Bonded laminated iron core, method for manufacturing the same, and rotating electrical machine
By adding an appropriate amount of inorganic filler to the adhesive to control the particle size, the problem of insufficient flatness and duty ratio of the bonded laminated iron core is solved, and the magnetic performance and accuracy stability of the iron core are improved.
Patent Information
- Application Number
- CN201980075988.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-17
- Filing Date
- 2019-12-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2039-12-17
AI Technical Summary
The existing bonded laminated iron cores have shortcomings in improving flatness and duty cycle, resulting in reduced magnetic characteristics and unstable accuracy.
By adding an inorganic filler to the adhesive, the bonding portion formed by combining organic resin is controlled to improve the flatness and dutyage of the iron core by 50% of the particle size and 90% of the particle size between 0.2-3.5 μm and 10.0 μm or less, and the bonding portion is formed by combining organic resin to improve the flatness and duty cycle of the iron core. coefficient.
The flatness and duty ratio of the bonded laminated core are significantly improved, and the magnetic performance and accuracy stability are improved.
Smart Images

Figure CN113056859B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a bonded laminated core, a method for manufacturing the same, and a rotating electrical machine.
[0002] This application claims priority based on Tokugan Application No. 2018-235871 filed in Japan on December 17, 2018, the contents of which are incorporated herein by reference. Background Art
[0003] In the past, a bonded laminated core for motors, transformers, etc. was known. The bonded laminated core is a structure obtained by stacking multiple thin electromagnetic steel plates and integrating them with an adhesive. In the bonded laminated core, it is difficult to maintain flatness as the number of stacked electromagnetic steel plates increases. In a bonded laminated core with poor flatness, there may be a risk that the bonded laminated core is not upright, the bonded laminated core is tilted, the accuracy of the bonded laminated core is unstable, and the magnetic properties of the bonded laminated core are reduced.
[0004] To address such a problem, for example, Patent Document 1 proposes a bonded laminated core in which electromagnetic steel sheets are bonded to each other with an adhesive containing an epoxy resin and a rubber component to suppress the amount of adhesive extruding from the outer periphery of the electromagnetic steel sheets. In the bonded laminated core of Patent Document 1, the accuracy of the film thickness of the bonding portion is improved.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-096429 Summary of the invention
[0008] [Technical problem to be solved by the invention]
[0009] However, the bonded laminated core of Patent Document 1 has room for improvement in terms of further improving flatness and increasing the space factor.
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a bonded laminated core capable of further improving flatness and space factor, a method for manufacturing the same, and a rotating electrical machine.
[0011] [Technical means for solving technical problems]
[0012] It is conceivable that if an inorganic filler is mixed in the bonding portion where the electromagnetic steel sheets are bonded to each other, expansion or contraction of the bonding portion can be suppressed.
[0013] By suppressing the expansion of the bonding portion, it is easy to increase the space factor of the bonded laminated core. A high space factor of the bonded laminated core means that the proportion of the electromagnetic steel sheet in the cross section of the bonded laminated core in the stacking direction is high. This means that when magnetic lines of force are generated inside the bonded laminated core by excitation from the winding current, the magnetic lines of force can be formed at a higher density. In other words, increasing the space factor of the bonded laminated core means improving the magnetic properties of the bonded laminated core.
[0014] It is conceivable that when the 50% particle size of the inorganic filler included in the bonding portion is small, the bonded laminated core is likely to stand upright, is likely to be flat, and has a high space factor.
[0015] However, the inventors of the present invention have found that the flatness of the bonded laminated core is determined not only by the 50% particle size (center particle size) of the inorganic filler and the average particle size of the inorganic filler (arithmetic mean of the particle sizes of all inorganic filler particles), but also by the 90% particle size of the inorganic filler and the maximum particle size of the inorganic filler. In other words, the inventors of the present invention have found that the flatness of the bonded laminated core is determined by the component with the largest particle size among all the particles of the inorganic filler.
[0016] This is considered to be because no matter how small the 50% particle size or average particle size of the inorganic filler is, if "coarse particles" exist in the total particles of the inorganic filler, the coarse particles dominate the gaps (interstices) between the electromagnetic steel sheets.
[0017] In order to solve the above technical problems, the inventors of the present invention have repeatedly conducted in-depth research. As a result, they found that by reducing the 50% particle size of the inorganic filler contained in the bonding portion and reducing the 90% particle size of the inorganic filler contained in the bonding portion, the flatness of the bonded laminated core can be further improved, and the space factor of the bonded laminated core can be improved, thereby completing the present invention.
[0018] That is, the present invention has the following aspects.
[0019] (1) A first embodiment of the present invention is a bonded laminated iron core comprising: a plurality of electromagnetic steel sheets stacked on each other, both surfaces of which are covered with an insulating film; and a bonding portion provided between the electromagnetic steel sheets adjacent to each other in a stacking direction, for bonding the electromagnetic steel sheets to each other, wherein an adhesive forming the bonding portion comprises an organic resin and an inorganic filler, wherein a 50% particle size of the inorganic filler is 0.2 to 3.5 μm, a 90% particle size of the inorganic filler is 10.0 μm or less, and the content of the inorganic filler is 5 to 50 parts by mass relative to 100 parts by mass of the organic resin.
[0020] (2) In the bonded laminated iron core described in (1), the maximum particle size of the inorganic filler may be 30.0 μm or less.
[0021] (3) In the bonded laminated iron core described in (1) or (2), the inorganic filler may include one or more selected from metal oxides and metal hydroxides.
[0022] (4) In the bonded laminated iron core described in any one of (1) to (3), the inorganic filler may include one or more selected from aluminum hydroxide and aluminum oxide.
[0023] (5) In the bonded laminated iron core described in any one of (1) to (4), the bonded laminated iron core may be for a stator.
[0024] (6) A second embodiment of the present invention is a method for manufacturing a bonded laminated iron core as described in any one of (1) to (5), which comprises repeating the operation of applying the adhesive to a portion of the surface of the electromagnetic steel sheet, overlapping it on another electromagnetic steel sheet and crimping it to form the bonding portion.
[0025] (7) A third aspect of the present invention is a rotating electrical machine including the bonded laminated iron core described in any one of (1) to (5).
[0026] [Effects of the invention]
[0027] According to the bonded laminated core of the present invention, the flatness can be further improved and the space factor can be increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a cross-sectional view of a rotating electrical machine including a bonded laminated core according to one embodiment of the present invention.
[0029] Figure 2 yes Figure 1 A side view of a bonded laminated core is shown.
[0030] Figure 3 yes Figure 2 AA section view.
[0031] Figure 4 It is a side view showing a schematic structure of a manufacturing apparatus for an adhesive laminated iron core. DETAILED DESCRIPTION
[0032] Hereinafter, a bonded laminated core and a rotating electrical machine having the bonded laminated core according to an embodiment of the present invention will be described with reference to the accompanying drawings. In addition, in this embodiment, as a rotating electrical machine, an electric motor, specifically an AC motor, more specifically a synchronous motor, and most specifically a permanent magnet field type motor will be cited as an example for description. Such an electric motor is preferably used in, for example, electric vehicles, etc.
[0033] like Figure 1 As shown, the rotary electric machine 10 includes a stator 20, a rotor 30, a housing 50, and a rotary shaft 60. The stator 20 and the rotor 30 are accommodated in the housing 50.
[0034] The stator 20 is fixed in the housing 50 .
[0035] In the present embodiment, an inner rotor type in which the rotor 30 is located inside the stator 20 is adopted as the rotating electrical machine 10. However, an outer rotor type in which the rotor 30 is located outside the stator 20 may be adopted as the rotating electrical machine 10. In addition, in the present embodiment, the rotating electrical machine 10 is a three-phase AC motor having 12 poles and 18 slots. However, the number of poles, the number of slots, the number of phases, etc. may be changed as appropriate.
[0036] For example, by applying an exciting current having an effective value of 10A and a frequency of 100 Hz to each phase, the rotating electric machine 10 can rotate at a rotation speed of 1000 rpm.
[0037] The stator 20 includes a stator core 21 and a winding (not shown).
[0038] The stator core 21 includes an annular core back 22 and a plurality of teeth 23. Hereinafter, the direction of the central axis O of the stator core 21 (or the core back 22) is referred to as the axial direction, the radial direction (the direction orthogonal to the central axis O) of the stator core 21 (or the core back 22) is referred to as the radial direction, and the circumferential direction (the direction around the central axis O) of the stator core 21 (or the core back 22) is referred to as the circumferential direction.
[0039] The core back 22 is formed in an annular shape in a plan view of the stator 20 viewed from the axial direction.
[0040] The plurality of teeth 23 protrude radially inward (radially toward the central axis O of the core back 22) from the core back 22. The plurality of teeth 23 are arranged at equal intervals in the circumferential direction. In the present embodiment, 18 teeth 23 are provided at a central angle of 20 degrees with the central axis O as the center. The plurality of teeth 23 are formed to have the same shape and the same size as each other.
[0041] The winding is wound around the teeth 23. The winding may be concentratedly wound or dispersedly wound.
[0042] The rotor 30 is arranged radially inward of the stator 20 (or the stator core 21 ). The rotor 30 includes a rotor core 31 and a plurality of permanent magnets 32 .
[0043] The rotor core 31 is formed in an annular shape (ring shape) arranged coaxially with the stator 20. The rotating shaft 60 is arranged in the rotor core 31. The rotating shaft 60 is fixed to the rotor core 31.
[0044] A plurality of permanent magnets 32 are fixed to the rotor core 31. In the present embodiment, a set of two permanent magnets 32 forms one magnetic pole. The plurality of sets of permanent magnets 32 are arranged at equal intervals in the circumferential direction. In the present embodiment, 12 sets (a total of 24) of permanent magnets 32 are arranged at a central angle of 30 degrees with the central axis O as the center.
[0045] In this embodiment, an embedded magnet type motor is used as the permanent magnet field type motor.
[0046] The rotor core 31 is provided with a plurality of through holes 33 that penetrate the rotor core 31 in the axial direction. The plurality of through holes 33 are provided corresponding to the plurality of permanent magnets 32. Each permanent magnet 32 is fixed to the rotor core 31 in a state of being arranged in the corresponding through hole 33. For example, each permanent magnet 32 can be fixed to the rotor core 31 by bonding the outer surface of the permanent magnet 32 to the inner surface of the through hole 33 with an adhesive. In addition, as a permanent magnet field type motor, a surface magnet type motor can also be used instead of an embedded magnet type motor.
[0047] The stator core 21 and the rotor core 31 are both bonded laminated cores. Figure 2 As shown, the stator 20 is formed by laminating a plurality of electromagnetic steel sheets 40 .
[0048] In the stator 20, bonding portions 41 for bonding the electromagnetic steel sheets 40 to each other are provided between electromagnetic steel sheets 40 adjacent to each other in the stacking direction, and the electromagnetic steel sheets 40 are bonded to each other via the bonding portions 41. That is, in the stator 20, a plurality of electromagnetic steel sheets 40 forming the stator core 21 are stacked with the bonding portions 41 interposed therebetween.
[0049] The stacking thickness of each of the stator core 21 and the rotor core 31 is set to 50.0 mm, for example. The outer diameter of the stator core 21 is set to 250.0 mm, for example. The inner diameter of the stator core 21 is set to 165.0 mm, for example. The outer diameter of the rotor core 31 is set to 163.0 mm, for example. The inner diameter of the rotor core 31 is set to 30.0 mm, for example. However, these values are examples, and the stacking thickness, outer diameter and inner diameter of the stator core 21, and the stacking thickness, outer diameter and inner diameter of the rotor core 31 are not limited to these values. Here, the inner diameter of the stator core 21 is based on the front end of the tooth portion 23 in the stator core 21. The inner diameter of the stator core 21 is the diameter of an imaginary circle inscribed in the front end of all the teeth 23.
[0050] Each electromagnetic steel sheet 40 forming the stator core 21 and the rotor core 31 is formed, for example, by punching an electromagnetic steel sheet as a base material. As the electromagnetic steel sheet 40, a known electromagnetic steel sheet can be used. The chemical composition of the electromagnetic steel sheet 40 is not particularly limited. In this embodiment, a non-oriented electromagnetic steel sheet is used as the electromagnetic steel sheet 40. As the non-oriented electromagnetic steel sheet, for example, a non-oriented electrical steel strip of JIS C2552:2014 can be used.
[0051] However, a oriented electromagnetic steel sheet may be used instead of a non-oriented electromagnetic steel sheet as the electromagnetic steel sheet 40. As the oriented electromagnetic steel sheet, for example, a oriented electrical steel strip according to JIS C2553:2012 may be used.
[0052] In order to improve the workability of the electromagnetic steel sheet or the iron loss of the bonded laminated core, both surfaces of the electromagnetic steel sheet 40 are covered with an insulating film. As the material constituting the insulating film, for example, (1) an inorganic compound, (2) an organic resin, (3) a mixture of an inorganic compound and an organic resin, etc. can be applied. As the inorganic compound, for example, (1) a complex of dichromate and boric acid, (2) a complex of phosphate and silicon dioxide, (3) phosphate, etc. can be cited. As the organic resin, for example, epoxy resin, acrylic resin, acrylic styrene resin, polyester resin, silicone resin, fluororesin, etc. can be cited.
[0053] The organic resin may be the same as or different from the organic resin contained in the adhesive described later.
[0054] In order to ensure the insulation performance between the electromagnetic steel sheets 40 stacked on each other, the thickness of the insulating film (the thickness per one surface of the electromagnetic steel sheet 40 ) is preferably 0.1 μm or more.
[0055] On the other hand, as the insulating film becomes thicker, the insulating effect is saturated. In addition, as the insulating film becomes thicker, the space factor decreases, and the performance as a bonded laminated core decreases. Therefore, it is better for the insulating film to be thinner within the range that can ensure the insulating performance. The thickness of the insulating film (the thickness of each surface of the electromagnetic steel sheet 40) is preferably 0.1 μm or more and 5 μm or less, and more preferably 0.1 μm or more and 2 μm or less.
[0056] The thickness of the insulating film can be measured by observing a cut surface obtained by cutting the electromagnetic steel sheet 40 in the thickness direction with a microscope or the like, for example.
[0057] The iron loss improvement effect gradually saturates as the electromagnetic steel sheet 40 becomes thinner. In addition, the manufacturing cost of the electromagnetic steel sheet 40 increases as the electromagnetic steel sheet 40 becomes thinner. Therefore, considering the iron loss improvement effect and the manufacturing cost, the thickness of the electromagnetic steel sheet 40 is preferably 0.10 mm or more.
[0058] On the other hand, if the electromagnetic steel sheet 40 is too thick, it is difficult to perform the press punching operation of the electromagnetic steel sheet 40. Therefore, in consideration of the press punching operation of the electromagnetic steel sheet 40, the thickness of the electromagnetic steel sheet 40 is preferably 0.65 mm or less.
[0059] In addition, when the electromagnetic steel sheet 40 becomes thicker, the iron loss increases. Therefore, considering the iron loss characteristics of the electromagnetic steel sheet 40, the thickness of the electromagnetic steel sheet 40 is preferably 0.35 mm or less, more preferably 0.25 mm or less, and further preferably 0.20 mm or less.
[0060] Considering the above aspects, the thickness of each electromagnetic steel sheet 40 is preferably, for example, 0.10 mm or more and 0.65 mm or less, more preferably 0.10 mm or more and 0.35 mm or less, further preferably 0.10 mm or more and 0.25 mm or less, and particularly preferably 0.10 mm or more and 0.20 mm or less. The thickness of the electromagnetic steel sheet 40 also includes the thickness of the insulating film.
[0061] The thickness of the electromagnetic steel sheet 40 can be measured by, for example, a micrometer or the like.
[0062] like Figure 3 As shown, a plurality of electromagnetic steel sheets 40 forming the stator core 21 are stacked via bonding portions 41. The bonding portions 41 are formed on the core back 22 and the teeth 23 of the stator core 21. The bonding portions 41 are formed as 41a, 41b, and 41c from the inner periphery of the core back 22 toward the radial inner side (radially toward the center axis O of the core back 22). The bonding portions 41b and 41c are respectively formed on the plurality of teeth 23. The bonding portions 41a are respectively formed on the core back 22 at positions corresponding to the plurality of teeth 23.
[0063] The adhesive portion 41 is a layer formed of an adhesive containing an organic resin and an inorganic filler.
[0064] The organic resin constituting the adhesive is not particularly limited, and examples thereof include polyolefin resins, acrylic resins, polyurethane resins, epoxy resins, polyamide resins, polyimide resins, polyester resins, silicone resins, and fluororesins.
[0065] As the organic resin, an acrylic-modified epoxy resin obtained by graft-polymerizing an acrylic resin onto an epoxy resin is preferred because the adhesive strength of the adhesive portion 41 can be easily increased.
[0066] Examples of the epoxy resin include an epoxy resin obtained by condensing epichlorohydrin and bisphenol in the presence of an alkali catalyst, and an epoxy resin obtained by condensing epichlorohydrin and bisphenol in the presence of an alkali catalyst to form a low molecular weight epoxy resin and subjecting the low molecular weight epoxy resin to an addition polymerization reaction with bisphenol, etc. Here, the "low molecular weight epoxy resin" refers to an epoxy resin having a number average molecular weight of less than 1,200.
[0067] The epoxy resin may be an epoxy ester resin in combination with a divalent carboxylic acid. Examples of the divalent carboxylic acid include succinic acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, dodecanoic acid, and hexahydrophthalic acid.
[0068] Examples of the bisphenol include bisphenol A, bisphenol F, and bisphenol AD, and bisphenol A and bisphenol F are preferred.
[0069] Examples of the alkaline catalyst include sodium hydroxide and potassium hydroxide.
[0070] These epoxy resins may be used alone or in combination of two or more.
[0071] The number average molecular weight of the epoxy resin is preferably 1200 to 8000, more preferably 2000 to 7000, and further preferably 2500 to 7000. When the number average molecular weight of the epoxy resin is greater than or equal to the lower limit, the bonding strength of the bonding portion 41 is easily improved. When the number average molecular weight of the epoxy resin is less than or equal to the upper limit, the stability of the bonding portion 41 is easily improved.
[0072] The number average molecular weight of the epoxy resin can be measured using polystyrene as a standard substance in accordance with the size exclusion chromatography (SEC: Size-Exclusion Chromatography) described in JIS K7252-1:2008.
[0073] The content of the epoxy resin is preferably 30 to 90 mass %, more preferably 40 to 80 mass %, and further preferably 50 to 70 mass % relative to the total mass of the adhesive. If the content of the epoxy resin is greater than the lower limit, it is easy to increase the bonding strength of the bonding portion 41. If the content of the epoxy resin is less than the upper limit, it is easy to relax the strain generated in the electromagnetic steel sheet 40.
[0074] Examples of the acrylic resin include an acrylic resin obtained by polymerizing or copolymerizing at least one selected from unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, and crotonic acid; an acrylic resin obtained by copolymerizing at least one monomer selected from unsaturated carboxylic acids and at least one selected from the following free radical polymerizable unsaturated monomers; and the like.
[0075] Examples of free radical polymerizable unsaturated monomers include (1) hydroxyalkyl esters of acrylic acid or methacrylic acid having 1 to 8 carbon atoms, such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, etc.; (2) alkyl esters or cycloalkyl esters of acrylic acid or methacrylic acid having 1 to 24 carbon atoms, such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, 2-ethyl ...methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, cyclohe (3) functional acrylamides or functional methacrylamides, such as acrylamide, methacrylamide, N-methylacrylamide, N-ethylacrylamide, diacetone acrylamide, N-hydroxymethyl acrylamide, N-methoxymethyl acrylamide, N-butoxymethyl acrylamide, etc.; (4) aromatic vinyl monomers, such as styrene, vinyl toluene, α-methylstyrene; (5) aliphatic vinyl monomers, such as vinyl acetate, vinyl propionate, acrylonitrile, methacrylonitrile, etc.
[0076] Preferred combinations of the unsaturated monomers include, for example, a combination of methyl methacrylate, 2-ethylhexyl acrylate and acrylic acid; a combination of styrene, methyl methacrylate, ethyl acrylate and methacrylic acid; a combination of styrene, ethyl acrylate and methacrylic acid; a combination of methyl methacrylate, ethyl acrylate and acrylic acid, and the like.
[0077] The number average molecular weight of the acrylic resin is preferably 5000 to 100000, more preferably 6000 to 80000, and further preferably 7000 to 60000. When the number average molecular weight of the acrylic resin is equal to or greater than the lower limit, it is easy to increase the bonding strength of the bonding portion 41. When the number average molecular weight of the acrylic resin is equal to or less than the upper limit, it is easy to suppress the adhesive from becoming highly viscous, and it is easy to make the bonding portion 41 flat.
[0078] The number average molecular weight of the acrylic resin can be measured by the same method as the number average molecular weight of the epoxy resin.
[0079] The content of the acrylic resin is preferably 10 to 40% by mass, more preferably 15 to 35% by mass, and further preferably 20 to 30% by mass relative to the total mass of the adhesive. If the content of the acrylic resin is greater than or equal to the above lower limit, the bonding strength of the bonding portion 41 can be easily improved. If the content of the acrylic resin is less than or equal to the above upper limit, it is easy to suppress the adhesive from becoming highly viscous and to make the bonding portion 41 flat. Therefore, it is easy to suppress the strain of the bonded laminated core.
[0080] The acrylic modified epoxy resin (hereinafter also referred to as a graft product) obtained by graft-polymerizing an acrylic resin onto an epoxy resin is obtained, for example, by subjecting the above-mentioned free radical polymerizable unsaturated monomer to a graft polymerization reaction with a high molecular weight epoxy resin in an organic solvent solution in the presence of a free radical generator such as benzoyl peroxide. Here, the "high molecular weight epoxy resin" refers to an epoxy resin having a number average molecular weight of 1,200 or more.
[0081] The radical generator used in the graft polymerization reaction is preferably contained in an amount of 3 to 15 parts by mass based on 100 parts by mass of the solid content of the radical polymerizable unsaturated monomer.
[0082] The graft polymerization reaction is carried out, for example, by adding a radical polymerizable unsaturated monomer uniformly mixed with a radical generator to an organic solvent solution of a high molecular weight epoxy resin heated to 80 to 150° C. over 1 to 3 hours, and further maintaining the solution at the same temperature for 1 to 3 hours.
[0083] The organic solvent used for the graft polymerization reaction may be an organic solvent that dissolves the high molecular weight epoxy resin and the free radical polymerizable unsaturated monomer and is miscible with water.
[0084] As such an organic solvent, for example, alcohol solvents such as isopropyl alcohol, butanol, 2-hydroxy-4-methylpentane, 2-ethylhexanol, cyclohexanol, ethylene glycol, diethylene glycol, 1,3-butylene glycol, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, ketone solvents such as acetone and methyl ethyl ketone, cellosolves, and carbitol solvents can be cited. In addition, an inert organic solvent that is immiscible with water can also be used. As such an organic solvent, for example, aromatic hydrocarbons such as toluene and xylene, and esters such as ethyl ester and butyl acetate can be cited.
[0085] When the adhesive contains epoxy resin, the curing agent can use a commonly used epoxy resin curing agent. As the epoxy resin curing agent, for example, at least one selected from the following can be used: aliphatic polyamines, alicyclic polyamines, aromatic polyamines, polyamide polyamines, modified polyamines and other polyamine curing agents; monofunctional acid anhydrides (phthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, chlorendic anhydride, etc.), difunctional acid anhydrides (pyromellitic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol bis (dehydrated trimellitic ester), methylcyclohexene tetracarboxylic anhydride, etc.), free acid anhydrides (trimellitic anhydride, polyazelaic anhydride, etc.); hydroxymethyl-containing initial condensation products, such as novolac type or phenolic type phenolic resins, urea resins, melamine resins, etc.; latent curing agents, etc.
[0086] As latent curing agents, for example, dicyandiamide, melamine, organic acid dihydrazide, amine imide, ketimine, tertiary amine, imidazole salt, boron trifluoride amine salt, microcapsule type curing agent (the curing agent is encapsulated in microcapsules formed by casein or the like, the microcapsules are broken by heating and pressurizing, and a curing reaction occurs with the resin) and molecular sieve type curing agent (the curing agent is adsorbed on the surface of an adsorption compound, the adsorbed molecules are released by heating, and a curing reaction occurs with the resin) are mentioned.
[0087] As the epoxy resin curing agent, a novolac phenolic resin (phenol novolac resin) is preferably used from the viewpoint of easily improving the bonding strength of the bonding portion 41. Here, a "novolac phenolic resin" refers to a resin obtained by condensing phenols and aldehydes using an acid catalyst.
[0088] Examples of the phenols include phenol.
[0089] Examples of the aldehydes include formaldehyde.
[0090] Examples of the acid catalyst include oxalic acid and divalent metal salts.
[0091] Novolac phenolic resin is solid at room temperature (25°C) and is classified as a thermoplastic resin. 2 The OH group is hardly bonded to the phenol nucleus (aromatic ring) constituting the phenol resin.
[0092] The content of the epoxy resin curing agent is preferably 1 to 20% by mass relative to the total mass of the adhesive. When the content of the epoxy resin curing agent is greater than or equal to the lower limit, the bonding strength of the bonding portion 41 is easily improved. When the content of the epoxy resin curing agent is less than or equal to the upper limit, the stability of the bonding portion 41 is easily improved.
[0093] The adhesive may contain an elastomer. Examples of the elastomer include natural rubber and synthetic rubber, and synthetic rubber is preferred.
[0094] Examples of the synthetic rubber include polybutadiene-based synthetic rubber, nitrile-based synthetic rubber, and chloroprene-based synthetic rubber.
[0095] Examples of the polybutadiene-based synthetic rubber include isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), polyisobutylene (butyl rubber, IIR), and ethylene-propylene-diene rubber (EPDM).
[0096] Examples of the nitrile synthetic rubber include nitrile rubber (NBR) and acrylic rubber (ACM).
[0097] Examples of the chloroprene-based synthetic rubber include chloroprene rubber (CR) and the like.
[0098] As the synthetic rubber, in addition to the above, polyurethane rubber, silicone rubber, fluororubber (FKM), chlorosulfonated polyethylene (CSM), epichlorohydrin rubber (ECO), etc. can also be used.
[0099] As the elastomer, SBR, EPDM, and NBR are preferred from the viewpoints of excellent heat resistance and ease of relaxing strain generated in the electromagnetic steel sheet 40 .
[0100] The elastomer may be used alone or in combination of two or more.
[0101] The content of the elastomer is preferably 5 to 30% by mass relative to the total mass of the adhesive. When the content of the elastomer is equal to or greater than the lower limit, strain generated in the electromagnetic steel sheet 40 can be easily alleviated.
[0102] When the content of the elastomer is equal to or less than the above upper limit, the bonding strength of the bonding portion 41 can be easily increased.
[0103] The content of the organic resin is preferably 40 to 95% by mass, more preferably 50 to 90% by mass, and further preferably 60 to 80% by mass relative to the total mass of the adhesive. If the content of the organic resin is above the lower limit, it is easy to increase the bonding strength of the bonding portion 41. If the content of the organic resin is below the upper limit, it is easy to suppress the adhesive from becoming highly viscous, and it is easy to make the bonding portion 41 flat. Therefore, it is easy to suppress the strain of the bonded laminated core.
[0104] As the inorganic filler, for example, there are metal oxides such as aluminum oxide (α-alumina), zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, and tin oxide; metal hydroxides such as aluminum hydroxide (gibbsite), calcium hydroxide, and magnesium hydroxide; silicon-containing materials such as silicon dioxide, diatomaceous earth, calcium silicate, and talc; sulfates such as calcium sulfate, magnesium sulfate, and barium sulfate, etc.
[0105] The inorganic filler may be used alone or in combination of two or more.
[0106] As the inorganic filler, from the viewpoint of low cost and easy availability, one or more selected from metal oxides and metal hydroxides are preferred, one or more selected from aluminum hydroxide and aluminum oxide are more preferred, and aluminum hydroxide is further preferred.
[0107] The 50% particle size of the inorganic filler is 0.2 to 3.5 μm, preferably 0.4 to 3.0 μm, and more preferably 0.6 to 2.5 μm. If the 50% particle size of the inorganic filler is greater than the lower limit, it is easy to suppress expansion or contraction of the bonding portion 41. If the 50% particle size of the inorganic filler is less than the upper limit, it is easy to increase the space factor of the bonded laminated core.
[0108] When the inorganic filler is a metal oxide, the 50% particle size of the inorganic filler is preferably 1.0 to 3.5 μm, more preferably 1.5 to 3.2 μm, and further preferably 2.0 to 3.0 μm.
[0109] When the inorganic filler is a metal hydroxide, the 50% particle size of the inorganic filler is preferably 0.2 to 3.0 μm, more preferably 0.5 to 2.5 μm, and further preferably 1.0 to 2.0 μm.
[0110] The 90% particle size of the inorganic filler is 10.0 μm or less, preferably 8.0 μm or less, and more preferably 6.0 μm or less. If the 90% particle size of the inorganic filler is below the upper limit, it is easy to make the bonding portion 41 flat. Therefore, it is easy to suppress the strain of the bonded laminated core. The lower limit of the 90% particle size of the inorganic filler is not particularly limited, but is substantially 2.0 μm.
[0111] When the inorganic filler is a metal oxide, the 90% particle size of the inorganic filler is preferably 10.0 μm or less, more preferably 9.5 μm or less, and even more preferably 9.0 μm or less.
[0112] When the inorganic filler is a metal hydroxide, the 90% particle size of the inorganic filler is preferably 9.0 μm or less, more preferably 8.0 μm or less, and further preferably 7.0 μm or less.
[0113] In this specification, the 50% particle size and the 90% particle size represent the particle size on a volume basis in the cumulative particle size distribution. The 50% particle size and the 90% particle size can be measured using a laser diffraction / scattering type particle size distribution measuring device. The 50% particle size represents the particle size when the cumulative amount accounts for 50% on a volume basis in the cumulative particle size curve of the particle size distribution measured using a laser diffraction / scattering type particle size distribution measuring device. The 90% particle size represents the particle size when the cumulative amount accounts for 90% on a volume basis in the cumulative particle size curve of the particle size distribution measured using a laser diffraction / scattering type particle size distribution measuring device.
[0114] The 90% particle size of the inorganic filler can be adjusted by using a sieve having a specific aperture or by an air classification method or the like.
[0115] The maximum particle size of the inorganic filler is preferably 30.0 μm or less, more preferably 20.0 μm or less, and further preferably 10.0 μm or less. When the maximum particle size of the inorganic filler is equal to or less than the upper limit, it is easy to make the bonding portion 41 flat. Therefore, it is easy to suppress the strain of the bonded laminated core.
[0116] The lower limit of the maximum particle size of the inorganic filler is not particularly limited, but is substantially 3.0 μm.
[0117] When the inorganic filler is a metal oxide, the maximum particle size of the inorganic filler is preferably 20.0 μm or less, more preferably 15.0 μm or less, and further preferably 10.0 μm or less.
[0118] When the inorganic filler is a metal hydroxide, the maximum particle size of the inorganic filler is preferably 15.0 μm or less, more preferably 10.0 μm or less, and further preferably 8.0 μm or less.
[0119] The maximum particle size of the inorganic filler can be measured using a laser diffraction / scattering type particle size distribution measuring device. The maximum particle size of the inorganic filler is given by the maximum value of all particles measured using a laser diffraction / scattering type particle size distribution measuring device.
[0120] The maximum particle size of the inorganic filler can be adjusted by using a sieve with a specific aperture or an air classification method.
[0121] The content of the inorganic filler is 5 to 50 parts by mass, preferably 5 to 40 parts by mass, more preferably 5 to 30 parts by mass, and further preferably 10 to 30 parts by mass, relative to 100 parts by mass of the organic resin. If the content of the inorganic filler is above the lower limit, it is easy to suppress the expansion or contraction of the bonding portion 41. If the content of the inorganic filler is below the upper limit, it is easy to increase the space factor of the bonded laminated core.
[0122] When the inorganic filler is a metal oxide, the content of the inorganic filler is preferably 10 to 50 parts by mass, more preferably 15 to 40 parts by mass, and even more preferably 20 to 30 parts by mass, based on 100 parts by mass of the organic resin.
[0123] When the inorganic filler is a metal hydroxide, the content of the inorganic filler is preferably 5 to 45 parts by mass, more preferably 10 to 40 parts by mass, and further preferably 15 to 35 parts by mass, based on 100 parts by mass of the organic resin.
[0124] The adhesive of the present embodiment may include any component in addition to the organic resin and the inorganic filler. As the optional component, conductive materials, rust-proof additives such as sparingly soluble chromates, coloring pigments (such as condensed polycyclic organic pigments, phthalocyanine organic pigments, etc.), coloring dyes (such as azo dyes, azo metal complex salt dyes, etc.), film-forming aids, dispersibility improvers, defoamers, etc. may be cited.
[0125] These optional components may be used alone or in combination of two or more.
[0126] When the adhesive contains an optional component, the content of the optional component is preferably 1 to 10 parts by mass based on 100 parts by mass of the organic resin.
[0127] As the adhesive of this embodiment, in addition to thermosetting adhesives, free radical polymerization adhesives and the like can also be used. From the perspective of productivity, it is preferred to use room temperature curing adhesives. Room temperature curing adhesives cure at 20°C to 30°C. As room temperature curing adhesives, acrylic adhesives are preferred. Representative acrylic adhesives include SGA (Second Generation Acrylic Adhesive) and the like. Any of anaerobic adhesives, instant adhesives and acrylic adhesives containing elastomers can be used within the scope of not impairing the effects of the present invention. In addition, the adhesive referred to here is a state before curing, and the adhesive becomes the bonding portion 41 after curing.
[0128] The average tensile modulus E of the adhesive portion 41 at room temperature (20°C to 30°C) is in the range of 1500MPa to 4500MPa. If the average tensile modulus E of the adhesive portion 41 is less than 1500MPa, the rigidity of the laminated core will be reduced. Therefore, the lower limit of the average tensile modulus E of the adhesive portion 41 is set to 1500MPa, and more preferably 1800MPa. On the contrary, if the average tensile modulus E of the adhesive portion 41 exceeds 4500MPa, the insulating film formed on the surface of the electromagnetic steel sheet 40 will be peeled off. Therefore, the upper limit of the average tensile modulus E of the adhesive portion 41 is set to 4500MPa, and more preferably 3650MPa.
[0129] Furthermore, the average tensile elastic modulus E was measured by a resonance method. Specifically, the tensile elastic modulus was measured in accordance with JIS R 1602:1995.
[0130] More specifically, first, a sample for measurement (not shown) is manufactured. The sample is obtained by bonding two electromagnetic steel plates 40 with an adhesive to be measured and curing the adhesive to form a bonding portion 41. When the adhesive is a thermosetting adhesive, the curing is performed by heating and pressurizing under the heating and pressurizing conditions in actual operation. On the other hand, when the adhesive is a room temperature curing adhesive, the curing is performed by pressurizing at room temperature.
[0131] Then, the tensile modulus of the sample is measured by the resonance method. The method for measuring the tensile modulus of the sample by the resonance method is as described above, and is performed in accordance with JIS R 1602: 1995. Thereafter, the tensile modulus of the bonding portion 41 alone is obtained by excluding the influence of the electromagnetic steel sheet 40 itself from the tensile modulus of the sample (measured value) by calculation.
[0132] Since the tensile modulus obtained from the sample in this way is equal to the average value of the laminated core as a whole, this value is regarded as the average tensile modulus E. The composition of the average tensile modulus E is set so that it does not change much at the stacking position along the stacking direction and the circumferential position around the central axis of the laminated core. Therefore, the value obtained by measuring the cured adhesive portion 41 located at the upper end of the laminated core can also be used as the value of the average tensile modulus E.
[0133] As a bonding method, for example, a method of applying an adhesive to the electromagnetic steel sheet 40 and then bonding by heating or pressing or both can be adopted. In addition, the heating means can be any means such as heating in a high temperature tank or electric furnace, or directly applying electricity.
[0134] In order to stably obtain sufficient bonding strength, the thickness of the bonding portion 41 is preferably 1 μm or more.
[0135] On the other hand, if the thickness of the adhesive portion 41 exceeds 100 μm, the adhesive force will be saturated. In addition, as the adhesive portion 41 becomes thicker, the space factor decreases, and the magnetic properties such as the iron loss of the bonded laminated core decrease. Therefore, the thickness of the adhesive portion 41 is preferably greater than 1 μm and less than 100 μm, and more preferably greater than 1 μm and less than 10 μm.
[0136] Furthermore, in the above, the thickness of the adhesive portion 41 means the average thickness of the adhesive portion 41 .
[0137] The average thickness of the adhesive portion 41 is preferably greater than 1.0 μm and less than 3.0 μm. If the average thickness of the adhesive portion 41 is less than 1.0 μm, sufficient bonding strength cannot be ensured as described above. Therefore, the lower limit of the average thickness of the adhesive portion 41 is 1.0 μm, and more preferably 1.2 μm. On the contrary, if the average thickness of the adhesive portion 41 becomes thicker than 3.0 μm, undesirable conditions such as a significant increase in the strain of the electromagnetic steel sheet 40 due to shrinkage during thermal curing may occur. Therefore, the upper limit of the average thickness of the adhesive portion 41 is set to 3.0 μm, and more preferably 2.6 μm.
[0138] The average thickness of the bonding portion 41 is the average value of the entire bonded laminated core. The average thickness of the bonding portion 41 hardly changes at the stacking position along the stacking direction or the circumferential position around the central axis of the bonded laminated core. Therefore, the average thickness of the bonding portion 41 can be measured at the upper end position of the bonded laminated core at more than 10 positions in the circumferential direction as its value.
[0139] In addition, the average thickness of the bonding portion 41 can be adjusted by, for example, changing the amount of adhesive applied. In addition, for example, in the case of a thermosetting adhesive, the average tensile elastic modulus E of the bonding portion 41 can be adjusted by changing one or both of the heating and pressurizing conditions applied during bonding and the type of curing agent.
[0140] In the present embodiment, the plurality of electromagnetic steel sheets 40 forming the rotor core 31 are fixed to each other by caulking (dowels) C. However, the plurality of electromagnetic steel sheets 40 forming the rotor core 31 may be bonded to each other by bonding portions 41 .
[0141] Furthermore, the bonded laminated core such as the stator core 21 or the rotor core 31 may be formed by so-called rotational lamination.
[0142] Hereinafter, a method for manufacturing a bonded laminated core according to an embodiment of the present invention will be described with reference to the drawings.
[0143] The stator core 21 can be manufactured by repeating the operation of applying adhesive to a part of the surface of the electromagnetic steel sheet 40 and then overlapping and press-bonding the electromagnetic steel sheet to another electromagnetic steel sheet to form the bonding portion 41 .
[0144] Next, we will use Figure 4 The manufacturing apparatus 100 shown will be used to explain a method of manufacturing the stator core 21.
[0145] First, the manufacturing device 100 is described. In the manufacturing device 100, while the original steel sheet P is fed from the steel coil Q (strip steel) in the direction of the arrow F, the original steel sheet P is gradually formed into the shape of the electromagnetic steel sheet 40 by multiple punching using dies arranged on each stage, and an adhesive is applied to a predetermined position on the lower surface of the electromagnetic steel sheet 40 after the second sheet, and the punched electromagnetic steel sheets 40 are sequentially stacked and crimped.
[0146] like Figure 4 As shown, the manufacturing device 100 includes: a first-level punching workstation 110 located closest to the steel coil Q; a second-level punching workstation 120 arranged adjacent to the punching workstation 110 on the downstream side along the conveying direction of the original steel plate P; and an adhesive coating workstation 130 arranged adjacent to the punching workstation 120 on the downstream side than the punching workstation 120.
[0147] The punching station 110 includes a female die 111 disposed below the original steel plate P and a male die 112 disposed above the original steel plate P.
[0148] The punching station 120 includes a female die 121 disposed below the original steel plate P and a male die 122 disposed above the original steel plate P.
[0149] The adhesive coating station 130 includes a coater 131 having a plurality of sprayers arranged according to a coating pattern of the adhesive.
[0150] The manufacturing apparatus 100 further includes a laminating station 140 at a position downstream of the adhesive coating station 130. The laminating station 140 includes a heating device 141, an outer peripheral punching female die 142, a heat insulating member 143, an outer peripheral punching male die 144, and a spring 145.
[0151] The heating device 141 , the outer peripheral punching female die 142 , and the heat insulating member 143 are arranged below the original steel sheet P. On the other hand, the outer peripheral punching male die 144 and the spring 145 are arranged above the original steel sheet P.
[0152] In the manufacturing apparatus 100, first, the original steel sheet P is cut from the steel coil Q along the Figure 4 Then, the original steel sheet P is firstly punched by the punching station 110. Then, the original steel sheet P is punched by the punching station 120. Through these punching processes, the original steel sheet P is obtained with Figure 3 The shape of the electromagnetic steel sheet 40 of the core back 22 and the plurality of teeth 23 shown in the figure (punching process). However, since it has not been completely punched out at this moment, it proceeds to the next process in the direction of arrow F. In the adhesive coating station 130 of the next process, the adhesive supplied from the respective injectors of the coater 131 is applied in a dotted manner (coating process).
[0153] Next, the original steel plate P is sent to the stacking workstation 140, punched out by the outer peripheral punching male die 144, and stacked with good precision (stacking process). During the stacking, the electromagnetic steel plate 40 is subjected to a certain pressure by the spring 145. By repeating the punching process, coating process and stacking process described above in sequence, a predetermined number of electromagnetic steel plates 40 can be stacked. Furthermore, the iron core formed by stacking the electromagnetic steel plates 40 in this way is heated by the heating device 141, for example, at 60°C to 200°C. The adhesive is cured by the heating to form the bonding portion 41 (curing process).
[0154] Through the above-mentioned steps, the stator core 21 is completed.
[0155] As described above, the rotating electric machine and the bonded laminated iron core of the present embodiment are composed of a plurality of electromagnetic steel sheets covered with insulating films on both sides, and the electromagnetic steel sheets adjacent to each other in the stacking direction are bonded to each other via a bonding portion formed by an adhesive containing an organic resin and an inorganic filler. The electromagnetic steel sheets are bonded to each other via the bonding portion, thereby obtaining a sufficient bonding strength. Since the bonding portion contains an inorganic filler, expansion or contraction of the bonding portion can be suppressed.
[0156] In addition, in each bonding portion, 5 to 50 parts by mass of inorganic filler, 50% of which has a particle size of 0.2 to 3.5 μm and 90% of which has a particle size of 10.0 μm or less, is contained relative to 100 parts by mass of the organic resin. Therefore, the rotating electric machine and the bonded laminated core of this embodiment can easily reduce the gap between the electromagnetic steel sheets. As a result, the flatness of the bonded laminated core can be further improved, and the space factor of the bonded laminated core can be increased.
[0157] The bonded laminated core of this embodiment can further improve flatness and space factor. Therefore, the bonded laminated core of this embodiment is suitable as a bonded laminated core (stator core) for a stator. The bonded laminated core can also be used as a rotor core.
[0158] In addition, the technical scope of the present invention is not limited to the above-mentioned embodiment, and various changes can be made within the scope not departing from the spirit of the present invention.
[0159] The shape of the stator core is not limited to the shape shown in the above embodiment. Specifically, the outer diameter and inner diameter of the stator core, the lamination thickness, the number of slots, the circumferential and radial dimension ratio of the tooth portion 23, the radial dimension ratio of the tooth portion 23 and the core back 22, etc. can be arbitrarily designed according to the desired characteristics of the rotating electrical machine.
[0160] In the rotor of the above embodiment, a set of two permanent magnets 32 forms one magnetic pole, but the present invention is not limited thereto. For example, one permanent magnet 32 may form one magnetic pole, or three or more permanent magnets 32 may form one magnetic pole.
[0161] In the above embodiment, a permanent magnet field type motor is described as an example of a rotating electrical machine, but the structure of the rotating electrical machine is shown in the following example and is not limited thereto, and various known structures not shown below may be adopted.
[0162] In the above embodiment, a permanent magnet field type motor is used as an example of a synchronous motor, but the present invention is not limited thereto. For example, the rotating electrical machine may be a reluctance type motor or an electromagnetic field type motor (winding field type motor).
[0163] In the above embodiment, a synchronous motor is described as an example of an AC motor, but the present invention is not limited thereto. For example, the rotating electrical machine may be an induction motor.
[0164] In the above embodiment, an AC motor is described as an example of a motor, but the present invention is not limited thereto. For example, the rotating electric machine may be a DC motor.
[0165] In the above-mentioned embodiment, although the electric motor is taken as an example as the rotating electric machine, the present invention is not limited thereto. For example, the rotating electric machine may be a generator.
[0166] In the above-mentioned embodiment, the case where the bonded laminated iron core of the present invention is applied to a stator core is exemplified, but it may also be applied to a rotor core.
[0167] Furthermore, the components in the above-described embodiments may be appropriately replaced with known components without departing from the spirit of the present invention, and the above-described modifications may be appropriately combined.
[0168] [Example]
[0169] [Examples 1 to 6, Comparative Examples 1 to 4]
[0170] A steel strip having a thickness of 0.25 mm was prepared, and an insulating coating treatment solution containing metal phosphate and acrylic resin emulsion was applied to both surfaces of the steel strip, and baked at 300° C. to form an insulating coating of 0.8 μm on a single surface.
[0171] The steel strip formed with the insulating film is wound up as a steel coil Q. The steel coil Q is placed in the above-mentioned manufacturing device 100, and the original steel sheet P is sent out from the steel coil Q in the direction of arrow F. Using the manufacturing device 100, a single plate (electromagnetic steel sheet 40) is formed by punching (punching process), and the single plate (electromagnetic steel sheet 40) has an annular shape with an outer diameter of 300 mm and an inner diameter of 240 mm, and a rectangular tooth portion with a length of 30 mm and a width of 15 mm is provided on the inner diameter side 18.
[0172] Next, the electromagnetic steel sheets after punching are transported in sequence. Figure 3 The adhesive of the composition shown in Table 1 was applied in dots at each location (5 mg per location) (application process), and then laminated (lamination process). The same operation was repeated to obtain a laminated body of 130 electromagnetic steel sheets. The obtained laminated plate was pressed at a pressure of 10 MPa and heated at 120°C to cure the adhesive (curing process), and the bonded laminated iron core of each example was manufactured.
[0173] The types of the components in Table 1 are as follows.
[0174] <Organic resin>
[0175] Acrylic modified epoxy resin (epoxy resin: bisphenol F type, 60 mass %; acrylic resin: acrylic acid polymer, 20 mass %; curing agent: novolac type phenolic resin, 20 mass %).
[0176] <Inorganic filler>
[0177] A1: aluminum hydroxide (50% particle size 1.5 μm, 90% particle size 6.5 μm, maximum particle size 7.0 μm).
[0178] A2: Alumina (50% particle size 2.5 μm, 90% particle size 8.5 μm, maximum particle size 9.5 μm).
[0179] A'1: silicon dioxide (50% particle size 1.5 μm, 90% particle size 12.0 μm, maximum particle size 15.0 μm).
[0180] A'2: magnesium oxide (50% particle size 2.5 μm, 90% particle size 15.5 μm, maximum particle size 21.0 μm).
[0181] In Table 1, the composition unit of each component is part by mass.
[0182] In Table 1, “-” means that the component is not contained.
[0183] <Evaluation of Flatness>
[0184] The bonded laminated core of each example was placed on a flat table and Figure 3 The height of the bonded laminated core is measured at 18 positions corresponding to the tooth portion 23. The difference between the maximum and minimum values of the height of the bonded laminated core (△H) is calculated and divided by the average value of the height of the bonded laminated core (average height) to find the flatness (△H / average height × 100 (%)). The average height is the arithmetic mean of the above 18 points. The flatness of the bonded laminated core is evaluated according to the following evaluation criteria. The smaller the flatness, the better the flatness. The results are shown in Table 1.
[0185] Evaluation Criteria
[0186] A: The flatness is less than 2%.
[0187] B: The flatness is 2% or more and less than 5%.
[0188] C: The flatness is 5% or more.
[0189] <Evaluation of Duty Factor>
[0190] The space factor (%) of the bonded laminated core of each example obtained was calculated.
[0191] In addition, in this specification, the space factor of the bonded laminated core is given by the following formula.
[0192] Duty factor (%) = M / (D·h·S) × 100
[0193] Here, M represents the mass of the bonded laminated core (kg), and D represents the density of the steel sheet (the electromagnetic steel sheet excluding the insulating film) (kg / m3 ), h represents the average height of the bonded laminated core (m), and S represents the area of the electromagnetic steel sheet when viewed from above (m 2 ). The area S of the electromagnetic steel sheet is obtained by taking the electromagnetic steel sheet before lamination as an image using a scanner and performing image analysis.
[0194] The duty factor was evaluated based on the calculated value of the duty factor according to the following evaluation criteria. The results are shown in Table 1.
[0195] Evaluation Criteria
[0196] A: The duty factor is more than 99%.
[0197] B: The duty factor is 98% or more and less than 99%.
[0198] C: Duty factor is less than 98%.
[0199] [Table 1]
[0200]
[0201] As shown in Table 1, in Examples 1 to 6 to which the present invention is applied, the flatness and the space factor are all "A" or "B".
[0202] On the other hand, in Comparative Example 1 in which the content of the inorganic filler was smaller than the range of the present invention, the space factor was "C".
[0203] In Comparative Example 2 in which the content of the inorganic filler was larger than the range of the present invention, the flatness and the space factor were "C".
[0204] In Comparative Examples 3 and 4 in which the 90% particle size of the inorganic filler was outside the range of the present invention, the flatness and the space factor were "C".
[0205] From the above results, it is understood that the bonded laminated core according to the present invention can further improve the flatness and the space factor.
[0206] [Industrial Applicability]
[0207] According to the present invention, the flatness of the bonded laminated core can be further improved, and the space factor can be increased. Therefore, the industrial applicability is very high.
[0208] [Explanation of Reference Numerals]
[0209] 10 Rotating motor
[0210] 20 Stator
[0211] 21. Stator core (bonded laminated core)
[0212] 40 Electromagnetic steel plate
[0213] 41 Bonding
Claims
1. A bonded laminated core comprising: A plurality of electromagnetic steel sheets are stacked one on top of the other, and both surfaces are covered with insulating films; and The bonding portion is provided between the electromagnetic steel sheets adjacent to each other in the stacking direction, and bonds the electromagnetic steel sheets to each other. The adhesive forming the bonding portion includes an organic resin and an inorganic filler. The 50% particle size of the inorganic filler is 0.2 to 3.5 μm, 90% of the inorganic filler has a particle size of 10.0 μm or less, The content of the inorganic filler is 5 to 50 parts by mass based on 100 parts by mass of the organic resin.
2. The bonded laminated core according to claim 1, The maximum particle size of the inorganic filler is 30.0 μm or less.
3. The bonded laminated core according to claim 1, The inorganic filler contains one or more selected from metal oxides and metal hydroxides.
4. The bonded laminated core according to claim 2, The inorganic filler contains one or more selected from metal oxides and metal hydroxides.
5. The bonded laminated core according to claim 1, The inorganic filler contains one or more selected from aluminum hydroxide and aluminum oxide.
6. The bonded laminated core according to claim 2, The inorganic filler contains one or more selected from aluminum hydroxide and aluminum oxide.
7. The bonded laminated core according to claim 3, The inorganic filler contains one or more selected from aluminum hydroxide and aluminum oxide.
8. The bonded laminated core according to claim 4, The inorganic filler contains one or more selected from aluminum hydroxide and aluminum oxide.
9. The bonded laminated core according to claim 1, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm. 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
10. The bonded laminated core according to claim 2, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm, 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
11. The bonded laminated core according to claim 3, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm. 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
12. The bonded laminated core according to claim 4, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm, 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
13. The bonded laminated core according to claim 5, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm. 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
14. The bonded laminated core according to claim 6, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm, 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
15. The bonded laminated core according to claim 7, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm. 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
16. The bonded laminated core according to claim 8, wherein the 50% particle size of the inorganic filler is 0.4 to 3.0 μm. 90% of the particle sizes of the inorganic filler are 2.0-10.0 μm.
17. The bonded laminated core according to claim 1, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
18. The bonded laminated core according to claim 2, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
19. The bonded laminated core according to claim 3, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
20. The bonded laminated core according to claim 4, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
21. The bonded laminated core according to claim 5, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
22. The bonded laminated core according to claim 6, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
23. The bonded laminated core according to claim 7, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
24. The bonded laminated core according to claim 8, wherein the 50% particle size of the inorganic filler is 1.5 to 2.5 μm. 90% of the particle sizes of the inorganic filler are 6.5-8.5 μm.
25. The bonded laminated core according to claim 1, The bonded laminated core is used for a stator.
26. The bonded laminated core according to claim 2, The bonded laminated iron core is used for a stator.
27. The bonded laminated core according to claim 3, The bonded laminated core is used for a stator.
28. The bonded laminated core according to claim 4, The bonded laminated iron core is used for a stator.
29. The bonded laminated core according to claim 5, The bonded laminated core is used for a stator.
30. The bonded laminated core according to claim 6, The bonded laminated iron core is used for a stator.
31. The bonded laminated core according to claim 7, The bonded laminated iron core is used for a stator.
32. The bonded laminated core according to claim 8, The bonded laminated iron core is used for a stator.
33. A method for manufacturing a bonded laminated iron core, the method for manufacturing a bonded laminated iron core according to any one of claims 1 to 32, The adhesive is applied to a part of the surface of the electromagnetic steel sheet, and then overlapped with another electromagnetic steel sheet and pressure-bonded to form the bonded portion.
34. A rotating electrical machine comprising: The bonded laminated iron core according to any one of claims 1 to 32.