.
[0055] Effects of the Invention
[0056] According to the positive electrode active material of one embodiment of the present invention, the plate-shaped surface with low reactivity is in contact with the electrolyte, whereby the decomposition reaction of the electrolyte on the positive electrode surface can be suppressed.
[0057] As such side reactions of the electrolyte are reduced, the thermal stability of the positive electrode active material is improved.
[0058] More specifically, the peak temperature during DSC analysis increases, the total calorific value decreases, and a positive electrode active material having improved thermal stability can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 is a schematic diagram of a secondary particle according to one embodiment of the present invention.
[0060] Figure 2 This is the shape of the primary particles present in the surface portion of the positive electrode active material of Example 1.
[0061] Figure 3 This is the shape of the primary particles present in the surface portion of the positive electrode active material of Example 3.
[0062] Figure 4 This is the shape of the primary particles present in the surface portion of the positive electrode active material of Comparative Example 1.
[0063] Figure 5 is the cross-sectional shape of the positive electrode active material of Example 1, Figure 6 is the cross-sectional shape of the positive electrode active material of Example 3, Figure 7 This is the cross-sectional shape of the positive electrode active material of Comparative Example 1. DETAILED DESCRIPTION
[0064] Hereinafter, embodiments of the present invention will be described in detail. However, the following embodiments are examples only, and the present invention is not limited to the embodiments described herein, and the scope of the present invention is subject to the claims.
[0065] (Example 1) Preparation of positive electrode active material containing 88 mol% Ni
[0066] 1) Preparation of metal salt solution
[0067] First, NiSO4.6H2O is used as a nickel raw material, CoSO4.7H2O is used as a cobalt raw material, and MnSO4.H2O is used as a manganese raw material to prepare two metal salt aqueous solutions having different concentrations of Ni, Co, and Mn.
[0068] For the first metal salt aqueous solution for forming the core, the raw materials are mixed in distilled water to satisfy (Ni 0.98 Co 0.01 Mn 0.01 )(OH)2 in a stoichiometric molar ratio.
[0069] Separately, for the second metal salt aqueous solution for forming the shell, the raw materials are mixed in distilled water to satisfy (Ni 0.64 Co 0.23 Mn 0.13 )(OH)2 in a stoichiometric molar ratio.
[0070] 2) Co-precipitation process
[0071] A co-precipitation reactor having two metal salt aqueous solution supply tanks connected in series is prepared, and each metal salt aqueous solution supply tank is filled with the first metal salt aqueous solution and the second metal salt aqueous solution.
[0072] After distilled water is put into the coprecipitation reactor, the temperature of the reactor is maintained constant and stirring is performed.
[0073] In addition, NH4(OH) was used as a chelating agent, and a NaOH solution was used as a pH adjuster.
[0074] At this time, the initial pH in the reactor undergoing the reaction was set to 11.2.
[0075] In the reactor in which the pH is thus kept constant and the chelating agent is supplied, the addition time and amount of each metal salt solution supplied from the two metal salt aqueous solution supply tanks connected in series are adjusted.
[0076] Specifically, the first metal salt aqueous solution is added at a rate of 0.4 liters / hour, and the coprecipitation reaction is carried out until the diameter of the precipitate reaches about 11.1 μm. At this time, by adjusting the flow rate, the average residence time of the solution in the reactor is about 10 hours. After the reaction reaches a normal state, the reactant is given a normal state duration to obtain a coprecipitated compound with a higher density.
[0077] Next, the mixing ratio of the first metal salt aqueous solution and the second metal salt aqueous solution was changed, and the total supply solution was added at a rate of 0.4 liters / hour, while the supply rate of the first metal salt aqueous solution was gradually reduced to 0.05 liters / hour, and the supply rate of the second metal salt aqueous solution was gradually increased to 0.35 liters / hour. At this time, by adjusting the flow rate, the average residence time of the solution in the reactor was within 20 hours, and the final coprecipitation reaction was carried out until the diameter of the precipitate reached 16.0 μm.
[0078] At this time, the pH was adjusted upward to the range of 12.0 1 hour before the end of the reaction, and the pH adjustment rate was 0.0133 pH / min.
[0079] 3) Post-processing process
[0080] The precipitate obtained according to the series of coprecipitation processes was filtered, washed with water, and dried in an oven at 100° C. for 24 hours to prepare particles having a composition of (Ni 0.88 Co 0.095 Mn 0.025 )(OH)2 and an active material precursor of large-size particles with an average particle size of 16.0 μm.
[0081] 4) Calcination process
[0082] There will be a core-shell concentration gradient and Ni 0.88 Co 0.095 Mn 0.025 The precursor of the (OH)2 component was uniformly mixed with ZrO2 (Aldrich, 4N, Zr concentration was 3400ppm) and Al(OH)3 (Aldrich, 4N, Al concentration was 140ppm), and then LiOH·H2O (Samchun Chemical, battery grade) was remixed in a molar ratio of 1:1.05, and then charged into a furnace and oxygen was introduced for calcination.
[0083] The resulting product was then naturally cooled, and the positive electrode active material was prepared by pulverizing and classifying.
[0084] (Example 2) Preparation of positive electrode active material containing 88 mol% Ni
[0085] The positive electrode active material was prepared by the same method as in Example 1, except for the following points: when preparing the raw material, the raw material was made to satisfy (Ni 0.88 Co 0.095 Mn 0.025 )(OH)2 molar ratio; in the co-precipitation process, the reaction start pH is adjusted to 11.2 during the reaction, and the pH is increased to 11.8 range 1 hour before the end of the reaction; and the pH adjustment rate is adjusted to 0.01pH / minute.
[0086] (Example 3) Preparation of positive electrode active material containing 88 mol% Ni
[0087] The positive electrode active material was prepared by the same method as Example 2, except for the following points: in the coprecipitation process, the reaction start pH was adjusted to 11.2 during the reaction, and the pH was adjusted to 11.6 range 1 hour before the end time of the reaction; and the pH adjustment rate was adjusted to 0.0066 pH / minute.
[0088] (Example 4) Preparation of positive electrode active material containing 88 mol% Ni
[0089] The positive electrode active material was prepared by the same method as Example 2, except for the following points: in the coprecipitation process, the reaction start pH was adjusted to 11.2 during the reaction, and the pH was adjusted to 11.4 range 1 hour before the end time of the reaction; and the pH adjustment rate was adjusted to 0.0033 pH / minute.
[0090] (Comparative Example 1) Preparation of positive electrode active material containing 88 mol% Ni
[0091] A positive electrode active material was prepared by the same method as in Example 2, except that the pH was maintained at 11.0 during the reaction in the coprecipitation process.
[0092] [Table 1]
[0093]
[0094] (Experimental Example 1) SEM analysis of the surface of the positive electrode active material
[0095] For the positive electrode active materials of Example 1, Example 3 and Comparative Example 1, the shapes of primary particles on the surface of the positive electrode active materials were observed by SEM analysis.
[0096] Figure 2This is the shape of the primary particles present in the surface portion of the positive electrode active material of Example 1, and it was confirmed that the plate-like primary particles uniformly covered the entire surface portion of the positive electrode active material. The plate-like surface (c-axis surface) of the primary particle is a surface where Li deintercalation / intercalation reactions do not occur, and it is expected that the electrolyte decomposition reaction will be suppressed on the positive electrode surface.
[0097] Figure 3 This is the shape of the primary particles existing in the surface portion of the positive electrode active material of Example 3, and the plate-like primary particles and the needle-like particles coexist in the surface portion of the positive electrode active material.
[0098] Figure 4 This is the shape of the primary particles present in the surface portion of the positive electrode active material of Comparative Example 1, and the needle-shaped primary particles are uniformly distributed. This is similar to the shape observed when a positive electrode active material is usually prepared.
[0099] (Experimental Example 2) Analysis of the cross-sectional shape of the positive electrode active material (TEM)
[0100] The positive electrode active materials of Example 1, Example 3 and Comparative Example 1 were cut into positive electrode material cross sections using FIB, and the primary particle shape distribution of the positive electrode material cross sections was observed using a TEM analysis device.
[0101] Figure 5 is the cross-sectional shape of the positive electrode active material of Example 1, Figure 6 is the cross-sectional shape of the positive electrode active material of Example 3, Figure 7 This is the cross-sectional shape of the positive electrode active material of Comparative Example 1.
[0102] As for the arrangement of primary particles inside the positive electrode active material, many needle-shaped particles can be seen in Example 1, Example 3, and Comparative Example 1, and the needle-shaped particles are arranged radially toward the center of the secondary particles.
[0103] However, as for the arrangement of primary particles on the surface of the positive electrode active material, Comparative Example 1 exhibited a needle-like shape similar to the inside, but in Example 3, it was confirmed that primary particles in a plate-like shape and primary particles in a needle-like shape coexisted.
[0104] It can be confirmed that the positive electrode active material of Example 1 has more plate-like particles.
[0105] How much area the primary particles having a plate-like shape in the surface portion of the positive electrode active materials of Examples 1 to 4 and Comparative Example 1 occupied within the surface portion was investigated.
[0106] This was confirmed by the following method.
[0107] like Figure 2As shown, based on the SEM image of the secondary particles, the area occupied by the plate-like particles was calculated relative to 100 area % of the area formed by a circle from the center point of the secondary particle to 50% of the radius of the secondary particle.
[0108] [Table 2]
[0109]
[0110] (Experimental Example 3) Differential Scanning Calorimetry (DSC) in Charged State
[0111] After button cells were prepared using the positive electrode active materials of Examples 1 to 4 and Comparative Example 1 and charged, the button cells were disassembled and the thermal stability of the positive electrode active materials was analyzed by DSC.
[0112] The slurry used for the plate is positive electrode: conductive material (Denka black): binder (PVDF, KF1100) = 92.5:3.5:4% by weight, and NMP (N-methyl-2-pyrrolidone) is added to make the solid content reach about 30% to adjust the slurry viscosity.
[0113] The prepared slurry was coated on an aluminum foil having a thickness of 15 μm by a doctor blade method, and then dried and pressed.
[0114] The electrode loading is 14.6 mg / cm 2 , compacted density is 3.1g / cm 3 The electrolyte used was a solution of 1M LiPF6 in ethylene carbonate: dimethyl carbonate: ethyl methyl carbonate = 3:4:3 (volume %), and a button cell was prepared using a polypropylene separator and a lithium negative electrode (200um, Bencheng Metal). The charging conditions were CC / CV 2.5~4.25V, 1 / 20C cut-off charging conditions.
[0115] Then, the button cell was removed from the dried product and 10 mg of the positive electrode active material was collected for DSC analysis.
[0116] In DSC analysis, the temperature was raised from 25°C to 400°C at 5°C / min, and the on-set temperature at which the exothermic reaction starts, the peak temperature at which the heat generation is maximum (Max), and the total heat generation were analyzed. The results are shown in Table 3 below.
[0117] (Experimental Example 4) Evaluation of electrochemical characteristics
[0118] After the positive electrode active materials of Examples 1 to 4 and Comparative Example 1 were used to prepare 2032 button-type half-cells in the same manner as in Experimental Example 3, they were aged at room temperature (25° C.) for 10 hours and then subjected to charge and discharge tests.
[0119] For capacity evaluation, 215 mAh / g was used as the reference capacity, and the charge and discharge conditions were CC / CV 2.5-4.25V, 1 / 20C cut-off. The initial capacity was evaluated under 0.2C charge / 0.2C discharge conditions.
[0120] [Table 3]
[0121]
[0122] As can be seen from Table 3 above, the peak temperature of the active material of the example increases, the total calorific value decreases, and the thermal stability is improved.
[0123] [Table 4]
[0124]
[0125] It can be seen from Table 4 above that although the thermal stability of the positive electrode active material according to the example of the present application is greatly improved as shown in Table 3, it still shows the same level of charge and discharge capacity and efficiency as Comparative Example 1.
[0126] The present invention can be implemented in various different ways and is not limited to the above-mentioned embodiments. It will be appreciated by those skilled in the art that the present invention can be implemented in other specific ways without changing the technical concept or essential features of the present invention. Therefore, the above-mentioned embodiments are exemplary in all aspects and are not restrictive.
Claims
1. A positive electrode active material, which is a lithium metal oxide particle in the form of a secondary particle including a primary particle, The secondary particle surface includes a plate-like primary particle whose narrowest angle between the c-axis of the primary particle and a straight line connecting a virtual point at the center of the primary particle and the center point of the secondary particle is 60° to 90°, The area occupied by the plate-like primary particles is greater than or equal to 20% by area relative to 100% by area of a circle defined by a circle extending from the center of the secondary particle to 50% by radius of the secondary particle.
2. The positive electrode active material according to claim 1, wherein With respect to the area formed by a circle from the center point of the secondary particle to 50% of the radius of the secondary particle as a reference, 100 area%, The average length of the plate-like primary particles present in the area is 750 nm to 1.25 μm.
3. The positive electrode active material according to claim 1, wherein The interior of the secondary particle includes a needle-shaped primary particle having a narrow angle of greater than or equal to 0° and less than 70° between the c-axis of the primary particle and a straight line connecting a virtual point at the center of the primary particle and the center point of the secondary particle.
4. The positive electrode active material according to claim 1, wherein The nickel content in the metal in the secondary particles is greater than or equal to 80 mol %.
5. A method for preparing a positive electrode active material according to claim 1, comprising: A step of adding a metal salt aqueous solution into a co-precipitation reactor to obtain a metal precursor; and The step of mixing the metal precursor and the lithium raw material and calcining them to obtain a positive electrode active material, In the step of adding a metal salt aqueous solution into the coprecipitation reactor to obtain a metal precursor, The pH condition is changed within the range of 1 hour % to 30 hour % at the end of the reaction, relative to the total reaction time of 100 hour %, Wherein, relative to the total reaction time of 100 hour%, the pH condition is increased by 0.1 to 0.8 within the range of 1 to 30 hour% at the end of the reaction.
6. The method for preparing a positive electrode active material according to claim 5, wherein: The difference between the reaction start pH and the reaction end pH of the step of adding the metal salt aqueous solution into the coprecipitation reactor to obtain the metal precursor is 0.1 to 0.
8.
7. The method for preparing a positive electrode active material according to claim 5, wherein: The upward adjustment speed of the pH condition is 0.0016 pH / min to 0.0133 pH / min.
8. A lithium secondary battery comprising: A positive electrode comprising the positive electrode active material according to any one of claims 1 to 4; a negative electrode comprising a negative electrode active material; and An electrolyte is located between the positive electrode and the negative electrode.
Citation Information
Patent Citations
Positive electrode material for lithium ion battery with nonaqueous electrolyte, and battery using the same
KR1020100099337A
Positive electrode active material precursor for secondary battery and positive electrode active material for secondary battery prepared by using the same
KR1020180063862A
Nickel manganese composite hydroxide, production method for nickel manganese composite hydroxide, positive electrode active material for non-aqueous electrolyte secondary battery, production method for positive electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
WO2018021557A1