Diamond-metal high temperature solid-state interface reaction sample preparation method
Through the diamond-metal high-temperature solid-state reaction sample preparation method, the problem in the existing technology that the diamond-metal interface reaction is mainly a solid-liquid reaction at a microscopic scale is solved. The high-temperature solid-state reaction between diamond and metal is realized and perfected. It has developed a diamond-metal reaction test process and is suitable for studying the high-temperature reaction mechanism between large-sized diamond and metal.
Patent Information
- Application Number
- CN202110517776.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In existing diamond processing methods, the diamond-metal interface reaction is mainly concentrated in the solid-liquid reaction system at the microscopic scale. There is a lack of research on solid-solid reaction systems, and the commonly used powdered metal reaction methods can easily lead to environmental pollution and powder oxidation.
The diamond-metal high-temperature solid-state interface reaction sample preparation method is adopted. The diamond and metal are processed into a flat block to ensure the parallelism of the contact surface, and a clamping device is used to fix the diamond and metal, and vacuum heating is performed to achieve high-temperature solid-state interface reaction.
It achieves full contact and high-temperature solid-state reaction between diamond and metal, avoids displacement, is suitable for research on the high-temperature reaction mechanism between large-sized diamond and metal, and improves the diamond-metal reaction test process.
Smart Images

Figure CN113311101B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of research on the reaction mechanism of diamond and metal, and in particular to a method for preparing a diamond-metal high-temperature solid-state interface reaction sample. Background Art
[0002] Diamond is the hardest substance in nature and has good physical and stable chemical properties. It can be widely used in the field of tool preparation. In addition, diamond has advantages such as wide bandgap and high thermal conductivity. It can be used to prepare optical and semiconductor components in extreme situations, such as lenses in Raman lasers and other precision instruments. Therefore, the processing of diamond semiconductors has become an urgent problem to be solved at this stage.
[0003] At present, the commonly used diamond processing methods are mainly the following: salt etching, metal solid catalytic processing, chemical processing, mechanical and chemical composite processing, etc. At present, the above processing methods are mostly concentrated on the research of process parameters and processing effects, but there are few studies on their processing mechanisms and catalytic mechanisms, especially on the changes in the properties of diamond itself caused by changes in temperature or pressure under different processing conditions.
[0004] The above method is based on the diamond phase change to achieve diamond processing. Due to the unique properties of diamond itself, such as high hardness and high wear resistance, diamond itself is extremely difficult to process, so it is necessary to reduce the hardness of diamond to achieve processing. The most direct way to reduce the hardness of diamond is to make the diamond surface undergo a phase change. Under normal circumstances, the diamond phase change needs to cross a very high potential barrier to achieve, and it can only be achieved under high temperature and high pressure or catalytic conditions of catalytic metals. Therefore, reducing the diamond phase change barrier is a necessary condition for achieving diamond processing. Currently, the commonly used methods to reduce the hardness of diamond, that is, to reduce the diamond phase change reaction conditions, are: mechanical methods and chemical methods. The mechanical method is to use pressure and rotation speed to reduce the diamond phase change barrier during the processing process; the chemical method is to use metal elements with similar crystal structure and structural parameters to diamond. When the metal element meets the "alignment principle", the metal will convert the sp3 hybridized carbon atoms into sp2 hybridized carbon atoms, reducing the energy required for the diamond phase change, so that the diamond undergoes a phase change or generates carbides under lower conditions. After the catalytic phase change occurs, a layer of graphite or carbide with a hardness lower than that of diamond itself is generated on the surface of diamond, making diamond easy to process.
[0005] Based on the above-mentioned process requirements, the research on diamond-metal interface reaction is the basis for realizing the process and optimizing the process parameters of different reaction systems. In the existing diamond-metal reaction system research, the test method of metal powder wrapped diamond is adopted, such as CN103231054B, CN102814749A, CN106312056B. However, in the metal powder and diamond reaction system, due to the size effect of the metal powder, most metals will form micro-droplets on the diamond surface, that is, what is established is the solid-state (diamond)-liquid (powder droplet) reaction system under microscopic scale, and the research on solid-state (diamond)-solid-state (solid metal) system is still less. At the same time, adopt powdered metal to react with diamond, which is very easy to cause environmental pollution and powder oxidation during the experiment. Summary of the invention
[0006] The present invention provides a method for preparing a diamond-metal high temperature solid-state interface reaction sample, which overcomes the shortcomings of the background technology.
[0007] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a diamond-metal high-temperature solid-state interface reaction sample, comprising:
[0008] Step 1, processing diamond and metal into flat blocks or sheets;
[0009] Step 2, processing the diamond and the metal so that the parallelism of the diamond and the metal reaches a predetermined requirement;
[0010] Step 3, grinding and polishing the contact surface of diamond and metal where a high-temperature solid-state interface reaction is about to occur;
[0011] Step 4, using acetone solution to ultrasonically clean the diamond and metal and dry them;
[0012] Step 5, assembling the diamond and the metal and ensuring that the contact surfaces of the diamond and the metal are in full contact;
[0013] Step 6, placing the assembled diamond and metal in a vacuum heating furnace for aging or temperature variation treatment to obtain a high-temperature solid-state interface reaction sample;
[0014] Step 7: Observe the sample morphology and analyze the sample composition.
[0015] In one embodiment: In step 2, a vernier caliper is used to measure the parallelism of the diamond and the metal. If the parallelism does not meet the predetermined requirement, rough grinding is performed to meet the requirement.
[0016] In one embodiment, the diamond is an artificial single crystal or polycrystalline diamond with a fixed plane size, and the metal is a sheet-like high-purity metal element or alloy.
[0017] In one embodiment: In step 5, a clamping device is used to mount the diamond and the metal. The clamping device includes a stage, a sample fixing pin, a pin holder and a fixed pressure head. The stage includes a stage body and two horizontally spaced columns fixed on the stage body. The facing side walls of the two columns are recessed with loading grooves. Both ends of the pin holder are inserted into the loading grooves. The sample fixing pin can pass through the pin holder so as to be adjusted up and down. The lower end of the sample fixing pin is connected to the fixed pressure head. The diamond and the metal are stacked up and down on the stage body. The sample fixing pin is rotated and the fixed pressure head is pressed against the diamond.
[0018] In one embodiment: the clamping device also includes a nail seat fixing nail, the top surface of the column is recessed with a through slot that penetrates the loading slot, the nail seat fixing nail passes through the through slot and is screwed to the nail seat so that the nail seat can be adjusted up and down by rotating the nail seat fixing nail.
[0019] In one embodiment: the clamping device also includes a nail seat fixing nail, the top surface of the column is recessed with a through slot that penetrates the loading slot, and the nail seat fixing nail passes through the through slot and presses against the nail seat.
[0020] In one embodiment: the bottom surface of the sample fixing nail is concavely provided with a revolving groove, the fixed pressure head includes a pressing part and a rotating shaft fixed on the top surface of the pressing part, the rotating shaft and the revolving groove are adapted and can rotate relatively, and the pressing part presses on the diamond.
[0021] In one embodiment: the clamping device is made of high-purity alumina ceramics.
[0022] In one embodiment, step 5 includes:
[0023] Step A, stacking diamond and metal on top of each other on a table;
[0024] Step B, placing a fixed indenter on the diamond;
[0025] Step C, attaching the sample fixing nail to the nail holder;
[0026] Step D, inserting the nail holder into the loading slot of the stage, and adjusting the sample fixing nail so that the sample fixing nail contacts the fixed pressure head;
[0027] Step E, gradually tightening the sample fixing pins so that the fixed pressure head is pressed tightly against the diamond;
[0028] Step F, tighten the nail base fixing nails to fix the nail base and the stage.
[0029] Compared with the background technology, this technical solution has the following advantages:
[0030] The present invention proposes a method for preparing diamond-metal high-temperature solid-state interface reaction samples. The diamond interface is in full contact with the metal interface and no displacement occurs. The diamond and metal react fully at high temperature. The method is suitable for the solid-solid reaction system in the diamond-metal reaction system, improves the diamond-metal reaction test process, improves the research process of the high-temperature reaction mechanism between large-size diamond and metal, and lays a good foundation for subsequent experimental research.
[0031] The clamping device includes a stage, a sample fixing pin, a pin holder and a fixed pressure head. The diamond and the metal are stacked on the stage. The sample fixing pin is rotated and the fixed pressure head is pressed against the diamond, which can firmly fix the diamond-metal to avoid displacement. At the same time, the slight deformation of the clamping device under higher temperature conditions will not affect the experimental results. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0033] Figure 1 It is a schematic structural diagram of a clamping device according to a specific implementation method.
[0034] Figure 2 It is a schematic front view of a loading platform of a specific implementation method.
[0035] Figure 3 It is a front view schematic diagram of a nail seat of a specific implementation method.
[0036] Figure 4 It is a top view schematic diagram of a nail seat of a specific implementation method.
[0037] Figure 5 It is a structural schematic diagram of the sample fixing nail and the fixed pressure head assembly according to a specific implementation method. DETAILED DESCRIPTION
[0038] Please refer to Figures 1 to 5 The clamping device includes a stage 1, a sample fixing pin 2, a pin seat 3, a pin seat fixing pin 4 and a fixed pressure head 5.
[0039] The stage 1 comprises a body and two columns fixed on the body at horizontal intervals, and the facing side walls of the two columns are both recessed with loading grooves 11; the two ends of the nail seat 3 are inserted into the loading grooves 11; the sample fixing nail 2 can pass through the nail seat 3 so as to be adjusted up and down, and the lower end of the sample fixing nail 2 is connected to the fixed pressure head 5, and the diamond 6 and the metal 7 are stacked up and down on the body. The sample fixing nail 2 is rotated and the fixed pressure head 5 is pressed against the diamond 6. On the one hand, it can adapt to different sample heights, and on the other hand, the pressing force can be adjusted to adapt to metals of different hardness; the top surface of the column is recessed with a through groove 12 that passes through the loading groove 11, and the nail seat fixing nail 4 is screwed into the through groove 12 and pressed against the nail seat 3. In the specific structure: a rotary groove 21 is concavely provided on the bottom surface of the sample fixing nail 2, and the fixed pressure head 5 includes a pressing portion 51 and a rotating shaft 52 fixed on the top surface of the pressing portion 51. The rotating shaft 52 and the rotary groove 21 are adapted and can rotate relative to each other so that the two can rotate relative to each other when the sample fixing nail 2 is rotated, so that the fixed pressure head 5 can be statically pressed against the diamond 6 to avoid the movement of the diamond and improve the reaction monitoring accuracy; the clamping device is made of high-purity alumina ceramics to withstand a high temperature of 1700°C, to meet the temperature conditions of most solid-phase interface reactions, and to perform mechanical micromachining to prepare a clamping device suitable for clamping diamond-metal samples.
[0040] The method for preparing diamond-metal high temperature solid-state interface reaction samples comprises:
[0041] Step 1, processing diamond 6 and metal 7 into flat blocks or sheets, such as rectangular or circular structures, wherein the diamond 6 is an artificial single crystal or polycrystalline diamond with a fixed plane size, and the metal 7 is a sheet-shaped high-purity metal element or alloy;
[0042] Step 2, processing the diamond 6 and the metal 7 so that the parallelism of the diamond 6 and the metal 7 reaches a predetermined requirement; specifically, using a vernier caliper to measure the parallelism of the diamond 6 and the metal 7, if the parallelism does not reach the predetermined requirement, rough grinding is used to meet the requirement;
[0043] Step 3, grinding and polishing the contact surface of the diamond 6 and the metal 7 where a high-temperature solid-state interface reaction is about to occur;
[0044] Step 4, using acetone solution to ultrasonically clean the diamond 6 and the metal 7 and dry them to remove oil stains on the sample surface and debris after grinding and polishing;
[0045] Step 5, assembling the diamond 6 and the metal 7 and ensuring that the contact surfaces of the diamond 6 and the metal 7 are in full contact;
[0046] Step 6, placing the assembled diamond 6 and metal 7 in a vacuum heating furnace for aging or temperature-changing treatment to obtain a high-temperature solid interface reaction sample; the aging or temperature-changing treatment is based on heating at 500, 600, 700, 800, 900° C. for a predetermined time, such as 1-5 hours;
[0047] Step 7: Observe the sample morphology and analyze the sample composition.
[0048] In this specific implementation mode: step 5 includes:
[0049] Step A, stacking diamond 6 and metal 7 on top of each other on a table;
[0050] Step B, placing the fixed pressure head 5 on the diamond 6;
[0051] Step C, attaching the sample fixing nail 2 to the nail seat 3;
[0052] Step D, insert the nail holder 3 into the loading slot 11 of the stage, and adjust the sample fixing nail 2 so that the sample fixing nail 2 contacts the fixed pressure head 5;
[0053] Step E, according to the hardness of the metal sample or the test requirements, gradually tighten the sample fixing pin 2 so that the fixed pressure head 5 is pressed tightly against the diamond 6, ensuring that the diamond 6 and the metal 7 will not be displaced during the tightening process; the total height of the diamond 6 and the metal 7 determines the tightening height of the sample fixing pin, so the device is suitable for the preparation of interface samples with different thicknesses, and samples of different thicknesses can be clamped by adjusting the height of the sample fixing pin;
[0054] Step F, tighten the nail base fixing nail 4 to fix the nail base 3 and the loading platform 1.
[0055] The above-mentioned assembly can avoid the movement of the diamond and the metal and can enhance the pressing force.
[0056] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. Diamond-metal high temperature solid-state interface reaction sample preparation method, Features: include: Step 1, processing diamond and metal into flat blocks or sheets; Step 2, processing the diamond and the metal so that the parallelism of the diamond and the metal reaches a predetermined requirement; Step 3, grinding and polishing the contact surface of diamond and metal where a high-temperature solid-state interface reaction is about to occur; Step 4, using acetone solution to ultrasonically clean the diamond and metal and dry them; Step 5, assembling the diamond and the metal and ensuring that the contact surfaces of the diamond and the metal are in full contact; Step 6, placing the assembled diamond and metal in a vacuum heating furnace for aging or temperature-changing treatment to obtain a temperature-changing solid-state interface reaction sample; Step 7, morphological observation of samples and analysis of sample components; Wherein: in step 5, a clamping device is used to mount the diamond and the metal, and the clamping device includes a stage, a sample fixing nail, a nail seat and a fixed pressure head. The stage includes a stage body and two columns fixedly arranged on the stage body at horizontal intervals, and the facing side walls of the two columns are both recessed with loading grooves, and the two ends of the nail seat are inserted into the loading grooves, and the sample fixing nail can pass through the nail seat to be adjusted up and down, and the lower end of the sample fixing nail is connected to the fixed pressure head, and the diamond and the metal are stacked up and down on the stage body, and the sample fixing nail is rotated and the fixed pressure head is pressed against the diamond; the clamping device also includes a nail seat fixing nail, and the top surface of the stage column is recessed with a through groove passing through the loading groove, and the nail seat fixing nail passes through the through groove and is screwed to the nail seat so as to adjust the nail seat up and down by rotating the nail seat fixing nail; the bottom surface of the sample fixing nail is recessed with a rotary groove, and the fixed pressure head includes a pressing portion and a rotating shaft fixedly arranged on the top surface of the pressing portion, and the rotating shaft and the rotary groove are adapted and can rotate relatively, and the pressing portion is pressed against the diamond; The step 5 includes: step A, stacking the diamond and the metal on the table; step B, placing the fixed pressure head on the diamond; step C, installing the sample fixing nail on the nail seat; step D, inserting the nail seat into the loading slot of the stage, adjusting the sample fixing nail so that the sample fixing nail contacts the fixed pressure head; step E, gradually tightening the sample fixing nail so that the fixed pressure head is pressed tightly against the diamond; step F, tightening the nail seat fixing nail to fix the nail seat and the stage.
2. The method for preparing diamond-metal high temperature solid state interface reaction samples according to claim 1, Features: In step 2, a vernier caliper is used to measure the parallelism of the diamond and the metal. If the parallelism does not meet the predetermined requirement, rough grinding is performed to meet the requirement.
3. The method for preparing diamond-metal high temperature solid state interface reaction samples according to claim 1, Features: The diamond is an artificial single crystal or polycrystalline diamond with a fixed plane size, and the metal is a flake-shaped high-purity metal single substance or alloy.
4. The method for preparing diamond-metal high temperature solid state interface reaction samples according to claim 1, 2 or 3, Features: The clamping device also includes a nail seat fixing nail. The top surface of the platform column is concavely provided with a through slot that penetrates the loading slot. The nail seat fixing nail passes through the through slot and is pressed against the nail seat.
5. The method for preparing diamond-metal high temperature solid state interface reaction samples according to claim 1, 2 or 3, Features: The clamping device is made of high-purity alumina ceramics.
Citation Information
Patent Citations
Metallic bond diamond grinding wheel with good self-sharpening performance
CN102814749A
Sintering-brazing method of metal matrix diamond segments
CN103231054B
A method for metallizing diamond surfaces
CN106312056B
Multipurpose scanning electron microscope sample platform
CN208284450U
Clamping device for preparing diamond-metal high-temperature solid interface reaction sample