Deep hanging core iron mold sand-coated casting process and sand-coated mold
By using deep core iron sand coating molds and tapered round hole perforation technology in the iron mold sand coating process, the problems of unstable molding of the inner cavity of the casting and difficulty in solidification of the coated sand in the traditional method are solved, and efficient The production of deep cavity castings improves the yield rate and casting quality.
Patent Information
- Application Number
- CN202110478034.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-04-28
AI Technical Summary
When using the iron mold sand coating process to cast large-scale deep cavity structural castings, the traditional method has problems such as unstable cavity molding, difficulty in demoulding, difficulty in solidifying the coated sand, and the formation of empty or loose shells, resulting in low yield.
Using a deep hanging core iron-shaped sand coating mold and process, multiple connected conical round hole perforations and nozzles are provided on the upper shape mold, and the coated sand is injected into the sand coating chamber through the nozzles. After solidification It comes out together with the upper iron type lifting core, which reduces the pre-sand filling and cleaning processes and improves the tightness and production efficiency of the casting.
It realizes the forming of deep cavity castings without manual sand filling, reduces top hole tooling and cleaning work, improves the yield and quality of castings, and is suitable for the production of large castings.
Smart Images

Figure CN113084093B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting, and particularly relates to a deep hanging core iron mold sand-coated casting process and a sand-coated mold thereof. Background Art
[0002] The iron mold sand coating process has its own technological advantages, but it also has many technological limitations.
[0003] At present, when large castings with deep inner cavities (such as large oil pans and large diesel engine flywheel housing castings) are produced using the iron mold sand coating process, the inner cavity is usually formed by inserting a sand core or using the iron mold hanging core process.
[0004] The molding method adopts the method of inserting sand cores, and the molding process quality is stable and reliable, but it needs to put in a core box, increase the core making process, and after the core is made, it needs to be brushed or soaked in paint and dried, and the process is very cumbersome.
[0005] The use of the upper iron core hanging process can save a set of core boxes and core making processes. However, due to the large height of the hanging sand, the ejector pin often bends during demolding, which makes production very difficult and dangerous. It also causes the coated sand at the perforation site to be too thick and unable to solidify, resulting in mold collapse. In order to avoid the difficulty of top hole caused by the long sand hole and the difficulty of solidifying the sand in the perforation, no perforation is arranged at the upper iron core, but the perforation of the hanging sand edge is adopted, and the coated sand is transported from the edges of the hanging core to the bottom of the hanging core by air pressure. However, during molding, after the coated sand passes through the narrow vertical gap of the hanging core, the fluidity of the coated sand deteriorates when it encounters heat, which often causes the flat area at the bottom of the hanging core to be empty or loose and porous. After demolding, it needs to be repaired manually or the mold needs to be scrapped and re-shot, which wastes a lot of labor and materials. Empty shells can be avoided by pre-laying a certain thickness of coated sand in the center of the bottom of the upper outer mold. However, the thickness of the coated sand placed in advance is difficult to control. Too much sand is often used, which causes the upper iron mold to be raised and unable to fit completely with the outer mold. On the other hand, the coated sand placed first and later is difficult to mature uniformly. The coated sand placed earlier has already solidified and is difficult to combine with the coated sand injected later, resulting in cavity stratification.
[0006] In summary, there are many inconveniences when using the iron mold sand covering process with an ultra-high inner cavity hanging core solution to cast large deep inner cavity castings, and the mold yield is very low. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a deep hanging core iron mold sand-coated casting process and a sand-coated mold thereof, and the specific scheme is as follows:
[0008] A deep hanging core iron mold sand-coated mold comprises an upper outer mold and an upper iron mold, wherein the lower surface of the upper outer mold is provided with a casting mold concave mold, and the upper surface of the upper iron mold is provided with an upper iron mold hanging core, and the upper outer mold and the upper iron mold are butted from top to bottom to form a sand-coated layer chamber between the casting mold concave mold and the upper iron mold hanging core, and the upper outer mold is provided with a plurality of perforations connecting the sand-coated layer chamber.
[0009] Furthermore, it comprises a shooting plate, on which a shooting nozzle for docking with the shooting hole is arranged, and a bushing is arranged on the shooting nozzle.
[0010] Furthermore, the perforations are tapered circular holes, the draft angle of the tapered circular holes is 1°~1.5°, the surface roughness of the perforation wall is 2~5, and multiple perforations are arranged on the upper outer mold corresponding to the horizontal and vertical surfaces of the upper iron core.
[0011] Furthermore, the upper surface of the upper outer shape mold is provided with a plurality of outer shape mold pits, and the plurality of outer shape mold pits are arranged on the upper surface of the upper outer shape mold corresponding to the horizontal plane and the vertical plane of the upper iron-type hanging core respectively, and each perforation is respectively arranged in each outer shape mold pit, and a plurality of electric heating pipe holes are respectively arranged on both sides of the upper outer shape mold, and an upper outer shape mold positioning pin hole is provided on the parting surface of the upper outer shape mold.
[0012] Furthermore, a horizontal runner is provided on one side of the upper surface of the upper iron mold, the horizontal runner is connected to the straight runner that runs through the upper iron mold, and ears are provided at both ends of the upper iron mold. Upper iron mold positioning pin holes corresponding to the upper outer mold positioning pin holes are provided on the upper iron mold separation surface, and multiple iron mold pits are provided on the lower surface of the upper iron mold.
[0013] The deep hanging core iron mold sand-coated casting process using the deep hanging core iron mold sand-coated mold comprises the following steps:
[0014] (1) During sand-shot molding, the upper iron mold is raised to dock with the upper outer mold;
[0015] (2) The nozzle is connected to the perforation on the outer mold, and the coated sand is shot into the perforation through the nozzle and enters the sand coating chamber;
[0016] (3) The coated sand in step (2) adheres to the upper iron mold after being heated and solidified, and the upper iron mold is lowered to separate it from the upper outer mold. The cured coated sand in the perforation follows the upper iron mold and escapes from the upper outer mold;
[0017] (4) After demolding, the residual perforated and solidified coated sand in step (3) is ground until it is flush with the bottom surface of the upper iron-type hanging core, thereby obtaining an upper outer mold cavity of the coated sand that is integrated with the upper iron-type hanging core.
[0018] Furthermore, the demoulding time is 150s to 200s.
[0019] Advantages of the present invention
[0020] 1. The iron mold sand-coated process without sand core and the sand-coated mold of the present invention can cast large castings with deep inner cavities (such as oversized oil pan castings, etc.). Compared with the traditional iron mold sand-coated molding process, it does not require auxiliary methods such as artificial sand filling to solve the pre-filling solution of the bottom surface of the upper iron mold hanging core.
[0021] 2. The perforation of the present invention is a tapered circular hole with an inclination and the perforation surface is very smooth. Since the perforation height is short, after demoulding, only the residual perforation solidified coated sand needs to be manually polished, thereby eliminating the solidification of the upper iron-type long perforation and the manual sand cleaning work and the perforation top hole cleaning scheme of the traditional sand coating process and reducing a set of upper iron-type top hole tooling procedures, and can also solve the empty shell and looseness of the bottom surface of the upper iron-type hanging sand.
[0022] 3. The casting process and sand-coated mold of the present invention can solve the defects of the traditional iron mold sand-coated process that the bottom surface of the upper iron mold hanging core is difficult to form or the surface of the molding sand is loose, and there is no need to manufacture the top hole tooling of the upper iron mold and the upper outer mold, which effectively improves the production efficiency, the qualified rate of the casting, and the quality of the casting, which is suitable for promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a cross-sectional view of the nozzle, the upper outer mold and the upper iron mold docking of the present invention.
[0024] Figure 2 It is a structural schematic diagram of the upper outer mold and the shooting plate docking of the present invention.
[0025] Figure 3 for Figure 2 A partial enlarged cross-sectional view of the upper outer mold and nozzle combination.
[0026] Figure 4 for Figure 1 Schematic diagram of the structure of the upper surface of the upper outer mold.
[0027] Figure 5 for Figure 4 Schematic diagram of the structure of the lower surface of the upper outer mold.
[0028] Figure 6 for Figure 2 A schematic diagram of the structure of the shooting plate;
[0029] Figure 7 for Figure 1 Schematic diagram of the structure of the upper surface of the upper iron mold.
[0030] Figure 8 for Figure 7 Schematic diagram of the structure of the lower surface of the upper iron mold.
[0031] In the figure:
[0032] 1. Upper outer mold; 101. Casting mold concave mold; 102. Upper outer mold positioning pin hole; 103. Outer mold pit; 104. Perforation; 105. Electric heating pipe hole; 2. Upper iron mold; 201. Upper iron mold hanging core; 202; Iron mold pit; 203. Horizontal runner; 204. Straight runner; 205. Lifting ear; 3. Shooting plate; 4. Sand coating chamber; 5. Shooting plate; 6. Nozzle. DETAILED DESCRIPTION
[0033] The invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be noted that this specific embodiment is not intended to limit the scope of rights of the invention.
[0034] like Figures 1 to 8 As shown, the deep hanging core iron mold sand-coated mold provided by this specific embodiment includes an upper outer mold 1, an upper iron mold 2 and a shooting plate 3. The lower surface of the upper outer mold 1 is provided with a casting mold die 101, and the upper outer mold 1 is provided with an upper outer mold positioning pin hole 102 on the parting surface. The upper iron mold 2 is provided with an upper iron mold hanging core 201 on the upper surface, and the upper iron mold 2 is provided with an upper iron mold positioning pin hole 202 corresponding to the upper outer mold positioning pin hole 102 on the parting surface. The upper iron mold 2 is lifted and connected to the upper outer mold 1, and the positioning pin is moved through the upper outer mold positioning pin hole 102 and the upper iron mold positioning pin hole 202 for fixation, so that a sand-coated layer chamber 4 is formed between the casting mold die 101 and the upper iron mold hanging core 201. A plurality of outer mold pits 103 are respectively provided on the upper surface of the upper outer mold 1 corresponding to the horizontal and vertical surfaces of the upper iron mold hanging core 201, and each outer mold pit 103 is respectively provided with a shooting hole 104 connected to the horizontal surface of the sand-coated layer chamber. Preferably, as Figure 2 , 4 As shown in Figures 6 and 7, multiple perforations 104 are arranged in three groups, one of which corresponds to the horizontal surface of the upper iron core 201, and the other two groups correspond to the vertical surfaces on both sides of the upper iron core 201. The purpose of setting the outer shape mold pit 103 is to firstly shorten the height of the perforations 104, reduce the solidified coated sand of the residual perforations 104, facilitate demoulding and manual grinding to be flush with the bottom surface of the upper iron core 201, and obtain a dense and compact coated sand upper outer shape model cavity integrated with the upper iron core 201; secondly, reduce the weight of the upper outer shape mold 1. Preferably, the perforation 104 is a tapered circular hole, the draft angle of the tapered circular hole is 1° to 1.5°, and the surface roughness of the perforation wall is 2 to 5. The purpose is to make the height of the tapered circular hole short (the height of the perforation is set to 10 mm) and to provide an inclination, and the perforation wall is smooth and has an inclination. Therefore, the length of the solidified coated sand in the perforation 104 is the height of the perforation 104 (that is, the length is 10 mm), so that the solidified coated sand remaining in the perforation 104 can be easily removed from the upper outer mold 1 along with the upper iron mold 2.
[0035] The nozzle 6 is provided with a bushing, and the nozzle 6 with the bushing is connected to the perforation 104 through a sealing ring. The nozzle 6 shoots sand into the perforation 104, and enters the sand coating chamber 4 from the horizontal and vertical surfaces of the upper iron-type hanging core 201, respectively, to ensure the compactness of the coating sand filling on the horizontal and vertical surfaces of the upper iron-type hanging core 201, and also ensure that the kinetic energy of the coating sand filling is not lost, forming a dense, compact, and complete sand coating chamber 4. At the same time, it avoids the situation in the traditional casting process where only the horizontal surface of the sand coating chamber 4 is filled and the kinetic energy of the coating sand is lost, resulting in the situation that the bottom plane area of the upper iron-type hanging core 201 is empty or loose and porous.
[0036] A plurality of iron mold pits 202 are provided on the lower surface of the upper iron mold 2, and the purpose of the iron mold pits 202 is to reduce the weight of the upper iron mold 2. A horizontal runner 203 is provided on one side of the upper surface of the upper iron mold 2, and the horizontal runner 203 is connected to the straight runner 204 that runs through the upper iron mold 2. Lifting ears 205 are also provided at both ends of the upper iron mold 2 for easy lifting.
[0037] A plurality of electric heating tube holes 105 are respectively provided on both sides of the upper outer shape mold 1, the purpose of which is to heat the upper outer shape mold 1 to a temperature of 190-230°C so that the coated sand injected into the coating sand layer chamber 4 is solidified.
[0038] After sand shooting, the solidified coated sand adheres to the upper iron mold 2, and the upper iron mold 2 is lowered to separate the upper iron mold 2 from the upper outer mold 1. Since the nozzle 6 is not heated, the coated sand is not solidified and will leak out after the upper iron mold 2 is lowered, leaving no residue at the nozzle 6. The perforation 104 is short in height and the perforation wall is smooth and inclined. Therefore, the solidified coated sand in the perforation 104 can follow the upper iron mold 2 to escape from the upper outer mold 1. After 150s to 200s, the mold is removed, and the solidified coated sand in the residual perforation 104 is polished to be flush with the bottom surface of the upper iron mold hanging core 201, so as to obtain a dense and tight upper outer mold cavity with a smooth surface, no empty shells and looseness, and an integrated coated sand upper outer mold cavity with the upper iron mold hanging core 201.
[0039] The deep hanging core iron mold sand-coated casting process using a deep hanging core iron mold sand-coated mold includes the following steps:
[0040] (1) During sand-shot molding, first fix the upper outer mold 1 on the motorized roller, then raise the upper iron mold 2 to dock with the upper outer mold 1;
[0041] (2) The nozzle 6 is connected to the perforation 104, and the coated sand is shot from the perforation 104 through the nozzle 6. The coated sand enters the sand coating chamber 4 from the horizontal surface of the upper iron-type hanging core 201, ensuring the compactness of the horizontal surface of the upper iron-type hanging core 201. The coated sand enters the sand coating chamber 4 from the vertical surface of the upper iron-type hanging core 201, avoiding the situation where the coated sand turns when filling the mold. The kinetic energy of the coated sand filling the mold is not lost, ensuring the compactness of the vertical surface of the upper iron-type hanging core 201, thereby obtaining a dense, compact and complete sand coating cavity 4;
[0042] (3) The coated sand in step (2) adheres to the upper iron mold 2 after being heated and solidified. The upper iron mold 2 is lowered to separate it from the upper outer mold 1. Since the nozzle 6 is not heated and the coated sand is not solidified, it will leak out after the upper iron mold 2 is lowered, leaving no residue in the nozzle 6. The perforation 104 is a conical circular hole with a short height and a smooth and inclined perforation wall. Therefore, the length of the solidified coated sand in the perforation 104 is the height of the perforation 104, and it can follow the upper iron mold 2 out of the upper outer mold 1.
[0043] (4) After 150s to 200s, the mold is removed and the residual perforated and solidified coated sand in step (3) is ground to be flush with the bottom surface of the upper iron-type hanging core 201 to obtain an upper outer mold cavity of the coated sand that is integrated with the upper iron-type hanging core 201.
[0044] Example 1: Production of M-26TU oil pan
[0045] The oil pan has a length of 2350 mm, a width of 685 mm, an inner cavity depth of 423 mm, and a casting weight of 475 kg. The deep hanging core iron mold sand-coated casting process of the present invention is adopted, and 32 nozzles 6 are opened on the upper outer mold 1. After sand-shooting molding, the mold is demolded after 170 seconds, and the nozzles 6 are smoothly removed from the upper outer mold 1. The height of the remaining perforations 104 is 10 mm, which is removed by manual grinding. After demolding, it is observed that the sand coating layer is dense and compact, and the surface of the upper iron-type hanging core 201 is smooth, without the defect of loose shell.
[0046] Example 2: Production of C3200 oil pan
[0047] The oil pan has a length of 2800 mm, a width of 600 mm, an inner cavity depth of 355 mm, and a casting weight of 510 kg. The deep hanging core iron mold sand-coated casting process of the present invention is adopted, and 38 nozzles 6 are opened on the upper outer mold 1. After sand-shooting molding, the mold is demolded after 160 seconds, and the nozzles 6 are smoothly removed from the upper outer mold 1. The height of the remaining perforations 104 is 10 mm, which is removed by manual grinding. After demolding, it is observed that the sand coating layer is dense and compact, and the surface of the upper iron-type hanging core 201 is smooth, without the defect of loose shell.
Claims
1. A deep hanging core iron mold covered with sand, comprising an upper outer mold and an upper iron mold, characterized in that: The lower surface of the upper outer mold is provided with a casting mold die, the upper surface of the upper iron mold is provided with an upper iron mold hanging core, the upper outer mold and the upper iron mold are butted from top to bottom to form a sand-coated layer chamber between the casting mold die and the upper iron mold hanging core, and the upper outer mold is provided with a plurality of perforations communicating with the sand-coated layer chamber; it includes a shooting plate, the shooting plate is provided with a nozzle butting the perforations, and the nozzle is provided with a bushing; the perforations are tapered circular holes, the draft angle of the tapered circular holes is 1°~1.5°, and the surface roughness of the perforation wall is 2~5, and the plurality of perforations are respectively arranged on the upper outer mold corresponding to the horizontal plane and the vertical plane of the upper iron mold hanging core; the upper surface of the upper outer mold is provided with a plurality of outer mold pits, and the plurality of outer mold pits are respectively arranged on the upper surface of the upper outer mold corresponding to the horizontal plane and the vertical plane of the upper iron mold hanging core, each perforation is respectively arranged in each outer mold pit, a plurality of electric heating pipe holes are respectively arranged on both sides of the upper outer mold, and an upper outer mold positioning pin hole is provided on the parting surface of the upper outer mold.
2. The deep hanging core iron mold sand-coated mold according to claim 1, characterized in that: A horizontal runner is provided on one side of the upper surface of the upper iron mold, and the horizontal runner is connected to the straight runner that runs through the upper iron mold. Lifting ears are also provided at both ends of the upper iron mold. An upper iron mold positioning pin hole corresponding to the upper outer mold positioning pin hole is provided on the parting surface of the upper iron mold, and a plurality of iron mold pits are provided on the lower surface of the upper iron mold.
3. A deep hanging core iron mold sand-coated casting process using the deep hanging core iron mold sand-coated mold according to claim 1 or 2, characterized in that: The steps include: (1) During sand-shot molding, the upper iron mold is raised to dock with the upper outer mold; (2) The nozzle is connected to the perforation on the outer mold, and the coated sand is shot into the perforation through the nozzle and enters the sand coating chamber; (3) The coated sand in step (2) adheres to the upper iron mold after being heated and solidified, and the upper iron mold is lowered to separate it from the upper outer mold. The cured coated sand in the perforation follows the upper iron mold and escapes from the upper outer mold; (4) After demolding, the residual perforated and solidified coated sand in step (3) is ground until it is flush with the bottom surface of the upper iron-type hanging core, thereby obtaining an upper outer mold cavity of the coated sand that is integrated with the upper iron-type hanging core.
4. The deep hanging core iron mold sand-coated casting process according to claim 3 is characterized in that: The demoulding time is 150s to 200s.
Citation Information
Cited By
Empty shell precoated sand core manufacturing process
CN121082828A