Lithium solid state battery
By using phosphate ester compounds and sulfide-based solid electrolytes in the negative electrode layer of the lithium solid battery, the decomposition and heat release of the negative electrode active substance are suppressed, and the problems of thermal stability and resistance improvement of lithium solid battery are solved, and high thermal stability is achieved and low resistance effect.
Patent Information
- Application Number
- CN202110244685.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-11
- Filing Date
- 2021-03-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-03-05
AI Technical Summary
The problem of the high resistance of existing lithium solid batteries when improving thermal stability.
In the negative electrode layer of lithium solid battery, phosphate compounds, such as phosphate esters, phosphonates, phosphinates and phosphate amides, are used to combine with sulfide-based solid electrolytes to inhibit the decomposition reaction and exothermic of the negative electrode active substance, and by The fluorinated alkyl group of the phosphorus-based ester compound fixes oxygen free radicals, thereby improving the thermal stability of the battery.
The high thermal stability and low resistance of lithium solid batteries are achieved, which avoids the increase in resistance and enhances the high temperature resistance of the battery.
Smart Images

Figure CN113394397B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to lithium solid state batteries. Background Art
[0002] In the field of solid batteries, attempts have been made to improve the thermal stability of solid batteries.
[0003] For example, Patent Document 1 discloses a lithium solid state battery containing phosphate ester in a positive electrode active material layer.
[0004] In addition, as a technology for using a phosphoric acid ester as a flame retardant, Patent Document 2 discloses a fluorine-containing phosphoric acid ester as a flame retardant composition for a polymer solid electrolyte.
[0005] Furthermore, Patent Document 3 discloses an electrolyte composition for lithium ion secondary batteries containing a phosphoric acid ester having a fluorinated alkyl group or the like as a flame retardant.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2017-112041
[0009] Patent Document 2: Japanese Patent Application Publication No. 2003-238821
[0010] Patent Document 3: Japanese Patent Application Publication No. 2019-079781 Summary of the invention
[0011] Problems to be solved by the invention
[0012] The inventors have conducted intensive studies and found that, as disclosed in Patent Document 1, when a phosphoric acid ester is included in a positive electrode active material layer of a lithium solid state battery, the thermal stability of the lithium solid state battery is improved, but the resistance increases.
[0013] The present disclosure is made in view of the above-mentioned actual situation, and an object of the present disclosure is to provide a lithium solid state battery having high thermal stability and low resistance.
[0014] Means for solving problems
[0015] The present disclosure provides a lithium solid state battery, characterized in that it comprises a positive electrode, a negative electrode and a solid electrolyte layer, wherein the positive electrode has a positive electrode layer containing an oxide-based positive electrode active material, the negative electrode has a negative electrode layer containing a negative electrode active material, and the solid electrolyte layer is disposed between the positive electrode layer and the negative electrode layer and contains a solid electrolyte.
[0016] At least one of the negative electrode layer and the solid electrolyte layer contains a sulfide-based solid electrolyte.
[0017] The negative electrode layer contains at least one phosphorus ester compound selected from the group consisting of phosphoric acid ester, phosphonic acid ester, phosphinate, phosphite and phosphoric acid ester amide.
[0018] In the lithium solid state battery of the present disclosure, the content of the phosphorus ester compound in the negative electrode layer may be 1% by mass or more and 10% by mass or less when the total mass of the negative electrode layer is 100% by mass.
[0019] In the lithium solid state battery of the present disclosure, the negative electrode active material may be at least one selected from Si single substance and Si alloy.
[0020] In the lithium solid state battery of the present disclosure, the phosphorus-based ester compound may have a fluorinated alkyl group.
[0021] Effects of the Invention
[0022] According to the present disclosure, a lithium solid state battery having high thermal stability and low resistance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic cross-sectional view showing an example of the lithium solid state battery of the present disclosure.
[0024] Description of Reference Numerals
[0025] 11 Solid electrolyte layer
[0026] 12. Positive electrode layer
[0027] 13 Negative electrode layer
[0028] 14. Positive electrode collector
[0029] 15 Negative electrode collector
[0030] 16 Positive electrode
[0031] 17 Negative electrode
[0032] 100 Lithium solid battery DETAILED DESCRIPTION
[0033] The present disclosure provides a lithium solid state battery, characterized in that it comprises a positive electrode, a negative electrode and a solid electrolyte layer, wherein the positive electrode has a positive electrode layer containing an oxide-based positive electrode active material, the negative electrode has a negative electrode layer containing a negative electrode active material, and the solid electrolyte layer is disposed between the positive electrode layer and the negative electrode layer and contains a solid electrolyte.
[0034] At least one of the negative electrode layer and the solid electrolyte layer contains a sulfide-based solid electrolyte.
[0035] The negative electrode layer contains at least one phosphorus ester compound selected from the group consisting of phosphoric acid ester, phosphonic acid ester, phosphinate, phosphite and phosphoric acid ester amide.
[0036] As described in Patent Document 1, conventionally, when phosphorus ester compounds such as phosphate esters are used for negative electrode layers of lithium solid state batteries, it is believed that once the phosphorus ester compounds penetrate into the negative electrode layer, reductive decomposition of the phosphorus ester compounds may occur.
[0037] However, the researchers unexpectedly found that the phosphorus ester compound exists stably in the negative electrode layer, and even if the phosphorus ester compound is contained in the negative electrode layer, it will not cause an increase in the resistance of the lithium solid battery. In addition, it was found that the lithium solid battery using the phosphorus ester compound in the negative electrode layer can inhibit the decomposition reaction and heat release of the negative electrode active material. Therefore, the lithium solid battery using the phosphorus ester compound in the negative electrode layer can ensure the desired thermal stability without causing resistance increase.
[0038] In the present disclosure, the exothermic peak temperature of a lithium solid state battery can be shifted to a higher temperature side by using a specific phosphorus ester compound. The mechanism is presumed to be as follows.
[0039] That is, due to overcharge of the lithium solid battery, the oxide-based positive electrode active material of the positive electrode layer decomposes, and oxygen is generated from the positive electrode layer. Thereafter, the oxygen moves to the negative electrode layer. Then, the active species (species) from the oxygen is captured (trapped) by the phosphorus ester compound contained in the negative electrode layer. Due to the above reasons, it is speculated that the occurrence of the exothermic reaction of the lithium solid battery caused by the generation of oxygen is suppressed.
[0040] In addition, in the case of phosphorus ester compounds, two or more phosphorus ester compounds condense to form a film on the surface of the negative electrode active material. Moreover, it is speculated that the presence of the film between the negative electrode active material and the sulfide-based solid electrolyte inhibits the reaction between the negative electrode active material and the sulfide-based solid electrolyte, thereby inhibiting the exothermic reaction of the lithium solid battery.
[0041] Furthermore, when the lithium solid battery is exposed to high temperature, oxygen free radicals (O free radicals) are generated from the oxide-based positive electrode active material. When the phosphorus ester compound has a fluorinated alkyl group, free radicals from the fluorinated alkyl group are also generated at the same time as the oxygen free radicals. The free radicals from the fluorinated alkyl group fix the oxygen free radicals, thereby suppressing the occurrence of the exothermic reaction of the lithium solid battery caused by the generation of oxygen free radicals, thereby presumably improving the thermal stability of the lithium solid battery.
[0042] Figure 1 This is a schematic cross-sectional view showing an example of a lithium solid state battery of the present disclosure.
[0043] The solid battery 100 includes a positive electrode 16 including a positive electrode layer 12 and a positive electrode current collector 14 , a negative electrode 17 including a negative electrode layer 13 and a negative electrode current collector 15 , and a solid electrolyte layer 11 disposed between the positive electrode 16 and the negative electrode 17 .
[0044] [positive electrode]
[0045] The positive electrode has at least a positive electrode layer and, if necessary, a positive electrode current collector for collecting current from the positive electrode layer.
[0046] The positive electrode layer contains at least an oxide-based positive electrode active material as a positive electrode active material, and contains a conductive material, a binder, a solid electrolyte, a phosphorus-based ester compound, and the like as necessary.
[0047] The oxide-based positive electrode active material may contain an O element.
[0048] Examples of the oxide-based positive electrode active material include Li 2 TiO 3 , Li 2 Ti 3 O 7 , Li 4 Ti 5 O 12 、LiCoO 2 、LiMnO 2 、LiNiO 2 、LiVO 2 、LiNi x Co 1-x O 2 (0 <x<1)、LiNi x Co y Mn z O 2 (x+y+z=1), LiMn 2 O 4 , Li 2 MnO 3 、LiMn 1.5 Ni 0.5 O 4 、LiMn 1.5 Al 0.5 O 4 、LiMn 1.5 Mg 0.5 O 4 、LiMn 1.5 Co 0.5 O 4 、LiMn 1.5 Fe 0.5 O 4 、LiMn 1.5 Zn 0.5 O 4、LiFePO 4 、LiMnPO 4 、LiCoPO 4 、LiNiPO 4 , Li 2 SiO 3 , Li 4 SiO 4 、V 2 O 5 、MoO 3 and SiO 2 wait.
[0049] As long as the positive electrode layer contains an oxide-based positive electrode active material as a main component, the positive electrode active material may contain a conventionally known non-oxide-based positive electrode active material.
[0050] Examples of the non-oxide positive electrode active material include Li simple substance, Li alloy, Si simple substance, Si alloy, LiCoN, TiS 2 and Mg 2 Sn、Mg 2 Ge、Mg 2 Sb and Cu 3 Sb et al.
[0051] Examples of Li alloys include Li-Au, Li-Mg, Li-Sn, Li-Si, Li-Al, Li-B, Li-C, Li-Ca, Li-Ga, Li-Ge, Li-As, Li-Se, Li-Ru, Li-Rh, Li-Pd, Li-Ag, Li-Cd, Li-In, Li-Sb, Li-Ir, Li-Pt, Li-Hg, Li-Pb, Li-Bi, Li-Zn, Li-Tl, Li-Te, and Li-At. Examples of Si alloys include alloys with metals such as Li, and alloys with at least one metal selected from Sn, Ge, and Al.
[0052] A coating containing a Li ion conductive oxide may be formed on the surface of the positive electrode active material. That is, the positive electrode active material may be a positive electrode active material complex having a coating formed on the surface of the positive electrode active material. This is because the reaction between the positive electrode active material and the solid electrolyte can be suppressed.
[0053] Examples of the Li ion conductive oxide include LiNbO 3 , Li 4 Ti 5 O 12 and Li 3 PO 4The thickness of the coating is, for example, 0.1 nm or more, and may be 1 nm or more. On the other hand, the thickness of the coating is, for example, 100 nm or less, and may be 20 nm or less. The coverage of the coating on the surface of the positive electrode active material is, for example, 70% or more, and may be 90% or more.
[0054] The method of coating the surface of the positive electrode active material with a Li ion conductive oxide is not particularly limited, and examples thereof include a method of coating the positive electrode active material with a Li ion conductive oxide in an atmospheric environment using a tumbling flow coating apparatus (manufactured by Pawleck Co., Ltd.), and calcining the positive electrode active material in an atmospheric environment, etc. In addition, examples thereof include a sputtering method, a sol-gel method, an electrostatic spray method, and a ball milling method, etc.
[0055] The shape of the positive electrode active material is not particularly limited, and examples thereof include a particle shape and a plate shape.
[0056] The content of the positive electrode active material in the positive electrode layer is not particularly limited, and can be, for example, 50% by mass to 90% by mass when the total mass of the positive electrode layer is 100% by mass.
[0057] Examples of the solid electrolyte include the materials exemplified in the solid electrolyte layer described later.
[0058] The content of the solid electrolyte in the positive electrode layer is not particularly limited, and can be, for example, 1% by mass to 80% by mass when the total mass of the positive electrode layer is 100% by mass.
[0059] The binder is not particularly limited, and examples thereof include acrylonitrile butadiene rubber (ABR), butadiene rubber (BR), polyvinylidene fluoride (PVdF), and styrene butadiene rubber (SBR). The content of the binder in the positive electrode layer is not particularly limited.
[0060] As the conductive material, a known conductive material can be used, for example, a carbon material and a metal material can be mentioned. As the carbon material, for example, at least one of carbon black selected from acetylene black and furnace black, vapor grown carbon fiber (VGCF), carbon nanotubes and carbon nanofibers can be mentioned, wherein, from the viewpoint of electronic conductivity, it can be at least one selected from VGCF, carbon nanotubes and carbon nanofibers. As the metal material, Ni, Cu, Fe and SUS can be mentioned.
[0061] The content of the conductive material in the positive electrode layer is not particularly limited.
[0062] Examples of the phosphorus-based ester compound include the materials exemplified in the negative electrode layer described later.
[0063] The content of the phosphorus ester compound in the positive electrode layer is not particularly limited, and may be, for example, 0.1 to 20% by mass, or 1 to 10% by mass, based on 100% by mass of the total mass of the positive electrode layer.
[0064] When the content of the phosphorus ester compound in the positive electrode layer is less than 0.1% by mass, it is possible that the thermal stability cannot be fully improved. On the other hand, when the content of the phosphorus ester compound in the positive electrode layer exceeds 20% by mass, the content of the positive electrode active material is relatively reduced, and it is possible that sufficient battery capacity cannot be obtained.
[0065] The thickness of the positive electrode layer is not particularly limited, and may be, for example, 10 to 250 μm.
[0066] As for the method for forming the positive electrode layer, for example, an oxide-based positive electrode active material and other components as needed are put into a solvent and stirred to prepare a slurry for the positive electrode layer. The slurry for the positive electrode layer is applied to one side of a support such as a positive electrode collector and dried to obtain the positive electrode layer.
[0067] Examples of the solvent include butyl acetate, butyl butyrate, heptane, and N-methyl-2-pyrrolidone.
[0068] The method for coating the positive electrode layer slurry on one side of a support such as a positive electrode current collector is not particularly limited, and examples thereof include doctor blade method, metal mask printing method, electrostatic coating method, dip coating method, spraying method, roll coating method, gravure coating method and screen printing method.
[0069] As the support, a self-supporting support can be appropriately selected and used without particular limitation, and for example, metal foil of Cu, Al, etc. can be used.
[0070] In addition, as another method for forming the positive electrode layer, the positive electrode layer can be formed by press-molding the powder of the positive electrode mixture containing the oxide-based positive electrode active material and other components as required. When the powder of the positive electrode mixture is press-molded, a pressing pressure of about 1 MPa or more and about 600 MPa or less is usually loaded.
[0071] The pressurizing method is not particularly limited, and examples thereof include a method of applying pressure using a plate press, a roll press, and the like.
[0072] The positive electrode current collector has the function of collecting current in the positive electrode layer. Examples of the material of the positive electrode current collector include metal materials such as SUS, Ni, Cr, Au, Pt, Al, Fe, Ti, and Zn.
[0073] Examples of the shape of the positive electrode current collector include a foil shape, a plate shape, and a mesh shape.
[0074] The positive electrode may further include a positive electrode lead connected to the positive electrode current collector.
[0075] [negative electrode]
[0076] The negative electrode has at least a negative electrode layer and, if necessary, a negative electrode current collector for collecting current from the negative electrode layer.
[0077] The negative electrode layer contains at least a negative electrode active material and a phosphorus ester compound, and contains a conductive material, a binder, a solid electrolyte, and the like as necessary.
[0078] Furthermore, at least one of the negative electrode layer and the solid electrolyte layer contains a sulfide-based solid electrolyte as a solid electrolyte.
[0079] Examples of the negative electrode active material include graphite, hard carbon, Li simple substance, Li alloy, Si simple substance, Si alloy, and Li 4 Ti 5 O 12 As the Li alloy and the Si alloy, the materials exemplified in the positive electrode active material and the like can be exemplified.
[0080] The shape of the negative electrode active material is not particularly limited, and examples thereof include a particle shape and a plate shape.
[0081] The content of the negative electrode active material in the negative electrode layer is not particularly limited, and may be, for example, 20% by mass to 90% by mass.
[0082] The phosphorus ester compound is at least one selected from the group consisting of phosphoric acid ester, phosphonic acid ester, phosphinate, phosphite and phosphoric acid ester amide.
[0083] Phosphate esters are represented by the following general formula (1). Phosphonates are represented by the following general formula (2). Phosphinates are represented by the following general formula (3). Phosphites are represented by the following general formula (4). Phosphate amides are represented by the following general formula (5).
[0084]
Chemical formula 1
[0085]
[0086]
Chemical formula 2
[0087]
[0088]
Chemical formula 3
[0089]
[0090]
Chemical formula 4
[0091]
[0092]
Chemical formula 5
[0093]
[0094] In the above general formulas (1) to (5), R 1 ~R 3 Each independently is a group containing at least carbon element.
[0095] R 1 ~R 3 The carbon number of is in the range of 1 to 10, for example.
[0096] In addition, R 1 ~R 3 It may be composed of only carbon and hydrogen, or may further contain other elements. 1 ~R 3 It may be composed of only carbon and fluorine, or may further contain other elements. 1 ~R 3 It may be composed of only carbon, hydrogen and fluorine, or may further contain other elements. 1 ~R 3 It may be a fluorinated alkyl group. In the fluorinated alkyl group, all hydrogen atoms (H) may be replaced by fluorine atoms. In the fluorinated alkyl group, part of the hydrogen atoms may be replaced by fluorine atoms.
[0097] In addition, R 1 ~R 3 It may have a chain structure, a cyclic structure (including an aromatic structure), or both a chain structure and a cyclic structure. The chain structure may be a straight chain structure or a branched chain structure.
[0098] In the above general formulas (1), (2) and (5), R 1 and R 2 , or R 1 and R 3 Replaced with alkylene (-R 10 -) ring structure.
[0099] R', R" and R* are directly bonded to a phosphorus atom (P) or a nitrogen atom (N). R', R" and R* are hydrogen atoms, alkyl groups or aromatic groups. R', R" and R* may not contain fluorine atoms. When R', R" and R* are alkyl groups or aromatic groups, R', R" and R* may contain fluorine atoms.
[0100]
Chemical formula 6
[0101]
[0102] The general formula (6) corresponds to a condensed product of the triphosphate ester represented by the general formula (1).
[0103] In the general formula (6), R 4 ~R 8 Each independently is a group containing at least carbon element.
[0104] R 4 ~R 8 The carbon number of is in the range of 1 to 10, for example.
[0105] In addition, R 4 ~R 8 It can be composed of only carbon and hydrogen, or it can further contain other elements. 4 ~R 8 It may be composed of only carbon and fluorine, or may further contain other elements. 4 ~R 8 It may be composed of only carbon, hydrogen and fluorine, or may further contain other elements. 4 ~R 8 It may be a fluorinated alkyl group. In the fluorinated alkyl group, all hydrogen atoms (H) may be replaced by fluorine atoms. In the fluorinated alkyl group, part of the hydrogen atoms may be replaced by fluorine atoms.
[0106] In addition, R 4 ~R 8 It may have a chain structure, a cyclic structure (including an aromatic structure), or both a chain structure and a cyclic structure. The chain structure may be a straight chain structure or a branched chain structure.
[0107] Examples of the phosphoric acid ester include triphenyl phosphate, tris(2,2,2-trifluoroethyl) phosphate, tris(2,2,3,3-tetrafluoropropyl) phosphate, tris(2,2,3,3,3-pentafluoropropyl) phosphate, tris(1H,1H-heptafluorobutyl) phosphate, and tris(1H,1H,5H-octafluoropentyl) phosphate.
[0108] Examples of the phosphoric acid ester having a cyclic structure include ethylene trifluoroethyl phosphate and the like.
[0109] Examples of the phosphonic acid ester include bis(2,2,2-trifluoroethyl)methylphosphonate, bis(2,2,2-trifluoroethyl)ethylphosphonate, and bis(2,2,2-trifluoroethyl)phosphonate.
[0110] Examples of the phosphinate include (2,2,2-trifluoroethyl) diethylphosphinate and the like.
[0111] Examples of the phosphite include tris(2,2,2-trifluoroethyl) phosphite, tris(2,2,3,3-tetrafluoropropyl) phosphite, tris(2,2,3,3,3-pentafluoropropyl) phosphite, tris(1H,1H-heptafluorobutyl) phosphite, and tris(1H,1H,5H-octafluoropentyl) phosphite.
[0112] Examples of the phosphoric acid ester amide include O,O-bis(2,2,2-trifluoroethyl)N,N-dimethylphosphonic acid amide and the like.
[0113] The phosphorus ester compound can be a liquid or a solid at 25°C, preferably a liquid. The liquid phosphorus ester compound is configured to fill the voids (especially the voids that are inevitably generated) of the negative electrode layer, so that the volume energy density can be maintained and the thermal stability of the battery can be improved. It should be noted that, based on the viewpoint of the battery use temperature, the phosphorus ester compound can be a liquid at any temperature in the range of -20°C to 100°C, and can be a liquid at all temperatures in the above range.
[0114] The content of the phosphorus-based ester compound in the negative electrode layer is not particularly limited, and may be, for example, 0.1% by mass to 20% by mass, or 1% by mass to 10% by mass.
[0115] When the content of the phosphorus ester compound in the negative electrode layer is less than 0.1% by mass, the thermal stability may not be sufficiently improved. On the other hand, when the content of the phosphorus ester compound in the negative electrode layer exceeds 20% by mass, the content of the negative electrode active material is relatively reduced, and sufficient battery capacity may not be obtained.
[0116] The conductive material and binder used in the negative electrode layer may be exemplified by the materials exemplified in the positive electrode layer, etc. The solid electrolyte used in the negative electrode layer may be exemplified by the materials exemplified in the solid electrolyte layer described later, etc.
[0117] The thickness of the negative electrode layer is not particularly limited, and may be, for example, 10 to 100 μm.
[0118] Examples of the material of the negative electrode current collector include metal materials such as SUS, Cu, Ni, Fe, Ti, Co, and Zn. Examples of the shape of the negative electrode current collector include the shapes exemplified for the positive electrode current collector.
[0119] [Solid electrolyte layer]
[0120] The solid electrolyte layer contains at least a solid electrolyte and may contain a binder and the like as necessary.
[0121] Furthermore, at least one of the negative electrode layer and the solid electrolyte layer contains a sulfide-based solid electrolyte.
[0122] Examples of the solid electrolyte include sulfide-based solid electrolytes and oxide-based solid electrolytes.
[0123] The sulfide-based solid electrolyte may contain Li element, A element (A is at least one of P, Ge, Si, Sn, B and Al) and S element. The sulfide-based solid electrolyte may further contain a halogen element. Examples of the halogen element include F element, Cl element, Br element and I element. In addition, the sulfide-based solid electrolyte may further contain O element.
[0124] Examples of sulfide-based solid electrolytes include Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -GeS 2 , Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 SP 2 S 5 -LiI-LiBr, Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n(wherein m and n are positive numbers. Z is any one of Ge, Zn or Ga.) 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 and Li 2 S-SiS 2 -Li x MO y (wherein x and y are positive numbers. M is any one of P, Si, Ge, B, Al, Ga, or In.) 2 SP 2 S 5 " refers to the use of Li 2 S and P 2 S 5 The same applies to the other descriptions.
[0125] The molar ratio of each element in the sulfide-based solid electrolyte can be controlled by adjusting the content of each element in the raw material. In addition, the molar ratio and composition of each element in the sulfide-based solid electrolyte can be measured by, for example, ICP emission spectrometry.
[0126] The sulfide-based solid electrolyte may be sulfide glass, crystallized sulfide glass (glass ceramic), or a crystalline material obtained by subjecting a raw material composition to a solid phase reaction treatment.
[0127] The crystal state of the sulfide-based solid electrolyte can be confirmed by, for example, performing powder X-ray diffraction measurement of the sulfide-based solid electrolyte using CuKα rays.
[0128] Sulfide glass can be prepared by adjusting the raw material composition (e.g. Li 2 S and P 2 S 5 The amorphous treatment may be, for example, mechanical grinding.
[0129] Glass ceramics can be obtained, for example, by heat treating sulfide glass.
[0130] The heat treatment temperature may be a temperature higher than the crystallization temperature (Tc) observed by thermal analysis of sulfide glass, and is usually 195° C. or higher. On the other hand, the upper limit of the heat treatment temperature is not particularly limited.
[0131] The crystallization temperature (Tc) of sulfide glass can be measured by differential thermal analysis (DTA).
[0132] The heat treatment time is not particularly limited as long as it is a time that can obtain the desired crystallinity of the glass ceramic, and is, for example, in the range of 1 minute to 24 hours, particularly in the range of 1 minute to 10 hours.
[0133] The method of heat treatment is not particularly limited, and an example thereof includes a method using a calcining furnace.
[0134] Examples of the oxide-based solid electrolyte include a substance having a garnet-type crystal structure containing Li element, La element, A element (A is at least one of Zr, Nb, Ta and Al) and O element, and Li 3+x PO 4-x N 4 (1≤x≤3) etc.
[0135] The shape of the solid electrolyte is not particularly limited, and examples thereof include a particle shape and a plate shape. From the viewpoint of good handling properties, the solid electrolyte may be in a particle shape.
[0136] The average particle size (D50) of the solid electrolyte particles is not particularly limited, but the lower limit may be 0.5 μm or more and the upper limit may be 2 μm or less.
[0137] In the present disclosure, unless otherwise specified, the average particle size of particles is the value of the volume-based median diameter (D50) measured by laser diffraction / scattering particle size distribution measurement. In addition, in the present disclosure, the median diameter (D50) refers to the diameter (volume average diameter) at which the cumulative volume of the particles becomes half (50%) of the total volume when the particles are arranged in order of the smallest particle size.
[0138] The solid electrolyte may be used alone or in combination of two or more. In addition, when two or more solid electrolytes are used, the two or more solid electrolytes may be mixed, or two or more layers of the solid electrolytes may be formed to form a multilayer structure.
[0139] The proportion of the solid electrolyte in the solid electrolyte layer is not particularly limited, and may be, for example, 50% by mass or more, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, or 100% by mass.
[0140] The binder used in the solid electrolyte layer can be exemplified by the materials exemplified in the above-mentioned positive electrode layer, etc. From the viewpoint of preventing excessive aggregation of the solid electrolyte and being able to form a solid electrolyte layer having a uniformly dispersed solid electrolyte to easily achieve high output, etc., the binder contained in the solid electrolyte layer can be set to 5% by mass or less.
[0141] [Other components]
[0142] The lithium solid state battery includes an outer casing that accommodates a positive electrode, a negative electrode, and a solid electrolyte layer as necessary.
[0143] The material of the outer casing is not particularly limited as long as it is stable to the electrolyte, and examples thereof include resins such as polypropylene, polyethylene, and acrylic resins.
[0144] [Lithium solid state battery]
[0145] The lithium solid battery disclosed herein can be a primary battery or a secondary battery, preferably a secondary battery. This is because it can be repeatedly charged and discharged, and is useful as a vehicle-mounted battery, for example. As the shape of the lithium solid battery, for example, a coin type, a laminated type, a cylindrical type, and a square type can be cited.
[0146] The manufacturing method of a lithium solid battery is, for example, firstly press-forming the powder of a solid electrolyte material to form a solid electrolyte layer. Then, on one side of the solid electrolyte layer, a powder of a positive electrode mixture containing an oxide-based positive electrode active material is press-formed to obtain a positive electrode layer. Thereafter, on the surface of the solid electrolyte layer opposite to the surface on which the positive electrode layer is formed, a powder of a negative electrode mixture containing a negative electrode active material and a phosphorus ester compound is press-formed to obtain a negative electrode layer. Then, a positive electrode collector and a negative electrode collector are installed as needed to make a lithium solid battery.
[0147] In this case, the pressing pressure when the powder of the solid electrolyte material, the powder of the positive electrode mixture, and the powder of the negative electrode mixture are press-molded is usually about 1 MPa or more and 600 MPa or less.
[0148] The pressurizing method is not particularly limited, and the pressurizing methods exemplified in the formation of the positive electrode layer may be mentioned.
[0149] Example
[0150] (Example 1)
[0151] [Production of positive electrode]
[0152] Butyl butyrate as a solvent and polyvinylidene fluoride as a binder were prepared. Then, polyvinylidene fluoride was dissolved in butyl butyrate to prepare a butyl butyrate solution containing 5% by mass of polyvinylidene fluoride.
[0153] As the positive electrode active material, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 of particles.
[0154] LiNbO was coated in an atmospheric environment using a tumble flow coating apparatus (manufactured by Pawleck Co., Ltd.). 3 Coated on LiNi1 / 3 Co 1 / 3 Mn 1 / 3 O 2 The surface of the particles was sintered in an atmospheric environment to obtain LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 The surface of the particles is LiNbO 3 The positive electrode active material complex is coated.
[0155] As a solid electrolyte, Li 2 SP 2 S 5 It is glass ceramic.
[0156] As a conductive additive, VGCF (vapor grown carbon fiber) was prepared.
[0157] A butyl butyrate solution, a positive electrode active material complex, a solid electrolyte, and a conductive aid were added to a polypropylene container, and the raw materials were stirred for 30 seconds with an ultrasonic disperser (manufactured by Esumetech, product name UH-50). Thereafter, the polypropylene container was vibrated for 3 minutes with an oscillator (manufactured by Shibata Technology Co., Ltd., product name TTM-1). Furthermore, these raw materials were stirred for 30 seconds with an ultrasonic disperser to prepare a positive electrode layer paste. Using an applicator, a doctor blade method was used to apply the positive electrode layer paste to an aluminum foil serving as a positive electrode collector, and then dried on a hot plate heated to 100°C for 30 minutes, thereby preparing a positive electrode layer on the positive electrode collector, and a positive electrode having a positive electrode collector and a positive electrode layer was obtained.
[0158] [Production of negative electrode]
[0159] Butyl butyrate as a solvent and polyvinylidene fluoride as a binder were prepared. Then, polyvinylidene fluoride was dissolved in butyl butyrate to prepare a butyl butyrate solution containing 5% by mass of polyvinylidene fluoride.
[0160] As the negative electrode active material, Si simple substance powder was prepared.
[0161] As a solid electrolyte, Li 2 SP 2 S 5 It is glass ceramic.
[0162] As a conductive additive, VGCF (vapor grown carbon fiber) was prepared.
[0163] As the phosphorus-based ester compound, tris(2,2,2-trifluoroethyl) phosphate was prepared in an amount of 5% by mass in the negative electrode layer when the total mass of the negative electrode layer was 100% by mass.
[0164] A butyl butyrate solution, a negative electrode active material, a solid electrolyte, a conductive aid, and a phosphorus ester compound were added to a polypropylene container, and these raw materials were stirred for 30 seconds using an ultrasonic disperser (manufactured by Esumetech, product name UH-50). Thereafter, the polypropylene container was vibrated for 3 minutes using an oscillator (manufactured by Shibata Technology Co., Ltd., product name TTM-1) to prepare a paste for the negative electrode layer. Using an applicator, the paste for the negative electrode layer was applied to a copper foil as a negative electrode collector by a doctor blade method, and then dried on a hot plate heated to 100°C for 30 minutes, thereby preparing a negative electrode layer on the negative electrode collector, and obtaining a negative electrode having a negative electrode collector and a negative electrode layer.
[0165] [Fabrication of Solid Electrolyte Layer]
[0166] Heptane as a solvent and butadiene rubber as a binder were prepared. Then, the butadiene rubber was dissolved in heptane to prepare a heptane solution containing 5% by mass of the butadiene rubber.
[0167] As a solid electrolyte, Li-ion battery containing lithium iodide was prepared. 2 SP 2 S 5 It is glass ceramic.
[0168] The heptane solution and the solid electrolyte were added to a polypropylene container, and the raw materials were stirred for 30 seconds using an ultrasonic dispersion device (manufactured by Esumetech, product name UH-50). Thereafter, the polypropylene container was vibrated for 30 minutes using an oscillator (manufactured by Shibata Tech Co., Ltd., product name TTM-1) to prepare a solid electrolyte layer paste. Using an applicator, the solid electrolyte layer paste was applied to an aluminum foil as a base using a doctor blade method, and then dried on a hot plate heated to 100°C for 30 minutes to prepare a solid electrolyte layer on the aluminum foil.
[0169] [Manufacturing of lithium solid state batteries]
[0170] The solid electrolyte layer was stacked on the positive electrode layer of the positive electrode so as to be in contact with the positive electrode layer, and roll-pressed to obtain a first stack having a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, and an aluminum foil in this order.
[0171] Thereafter, the aluminum foil serving as the base of the solid electrolyte layer was peeled off, and the negative electrode layer was stacked on the solid electrolyte layer in such a manner that the solid electrolyte layer and the negative electrode layer were in contact, thereby producing a second stack having a positive electrode collector, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode collector in sequence. A terminal was provided to the produced second stack, and the second stack was packaged with a laminate film to produce a lithium solid battery.
[0172] (Example 2)
[0173] In the above-mentioned [Preparation of the Negative Electrode], a lithium solid state battery was manufactured in the same manner as in Example 1 except that a negative electrode layer was prepared using tris(2,2,2-trifluoroethyl) phosphate in an amount of 1% by mass when the total mass of the negative electrode layer was set to 100% by mass as a phosphorus ester compound.
[0174] (Example 3)
[0175] In the above-mentioned [Preparation of the Negative Electrode], a lithium solid state battery was manufactured in the same manner as in Example 1 except that a negative electrode layer was prepared using tri(2,2,2-trifluoroethyl) phosphate in an amount of 10 mass % when the total mass of the negative electrode layer was set to 100 mass %.
[0176] (Example 4)
[0177] In the above-mentioned [Preparation of Negative Electrode], a lithium solid state battery was manufactured in the same manner as in Example 1 except that the negative electrode layer was manufactured using triphenyl phosphate in an amount of 5 mass % when the total mass of the negative electrode layer was set to 100 mass % as the phosphorus ester compound.
[0178] (Example 5)
[0179] In the above-mentioned [Preparation of the positive electrode], as the phosphorus ester compound, a positive electrode layer was prepared using tri(2,2,2-trifluoroethyl) phosphate in an amount of 5 mass % when the total mass of the positive electrode layer was set to 100 mass %, so that both the positive electrode layer and the negative electrode layer contained the phosphorus ester compound. Except for this, a lithium solid state battery was manufactured in the same manner as in Example 1.
[0180] (Comparative Example 1)
[0181] A lithium solid state battery was produced in the same manner as in Example 1 except that the negative electrode layer was produced without using a phosphorus ester compound in the above-mentioned [Production of Negative Electrode].
[0182] (Comparative Example 2)
[0183] In the above-mentioned [production of the positive electrode], the positive electrode layer was produced using tri(2,2,2-trifluoroethyl) phosphate in an amount of 5 mass % when the total mass of the positive electrode layer was set to 100 mass % as the phosphorus ester compound. In the above-mentioned [production of the negative electrode], the negative electrode layer was produced without using a phosphorus ester compound, and only the positive electrode layer was made to contain a phosphorus ester compound. Except for this, a lithium solid battery was produced in the same manner as Example 1.
[0184] [Differential Scanning Calorimetry (DSC) of Simulated Battery]
[0185] The lithium solid state battery obtained in Example 1 was constrained at a predetermined pressure and charged to 4.55 V at a constant current of 0.1 C in an inert atmosphere.
[0186] Afterwards, the lithium solid battery was disassembled in an inactive atmosphere in a manner that did not cause a short circuit, and the positive electrode layer and the negative electrode layer in a charged state were taken out. Then, the positive electrode layer and the negative electrode layer were processed into a size that could be placed in a stainless steel container for DSC, and a positive electrode layer sample and a negative electrode layer sample were obtained. The positive electrode layer sample was placed in a container for DSC, and then a plate-shaped electrolyte was placed. Next, the negative electrode layer sample was placed in a container for DSC in a manner that did not cause a short circuit, and the container was sealed to make a simulated battery. The sealed container was placed in a DSC device (manufactured by Shimadzu Corporation), and the heat release behavior of the simulated battery was measured. An empty container was used for reference, the heating rate was set to 10°C / min, and the end temperature was set to 500°C.
[0187] Based on the DSC results, the exothermic peak temperature of the simulated battery was measured. The exothermic peak temperature refers to the peak temperature at which the heat flow reaches the maximum in the exothermic behavior.
[0188] For the lithium solid state batteries obtained in Examples 2 to 5 and Comparative Examples 1 to 2, simulated batteries were prepared in the same manner as in the lithium solid state battery of Example 1, and the exothermic peak temperatures of the simulated batteries were measured.
[0189] [Measurement of DC resistance of lithium solid state batteries]
[0190] The lithium solid state battery obtained in Example 1 was constrained at a predetermined pressure and charged at a constant current of 0.1 C to 4.55 V in an inert atmosphere.
[0191] Thereafter, the lithium solid state battery was discharged at 0.1 C to 3 V, and then charged at 0.1 C to 3.8 V by constant current constant voltage (CCCV), and the DC resistance of the lithium solid state battery was measured.
[0192] The lithium solid state batteries obtained in Examples 2 to 5 and Comparative Examples 1 to 2 were also measured for DC resistance in the same manner as in the lithium solid state battery of Example 1. The results are shown in Table 1. In Table 1, the lithium solid state batteries are simply referred to as batteries.
[0193] Table 1
[0194]
[0195] As shown in Table 1, the exothermic peaks of the simulated batteries observed in DSC of Examples 1 to 5 and Comparative Examples 1 and 2 are considered to be generated by the reaction of oxygen generated from the thermally decomposed positive electrode active material with the negative electrode layer in a charged state.
[0196] When the exothermic peak temperature of each simulated battery of Examples 1 to 5 was compared with the exothermic peak temperature of each simulated battery of Comparative Examples 1 to 2, it was confirmed that the exothermic peak temperature of each simulated battery of Examples 1 to 5 was shifted to the high temperature side compared with the exothermic peak temperature of each simulated battery of Comparative Examples 1 to 2. The phosphorus-based ester compound has a function as a flame retardant, and it is believed that by adding the phosphorus-based ester compound to the negative electrode layer, the decomposition reaction of the negative electrode active material caused by oxygen can be suppressed, and the thermal stability of the lithium solid battery is improved.
[0197] In addition, the results of Comparative Example 2 confirmed that when only the phosphorus ester compound was added to the positive electrode layer, the DC resistance of the lithium solid battery increased compared to the case of Comparative Example 1 in which the phosphorus ester compound was not added. This is believed to be because the positive electrode layer is exposed to high temperature during the charge and discharge of the lithium solid battery, thereby decomposing the phosphorus ester compound in the positive electrode layer.
[0198] On the other hand, the results of Examples 1 to 5 show that, when a phosphorus ester compound is added to at least the negative electrode layer, an increase in resistance of the lithium solid state battery can be suppressed, although the reason is unclear.
[0199] From the above results, it was confirmed that when a phosphorus ester compound is added to at least the negative electrode layer, the thermal stability of the lithium solid state battery is improved and an increase in resistance can be suppressed.
Claims
1. Lithium solid state battery, It is characterized in that The invention comprises a positive electrode, a negative electrode and a solid electrolyte layer, wherein the positive electrode comprises a positive electrode layer containing an oxide-based positive electrode active material, the negative electrode comprises a negative electrode layer containing a negative electrode active material, and the solid electrolyte layer is arranged between the positive electrode layer and the negative electrode layer and contains a solid electrolyte. The above oxide-based positive electrode active material is LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 , The negative electrode active material is Si single substance. The solid electrolyte layer includes Li containing lithium iodide 2 SP 2 S 5 Glass ceramics are used as solid electrolytes. The negative electrode layer contains a sulfide-based solid electrolyte. The negative electrode layer further comprises tris(2,2,2-trifluoroethyl) phosphate, The content of the tris(2,2,2-trifluoroethyl)phosphate in the negative electrode layer is 1% by mass or more and 10% by mass or less, when the total mass of the negative electrode layer is 100% by mass.
2. The lithium solid state battery according to claim 1, It is characterized in that The content of the tris(2,2,2-trifluoroethyl)phosphate in the negative electrode layer was 5% by mass when the total mass of the negative electrode layer was 100% by mass.
Citation Information
Patent Citations
Flame retardant composition for polymer solid electrolyte
JP2003238821A
Lithium solid battery
JP2017112041A
Lithium secondary battery
CN104247139A
Nonaqueous electrolyte secondary battery
CN105322174A
Solid-state lithium battery
CN106898827A