Polymer formulations for lining metal cores and methods for producing composite piezoelectric fibers
By using a solvent-based coating method during spinning, combined with P(VDF-TrFE) copolymer, surfactant and adhesion promoter, the problems of conductivity and thickness control are solved, and efficient and simplified piezoelectricity is achieved. Fiber manufacturing, suitable for industrial applications.
Patent Information
- Application Number
- CN201980089148.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-20
- Filing Date
- 2019-12-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-12-11
AI Technical Summary
The prior art is difficult to obtain polymer layers of high conductivity and low thickness during spinning, especially when fluorine-containing polymers are used, and the alignment of the conductive fillers results in a reduced conductivity, and the use of complex electrowetting methods requires High voltage and difficult to control thickness.
Using a solvent-based coating method, 10-30% by mass of P(VDF-TrFE) copolymer solution, surfactant and adhesion promoter are used to improve the wetting of the polymer layer by volatile solvents and adhesion promoters. and adhesion, realize the method of continuous manufacturing of piezoelectric fibers.
The optimal adhesion and homogenous polymer layer are achieved on exposed wires, reducing the polymer layer thickness, avoiding the use of high voltages, and simplifying the manufacturing process, suitable for industrial production.
Smart Images

Figure HDA0003164035830000011 
Figure HDA0003164035830000021 
Figure HDA0003164035830000022
Abstract
Description
Technical Field
[0001] The present invention relates to the field of composite piezoelectric fibers. More particularly, the present invention relates to multicomponent fibers with piezoelectric effect, comprising an electroactive fluoropolymer shell adhered to a metal core. The present invention also relates to a solvent-based fluoropolymer formulation that enables optimal adhesion to bare conductive metal filaments to be obtained. The present invention also relates to a method for making these composite fibers, as well as their use in different fields of technical textiles, composite materials, filtration and electronics. Background Art
[0002] Ferroelectric and relaxor ferroelectric materials that generate mechanical effects induced by external electric fields have attracted widespread attention and have been recognized for applications in various transducers, actuators, and transformers.
[0003] Among piezoelectric materials, ceramics are the most commonly used materials due to their good actuation properties and their very wide bandwidth. However, they have brittleness, which hinders their application to curved or complex surfaces.
[0004] Other conductive devices use a polymer film sandwiched between two electrodes. Among the polymers that can be used, fluoropolymers based on vinylidene fluoride (VDF) in particular represent a class of compounds with outstanding properties for a large number of applications. Polyvinylidene fluoride (PVDF) and copolymers containing VDF and trifluoroethylene (TrFE) are of particular interest due to their piezoelectric properties.
[0005] These flexible piezoelectric structures are commercially available only in the form of films. However, certain applications require the availability of polymer piezoelectric fibers, which can be directly implanted into certain materials to form "smart" materials.
[0006] Such fibers have been made in the laboratory in either single-component or multi-component forms.
[0007] Multicomponent spinning of conductive polymers and piezoelectrically active polymers simultaneously allows the production of 100% polymer multilayer fibers. For example, the applicant has described such fibers in patent application WO 2018 / 224583, which relates to piezoelectric polymer fibers composed of three different polymer layers: a layer composed of at least one fluoropolymer, a layer comprising at least one polyolefin, and a polyamide layer.
[0008] In general, conductive polymers used as electrodes must meet the following criteria: be able to be used by extrusion; be sufficiently fluid to be used in a spinning process; have a spinning temperature close to that of the constituent piezoelectric material of the fiber, and be sufficiently conductive to ensure biasing of the fiber and efficient recovery of the charge generated during deformation of the piezoelectric material.
[0009] To meet all these criteria, the use of conductive polymer compounds (abbreviated CPC) is generally favored. However, intrinsically conductive polymers such as polyaniline; the mixture PEDOT:PSS, where PEDOT stands for poly(3,4-ethylenedioxythiophene) and PSS stands for poly(styrenesulfonate); or polypyrrole cannot be used in the melt route. Therefore, the skilled person will make CPC as follows: using spinning grade polymers such as polyamide (PA), polyethylene (PE), poly(ethylene oxide) (PEO) or poly(ethylene terephthalate) (PET), combining them with conductive fillers such as carbon black, carbon nanotubes, graphene, silver nanowires or metal nanowires, gold nanoparticles, etc.
[0010] Although the conductivity of CPC particles is generally acceptable (e.g., up to 1000 S / m), this value is greatly reduced when the material is used in filament form, in some cases by 10%. 3 or even 10 6 This phenomenon is mainly due to the alignment of the conductive fillers during the spinning process, which leads to a decrease in the electrical permeation of these fillers and, thus, a decrease in the overall conductivity of the CPC filaments.
[0011] In order to solve this problem, it has been proposed to use a metal core (for example made of stainless steel) coated with a piezoactive polymer provided by extrusion, a technique known as melt cladding. This technique is difficult to implement in practice. It requires a piezoactive polymer with a low melt viscosity and leads to substantial coating thicknesses of more than 100 μm. Another problem is the centering of the metal core in the polymer coating, which makes it more difficult to control a smaller desired thickness.
[0012] In the case of piezoelectric fibers, polymer layer thicknesses of less than 50 μm are desired to obtain a linear piezoelectric response of deformation by overcoming the viscoelastic behavior of PVDF-type polymers. Furthermore, excessive polymer thicknesses require the application of high bias voltages, which can be problematic because they lead to air breakdown or require complex equipment.
[0013] The use of solvent-based coating methods makes it possible to overcome these viscosity problems and obtain fluoropolymer layers of lower thickness, typically between 1 and 30 μm.The main challenge of this technology is to produce an adhesive polymer layer at the surface of the metal wire, especially when using fluoropolymers.
[0014] The publication "Polymeric piezoelectric fiber with metal core produced by electrowetting-aided dry spinning method." J. Appl. Polym. Sci. 133, n / an / a (2016) by Liu, W., Chen, R., Ruan, X. and Fu, X. describes electrowetting-assisted solvent-based coating (layer) of PVDF or P (VDF-TrFE) copolymer on a metal core. A copper wire with a diameter of 100 μm enameled with polyester-imide (6 μm thick) was used as a central core. PVDF (Mw = 5340 000) and P (VDF-TrFE) (VDF / TrFE mass ratio: 70 / 30) copolymer in powder form were dissolved in a 1 / 1 dimethylformamide / acetone mixture at concentrations of 10, 15 and 20 w%. The glazed wire was passed through a solution of the polymer and through a copper needle with a diameter of 1 mm, and then through a series of concentric electrodes from 3.5 mm to 0.5 mm. The coating nozzle is biased at 1 kV. The copper core stripped of its glaze is grounded and the electrodes are connected to a continuous high voltage of 4 kV. The applied field is less than 20 MV / m. Crystallization of the polymer is carried out by solvent evaporation. The obtained fibers are metallized with gold by cathode sputtering. The authors show that the use of the electrowetting method makes it possible to obtain polymer layers on copper that are more homogeneous, smoother and more adhesive than in the absence of high voltage. The layer using 15% P(VDF-TrFE) is more homogeneous than the PVDF layer. The β phase is obtained when an electric field is applied. Coating thicknesses between 3 and 8 μm are obtained with most of the solutions used. The thickness uniformity is improved by using high voltages. However, the method remains complex to use and involves high voltages during manufacturing. In addition, no proof of adhesion of the fluoropolymer to the glazed wires is provided, such as microscopic images of parts of the obtained silk.
[0015] It is therefore desirable to develop a fluoropolymer-based coating formulation that allows for optimal adhesion to bare conductive metal wires to be obtained by a simple solvent-based process for continuous coating of the wires with a piezoelectric polymer without prior glazing or cladding. The present invention is also directed to providing a multicomponent fiber having a piezoelectric effect comprising an electroactive fluoropolymer shell adhered to a metal core. Summary of the invention
[0016] The present invention firstly relates to a polymer formulation for coating a metal core, comprising the following components:
[0017] a) a 10-30% by mass solution of a P(VDF-TrFE) copolymer in a volatile solvent,
[0018] b) a surfactant, and
[0019] c) Adhesion promoters.
[0020] According to one embodiment, the P(VDF-TrFE) copolymer consists of units derived from VDF and TrFE, and the proportion of the units derived from TrFE ranges from 5 mol% to 95 mol% relative to the sum of the units derived from VDF and TrFE.
[0021] According to one embodiment, the volatile solvent is selected from the following list:
[0022] - ketones, in particular methyl isobutyl ketone, methyl ethyl ketone (MEK), cyclopentanone and acetone,
[0023] - esters, in particular ethyl acetate, methyl acetate, propyl acetate, butyl acetate and propylene glycol methyl ether acetate,
[0024] - amides such as dimethylformamide and dimethylacetamide,
[0025] - dimethyl sulfoxide,
[0026] - furans, especially tetrahydrofuran,
[0027] - carbonates, especially dimethyl carbonate,
[0028] - phosphate esters, especially triethyl phosphate,
[0029] - and mixtures thereof.
[0030] The surfactant ensures optimal wetting of the solution of the fluorinated copolymer on the metal core. According to one embodiment, the surfactant is non-ionic, preferably based on an acrylic copolymer.
[0031] Adhesion promoters help improve the wetting of the solution of fluorinated copolymer on the metal core and also make it possible to obtain an adhesive coating of the copolymer on the wire. It is a polymer functionalized with associative groups such as -NH2, -OH, -COOH or other.
[0032] According to one embodiment, the adhesion promoter comprises a functional copolymer of the hydroxyl type having acid groups or an adhesive of the ethoxysilane type.
[0033] According to one embodiment, for 10s -1 At a shear rate of 1.5 Å, the viscosity of the coating formulation is between 1 and 500 Pa.s. Preferably, the viscosity of the coating solution is between 10 and 100 Pa.s. Finally, solutions that show shear-thickening behavior are advantageous.
[0034] The present invention also relates to a solvent-based method for continuously manufacturing a composite piezoelectric fiber comprising a metal filament covered with a piezoelectric fluoropolymer layer, the method comprising the steps of:
[0035] i) provide bare metal wires,
[0036] ii) coating the metal wire with a coating formulation according to the invention, comprising passing the metal wire through a coating nozzle into which the coating formulation is injected, to obtain a coated metal wire,
[0037] iii) drying the coated metal wire to evaporate the solvent,
[0038] iv) heating the dried coated metal film to achieve thermal annealing.
[0039] The method further comprises a step v) of winding the coated metal wire, which can be performed before or after the thermal annealing step.
[0040] The metal wire acts as the internal electrode. Various uses of the composite piezoelectric wire require the deposition of external electrodes on the polymer sheath.
[0041] According to one embodiment, the method according to the invention comprises a further step vi) of continuously covering the coated metal wire with a counter electrode. This operation for depositing the external electrode can advantageously be carried out in-line, after the drying and annealing steps previously described, and before the winding step.
[0042] The method according to the invention further comprises a step vii) of biasing the piezoelectric polymer deposited on the surface of the metal core. This biasing can be done in various ways before or after the deposition of the external electrodes.
[0043] The invention also relates to a composite piezoelectric fiber comprising an electroactive fluoropolymer shell adhered to a metallic core. Advantageously, the fiber according to the invention has an elastic deformation of between 1% and 5%.
[0044] Another subject matter of the invention relates to the use of composite piezoelectric fibers in various applications, such as instrumented composites, the manufacture of technical textiles, the manufacture of textile products, fluid filtration and electronics.
[0045] The present invention makes it possible to overcome the disadvantages of the prior art. In particular, the present invention provides a coating formulation based on fluoropolymers that makes it possible to obtain optimal adhesion on bare conductive metal wires without the need for prior glazing or coating for attachment. The coating formulation is used by a simple solvent-based process for the continuous manufacture of wire coatings with piezoelectric polymers. The process is easy to industrialize and does not require the properties of the surface for wetting the bare metal wire to be changed by applying a voltage (electrowetting). BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 Scanning electron microscope images of a copper wire with a diameter of 700 μm, coated with a layer of a formulation based on 20% P(VDF-TrFE) copolymer in MEK are shown. Images b and d relate to fibers according to the invention, whose coating contains a surfactant (1%) and an adhesion promoter (0.25%). Images a and c relate to comparative fibers, whose coating contains no surfactant and no adhesion promoter. Figure 1 c is Figure 1 Enlarged view of a. Figure 1 d is Figure 1 Enlarged view of b.
[0047] Figure 2 Six bias curves obtained by gradually increasing the electric field at the end of the piezoelectric fiber are shown. The ferroelectric effect is clearly demonstrated by the hysteresis phenomenon and the increase of the zero-field permanent bias. These curves are obtained by changing the electric field at a frequency of 1 Hz.
[0048] Figure 3 The values in μC / cm obtained for the maximum electric field values of +86 MV / m and -86 MV / m are shown. 2 The figure also shows the curve of the current (in μA) obtained during this bias. The current peak corresponds to the value of the coercive field, which is the field required for the electric dipoles to align, and is additional evidence of the ferroelectric and piezoelectric behavior obtained.
[0049] Figure 4 is a schematic diagram illustrating one-step DC biasing of a wrap having a piezoelectrically active polymer and a counter electrode. DETAILED DESCRIPTION
[0050] The invention is now described in more detail and in a non-limiting manner in the following description.
[0051] According to a first aspect, the present invention relates to a coating formulation comprising the following components:
[0052] a) a 10-30% by mass solution of a P(VDF-TrFE) copolymer in a volatile solvent,
[0053] b) a surfactant, and
[0054] c) Adhesion promoters.
[0055] According to various embodiments, the formulation comprises the following features, in combination where appropriate.
[0056] Fluorinated copolymer
[0057] The fluorinated copolymer of formula P (VDF-TrFE) is composed of units derived from vinylidene fluoride and units derived from trifluoroethylene. The proportion of units derived from TrFE relative to the sum of units derived from VDF and TrFE is preferably 5 mol% to 95 mol%, and in particular: 5 mol% to 10 mol%; or 10 to 15 mol%; or 15 to 20 mol%; or 20 to 25 mol%; or 25 to 30 mol%; or 30 to 35 mol%; or 35 to 40 mol%; or 40 to 45 mol%; or 45 to 50 mol%; or 50 to 55 mol%; or 55 to 60 mol%; or 10 or 60 to 65 mol%; or 65 to 70 mol%; or 70 to 75 mol%; or 75 to 80 mol%; or 80 to 85 mol%; or 85 to 90 mol%; or 90 to 95 mol%.
[0058] Particularly preferred is a range of 15 to 55 mol %.
[0059] The molar composition of the units in the P(VDF-TrFE) copolymer can be determined in various ways (e.g. infrared spectroscopy or Raman spectroscopy). Conventional methods of elemental analysis of the elements carbon, fluorine and chlorine or bromine or iodine (e.g. X-ray fluorescence spectroscopy) allow the calculation of the mass composition of the polymer, from which the molar composition is derived. The polynuclear (especially proton ( 1 H) and fluorine ( 19 F))NMR technique.
[0060] The P(VDF-TrFE) copolymer is preferably random and linear. It can be homogeneous or heterogeneous. A homogeneous polymer has a uniform chain structure.
[0061] The random distribution of units derived from various monomers has little variation from chain to chain. In a heterogeneous polymer, the chains have a multimodal or expanded distribution of units derived from various monomers. Thus, a heterogeneous polymer contains chains that are richer in a given unit and chains that are poorer in that unit.
[0062] The Curie temperature of the copolymers is between 50° C. and 145° C. The Curie temperature of the polymers of the invention can be measured by differential scanning calorimetry or dielectric spectroscopy.
[0063] The copolymer of the present invention can be produced by using any known method such as emulsion polymerization, mini-emulsion polymerization, suspension polymerization and solution polymerization.
[0064] According to one embodiment, the weight average molar mass, which in the context of this patent application is also referred to as the "molecular weight" (Mw) of the copolymer, ranges from 200 000 g / mol to 1 500 000 g / mol, preferably from 250 000 g / mol to 1 000 000 g / mol and more particularly from 300 000 g / mol to 700 000 g / mol.
[0065] The latter can be adjusted by varying certain parameters of the process (eg the temperature in the reactor) or by adding transfer agents.
[0066] The molecular weight distribution can be estimated by SEC (size exclusion chromatography) with dimethylformamide (DMF) as eluent using a set of three columns of increasing porosity. The stationary phase is styrene-DVB gel. The detection method is based on measuring the refractive index and calibrated with polystyrene standards. The sample is dissolved in DMF at 0.5 g / l and filtered through a 0.45 μm nylon filter.
[0067] The molecular weight can also be evaluated by measuring the melt flow index at 230° C. under a load of 5 kg according to ASTM D1238 (ISO 1133).
[0068] Furthermore, the molecular weight can also be characterized by measuring the viscosity in solution according to standard ISO 1628. Methyl ethyl ketone (MEK) is the preferred solvent for determining the viscosity index.
[0069] In the coating formulation, the P(VDF-TrFE) copolymer is dissolved in a volatile solvent at 10-30 mass %.
[0070] According to one embodiment, the volatile solvent is selected from the following list:
[0071] - ketones, in particular methyl isobutyl ketone, methyl ethyl ketone (MEK), cyclopentanone and acetone,
[0072] - esters, in particular ethyl acetate, methyl acetate, propyl acetate, butyl acetate and propylene glycol methyl ether acetate,
[0073] - amides such as dimethylformamide and dimethylacetamide,
[0074] - dimethyl sulfoxide,
[0075] - furans, especially tetrahydrofuran,
[0076] - carbonates, especially dimethyl carbonate,
[0077] - phosphate esters, especially triethyl phosphate,
[0078] - and mixtures thereof.
[0079] According to one embodiment, the volatile solvent is selected from the group consisting of methyl ethyl ketone, cyclopentanone, acetone, ethyl acetate.
[0080] Surfactants
[0081] The surfactant ensures optimal wetting of the solution of the fluorinated copolymer on the metal core. According to one embodiment, the surfactant is non-ionic.
[0082] According to one embodiment, the surfactant is based on an acrylic copolymer (eg BYK 3440) or on a high molecular weight block acrylic copolymer (eg Disperbyk 163).
[0083] The content of the surfactant ranges from 0.05 wt % to 1 wt % and preferably from 0.1 wt % to 0.5 wt %, inclusive, relative to the weight of the coating formulation.
[0084] Adhesion Promoters
[0085] Adhesion promoters help improve the wetting of the solution of fluorinated copolymer on the metal core and also make it possible to obtain an adhesive coating of the copolymer on the wire. It is a polymer functionalized with associative groups such as -NH2, -OH, -COOH or other.
[0086] According to one embodiment, the adhesion promoter comprises a functional copolymer of the hydroxyl type having acid groups (eg BYK 4510) or an adhesive of the ethoxysilane type, such as 3-aminopropyltriethoxysilane (Dynasylan AMEO).
[0087] The mass content of the adhesion promoter in the coating formulation is between 0.05% and 3%, preferably between 0.2% and 0.5%, inclusive, relative to the weight of the coating formulation.
[0088] According to one embodiment, for 10s -1 At a shear rate of 1.500 Å, the viscosity of the coating formulation is between 1 and 500 Pa.s and preferably between 10 and 100 Pa.s. It is advantageous to use a coating solution that exhibits shear-thickening behavior. The viscosity is measured at an ambient temperature between 20 and 25° C. using a Brookfield viscometer according to standard ASTM D2983.
[0089] According to one embodiment, the coating formulation according to the invention consists of the three components a, b and c.
[0090] The present invention also relates to a solvent-based method for continuously manufacturing a composite piezoelectric fiber comprising a metal filament covered with a piezoelectric fluoropolymer layer, the method comprising the steps of:
[0091] i) provide bare metal wires,
[0092] ii) coating the metal wire with a coating formulation according to the invention, comprising passing the metal wire through a coating nozzle into which the coating formulation is injected, to obtain a coated metal wire,
[0093] iii) drying the coated metal wire to evaporate the solvent,
[0094] iv) heating the dried coated metal film to achieve thermal annealing.
[0095] The method starts with unwinding a bare metal wire. The metal must preferably have an electrical conductivity greater than 0.5 MS / m and be selected from the following list: copper, platinum, stainless steel, molybdenum. The diameter of the metal wire ranges from 50 to 900 μm, preferably 80 to 300 μm and has a Young's modulus greater than 1 GPa and an elastic elongation between 1% and 10%.
[0096] Advantageously, the metal wire is degreased in a tank using an alkaline, acidic or detergent solution or with an alcohol. The degreased wire is subsequently dried and then passed through a coating nozzle, wherein the wire is covered with a layer of the coating formulation according to the invention as described above.
[0097] Preferably, the process is performed vertically to allow optimal centering of the coating formulation on the filament.The injection rate is adjusted according to the coated filament diameter, the diameter of the hollow tube, the outlet diameter of the coating nozzle, the viscosity of the injection solution and the production speed of the filament.
[0098] Several successive passes through the coating head make it possible to adjust the thickness of the coating formulation on the surface of the wire.
[0099] The thickness of the piezoelectric polymer obtained by the solvent-based coating method described herein is between 5 and 100 μm and preferably between 10 and 30 μm.
[0100] For 10s -1 The shear rate of 1000 μm / s makes it possible to obtain a coating solution with a viscosity of 1000 μm / s or a coating solution with a shear-thickening behavior, which is advantageous for obtaining an adherent polymer coating of controlled thickness centered on the metal core.
[0101] Adjusting the rheology of the coating formulation solution makes it possible to optimize the thickness of the polymer layer on the metal wire and the uniformity of this layer, as well as to prevent the formation of pores. This thickness ranges between 5 and 100 μm and is preferably between 10 and 30 μm.
[0102] Drying Steps
[0103] The drying process may include passing the coated filaments through a channel of hot air blown at a temperature between 50°C and 150°C so that the solvent used for the coating can be evaporated.
[0104] Annealing step
[0105] Once the metal wires are covered with the piezoelectric polymer layer, a thermal annealing step makes it possible to homogenize the structure and promote adhesion and piezoelectric behavior properties. This annealing step is preferably carried out at a temperature between 80 and 200° C. for 10 minutes and advantageously at a temperature between 130 and 180° C. for 5 minutes.
[0106] This annealing can also be performed in-line during a one-step procedure, after drying the polymer layer, by evaporating the solvent and before the winding step.
[0107] The method further comprises a step v) of winding the coated metal wire, which can be performed before or after the thermal annealing step.
[0108] In a piezoelectric composite fiber comprising a metal wire and a fluoropolymer layer, the metal wire acts as an internal electrode. Various uses of the composite piezoelectric fiber require the deposition of an external electrode on the polymer sheath.
[0109] According to one embodiment, the method according to the invention comprises the further step vi) of continuously covering the coated metal wire with a counter electrode.
[0110] Deposition of external electrodes
[0111] The metal and P(VDF-TrFE) copolymer filaments prepared as described above can be successively covered with a counter electrode according to one of the routes shown below:
[0112] - solvent-based coating with a solution of a conductive polymer, for example a solution of PEDOT:PSS (PEDOT stands for poly(3,4-ethylenedioxythiophene) and PSS stands for poly(styrenesulfonate)) in a bath (immersion) or in a coating nozzle; or
[0113] - Liquid-based coating using conductive inks of the silver paint or carbon varnish type (carbon or nanocarbon black) by dipping or in a coating nozzle; or
[0114] - melt path sheathing with CPC polymer; in this case, without stretching and alignment of the filler, the conductivity is greater than 100 S / m; or
[0115] - Metallization by evaporation of gold or other conductive metals; or
[0116] - bonding a conductive metal wire around the piezoelectrically active coating; or
[0117] - Braiding of metal wires (wires, cables, etc.) around the piezoelectrically active coating.
[0118] A particularly advantageous way to obtain a conductive external electrode deposited continuously on the piezoelectric polymer consists in using a film-forming PEDOT:PSS aqueous solution. This can be obtained, for example, by passing the wire to be covered through the conductive polymer solution mentioned and subsequently drying it by evaporation before winding.
[0119] This operation for depositing the external electrodes can advantageously be carried out in-line, after the drying and annealing steps previously described, and before the winding step.
[0120] The method according to the invention further comprises a step vii) of biasing the piezoelectric polymer deposited on the surface of the metal core.
[0121] Once the piezoelectric polymer is deposited on the surface of the metal core, the fluorinated material must be biased under an electric field in order to obtain a macroscopic piezoelectric response from the device.
[0122] This biasing can be accomplished in a variety of ways, either before or after deposition of the outer electrodes.
[0123] DC bias without counter electrode
[0124] This operation consists in applying an electric field between the surface of the adhered polymer layer and the central metal core. To this end, two methods are conventionally used by those skilled in the art: direct contact biasing and non-contact biasing.
[0125] According to one embodiment, the DC bias is direct contact and comprises the following steps:
[0126] - Connecting the bare conductor to zero potential (ground-ground) by grounding the wire coil or by a system of contact rollers which are themselves grounded;
[0127] - coating the piezoelectrically active polymer by covering the wire with a polymer solution followed by evaporation of the solvent as previously described; and
[0128] - Passing the coated wire over a system of conductive rollers, maintained at a high potential, so that the electric field at the end of the polymer coating is between 20 and 200 MV / m.
[0129] According to another embodiment, the DC bias is contactless and uses the corona effect. Effective biasing of the fluoropolymers of the present invention is achieved at high electric field values of the order of 100 V / μm. However, the maximum electric field that can be applied in air between breakdowns is about 3 V / μm. Beyond this value, discharges are observed by ionization of the air between the two poles, experiencing the influence of the high potential difference, generating atmospheric plasma and releasing ozone. It is this mechanism that is used in the corona bias method.
[0130] WO 2014 / 161920 describes a device for DC biasing fibers, in which a corona tunnel is used as an external electrode. This corona tunnel consists of a number of conducting needles that experience a high potential. The conducting core of the piezoelectric fiber itself is grounded. The distance between the needle electrode and the fluorinated surface of the fiber is kept constant, and an electric field greater than 3 V / μm is applied between the two electrodes of the system. A discharge is obtained by ionization of the air between the needle and the fluorinated surface. Due to the influence of this discharge, the fluorinated surface then becomes charged to a high potential, which thereby helps to locally bias the polymer to a field much greater than 3 V / μm.
[0131] According to one embodiment, a field / plasma diffuser is inserted between the corona needle and the surface to be biased; it is a conductive metal grid. This grid acts as a diffuser of the excessive local electric field generated by the corona needle and allows a more uniform bias to be obtained on the surface facing the electrode.
[0132] DC bias with counter electrode
[0133] The counter electrode was deposited in DC mode as described above.
[0134] According to one embodiment, online biasing comprises the following steps:
[0135] - Connecting the bare conductor to zero potential (ground-ground) by grounding the wire coil or by a system of contact rollers which are themselves grounded;
[0136] - coating of the piezoelectrically active polymer by covering the wire with a polymer solution followed by evaporation of the solvent as previously described;
[0137] - depositing a counter electrode; and
[0138] - Passing the coated wire over a system of conductive rollers, maintained at a high potential, so that the electric field at the end of the polymer coating is between 20 and 200 MV / m.
[0139] According to another embodiment, the biasing is performed in one step at the end of the in-line deposition of the counter electrode.
[0140] This implementation plan Figure 4 The scheme is shown in FIG.
[0141] The invention also relates to a composite piezoelectric fiber comprising an electroactive fluoropolymer shell adhered to a metal core. Advantageously, the fiber according to the invention has an elastic deformation between 1% and 5%. The fluoropolymer layer is biased and can be covered with an external electrode made of metal or a conductive polymer.
[0142] Another subject matter of the invention relates to the use of composite piezoelectric fibers in various applications, such as the production of technical textiles, fluid filtration and electronics.
[0143] The fiber according to the invention, comprising a fluoropolymer and having a conductive core constituting a first electrode and a conductive outer cladding constituting a second electrode, can thus constitute an actuator. The application of an electric field between these electrodes makes it possible to modify the mechanical properties of the fiber. If the fiber is incorporated into a textile structure, the application of this electric field makes it possible to modify the mechanical properties of the textile structure.
[0144] A subject of the invention is also a piezoelectric device comprising a piezoelectric fiber according to the invention.
[0145] The invention also relates to a textile material comprising said piezoelectric fibers.
[0146] Example
[0147] The following examples illustrate the invention without limiting it.
[0148] Example 1. Fabrication of Fibers Figure 1 SEM image of .
[0149] A concentrated solution containing 20 w% of VDF-TrFE (80 / 20) copolymer in MEK was obtained by dissolving without heating. 1% of Disperbyk 3440 and 0.2% of DynaSylan Ameo adhesion promoter (triethoxysilane) were added to the solution without heating.
[0150] This solution was used for DC coating of copper wires of 700 μm diameter, followed by a drying step at 80° C. and then in-line annealing in two separate ovens at 135° C. The fibers were finally wound.
[0151] The optimized formulation and solvent-based coating method make it possible to obtain bare copper wires adhesively coated with the copolymer without the use of insulating glazes or by a wetting process with applied electric fields.
[0152] Example 2: Fabrication of a piezoelectric fiber device with a metal core
[0153] A piezoelectric fiber was manufactured according to the invention. It consisted of a copper wire of 200 μm in diameter, constituting the internal electrode, a 20 μm layer of a P(VDF-TrFE) copolymer containing 20 mol% of TrFE, adhered to the wire, and a layer of conductive carbon varnish manually deposited onto the surface of the fluoropolymer, constituting the external electrode.
[0154] The device is electrically connected, with electrical contacts provided by compatible high voltage pins or flat alligator clips. One pin is connected to the metal core and is grounded, while the other pin is in contact with an external electrode and experiences a variable potential.
[0155] The area facing the two electrodes is expressed by the following equation:
[0156] S=πφL
[0157] Where: f is the diameter of the metal core, and L is the distance between the electrodes
[0158] When L = 5 cm, this gives: S = π × 200 × 10 -6 ×5×10 -2 =31.42mm 2 .
[0159] The device was then biased "offline" by applying an increasing sinusoidal voltage with a frequency of 1 Hz (up to 100 Mv / m, ie 2000 V for a 20 μm thick sample). During the biasing, the electric field and current values were recorded.
[0160] The ferroelectric effect is clearly demonstrated by the hysteresis phenomenon and the increase in the zero-field permanent bias (see Figure 2 ). The measured current peak corresponds to the value of the coercive field, which is the field required for the electric dipoles to align, indicating the acquisition of ferroelectric and piezoelectric behavior ( Figure 3 ).
[0161] These devices may also be subjected to cyclic mechanical stresses (DMA, traction, bending, etc.).
Claims
1. A polymer formulation for coating a metal core, comprising the following components: a) a 10-30% by mass solution of a P(VDF-TrFE) copolymer in a volatile solvent, b) a surfactant, and c) an adhesion promoter, wherein the adhesion promoter is a polymer functionalized with a group selected from -NH2, -OH, or -COOH, or an adhesive of the ethoxysilane type, For 10s -1 The shear rate of the coating formulation is between 1 and 500 Pa.s. The surfactant is based on an acrylic copolymer or a high molecular weight block copolymer and its content ranges from 0.05 wt % to 1 wt % relative to the weight of the coating formulation.
2. The formulation of claim 1, wherein for 10s -1 The shear rate of the coating formulation is between 10 and 100 Pa.s.
3. The formulation of claim 1, wherein the ethoxysilane-based binder is 3-aminopropyltriethoxysilane.
4. The formulation of claim 1, wherein the P(VDF-TrFE) copolymer consists of units derived from VDF and TrFE, and the proportion of the units derived from TrFE ranges from 5 mol% to 95 mol% relative to the sum of the units derived from VDF and TrFE.
5. The formulation according to claim 4, wherein the proportion of the unit derived from TrFE relative to the sum of the units derived from VDF and TrFE ranges from 15 mol% to 55 mol%.
6. The formulation according to any one of claims 1 and 5, wherein the volatile solvent is selected from the following list: -ketone, -ester, -amide, - dimethyl sulfoxide, - Furan, - carbonates, - phosphate esters, - and mixtures thereof.
7. The formulation of claim 6, wherein the amide is selected from dimethylformamide or dimethylacetamide.
8. The formulation of claim 6, wherein the ketone is selected from methyl isobutyl ketone, methyl ethyl ketone (MEK), cyclopentanone and acetone.
9. The formulation of claim 6, wherein the ester is selected from the group consisting of ethyl acetate, methyl acetate, propyl acetate, butyl acetate and propylene glycol methyl ether acetate.
10. The formulation of claim 6, wherein the furan is tetrahydrofuran.
11. The formulation of claim 6, wherein the carbonate is dimethyl carbonate.
12. The formulation of claim 6, wherein the phosphate ester is triethyl phosphate.
13. The formulation according to claim 1, wherein the surfactant is based on an acrylic copolymer or on a high molecular weight block copolymer and is present in an amount ranging from 0.1% to 0.5% by weight relative to the weight of the coating formulation.
14. The formulation according to any one of claims 1 to 5, wherein the adhesion promoter comprises a functional copolymer of the hydroxyl type with acid groups or a binder of the ethoxysilane type, in an amount between 0.05% and 3% by mass relative to the weight of the coating formulation.
15. The formulation according to claim 14, wherein the adhesion promoter comprises a functional copolymer of the hydroxyl type with acid groups or an adhesive of the ethoxysilane type, in an amount between 0.2% and 0.5% by mass relative to the weight of the coating formulation.
16. Formulation according to one of claims 1 to 5, consisting of components a), b) and c).
17. A solvent-based method for the continuous manufacture of a composite piezoelectric fiber comprising a metal filament covered with a piezoelectric fluoropolymer layer, the method comprising the steps of: i) provide bare metal wires, ii) coating the metal wire with a coating formulation according to one of claims 1 to 16, comprising passing the metal wire through a coating nozzle into which the coating formulation is injected, to obtain a coated metal wire, iii) drying the coated metal wire to evaporate the solvent, iv) heating the dried coated metal film to achieve thermal annealing.
18. The method of claim 17, wherein the bare metal wire is selected from the following list: copper, platinum, stainless steel, molybdenum, and has a diameter ranging from 50 to 900 μm.
19. The method of claim 18, wherein the bare metal wire is selected from the following list: copper, platinum, stainless steel, molybdenum, and has a diameter ranging from 80 to 300 μm.
20. A method as claimed in any one of claims 17 to 19, wherein the thickness of the coating formulation at the surface of the filaments is adjusted by successive passes through the coating head, said thickness being between 5 and 100 μm.
21. A method as claimed in claim 20, wherein the thickness of the coating formulation at the surface of the filaments is adjusted by successive passes through the coating head, said thickness being between 10 and 30 μm.
22. The method according to one of claims 17 to 19, comprising a step v) of winding the coated metal wire, which is carried out before or after the thermal annealing step.
23. The method of claim 22, comprising the step vi) of continuously covering the coated metal wire with a counter electrode.
24. The method of claim 23, wherein the forming of the external electrode is performed according to one of the following routes: - solvent-based coating with a solution of a conductive polymer or in a coating nozzle; - Liquid-based coating using conductive inks of the silver paint or carbon varnish type, either by dipping or in a coating nozzle; - Melt path coating with CPC polymer; -Metallization by evaporation of gold or other conductive metals; - bonding a conductive metal wire around the piezoelectrically active coating; - Braiding metal wires around the piezoelectrically active coating.
25. The method of claim 23, further comprising the step vii) of DC biasing the piezoelectric polymer deposited on the surface of the metal core, the step being performed before or after deposition of the external electrodes.
26. The method of claim 25, wherein the DC biasing without external electrodes employs direct contact and comprises the steps of: - Connecting the bare conductor to zero potential (ground-ground) by grounding the wire coil or by a system of contact rollers which are themselves grounded; - coated with piezoelectrically active polymer; - Passing the coated wire over a system of conductive rollers which is itself kept at a high potential.
27. The method of claim 25, wherein the DC biasing without external electrodes is contactless and comprises the steps of: - Creation of a corona tunnel consisting of conductive needles experiencing a high electrical potential; - grounding the conductive core of the piezoelectric fiber; -Maintaining a constant distance between the needle electrode and the fluoropolymer layer of the fiber; - Application of an electric field greater than 3 V / μm between the two electrodes of the system leads to the formation of an ionized discharge through the air between the needle and the fluorinated surface which becomes charged.
28. The method of claim 25, wherein the DC biasing is performed after deposition of the external electrodes.