Flexible copper-clad laminate, electronic device including the same, and method for manufacturing the same
By using a non-conductive polymer substrate and nickel and copper plating formed by electroless plating in flexible copper clad plates, the dimensional instability and interlayer peeling problems are solved, and high adhesion and durability are achieved, ensuring that after heat treatment Dimensional stability and crystallinity.
Patent Information
- Application Number
- CN202080006005.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-08-26
AI Technical Summary
The existing flexible copper clad plates have dimensional instability and interlayer peeling problems during microcircuit patterning, especially inadequate adhesion between the substrate and the metal layer, resulting in high thermal damage and dimensional change rates.
Using a combination of a non-conductive polymer substrate and nickel-containing and copper plating layer, copper and nickel plating are formed by electroless plating method to ensure that the half-value width change rate of copper plating in the X-ray diffraction spectrum is less than 0.01° and at 150°C. The dimensional change rate of 0.015 or less is maintained after heat treatment.
The dimensional stability and crystallinity of flexible copper clad plate are improved, heat damage is avoided, and adhesion and durability between the substrate and the metal layer are improved.
Smart Images

Figure CN113303034B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a flexible copper-clad laminate, an electronic device comprising the flexible copper-clad laminate, and a method for manufacturing the flexible copper-clad laminate. Background Art
[0002] As the growth of the mobile market accelerates and the demand for LCD TV monitors increases, the development of materials with thinner, smaller, lighter, more durable and higher resolution characteristics in electronic products, semiconductor integrated circuits and the like is promoted. Even in the field of flexible copper clad laminates (FCCL) used in driver body circuits (ICs) of LCDs, fine patterning, thinning and durability are increasingly required.
[0003] Flexible copper clad laminate (FCCL) has a structure in which a circuit pattern is formed on a surface of the structure and an electronic device such as a semiconductor chip is mounted on the circuit pattern. Recently, products including circuit patterns having a pitch of 23 μm or less have been increasing, and instability of dimensional changes has become a problem due to the reduction in pitch and line width.
[0004] In order to solve this problem, microcircuit patterning technology is also being developed. However, for microcircuit patterning, it is necessary to maintain high adhesion between the substrate and the metal layer, and to solve the problem of interlayer delamination of the flexible copper clad laminate (FCCL).
[0005] Therefore, there is still a need for a flexible copper clad laminate having excellent dimensional stability between a substrate and a metal layer, an electronic device including the flexible copper clad laminate, and a method for manufacturing the flexible copper clad laminate. Summary of the invention
[0006] Technical issues
[0007] One aspect provides a flexible copper clad laminate having improved crystallinity and dimensional stability.
[0008] Another aspect provides an electronic device including the flexible copper clad laminate.
[0009] Another aspect provides a method for manufacturing the flexible copper clad laminate.
[0010] Means of solving problems
[0011] According to one aspect, a flexible copper clad laminate is provided, comprising:
[0012] Non-conductive polymer substrate;
[0013] a nickel-containing plating layer disposed on at least one surface of the non-conductive polymer substrate; and
[0014] a copper plating layer disposed on the nickel-containing plating layer,
[0015] In the X-ray diffraction spectrum, the peak of the copper plating layer relative to the (111) plane has a half-value width change rate calculated by Mathematical Formula 1 of 0.01° or less.
[0016] In an X-ray diffraction spectrum, the copper plating layer may have a half-value width of 0.20° to 0.35° relative to the peak of the (111) plane.
[0017] Each of the nickel-containing plating layer and the copper plating layer may be an electroless plating layer.
[0018] The copper plating layer may have a thickness of 40 nm to 150 nm.
[0019] When the flexible copper clad laminate is left for one to 60 days and then heat-treated at 150° C. for 30 minutes to obtain dimensions, the flexible copper clad laminate can have a dimensional change rate of 0.015 or less relative to the non-conductive polymer substrate, the dimensional change rate being a value obtained by subtracting the minimum dimension from the maximum dimension among the dimensions.
[0020] The nickel-containing plating layer may include a nickel layer.
[0021] The nickel-containing plating layer may have a thickness of 40 nm to 250 nm.
[0022] The non-conductive polymer substrate may include at least one selected from the group consisting of a phenol-based resin, a novolac-based resin, an allyl-based resin, an epoxy-based resin, a polyethylene-based resin, a polypropylene-based resin, a polyester-based resin, and a polyimide-based resin.
[0023] According to another approach,
[0024] An electronic device including the flexible copper clad laminate described above is provided.
[0025] According to another aspect, a method for manufacturing a flexible copper clad laminate is provided, the method comprising the following steps:
[0026] preparing a non-conductive polymer substrate;
[0027] forming an electroless plating layer containing nickel on at least one surface of the non-conductive polymer substrate; and
[0028] A copper electroless plated layer is formed on one surface of the nickel-containing electroless plated layer to manufacture the flexible copper clad laminate described above.
[0029] Effects of the Invention
[0030] A flexible copper clad laminate according to one aspect is a film in which an electroless plating layer is used for electroplating a metal in an aqueous solution state without thermal damage, and can have improved crystallinity and dimensional stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a schematic diagram of a flexible copper clad laminate according to an embodiment.
[0032] Figure 2 The results of XRD analysis of the flexible copper clad laminate according to Example 1 are shown.
[0033] Figure 3a A sample of eight standard points obtained by cutting the flexible copper clad laminate according to Example 1 into a size of 295 mm×235 mm is shown.
[0034] Figure 3b Show the above Figure 3a A method of measuring the distance between the standard points using a three-dimensional measuring instrument. DETAILED DESCRIPTION
[0035] A flexible copper clad laminate, an electronic device including the flexible copper clad laminate, and a method for manufacturing the flexible copper clad laminate will be described in detail with reference to the embodiments and drawings of the present invention. These embodiments are only presented to explain the present invention in more detail, and those skilled in the art will understand that the scope of the present invention is not limited by these embodiments.
[0036] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. In the event of a conflict, the present specification (including definitions) will control.
[0037] Although methods and materials similar or equivalent to those described in this specification can be used in the practice or testing of the present invention, suitable methods and materials are described in this specification.
[0038] In this specification, the expression "at least one side" preceding an element refers to "one side" and "both sides" of the element. Expressions such as "at least one of..." when placed before a list of elements, modify the entire list of elements and do not modify the individual elements of the list.
[0039] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. As used herein, the term "or" means "and / or".
[0040] As used herein, the term "comprising" is used to indicate that other components may be added or / and inserted, rather than excluding other components, unless specifically stated to the contrary. As used herein, the term "combination thereof" is used to refer to a mixture or alloy of two or more components described above. As used herein, the term "resin based on..." is used to refer to a broad concept including "resin..." or / and "resin derivative...". As used herein, the term "phosphorus flame retardant" is used to refer to a broad concept of flame retardants containing phosphorus.
[0041] As used herein, unless otherwise specified, the unit "parts by weight" refers to the weight ratio between components.
[0042] As used herein, when referring to a component being disposed "on" another component, a component may be placed directly on the other component or there may be components interposed between the components. In contrast, when a component is referred to as being placed "directly" on another component, there may be no intervening components.
[0043] The flexible copper clad laminate manufactured by the sputtering process has limitations in processability due to thermal damage to its surface. The inventors of the present invention intend to propose the following flexible copper clad laminate in order to solve the above problems.
[0044] A flexible copper clad laminate according to an embodiment may include: a non-conductive polymer substrate; a nickel-containing plated layer located on at least one surface of the non-conductive polymer substrate; and a copper plated layer located on the nickel-containing plated layer, wherein in an X-ray diffraction spectrum, the copper plated layer may have a half-value width change rate of 0.01° or less calculated by Mathematical Formula 1 relative to a peak of a (111) plane:
[0045] <Mathematical formula 1>
[0046] Half-value width (111) change rate = {(half-value width after leaving for 60 days) - (initial half-value width)}.
[0047] Figure 1 is a schematic diagram of a flexible copper clad laminate according to an embodiment.
[0048] refer to Figure 1 According to an embodiment, the flexible copper clad laminate 10 may be a double-sided flexible copper clad laminate 10. In the flexible copper clad laminate 10, the nickel-containing plating layers 2 and 2' and the copper plating layers 3 and 3' are sequentially disposed on two surfaces of the non-conductive polymer substrate 1, respectively.
[0049] The flexible copper clad laminate 10 according to an embodiment may have a half-value width change rate of 0.01° or less and may have excellent crystallinity. Therefore, the flexible copper clad laminate 10 according to an embodiment may have improved dimensional stability. In the X-ray diffraction spectrum, the peak of the copper plating layer relative to the (111) plane has a half-value width of 0.20° to 0.35°: This result can be obtained from Figure 2 This is confirmed by the analytical example 1 which will be described later.
[0050] Hereinafter, each of the non-conductive polymer substrate 1 , the nickel-containing plating layers 2 and 2 ′, and the copper plating layers 3 and 3 ′ constituting the flexible copper clad laminate 10 will be described in detail.
[0051] <Non-conductive polymer substrate 1>
[0052] The non-conductive polymer substrate 1 may include at least one selected from phenol-based resins, novolac-based resins, allyl-based resins, epoxy-based resins, polyethylene-based resins, polypropylene-based resins, polyester-based resins, and polyimide-based resins.
[0053] For example, the non-conductive polymer substrate 1 may include a polyimide resin in consideration of adhesion strength, tensile strength, and peel strength. For example, the non-conductive polymer substrate 1 containing a polyimide-based resin may be prepared by extruding polyamic acid as a polyimide precursor into a film and heat-treating the film to imidize the polyamic acid.
[0054] The non-conductive polymer substrate 1 can be dried by a method commonly used in the art to remove moisture and residual gas. For example, the drying of the non-conductive polymer substrate 1 can be performed by roll-to-roll heat treatment under normal pressure, or can be performed by using an infrared (IR) heater under a vacuum atmosphere.
[0055] The thickness of the non-conductive polymer substrate 1 may be 5 μm to 100 μm, for example 10 μm to 400 μm or 20 μm to 30 μm. Within the above thickness range, the non-conductive polymer substrate 1 may have excellent ductility and adhesion while preventing thermal damage.
[0056] <Nickel-containing plating layers 2 and 2'>
[0057] In the plasma treatment using sputtering, adhesion between the non-conductive polymer substrate 1 and the copper plating layers 3 and 3' can be ensured, but thermal damage may occur when processing a thin film type non-conductive polymer substrate 1 having a thickness of 25 μm or less. Due to this thermal damage, the size of the non-conductive polymer substrate 1 may be significantly changed.
[0058] In order to solve this problem, each of the nickel-containing plating layers 2 and 2' may be an electroless plating layer formed by an electroless plating method in which a metal in a state of an aqueous solution is deposited. Each of the nickel-containing plating layers 2 and 2' may include a nickel layer. If necessary, the nickel-containing plating layer may include a nickel alloy layer. The nickel alloy layer may include Ni and at least one selected from the following: Cr, Mo, and Nb. While preventing thermal damage, the dimensional stability of the electroless plating layer relative to the non-conductive polymer substrate 1 can be improved.
[0059] Each of the nickel-containing plated layers 2 and 2' may be formed by using the following electroplating solution through an electroless plating method. In the electroless plating method, both horizontal and / or vertical electroless plating methods may be used.
[0060] The electroplating solution may include a water-soluble nickel salt, a reducing agent, and a complexing agent, and the water-soluble nickel salt may include at least one selected from the following: nickel sulfate, nickel chloride, nickel hypophosphite, nickel acetate, nickel malate, and dehydrates thereof. The water-soluble nickel salt may be included in the electroplating solution at a concentration of 3 g / l to 50 g / l (e.g., 3 g / l to 35 g / l, or 3 g / l to 15 g / l). Within the above range, the water-soluble nickel salt may be improved in terms of the precipitation rate and fluidity of the nickel plating film, and the occurrence of pits in the nickel plating film may be reduced.
[0061] The reducing agent may be a reducing agent commonly used in the art. For example, the reducing agent may include: a hypophosphite, such as sodium hypophosphite or potassium hypophosphite; a borohydride compound, such as sodium borohydride or potassium borohydride; or an amine borane compound, such as dimethylamine borane (DMAB), trimethylamine borane, or triethylamine borane.
[0062] The concentration of the reducing agent in the electroplating solution may vary depending on the type of reducing agent used. For example, when sodium hypophosphite is used as a reducing agent, its concentration may be 20 g / l to 50 g / l. For example, when dimethylamine borane (DMAB), which is a boron compound, is used as a reducing agent, its concentration may be 1 g / l to 10 g / l, such as 3 g / l to 5 g / l. Within the above concentration range, it is possible to prevent the problem that the electroplating solution takes a long time to decompose or form a film.
[0063] In addition, the electroplating solution may further include a complexing agent for preventing the precipitation of nickel compounds and controlling the precipitation reaction of nickel.
[0064] Examples of the complexing agent may include: dicarboxylic acids, such as malic acid, succinic acid, tartaric acid, malonic acid, oxalic acid and adipic acid; aminocarboxylic acids, such as glycine, glutamic acid, aspartic acid and alanine; ethylenediamine derivatives, such as ethylenediaminetetraacetic acid, versenol (N-hydroxyethylethylenediamine-N,N,N-triacetic acid) and tetraol (N,N,N',N'-tetrahydroxyethylethylenediamine); phosphonic acids, such as 1-hydroxyethane-1,1-diphosphonic acid and ethylenediaminetetramethylenephosphonic acid; and soluble salts thereof.
[0065] The complexing agent may be included in the electroplating solution at a concentration of 0.001 mol / l to 2 mol / l (eg, 0.002 mol / l to 1 mol / l). Even within the above concentration range, the complexing agent may prevent decomposition of the electroplating solution and precipitation of nickel hydroxide.
[0066] The electroplating solution may further include a sulfur-containing benzothiazole-based compound represented by the following Chemical Formula 1.
[0067] <Chemical Formula 1>
[0068]
[0069] (Herein, X is a halogen atom, a C1-C10 alkoxy group, a C2-C10 alkoxyalkyl group, a C1-C10 heteroalkyl group, a C6-C20 aryl group, a C6-C20 aralkyl group, a C6-C20 heteroaryl group, a C2-C30 alkyl group substituted with or substituted by a C7-C20 heteroaralkyl group, or a salt thereof.
[0070] The "halogen atom" includes fluorine, bromine, chlorine and iodine.
[0071] "Alkyl" refers to a fully saturated branched or unbranched (or straight chain or linear) hydrocarbon. Non-limiting examples of "alkyl" include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, secondary butyl, n-pentyl, isopentyl, neopentyl, isopentyl (iso-amyl), n-hexyl, 3-methylhexyl, 2,2-dimethylpentyl, 2,3-dimethylpentyl, and n-heptyl.
[0072] "Alkoxy" refers to an alkyl group bonded to an oxygen atom.
[0073] "Aryl" also includes groups in which an aromatic ring is fused to at least one carbocyclic ring. Non-limiting examples of "aryl" include phenyl, naphthyl, and tetrahydronaphthyl.
[0074] "Heteroaryl" refers to a monocyclic or bicyclic organic compound containing one or more heteroatoms selected from N, O, P or S and including carbon atoms as residual ring atoms. The heteroaryl group may contain, for example, 1 to 5 heteroatoms and may contain 5 to 10 ring members. S or N may be oxidized to have various oxidation states.
[0075] Non-limiting examples of “heteroaryl” include thienyl, furanyl, pyrrolyl, imidazolyl, pyrazolyl, thiazolyl, isothiazolyl, 1,2,3-oxadiazolyl, 1,2,4-oxadiazolyl, 1,2,5-oxadiazolyl, 1,3,4-oxadiazolyl, 1,2,3-thiadiazolyl, 1,2,4-thiadiazolyl, 1,2,5-thiadiazolyl, 1,3,4-thiadiazolyl, isothiazol-3-yl, isothiazol-4-yl, isothiazol-5-yl, oxadiazol-2-yl, oxadiazol-3-yl, oxadiazol-4-yl, oxadi ... -yl, oxazol-4-yl, oxazol-5-yl, isoxazol-3-yl, isoxazol-4-yl, isoxazol-5-yl, 1,2,4-triazol-3-yl, 1,2,4-triazol-5-yl, 1,2,3-triazol-4-yl, 1,2,3-triazol-5-yl, tetrazolyl, pyridin-2-yl, pyridin-3-yl, 2-pyrazin-2-yl, pyrazin-4-yl, pyrazin-5-yl, 2-pyrimidin-2-yl, 4-pyrimidin-2-yl and 5-pyrimidin-2-yl.
[0076] The concentration of the sulfur-containing benzothiazole-based compound in the electroplating solution may be 0.1 g / l to 1 g / l. The sulfur-containing benzothiazole-based compound may obtain improved film flexibility within the above concentration range.
[0077] The electroplating solution may further include a stabilizer. Examples of the stabilizer may include: inorganic compounds such as Pb compounds (such as lead acetate) and Bi compounds (such as bismuth acetate); and organic compounds such as butanediol. These compounds may be used alone or as a mixture of two or more.
[0078] The nickel electroless plating solution may have a pH of 4 to 8. For example, the nickel electroless plating solution may have a pH of 4 to 7.5. Within the above pH range, the nickel electroless plating solution may obtain a stable precipitation rate while preventing decomposition of the electroplating solution.
[0079] The thickness of each of the nickel-containing plating layers 2 and 2' may be 40 nm to 250 nm, for example 40 nm to 200 nm, or 40 nm to 150 um. Within the above thickness range, each of the nickel-containing plating layers 2 and 2' may be easily electroplated, and the dimensional stability of each of the nickel-containing plating layers 2 and 2' relative to the non-conductive polymer substrate 1 may be improved.
[0080] <Copper plating 3 and 3'>
[0081] Like each of the nickel-containing plating layers 2 and 2 ′, each of the copper plating layers 3 and 3 ′ may be an electroless plating layer formed by an electroless plating method in which a metal in a state of an aqueous solution is deposited.
[0082] Each of the copper plating layers 3 and 3 ′ may be formed by using the following plating solution through an electroless plating method.
[0083] The electroless plating can be performed by a method commonly used in the art. In the electroless plating method, both horizontal and / or vertical electroless plating methods are used.
[0084] The electroplating solution may include a copper ion source, a complexing or chelating agent, a reducing agent, water, optionally at least one surfactant, and optionally at least one pH adjuster.
[0085] Examples of copper ion sources may include, but are not limited to, water-soluble halides, nitrates, acetates, sulfates, and other organic and inorganic salts of copper. The copper ion source may be used alone or in combination to provide copper ions. Examples of copper ion sources may include copper sulfate, copper sulfate pentahydrate, copper chloride, copper nitride, copper hydroxide, copper sulfamate, and combinations thereof. The copper ion source may be included in the electroplating solution at a concentration of 0.5 g / l to 30 g / l (e.g., 1 g / l to 25 g / l, e.g., 5 g / l to 20 g / l, e.g., 5 g / l to 15 g / l, e.g., 10 g / l to 15 g / l).
[0086] Examples of complexing agents or chelating agents may include, but are not limited to, sodium potassium tartrate, sodium tartrate, sodium salicylate, sodium salts of ethylenediaminetetraacetic acid (EDTA), nitriloacetic acid and its alkaline metal salts, gluconic acid, gluconate, triethanolamine, modified ethylenediaminetetraacetic acid, S, S-ethylenediamine disuccinic acid, hydantoin and hydantoin derivatives, and combinations thereof. Hydantoin derivatives may include, but are not limited to, 1-methylhydantoin, 1,3-dimethylhydantoin and 5,5-dimethylhydantoin. Complexing agents may be included in the electroplating solution at a concentration of 10 g / l to 150 g / l (e.g., 20 g / l to 150 g / l, e.g., 30 g / l to 100 g / l, e.g., 35 g / l to 80 g / l, and e.g., 35 g / l to 55 g / l). Examples of reducing agents may include, but are not limited to, formaldehyde, formaldehyde precursors and formaldehyde derivatives, such as paraformaldehyde; borohydrides, such as sodium borohydride and substituted borohydrides; boranes, such as dimethylamine borane (DMAB); sugars, such as glucose, sorbitol, cellulose, sucrose, mannitol and gluconolactone; hypophosphites and their salts, such as sodium hypophosphite; hydroquinone; catechol; resorcinol; quinol; pyrogallol; trimellitol; fluorinated sweet alcohol, queacol; gallic acid; 3,4-dihydroxybenzoic acid; phenolsulfonic acid; toluenesulfonic acid; hydroquinonesulfonic acid; catecholsulfonic acid; tyrone; and salts of the foregoing reducing agents. The reducing agent may be included in the electroplating solution at a concentration of 0.5 g / l to 100 g / l, such as 0.5 g / l to 60 g / l, such as 1 g / l to 50 g / l, such as 1 g / l to 20 g / l, such as 1 g / 1 to 10 g / l, such as 1 g / 1 to 5 g / l.
[0087] The pH of the electroplating solution may exceed 7. Optionally, at least one pH adjusting agent is included in the electroplating solution so that the pH of the electroplating solution can be adjusted to an alkaline pH. The pH adjusting agent may include an organic acid, an inorganic acid, an organic base, an inorganic base, or a mixture thereof. For example, the inorganic acid may include phosphoric acid, nitric acid, sulfuric acid, hydrochloric acid, or a combination thereof. For example, the inorganic base may include ammonium hydroxide, sodium hydroxide, potassium hydroxide, or a combination thereof.
[0088] Optionally, at least one surfactant may be included in the electroplating solution. Examples of surfactants may include ionic (e.g., cationic and anionic) surfactants, nonionic and amphoteric surfactants. These surfactants may be used alone or as a mixture thereof. The surfactant may be included in the electroplating solution at a concentration of 0.001 g / l to 50 g / l (e.g., 0.001 g / l to 50 g / l). Cationic surfactants may include, but are not limited to, tetraalkylammonium halides, alkyltrimethylammonium halides, hydroxyethylalkylimidazolines, alkylbenzenemethylammonium halides, alkylamine acetates, alkylamine oleates, and alkylaminoethylglycine. Anionic surfactants may include, but are not limited to, alkylbenzene sulfonates, alkyl or alkoxynaphthalene sulfonates, alkyldiphenylether sulfonates, alkylether sulfonates, alkyl sulfates, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkylphenol ether sulfates, higher alcohol monoesters, polyoxyalkylene alkyl ether phosphonic acids (phosphates), and alkylsulfosuccinates. The nonionic surfactant may include, but is not limited to, alkylphenoxypolyethoxyethanols having 20 to 150 repeating units, polyoxyethylene polymers, and random and block copolymers of polyoxyethylene and polyoxypropylene. The amphoteric surfactant may include, but is not limited to, 2-alkyl-N-carboxymethyl or ethyl-N-hydroxyethyl or methyl imidazolium betaine, 2-alkyl-N-carboxymethyl or ethyl-N-carboxymethyloxyethyl imidazolium betaine, dimethyl alkyl betaine, N-alkyl-β-aminopropionic acid or its salt, and fatty acid amide propyl dimethylaminoacetic acid betaine.
[0089] The thickness of each of the copper plating layers 3 and 3 ′ may be 40 nm to 150 nm, such as 50 nm to 140 nm, or 60 nm to 140 μm. Within the above thickness range, each of the copper plating layers 3 and 3 ′ may be easily electroplated and may have improved dimensional stability with respect to the non-conductive polymer substrate 1 .
[0090] In this specification, the thickness of each layer can be measured by a conventional method known in the art. For example, the thickness of each layer can be measured using an X-ray fluorescence (XRF) analysis method. The X-ray fluorescence analysis method is an analysis method using the following principle: by irradiating a target material with primary X-rays having a constant energy, the amount of specific X-ray energy emitted during the position transfer of external electrons to electrons emitted due to excitation inside the target material is detected, and thus the energy intensity varies depending on the plating thickness.
[0091] <Flexible copper clad laminate 10>
[0092] When the flexible copper clad laminate is left for 1 to 60 days and then heat-treated at 150°C for 30 minutes to obtain an initial size, the flexible copper clad laminate has a dimensional change rate of 0.015 or less relative to the non-conductive polymer substrate, the dimensional change rate being a value obtained by subtracting the minimum size from the maximum size among the initial sizes.
[0093] “Initial size” refers to the average value obtained by measuring the distance between a plurality of standard points marked in a sample cut into a predetermined size, and “size after standing for 1 to 60 days” refers to the average value obtained by measuring the distance between the plurality of standard points after the sample marked with the plurality of standard points is left for 1 to 60 days and then heat-treated at 150°C for 30 minutes.
[0094] <Electronic Devices>
[0095] The electronic device may include the flexible copper clad laminate described above. Examples of the electronic device may include electronic circuit devices and electronic components. Examples of the electronic circuit device may include semiconductor boards, printed circuit boards, and wiring boards. Examples of the electronic device may include display devices such as LCDs and OLEDs.
[0096] <Method of Manufacturing Flexible Copper Clad Laminate 10>
[0097] A method for manufacturing a flexible copper clad laminate may include the following steps: preparing a non-conductive polymer substrate; forming a nickel-containing electroless plating layer on at least one surface of the non-conductive polymer substrate; and forming a copper electroless plating layer on one surface of the nickel-containing electroless plating layer to manufacture the flexible copper clad laminate described above.
[0098] The step of preparing the non-conductive polymer substrate may include a step of drying the non-conductive polymer substrate to remove moisture and residual gas from the non-conductive polymer substrate.
[0099] The step of drying the non-conductive polymer substrate may be performed at 50° C. to 300° C. (e.g., 60° C. to 280° C. or 70° C. to 270° C.) using infrared (IR) heating in a vacuum atmosphere. Within the above drying temperature range, there is an effect of properly removing moisture without deteriorating the quality by damaging the non-conductive polymer substrate.
[0100] In the step of forming the nickel-containing electroless plating layer, the nickel-containing plating layer may be formed by a wet electroless plating method.
[0101] The wet electroless plating method can be performed without being limited to the electroplating conditions and electroplating equipment, and can be appropriately selected and performed according to the conventional method. For example, the wet electroless plating method can be performed by immersing the object to be plated in a nickel-containing electroless plating solution having the above composition or contacting the object with the electroplating solution. In this case, the electroplating treatment temperature can be 45°C to 90°C, such as 47°C to 87°C or 50°C to 85°C. The electroplating treatment time can be appropriately set depending on the thickness of the nickel-plated film to be formed, and can be, for example, 0.1 minutes to 60 minutes, such as 0.5 minutes to 10 minutes. Within the above electroplating treatment temperature and electroplating treatment time, a stable nickel-containing coating can be formed.
[0102] In the step of forming a copper electroless plating layer to manufacture the flexible copper clad laminate described above, a copper plating layer can be formed by a wet electroless plating method. The method for forming a copper plating layer is not limited to electroplating conditions and electroplating equipment, and can be appropriately selected and performed according to conventional methods. For example, the method for forming a copper plating layer can be performed by immersing the object to be electroplated in a copper electroless plating solution having the above composition or contacting the object with the electroplating solution. In this case, the electroplating treatment temperature can be, for example, room temperature to about 50°C. The electroplating treatment time can be appropriately set depending on the thickness of the copper-plated film to be formed, and can be, for example, 0.1 minutes to 60 minutes, for example, 0.5 minutes to 30 minutes. At the above electroplating treatment temperature and electroplating treatment time, a stable copper plating layer can be formed.
[0103] Hereinafter, examples and comparative examples will be described. However, the following example is only one embodiment of the present invention, and it is obvious to those skilled in the art that various changes and modifications can be made within the scope of the scope and technical ideas of the present invention. Naturally, the embodiments to which such changes and modifications are attached belong to the scope of the patent application.
[0104] [Example]
[0105] Example 1: Flexible copper clad laminate
[0106] As a non-conductive polymer substrate, a polyimide film (Kapton 100ECN, manufactured by TDC Corporation) having a thickness of 25 μm was used. Nickel electroless plating layers 2 and 2′ (thickness: about 100 nm) and copper electroless plating layers 3 and 3′ (thickness: about 100 nm) were sequentially formed on both surfaces of the polyimide film substrate 1 by a horizontal electroless plating process to manufacture a flexible copper clad laminate 10, such as Figure 1 As shown in .
[0107] (Nickel Electroless Plating Solution)
[0108] Electroplating solution: The solution is set to have a nickel ion concentration of about 5 g / L in the hydrated nickel salt NiSO4·6H2O.
[0109] Bath temperature: about 60℃
[0110] Nickel precipitation time: about 1 minute
[0111] pH concentration: about 7.3
[0112] (Copper electroless plating solution)
[0113] Electroplating solution: copper sulfate 16.25ml / L, sulfuric acid 3.25ml / L
[0114] Bath temperature: about 34°C
[0115] Nickel precipitation time: about 2.5 minutes
[0116] pH concentration: about 13.0
[0117] Comparative Example 1: Flexible Copper Clad Laminate
[0118] As a non-conductive polymer substrate, a polyimide film (Kapton 100ECN, manufactured by TDC Corporation) having a thickness of 25 μm was used. A Ni—Cr alloy bonding layer and a Cu seed layer were sequentially formed on one surface of the polyimide film substrate 1 by physical vapor deposition (PVD) using a roll-to-roll sputtering apparatus. In this case, the Ni—Cr alloy bonding layer was formed to have a thickness of about 100 μm. The thickness of the Cu seed layer is formed to have a Ni:Cr weight ratio of 80:20 (purity: 99.9% or more), and the Cu seed layer is formed to have a purity of 99.995% using copper. thickness to manufacture flexible copper clad laminates.
[0119] Comparative Example 2: Flexible Copper Clad Laminate
[0120] A copper plating layer having a thickness of about 4 μm was formed on the copper seed layer by an electroplating method using a copper sulfate plating solution. In this case, as the copper sulfate plating solution, a copper plating layer containing Cu at a concentration of about 26 g / L was used. 2+ and a solution of sulfuric acid at a concentration of about 188 g / L. A flexible copper clad laminate was manufactured in the same manner as in Comparative Example 1, except that the substrate was heated at a bath temperature of about 30° C. and at a temperature of about 1.7 A / dm 2 An electric current was applied at a current density of 100 Å to form a copper electroplating layer having a thickness of about 4 μm.
[0121] Analysis Example 1: XRD Analysis
[0122] XRD analysis experiments were performed on the flexible copper clad laminates according to Example 1, Comparative Example 1 and Comparative Example 2. XRD analysis was performed at a CuK-α characteristic X-ray wavelength. In the flexible copper-clad laminate according to Example 1, the peak of the (111) plane was observed at an angle of 43° of Bragg 2θ, as shown in FIG. Figure 2 After each of the flexible copper clad laminates according to Example 1, Comparative Example 1 and Comparative Example 2 was left for 60 days, the half-value width (FWHM) obtained from the peak value of the (111) plane by the following mathematical formula 1 was used to calculate the half-value width change rate thereof. The results are given in the following Table 1.
[0123] <Mathematical formula 1>
[0124] Half-value width (111) change rate = {(half-value width after leaving for 60 days) - (initial half-value width)}.
[0125] [Table 1]
[0126]
[0127] Referring to Table 1, after the flexible copper clad laminate according to Example 1 was left for 60 days, the half-value width change rate of its peak value relative to the (111) plane was almost unchanged (0.01), but in the flexible copper clad laminates according to Comparative Examples 1 and 2, the half-value width change rate of its peak value relative to the (111) plane changed to some extent by 0.095 and 0.024, respectively.
[0128] According to these results, it can be found that the flexible copper clad laminate according to Example 1 is improved in crystallinity compared to the flexible copper clad laminates according to Comparative Examples 1 and 2.
[0129] Analysis Example 2: Dimensional Stability Analysis
[0130] The dimensional stability of the flexible copper clad laminates according to Example 1, Comparative Example 1 and Comparative Example 2 relative to the polyimide substrate film within 60 days was analyzed. The results are given in Table 2 below.
[0131] The dimensional stability was analyzed by the following method.
[0132] Each of the flexible copper clad laminates according to Example 1, Comparative Example 1 and Comparative Example 2 was cut to a size of 295 mm×235 mm to prepare a sample. The sample was marked with eight standard points ( Figure 3a ). Use a three-dimensional measuring instrument to measure the distance between standard points ( Figure 3b) to obtain an average value (initial value). Eight points corresponding to the standard points are punched out on the surface of the polyimide substrate film of the sample, and the sample is placed in a constant temperature and humidity chamber (23°C ± 2°C, 50% ± 5%) for 1 to 60 days. Thereafter, the sample is heat treated at 150°C for 30 minutes and the sample is placed in a constant temperature and humidity chamber for 24 hours, and then the distance between the eight points corresponding to the standard points relative to the polyimide substrate film is measured by a three-dimensional measuring instrument to obtain an average value (the size after being placed for 1 to 60 days), and the value obtained by subtracting the minimum size from the maximum size among the sizes is defined as the size change rate.
[0133] [Table 2]
[0134] Example 1 Comparative Example 1 Comparative Example 2 initial 0.107 0.065 0.054 Size after 5 days of storage 0.104 0.071 0.059 Size after 7 days of storage 0.106 0.067 0.061 Size after 10 days of storage 0.096 0.068 0.055 Dimensions after 15 days of storage 0.099 0.069 0.056 Dimensions after 20 days of storage 0.097 0.057 0.064 Dimensions after 30 days of storage 0.110 0.053 0.059 Dimensions after 45 days of storage 0.098 0.056 0.047 Dimensions after 60 days of storage 0.099 0.053 0.049
[0135] Referring to Table 2, it can be found that the dimensional change rate of the flexible copper clad laminate according to Example 1 relative to the polyimide substrate film is 0.014. It can be found that the dimensional change rates of the flexible copper clad laminates according to Comparative Examples 1 and 2 relative to the polyimide substrate film are 0.018 and 0.017, respectively. Based on these structures, it can be found that the flexible copper clad laminate according to Example 1 has excellent dimensional stability relative to the polyimide substrate film within 60 days compared with the flexible copper clad laminates according to Comparative Examples 1 and 2.
Claims
1. A double-sided flexible copper-clad laminate, comprising: Non-conductive polymer substrate; an electroless nickel-containing layer disposed on both surfaces of the non-conductive polymer substrate; and an electroless copper layer disposed on both surfaces of the electroless nickel layer, Wherein, in the X-ray diffraction spectrum, the peak of the copper electroless plating layer relative to the (111) plane has a half-value width change rate of 0.01° or less calculated by Mathematical Formula 1: <Mathematical formula 1> Half-value width (111) change rate = {(half-value width after 60 days of storage) - (initial half-value width)}, Wherein, the storage is carried out at a temperature of 21° C. to 25° C. and a humidity of 45% to 55%.
2. The double-sided flexible copper clad laminate according to claim 1, wherein: In an X-ray diffraction spectrum, the peak of the electroless copper layer relative to the (111) plane has a half-value width of 0.20° to 0.35°. 3 . The double-sided flexible copper clad laminate as claimed in claim 1 , wherein the copper electroless plating layer has a thickness of 40 nm to 150 nm.
4. The double-sided flexible copper clad laminate according to claim 1, wherein: When the double-sided flexible copper clad laminate is left for 1 to 60 days and then heat-treated at 150°C for 30 minutes, the double-sided flexible copper clad laminate has a dimensional change rate of 0.015 or less relative to the non-conductive polymer substrate, the dimensional change rate being a value obtained by subtracting the minimum dimension from the maximum dimension among the dimensions of the double-sided flexible copper clad laminate. The double-sided flexible copper clad laminate as claimed in claim 1 , wherein the nickel-containing electroless plating layer comprises a nickel layer. The double-sided flexible copper clad laminate as claimed in claim 1 , wherein the nickel-containing electroless plating layer has a thickness of 40 nm to 250 nm.
7. The double-sided flexible copper clad laminate as claimed in claim 1, wherein the non-conductive polymer substrate comprises at least one selected from the group consisting of phenol-based resins, novolac-based resins, allyl-based resins, epoxy-based resins, polyethylene-based resins, polypropylene-based resins, polyester-based resins, and polyimide-based resins.
8. An electronic device comprising the double-sided flexible copper clad laminate according to any one of claims 1 to 7.
9. A method for manufacturing a double-sided flexible copper clad laminate, the method comprising: preparing a non-conductive polymer substrate; forming an electroless plating layer containing nickel on both surfaces of the non-conductive polymer substrate; and A copper electroless plated layer is formed on both surfaces of the nickel-containing electroless plated layer to produce a double-sided flexible copper clad laminate according to any one of claims 1 to 7.