Battery and method for manufacturing battery

By combining tubular pressing components and a pressure reducing pump system, the problem of spatter during welding of the negative electrode lead to the casing was solved, achieving high-reliability and high-efficiency battery manufacturing.

CN113302769BActive Publication Date: 2024-11-26PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080009370.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-17
Publication Date
2024-11-26
Estimated Expiration
2040-03-17

AI Technical Summary

Technical Problem

Existing technologies are prone to generating spatter when welding the negative electrode lead to the casing, which can lead to short circuit risks. Furthermore, laser output control is difficult and affects productivity.

Method used

A tubular pressing component and a pressure reducing pump system are used to weld the negative electrode lead to the inner surface of the housing by sucking in smoke and splatter in the tube, combined with laser welding, to form a stable molten mark.

Benefits of technology

It reduces the generation of spatter, improves battery reliability and production efficiency, avoids short circuit risks, and simplifies the welding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113302769B_ABST
    Figure CN113302769B_ABST
Patent Text Reader

Abstract

The manufacturing method of the present invention includes: a process of preparing a shell having an opening at one end and a bottom at the other end; a process of preparing an electrode group having a first electrode, a second electrode and a collecting lead electrically connected to the first electrode; a process of accommodating the electrode group in the shell; and a process of joining the inner surface of the shell to the collecting lead, wherein the joining process includes the following steps: pressing a tubular pressing member against the collecting lead so that the collecting lead abuts against the inner surface of the shell; and welding the shell to the collecting lead while the pressure inside the tube of the pressing member is reduced by a suction portion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a battery and a method for manufacturing the battery, and more particularly to a battery in which a current collector lead of a current collector is electrically connected to a housing by welding and a method for manufacturing the battery. Background Art

[0002] Patent document 1 discloses the following manufacturing method: when joining and fixing a collector tab (positive electrode tab or negative electrode tab) to the inner surface of the bottom of a shell, a center column is inserted into the center of the electrode assembly to press the collector tab to the bottom surface of the shell, while laser welding is performed by irradiating a laser from the outside of the shell.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2006-012787 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] However, in the case where the negative electrode lead and the shell are joined by welding as in Patent Document 1, it is required to perform welding without penetrating the negative electrode lead. This is because there is a concern that when the negative electrode lead and the shell are welded in such a way that the molten portion penetrates the negative electrode lead, spatter will be generated from the upper surface of the molten portion of the negative electrode lead. Moreover, there is a concern that when the conductive spatter is mixed into the electrode assembly, it will cause a short circuit, and the reliability of the battery may be reduced. In addition, on the other hand, when the negative electrode lead and the shell are welded in such a way that the negative electrode lead is not penetrated, it is required to strictly control the output of the laser, or to perform welding within the application range of the limited laser output, so the productivity may be reduced.

[0008] Therefore, an object of the battery and the method for manufacturing the battery disclosed herein is to provide a battery having higher reliability and excellent workability.

[0009] Solutions for solving problems

[0010] The first method involved in the present disclosure relates to a method for manufacturing a battery, which includes: a process of preparing a shell having an opening at one end and a bottom at the other end; a process of preparing an electrode group having a first electrode, a second electrode and a collecting lead electrically connected to the first electrode; a process of accommodating the electrode group in the shell; and a process of joining the inner surface of the shell to the collecting lead, wherein the joining process includes the following steps: pressing a tubular pressing member against the collecting lead so that the collecting lead abuts against the inner surface of the shell; and welding the shell to the collecting lead while suction is applied to the inside of the tube of the pressing member using a suction portion.

[0011] A second embodiment of the present disclosure relates to a battery, comprising: an electrode group having a first electrode and a second electrode; a shell that accommodates the electrode group, the shell having an opening at one end and a bottom at the other end; and a collector lead that is electrically connected to the first electrode and to an inner surface of the shell, the collector lead having melt marks formed on a first surface of the collector lead and a second surface that is the back side of the first surface, the first surface of the collector lead facing the shell.

[0012] Effects of the Invention

[0013] According to the aspect of the present disclosure, when the case and the current collecting lead are laser welded, smoke and / or splashes generated by melting of the current collecting lead are reduced, thereby making it possible to manufacture a highly reliable battery more cheaply and by a simple method. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a front cross-sectional view of the battery according to the present embodiment as viewed from a vertical plane.

[0015] Figure 2 It is the process of laser welding the negative electrode lead to the shell. Figure 1 The same enlarged cross-sectional view from the front.

[0016] Figure 3 yes Figure 2 An enlarged cross-sectional view of a portion surrounded by a dotted ellipse is shown in FIG.

[0017] Figure 4 (a) is a top view showing the second surface of the negative electrode lead, Figure 4 (b) is a bottom view showing the first surface of the negative electrode lead.

[0018] Figure 5 (a)~ Figure 5(c) is a bottom perspective view, a cross-sectional view from a vertical plane, and a bottom view showing, in an enlarged manner, a part of a pressing member according to a modification of the present embodiment.

[0019] Figure 6 This is a block diagram showing the configuration of a manufacturing system that executes the battery manufacturing method according to the present embodiment. DETAILED DESCRIPTION

[0020] Below, embodiments of the battery and the method for manufacturing the battery involved in the present disclosure are described with reference to the accompanying drawings. In the description of the embodiments, terms indicating directions (such as "vertical", "horizontal", and "left and right", etc.) are appropriately used to facilitate understanding, but these terms are used to illustrate the directions in the drawings and are not used to limit the present disclosure. In addition, in each of the drawings, the various structural components of the battery are illustrated with relative sizes, and are not necessarily represented by the same scale, so as to clarify the shape or characteristics of the various structural components of the battery. In addition, the same symbols are used to represent the same structural components in each of the drawings.

[0021] After first describing the structure of the battery 1, the manufacturing method of the battery 1 according to this embodiment and the specific structure of the battery 1 obtained by the manufacturing method are described below. The manufacturing method and battery of the present invention are not limited to the structures and methods of the following embodiments.

[0022] (Battery structure)

[0023] Figure 1 It is a front cross-sectional view of the battery 1 according to the present embodiment. Figure 1 The battery 1 shown includes an electrode group 10, a shell 30 for accommodating the electrode group 10, and a sealing body 70 for blocking the opening of the shell 30. The electrode group 10 has, for example, a winding structure in which the first electrode 12 and the second electrode 22 are wound with the separator 11 sandwiched therebetween. That is, the battery 1 is a so-called cylindrical battery. In this embodiment, a cylindrical battery is exemplified, but the application of the present invention is not limited thereto. Next, each structural component will be described.

[0024] (Electrode Group)

[0025] After the first electrode 12 and the second electrode 22 sandwiching the separator 11 are wound around a winding core (not shown), the winding core is pulled out, and the electrode group 10 is formed into a columnar body having a hollow portion 20 extending along the winding axis direction. The first electrode 12 usually has a first current collector sheet and a first active material layer formed on the surface of the first current collector sheet (both are not shown). On the other hand, the second electrode 22 usually has a second current collector sheet and a second active material layer formed on the surface of the second current collector sheet (both are not shown).

[0026] The first electrode 12 is electrically connected to the conductive sealing body 70 via the first lead 14 made of conductive foil. On the other hand, the second electrode 22 is electrically connected to the inner surface of the case 30 via the second lead 24 also made of conductive foil.

[0027] In the present embodiment, the inner surface of the shell 30 is described as the central portion of the inner surface of the bottom 34 of the shell 30, but is not limited to this. The inner surface of the shell 30 may also be the side peripheral surface of the shell 30, or may be a portion of the bottom 34 other than the center (for example, the bottom surface biased toward the peripheral side), as long as the second lead 24 is electrically connected to the shell 30.

[0028] In addition, according to the present embodiment, such electrical connection is achieved by laser welding the case 30 and the second lead 24, and the second lead 24 has a melting mark 38 that is laser welded to the case 30. The melting mark 38 of the second lead 24 can be configured to overlap with the hollow portion 20 of the electrode group 10 in the winding axis direction.

[0029] In addition, as described in detail later, the second lead 24 has a first surface 24a facing downward and a second surface 24b facing upward as the back of the first surface 24a. The second lead 24 is welded to the housing 30 in such a manner that the first surface 24a faces the bottom of the housing 30. In addition, the melting mark 38 has a first melting mark 38a and a second melting mark 38b formed by laser welding on the first surface 24a and the second surface 24b of the second lead 24, and the area of ​​the first melting mark 38a is larger than the area of ​​the second melting mark 38b ( Figure 4 ).

[0030] In the battery 1 thus configured, the sealing body 70 functions as a first terminal (e.g., a positive electrode terminal) of the battery 1, and the case 30 functions as a second terminal (e.g., a negative electrode terminal) of the battery 1. Here, each structural element in the case where the first electrode 12 and the second electrode 22 are the positive electrode 12 and the negative electrode 22, respectively, will be described in further detail below.

[0031] The positive electrode 12 includes a positive electrode current collector sheet and positive electrode active material layers (not shown) formed on both sides of the positive electrode current collector sheet. When the battery 1 is a lithium ion battery, the positive electrode current collector sheet is made of metal foil such as aluminum or aluminum alloy, and its thickness can be, for example, 10 μm to 20 μm, but is not limited thereto.

[0032] The positive electrode active material layer includes, for example, a positive electrode active material, a binder, a conductive agent, etc. As the positive electrode active material of the lithium ion secondary battery, a lithium-containing composite oxide is preferably used, for example, LiCoO2, LiNiO2, LiMn2O4, etc. As the positive electrode active material of the lithium ion primary battery, manganese dioxide, graphite fluoride, etc. are used. The thickness of the positive electrode active material layer can be, for example, 70 μm to 130 μm, but is not limited thereto.

[0033] The positive lead 14 of the lithium ion secondary battery is made of aluminum, aluminum alloy, nickel, nickel alloy, iron, stainless steel, etc., and has a thickness of 10 μm to 120 μm. The positive lead 14 is connected to the bottom surface of the sealing body 70 also serving as the positive terminal.

[0034] The negative electrode 22 includes a negative electrode current collector sheet and negative electrode active material layers (not shown) formed on both sides of the negative electrode current collector sheet. When the battery is a lithium ion battery, the negative electrode current collector sheet is made of metal foil such as stainless steel, nickel, copper, copper alloy, etc., and its thickness can be, for example, 5 μm to 20 μm, but is not limited thereto.

[0035] The negative electrode active material layer includes, for example, a negative electrode active material, a binder, a conductive agent, etc. As the negative electrode active material of the lithium ion battery, metallic lithium, alloys (silicon alloys, tin alloys, etc.), carbon materials (graphite, hard carbon, etc.), silicon compounds, tin compounds, lithium titanate, etc. are used. The thickness of the negative electrode active material layer can be, for example, 70 μm to 150 μm, but is not limited thereto.

[0036] The negative electrode lead 24 of the lithium ion battery is formed of materials such as nickel, nickel alloy, iron, stainless steel, copper, copper alloy, etc., and its thickness can be, for example, 10μm to 200μm. In addition, the width of the negative electrode lead 24 is not particularly limited, as long as it is a size that can be accommodated in the shell 30. The width of the negative electrode lead 24 can be, for example, 2mm to 5mm. In addition, the negative electrode lead 24 can be a single-layer structure composed of one metal, or a multi-layer structure in which each layer is composed of different metals. For example, a double-layer structure composed of a Cu layer and a Ni layer, a three-layer structure of a Ni layer, a Cu layer, and a Ni layer are listed. In addition, the negative electrode lead 24 of the battery 1 can also be composed of more than one lead. For example, a plurality of negative electrode leads 24 can be provided. The plurality of negative electrode leads 24 can be individually joined to the bottom 34 of the shell 30, or the front ends of the plurality of leads 24 can be overlapped with each other, and the overlapping portion can be joined to one point of the bottom 34 of the shell 30.

[0037] The separator 11 sandwiched between the positive electrode 12 and the negative electrode 22 is formed of an insulating microporous film, woven fabric or nonwoven fabric. The separator of the lithium ion battery can be formed of polyolefin such as polypropylene and polyethylene, and its thickness is preferably 10 μm to 50 μm, more preferably 10 μm to 30 μm.

[0038] (Electrolyte)

[0039] The electrolyte solution is composed of, for example, a lithium salt and a non-aqueous solvent that can dissolve the lithium salt. As the non-aqueous solvent, cyclic carbonates, chain carbonates, cyclic carboxylates, etc. are used, and as the lithium salt, for example, LiPF6, LiBF4, etc. are used, but are not limited to these.

[0040] (case)

[0041] Figure 1 The shell 30 shown in has a cylindrical shape, has an opening at one end, and has a sealed bottom 34 at the other end. An annular groove 32 is formed near the end of the shell 30 where the opening is formed. In addition, the shell 30 only needs to be cylindrical in shape, and can be an elliptical column in shape in addition to a cylindrical shape. In addition, the shell 30 is made of a conductive material, for example, stainless steel with a thickness of 0.1 mm to 1.0 mm, but is not limited to this. In addition, a lower insulating plate 42 may be provided between the bottom 34 of the shell 30 and the electrode group 10. In addition, an upper insulating plate 43 may be provided between the upper part of the electrode group 10 and the shell 30.

[0042] (Sealing body)

[0043] The sealing body 70 can be formed by overlapping multiple components, for example. The sealing body 70 can be formed by overlapping the filter 71, the lower valve body 72, the insulating ring 73, the upper valve body 74 and the cover 75 in order from bottom to top. Specifically, the filter 71 and the lower valve body 72 are joined to each other at their respective peripheral portions. The central portion of the lower valve body 72 is joined to the central portion of the upper valve body 74. An insulating ring 73 is provided between the peripheral portion of the lower valve body 72 and the peripheral portion of the upper valve body 74. The peripheral portion of the upper valve body 74 is joined to the peripheral portion of the cover 75. The lower valve body 72 and the upper valve body 74 function as a safety mechanism of the battery 1. When the internal pressure of the housing 30 rises, the lower valve body 72 breaks. Then, the upper valve body 74 is pushed upward by the gas, whereby the joint position of the lower valve body 72 and the upper valve body 74 breaks, and the electrical connection between the upper valve body 74 and the lower valve body 72 is cut off. When the internal pressure of the case 30 further increases, the upper valve body 74 breaks, and the gas in the case 30 is released to the outside of the battery 1 through the lid 75. In addition, an insulating gasket 50 may be provided between the sealing body 70 and the opening of the case 30. The gasket 50 insulates the sealing body 70 from the case 30 and has a function of sealing the opening of the case 30 together with the sealing body 70.

[0044] (Battery Manufacturing Method)

[0045] Next, a method for manufacturing the battery according to this embodiment will be described.

[0046] First, the electrode group 10 described above is prepared. The positive electrode lead 14 is arranged relative to the case 30 so as to extend toward the opening of the case 30 and the negative electrode lead 24 is extended toward the bottom 34 of the case 30. Furthermore, the portion of the negative electrode lead 24 extending toward the bottom 34 of the case 30 further than the electrode group 10 is bent so as to be substantially parallel to the inner surface of the bottom. Then, the annular lower insulating plate 42 having a hole in the center is disposed between the bottom 34 of the case 30 and the electrode group 10, and then the electrode group 10 is inserted into the case 30 from the opening.

[0047] Figure 2 This is a process of laser welding the negative electrode lead 24 to the bottom 34 of the case 30. Figure 1 As described above, the position where the negative electrode lead 24 is laser welded to the case 30 is not limited to the central position of the bottom 34 of the case 30 as shown in the figure, but may be the peripheral side surface or the bottom surface adjacent to the peripheral side surface.

[0048] Next, a tubular pressing member 44 is prepared. The pressing member 44 may be, for example, a conduit formed of stainless steel. Then, the pressing member 44 is inserted into the hollow of the electrode group 10 disposed in the housing 30. The outer diameter of the tubular pressing member 44 may be, for example, greater than 2 mm and less than 4 mm. In addition, the inner diameter of the pressing member 44 may be, for example, greater than 1.5 mm and less than 3 mm. Figure 2 In the figure, the tubular pressing member 44 is shown exaggeratedly larger than its actual size to facilitate understanding of its features.

[0049] The tubular pressing member 44 is connected to a suction unit (not shown) such as a pressure reducing pump, and is configured to suck out the fluid and splashes P from the tube 45 of the pressing member 44 along with the operation of the pressure reducing pump. In addition, the suction pressure of the suction unit sucking the tube 45 can be, for example, 50 kPa or more, or, for example, 70 kPa or more.

[0050] The pressing member 44 is pressed so that the negative electrode lead 24 faces the case 30, and the negative electrode lead 24 abuts against (the inner surface of) the case 30. Such insertion and pressing actions of the pressing member 44 may be performed manually by an operator or automatically using a robot (not shown) driven by a stepping motor.

[0051] After pressing member 44 is pressed against negative lead 24 to make negative lead 24 contact with (the inner surface of) case 30 , laser beam LB is irradiated from the laser output unit toward bottom 34 of case 30 , thereby laser welding case 30 to negative lead 24 .

[0052] Figure 3 yes Figure 2 : is an enlarged cross-sectional view of the portion surrounded by the dotted ellipse α shown in FIG. In addition, in the present disclosure, the region or portion of the case 30 that faces the negative electrode lead 24 and is irradiated with the laser beam LB is referred to as the facing portion. In addition, in the present application, a melt (including a melt having continuity and integrity) composed of the constituent materials of the case 30 and the negative electrode lead 24 is formed, and the region or portion that is considered to be melted in appearance in the first surface 24a and the second surface 24b of the negative electrode lead 24 is referred to as a melt mark 38a, 38b.

[0053] The laser beam LB may be a continuous oscillation laser beam or a pulsed laser beam. In addition, regarding the laser output unit, there is no particular limitation on its laser oscillation mechanism, but it is preferably a laser oscillator using a fiber laser. Furthermore, it is preferred that the plurality of facing portions of the housing 30 at the bottom 34 (at Figure 2 and Figure 3 The laser beam LB is irradiated at 3 positions (in the figure).

[0054] In addition, in order to continuously and integrally form the melting mark composed of the constituent materials of the case 30 and the negative electrode lead 24, and to connect the case 30 and the negative electrode lead 24 in a manner that reduces the resistance between the case 30 and the negative electrode lead 24, it is necessary to irradiate the outer surface of the bottom of the case 30 with a laser beam LB having an appropriate light intensity. However, as described above, the thickness of the case 30 is, for example, 0.1 mm to 1.0 mm. On the other hand, the thickness of the negative electrode lead 24 is, for example, 10 μm to 200 μm, and in many cases, the negative electrode lead 24 is thinner than the case 30. Therefore, it is difficult to perform laser welding while maintaining the appropriate light intensity of the laser beam LB. In particular, when the light intensity of the laser beam LB is lower than the appropriate intensity, the resistance between the case 30 and the negative electrode lead 24 increases, which significantly impairs the characteristics of the battery 1. On the other hand, when the light intensity of the laser beam LB is much higher than the appropriate intensity, a hole penetrating the case 30 and the negative electrode lead 24 is formed, and the bonding strength and mechanical strength may be reduced.

[0055] In addition, although the light intensity of the laser beam LB is not strong enough to form a through hole, splashes P consisting of smoke and / or splashes may be formed from the second surface 24b of the negative electrode lead 24. Such splashes P are conductive and may move inside the battery 1 filled with the electrolyte, thereby generating a leakage current between the positive electrode 12 and the negative electrode 22 or causing a short circuit between the positive electrode 12 and the negative electrode 22.

[0056] Therefore, the manufacturing method of the battery 1 according to the present embodiment includes a step of exhausting the air in the tube 45 of the pressing member 44 using a pressure reducing pump. This can reduce smoke and / or splashes generated from the second surface 24b of the negative electrode lead 24 due to laser welding from the inside of the battery 1, and prevent leakage current / short circuit between the positive electrode 12 and the negative electrode 22.

[0057] After the negative electrode lead 24 is welded to the case 30, an upper insulating plate 43 is provided above the electrode group 10. Then, the positive electrode lead 14 is inserted into the hole formed in the upper insulating plate 43. The positive electrode lead 14 passing through the upper insulating plate 43 is led out from the opening of the case 30 and welded to the filter 71 of the sealing body 70 arranged in the gasket 50. The electrolyte is injected into the interior of the case 30 by decompression. Then, an annular groove 32 is formed on the side wall of the case 30. Finally, the sealing body 70 is arranged on the inner surface of the groove 32 together with the gasket 50, and the end of the case 30 is pressed and fastened to the peripheral edge of the sealing body 70 via the gasket 50, thereby manufacturing a cylindrical battery 1.

[0058] (Negative lead method)

[0059] Figure 4(a) is a top view showing the second surface 24b of the negative electrode lead 24, Figure 4 (b) is a bottom view showing the first surface 24a of the negative electrode lead 24. Figure 4 (a) and Figure 4 (b) shows a plurality of melt marks 38 formed by irradiation with the laser beam LB, the melt being composed of the constituent materials of the case 30 and the negative electrode lead 24. Figure 4 In (a) and (b), the outline of a portion of the structural member appearing in the figure is indicated by a dotted line to emphasize the shape of the melting mark 38 in the figure.

[0060] As shown in the figure, the area of ​​the melting mark 38b (also referred to as the second melting mark) formed on the second surface 24b of the negative lead 24 is smaller than the area of ​​the melting mark 38a (also referred to as the first melting mark) formed on the first surface 24a. In addition, a plurality of melting marks 38 can be formed on the first surface 24a and the second surface 24b in a manner that is separated from each other and extends linearly. By forming the melting mark 38b on the second surface 24b of the negative lead 24, it is possible to observe whether there is a melting mark 38b on the second surface 24b to confirm the melting condition of the negative lead 24 that was previously covered and invisible by the shell 30, and the bonding state of the negative lead 24 and the shell 30. Therefore, the inspection process for confirming this bonding state can be simplified.

[0061] In addition, the shape of the melting mark 38 may not extend linearly as described above. For example, a plurality of melting marks 38 may be formed in a dotted (spotted) shape on the first surface 24a and the second surface 24b. Figure 4 The linearly extending fusion mark 38 as shown in (a) and (b) also extends in a direction perpendicular to the direction in which the negative electrode lead 24 extends, and the negative electrode lead 24 extends substantially in parallel with the bottom 34 of the case 30 .

[0062] Figure 5 (a) is a bottom perspective view showing in an enlarged manner a portion of a pressing member 44 according to a modified example of the present embodiment, Figure 5 (b) is a front cross-sectional view showing, in an enlarged manner, a portion of the pressing member 44 according to the modification example. Figure 5 (c) is a bottom view of the pressing member 44 involved in this modification. Figure 5 (b) is from Figure 5 (c) is a front cross-sectional view of the VB-VB line. Figure 5As shown, a notch 45a may be formed at the front end of the tube 45. This structure can prevent the tube 45 from being blocked by the negative lead 24 when the pressing member 44 is brought into contact with the negative lead 24 and the inside of the tube of the pressing member 44 is sucked. Therefore, a gas flow is generated from the shell 30 through the notch 45a and flows into the tube 45 of the pressing member 44, so that an air flow is easily generated in the tube of the pressing member 44. Therefore, it is easy to suck splashes and the like. In addition, the inner diameter of the tube 45 may be wider than the width of the negative lead 24. This structure can also prevent the tube 45 of the pressing member 44 from being sealed by the negative lead 24.

[0063] (Manufacturing System)

[0064] The manufacturing method according to the present embodiment is preferably performed inline (automatically). Figure 6 1 is a block diagram showing the structure of a manufacturing system 100 for executing the manufacturing method of the battery involved in the present disclosure. As described above, the manufacturing system 100 includes: a pressure reducing pump 102 for exhausting the air in the tube 45 of the pressing member 44; a robot 104 for driving the insertion action of the pressing member 44 into the hollow portion 20 and the pressing action of the pressing member 44 against the negative electrode lead 24; and a laser output unit 106 for laser welding the shell 30 to the negative electrode lead 24 by irradiating the bottom surface of the shell 30 with a laser beam LB. In addition, the manufacturing system 100 includes a control unit 110, which controls the actions of the pressure reducing pump 102, the robot 104, and the laser output unit 106. The manufacturing system 100 also includes an input / output unit 114 (machine interface) and a pressure sensor 112 for monitoring the air pressure in the tube 45 of the pressing member 44. The input / output unit 114 is used to set the light intensity of the laser beam LB output from the laser output unit 106 during laser welding, as well as the decompression degree (vacuum degree) and flow rate in the tube 45 of the pressing member 44 , and is configured to display the air pressure in the tube 45 detected by the pressure sensor 112 .

[0065] The operator can use the input / output unit 114 to set the pressing force with which the pressing member 44 presses the negative lead 24 downward during the pressing action, the light intensity of the laser beam LB output from the laser output unit 106 during laser welding, and the decompression degree (vacuum degree) and flow rate in the tube 45 of the pressing member 44.

[0066] The control unit 110 of the manufacturing system 100 controls the robot 104 so that the pressing member 44 presses the negative lead 24 with a pressing force set by the input and output unit 114, the control unit 110 controls the laser output unit 106 so that a laser beam LB with a similarly set light intensity is output during laser welding, and the control unit 110 decompresses the inside of the tube 45 of the pressing member 44 at a desired decompression degree.

[0067] As the laser welding progresses, a portion of the negative electrode lead 24 (the portion corresponding to the melting mark 38) melts, and splashes and the like are generated in the tube 45 of the pressing member 44. At this time, the degree of decompression in the tube 45 decreases (the pressure increases). The pressure sensor 112 monitors the air pressure in the tube 45 of the pressing member 44 and feeds back to the control unit 110. The control unit 110 is configured to control the decompression pump 102 so that the pressure in the monitored tube 45 is substantially stable. In this way, the manufacturing method according to the present embodiment can be performed online.

[0068] Industrial Applicability

[0069] The present invention discloses a battery and a method for manufacturing the battery that can be used to perform laser welding between a case and a lead.

[0070] Description of Reference Numerals

[0071] 1: battery; 10: electrode group; 11: separator; 12: first electrode (positive electrode); 14: first lead (positive electrode lead); 20: hollow portion; 22: second electrode (negative electrode); 24: second lead (negative electrode lead); 24a: first surface; 24b: second surface; 30: shell; 32: groove; 34: bottom; 38: melting mark; 38a: first melting mark; 38b: second melting mark; 42: lower insulating plate; 43 : Upper insulating plate; 44: pressing member; 45: tube; 45a: notch; 50: gasket; 70: sealing body; 71: filter; 72: lower valve body; 73: insulating ring; 74: upper valve body; 75: cover; 100: manufacturing system; 102: pressure reducing pump; 104: robot; 106: laser output unit; 110: control unit; 112: pressure sensor; 114: input and output unit (machine interface); LB: laser beam; P: spatter.

Claims

1. A method for manufacturing a battery, comprising: The step of preparing a housing having an opening at one end and a bottom at the other end; A step of preparing an electrode group including a first electrode, a second electrode, and a current collecting lead electrically connected to the first electrode; The step of housing the electrode group in the housing; as well as a step of joining the inner surface of the housing to the current collecting lead, Wherein, the bonding process includes the following steps: pressing a tubular pressing member against the current collecting lead so that the current collecting lead abuts against the inner surface of the housing; The housing and the current collecting lead are welded while the inside of the tube of the pressing member is sucked by the suction unit. The inner surface of the shell has a facing portion facing the current collecting lead. The current collecting lead is welded to the case by irradiating the facing portion with laser light from outside the case, The current collecting lead has a first surface that abuts against the housing and a second surface that is a back surface of the first surface. In the joining step, when the case and the current collecting lead are welded, the current collecting lead is melted from the first surface to the second surface. When the current collecting lead is welded to the case, smoke and / or splashes generated on the second surface due to melting of the current collecting lead are sucked.

2. The method for manufacturing a battery according to claim 1, wherein: The electrode group is formed by winding the first electrode and the second electrode with a separator interposed therebetween, and the electrode group has a hollow portion extending in a winding axis direction. In the bonding process, The pressing member presses the current collecting lead while being inserted into the hollow portion. The housing and the current collecting lead are welded.

3. The method for manufacturing a battery according to claim 1, further comprising the following steps: monitoring the pressure or flow rate in the tube of the pressing member; The pressure or flow rate in the pressing member is adjusted so that the pressure or flow rate in the tube of the pressing member being monitored is substantially stable.