High energy density lithium battery for power tools
Through the composite cathode material of Li(NixCoyMn1-x-y)O2, metal MOF material and lithium iron phosphate, the problem of lithium battery being unable to meet high specific energy and high cycleability at the same time is solved, and high energy density and cycle performance are improved, which is suitable for Power tools.
Patent Information
- Application Number
- CN202110823202.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-07-21
AI Technical Summary
Existing lithium batteries cannot meet the requirements of high specific energy and high cycleability at the same time, and high-nickel materials have gas production problems and poor low-temperature performance. The synthesis of metal MOF materials is complex and costly, and has poor conductivity, which limits its application.
A composite cathode material of Li(NixCoyMn1-x-y)O2, metal MOF material and lithium iron phosphate is used to prepare the metal MOF material through electrodeposition and roasting to form a conductive network structure and improve the conductivity and cycle performance of lithium batteries.
Significantly improves the energy density and cycle performance of lithium batteries, has both good conductivity and cycleability, and is suitable for power tools.
Smart Images

Figure BDA0003172612650000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of lithium batteries, and in particular to a high specific energy lithium battery for electric tools. Background Art
[0002] With the continuous development of technology, the use of power tools is becoming more and more widespread, such as lawn mowers, drills, sanders, multi-functional woodworking power tools, etc. The use of power tools has greatly improved people's work efficiency and work comfort. In the prior art, power tools generally use battery packs to provide power, making the power tools easy to carry. As a power reserve source, secondary batteries are the first choice for battery packs. In addition, among the existing secondary batteries, lithium secondary batteries with high energy density and working voltage, long cycle life and low self-discharge rate are widely used.
[0003] Currently, the cathode materials LiCoO2 and ternary materials (NCM) on the market cannot meet the requirements of high specific energy and high cyclability at the same time. In addition, the development of high-nickel materials is further restricted by the serious gas production problem and poor low-temperature performance. There are also some studies that use metal MOF materials directly as battery cathode materials, but on the one hand, the synthesis of metal MOF materials is complex and the cost is high, and on the other hand, the poor conductivity of metal MOF materials also restricts the further application of metal MOF materials.
[0004] Therefore, it is particularly important to find a lithium battery with both high specific energy and high cyclability. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem that the existing lithium batteries in the prior art cannot have both high specific energy and high cyclability, and to provide a high specific energy lithium battery for electric tools.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A high specific energy lithium battery for electric tools, the high specific energy lithium battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, the positive electrode comprising a positive electrode collector and a positive electrode material coated on the positive electrode collector;
[0008] The positive electrode material comprises 1-30 wt % of Li(Ni x Co y Mn 1-x-y )O2, 20-30 wt% of a metal MOF material and 40-79 wt% of lithium iron phosphate; wherein 0≤x≤1, 0≤y≤1, and x+y≤1;
[0009] The preparation method of the metal MOF material comprises:
[0010] The metal salt, the organic ligand and the conductive medium are uniformly mixed in an organic solvent to obtain a mixed solution;
[0011] Electrodepositing the mixed solution to obtain a precursor;
[0012] calcining the precursor in a protective atmosphere to obtain a metal MOF material;
[0013] The metal salt is selected from at least one of lithium salts, cobalt salts, barium salts, gallium salts and molybdenum salts.
[0014] Preferably, the metal salt is composed of lithium salt, cobalt salt and molybdenum salt in a molar ratio of 1:0.5-1.5:0.001-0.005.
[0015] Preferably, the organic ligand is selected from at least one of p-dibenzoic acid, 1,3,5-tris(3,5-m-dicarboxyphenyl)benzene, 2,3',3",5,5',5"-terphenylhexacarboxylic acid, mellitic acid, tetrakis[4-(3,5-dicarboxyphenyl)]tetraphenylethylene and 2,4,6-tris(3,5-dicarboxyphenylamino)-1,3,5-triazine.
[0016] Preferably, the concentration of the conductive medium is 0.3-0.5 g / mL.
[0017] Preferably, the conductive medium is selected from at least one of 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethylpyridine tetrafluoroborate, 1-butyl-3-methylimidazolium tetracyanoborate, 1-ethylpyridine tetracyanoborate, 1-methyl-3-ethylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-butylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-hexylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-octylimidazole disalicylate chelated boron ionic liquid, tetrabutylphosphonium chloride, tetraethylphosphonium chloride, 1-ethyl-3-methylimidazolium dihexyl phosphate, 1-butyl-3-methylimidazolium methanesulfonate, 1-ethyl-3-methylimidazolium toluenesulfonate, and 1-ethylpyridine thiocyanate.
[0018] Preferably, the organic solvent is selected from at least one of acetone, DMF, tetrahydrofuran, dimethyl sulfoxide, dimethylacetamide, dichloromethane, acetonitrile, N-methylpyrrolidone and butyrolactone.
[0019] Preferably, the concentration of the metal salt is 0.1-0.8 mol / L; the concentration of the organic ligand is 0.1-0.5 mol / L.
[0020] Preferably, the particle size of the metal MOF material is 3-5 μm.
[0021] Preferably, the Li(Ni x Co y Mn 1-x-y )The particle size of O2 is 5-8μm.
[0022] Preferably, the particle size of the lithium iron phosphate is 0.3-1.2 μm.
[0023] Compared with the prior art, the present invention has the following technical effects:
[0024] Through the above technical solution, the present invention is through Li (Ni x Co y Mn 1-x-y )O2, metal MOF materials and lithium iron phosphate materials are combined to make the positive electrode of lithium batteries have good conductivity, cyclability and high specific energy. In addition, Li(Ni x Co y Mn 1-x-y The energy density and cycle performance of lithium batteries can be significantly improved by combining )O2, metal MOF materials of a specific particle size and lithium iron phosphate materials of a specific particle size. DETAILED DESCRIPTION
[0025] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific embodiments.
[0026] As mentioned above, the present invention provides a high specific energy lithium battery for electric tools, the high specific energy lithium battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, the positive electrode comprising a positive electrode collector and a positive electrode material coated on the positive electrode collector;
[0027] The positive electrode material comprises 1-30 wt % of Li(Ni x Co y Mn 1-x-y )O2, 20-30 wt% of a metal MOF material and 40-79 wt% of lithium iron phosphate; wherein 0≤x≤1, 0≤y≤1, and x+y≤1;
[0028] The preparation method of the metal MOF material comprises:
[0029] The metal salt, the organic ligand and the conductive medium are uniformly mixed in an organic solvent to obtain a mixed solution;
[0030] Electrodepositing the mixed solution to obtain a precursor;
[0031] calcining the precursor in a protective atmosphere to obtain a metal MOF material;
[0032] The metal salt is selected from at least one of lithium salts, cobalt salts, barium salts, gallium salts and molybdenum salts.
[0033] In the present invention, a metal salt, an organic ligand and a conductive medium are mixed and then electrodeposited to form a metal organic framework material. The metal organic framework material forms a three-dimensional skeleton structure after calcination, and can form a conductive and mass-conducting network structure, which helps to improve the conductivity of the lithium battery and reduce the impedance of the positive electrode material.
[0034] In the present invention, the metal salt can be the one commonly used by people in the art. In particular, the metal salt is composed of lithium salt, cobalt salt and molybdenum salt in a molar ratio of 1:0.5-1.5:0.001-0.005.
[0035] In the present invention, the organic ligand can be specifically selected from at least one of p-dibenzoic acid, 1,3,5-tris(3,5-m-dicarboxyphenyl)benzene, 2,3',3",5,5',5"-terphenylhexacarboxylic acid, mellitic acid, tetrakis[4-(3,5-dicarboxyphenyl)]tetraphenylethylene and 2,4,6-tris(3,5-dicarboxyphenylamino)-1,3,5-triazine.
[0036] The concentration of the conductive medium is 0.3-0.5 g / mL.
[0037] In the present invention, the conductive medium can be specifically selected from at least one of 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethylpyridine tetrafluoroborate, 1-butyl-3-methylimidazolium tetracyanoborate, 1-ethylpyridine tetracyanoborate, 1-methyl-3-ethylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-butylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-hexylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-octylimidazole disalicylate chelated boron ionic liquid, tetrabutylphosphonium chloride, tetraethylphosphonium chloride, 1-ethyl-3-methylimidazolium dihexyl phosphate, 1-butyl-3-methylimidazolium methanesulfonate, 1-ethyl-3-methylimidazolium toluenesulfonate, and 1-ethylpyridine thiocyanate.
[0038] The organic solvent is selected from at least one of acetone, DMF, tetrahydrofuran, dimethyl sulfoxide, dimethylacetamide, dichloromethane, acetonitrile, N-methylpyrrolidone and butyrolactone.
[0039] The concentration of the metal salt is 0.1-0.8 mol / L; the concentration of the organic ligand is 0.1-0.5 mol / L.
[0040] The particle size of the metal MOF material is 3-5 μm.
[0041] The Li(Ni x Co y Mn 1-x-y )The particle size of O2 is 5-8μm.
[0042] The particle size of the lithium iron phosphate is 0.3-1.2 μm.
[0043] The present invention will be described in detail below through examples.
[0044] Example 1
[0045] (1) Preparation of metal MOF materials
[0046] 5 mmol lithium nitrate, 5 mmol cobalt nitrate and 0.01 mmol ammonium molybdate, 5 mL organic ligand 2,3',3",5,5',5"-terphenylhexacarboxylic acid (0.3 mol / L) and 5 mL conductive medium 1-butyl-3-methylimidazolium hexafluorophosphate (0.4 g / mL) were mixed in DMF to obtain a mixed solution;
[0047] Two copper sheets were used as anode and cathode respectively, and the current density was 0.05A / cm 2 Under the condition of , electricity is supplied for 4 hours to carry out electrodeposition, and a precursor is deposited at the bottom of the container;
[0048] The precursor was calcined in a tube furnace (under nitrogen protection) at a temperature of 650° C. for 3 h to obtain a metal MOF material with a particle size of 5 μm.
[0049] (2) Preparation of positive electrode materials
[0050] Positive electrode active material: 25 wt% Li(Ni 0.33 Co 0.33 Mn 0.34 )O2 (particle size 8 μm), 25 wt% metal MOF material and 50 wt% lithium iron phosphate (1 μm);
[0051] 98 wt % of positive electrode active material, 1 wt % of conductive agent carbon black, and 1 wt % of binder PVDF are mixed evenly in NMP to obtain positive electrode slurry, and then the positive electrode slurry is coated on an Al sheet, and then dried and rolled to obtain a positive electrode;
[0052] (3) Assembly of lithium batteries
[0053] The positive electrode obtained in step (2) is used as the positive electrode, lithium metal is used as the negative electrode, the separator is a polymer separator (PP / / PE / / PP), and the electrolyte is 1M LiBF4 / PC:DME (1:1).
[0054] Example 2
[0055] The method of Example 1 is followed, except that ammonium molybdate is not added in the preparation of the metal MOF material; the rest remains unchanged, and a lithium battery is assembled.
[0056] Example 3
[0057] The method of Example 1 is followed, except that cobalt nitrate is not added during the preparation of the metal MOF material; the rest remains unchanged, and a lithium battery is assembled.
[0058] Example 4
[0059] The method of Example 1 is followed, except that the positive electrode material is composed of 50 wt% Li(Ni 0.33 Co 0.33 Mn 0.34 )O2 (particle size 8 μm) and 50 wt% lithium iron phosphate (1 μm).
[0060] Example 5
[0061] The method of Example 1 is followed, except that the positive electrode material is composed of 50 wt % metal MOF material (particle size of 5 μm) and 50 wt % lithium iron phosphate (1 μm).
[0062] Example 6
[0063] The method of Example 1 is followed, except that the positive electrode material is composed of 50 wt% metal MOF material (particle size 5 μm) and 50 wt% Li (Ni 0.33 Co 0.33 Mn 0.34 )O2 (particle size is 8μm).
[0064] Example 7
[0065] The method of Example 1 is followed, except that Li(Ni 0.33 Co 0.33 Mn 0.34 )The particle size of O2 is 20μm.
[0066] Example 8
[0067] The method of Example 1 is followed, except that Li(Ni 0.33 Co 0.33 Mn 0.34 )The particle size of O2 is 3μm.
[0068] Example 9
[0069] The method of Example 1 is followed, except that the particle size of the lithium iron phosphate is 5 μm.
[0070] Example 10
[0071] The method of Example 1 is followed, except that the particle size of the lithium iron phosphate is 0.1 μm.
[0072] Electrochemical testing
[0073] (1) The charge and discharge voltage range is 3-4.5V for cycle testing, the cycle number is 800 cycles, and the capacity retention rate of the lithium battery is recorded after 800 cycles. The experimental results are shown in Tables 1 and 2.
[0074] 1C / Ah / kg 2C / Ah / kg 5C / Ah / kg 10C / Ah / kg 20C / Ah / kg Example 1 892 872 846 806 759 Example 2 870 833 768 689 633 Example 3 851 825 788 730 682 Example 4 793 762 733 692 642 Example 5 734 715 882 840 785 Example 6 764 746 710 672 617 Example 7 782 760 734 684 627 Example 8 826 801 775 732 576 Example 9 683 657 624 579 527 Example 10 831 806 768 718 674
[0075] Table 2
[0076]
[0077] It can be seen from Table 1 and Table 2 that in the present invention, the particle size of the metal MOF material with a particle size of 3-5 μm is similar to that of the Li(Ni) with a particle size of 5-8 μm. x Co y Mn 1-x-y )O2 and lithium iron phosphate with a particle size of 0.3-1.2μm can significantly improve the specific energy, rate discharge performance and cycle performance of lithium batteries.
[0078] The above shows and describes the basic principles, main features and characteristics of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of the present invention to be protected is defined by the attached claims and their equivalents.
Claims
1. A high specific energy lithium battery for electric tools, characterized in that: The high specific energy lithium battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode material coated on the positive electrode current collector; The positive electrode material comprises 1-30 wt % of Li(Ni x Co y Mn 1-x-y )O2, 20-30 wt% of a metal MOF material and 40-79 wt% of lithium iron phosphate; wherein 0≤x≤1, 0≤y≤1, and x+y≤1; The preparation method of the metal MOF material comprises: The metal salt, the organic ligand and the conductive medium are uniformly mixed in an organic solvent to obtain a mixed solution; Electrodepositing the mixed solution to obtain a precursor; calcining the precursor in a protective atmosphere to obtain a metal MOF material; The metal salt is composed of lithium nitrate, cobalt nitrate and ammonium molybdate in a molar ratio of 1:0.5-1.5:0.001-0.005; The particle size of the metal MOF material is 3-5 μm; The Li(Ni x Co y Mn 1-x-y ) The particle size of O2 is 5-8 μm; The particle size of the lithium iron phosphate is 0.3-1.2 μm.
2. The high specific energy lithium battery for electric tools according to claim 1, characterized in that: The organic ligand is selected from at least one of p-dibenzoic acid, 1,3,5-tris(3,5-m-dicarboxyphenyl)benzene, 2,3',3",5,5',5"-terphenylhexacarboxylic acid, mellitic acid, tetrakis[4-(3,5-dicarboxyphenyl)]tetraphenylethylene and 2,4,6-tris(3,5-dicarboxyphenylamino)-1,3,5-triazine.
3. The high specific energy lithium battery for electric tools according to claim 1, characterized in that: The concentration of the conductive medium is 0.3-0.5 g / mL.
4. The high specific energy lithium battery for electric tools according to claim 1, characterized in that: The conductive medium is selected from at least one of 1-butyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethylpyridine tetrafluoroborate, 1-butyl-3-methylimidazolium tetracyanoborate, 1-ethylpyridine tetracyanoborate, 1-methyl-3-ethylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-butylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-hexylimidazolium disalicylate chelated boron ionic liquid, 1-methyl-3-octylimidazole disalicylate chelated boron ionic liquid, tetrabutylphosphonium chloride, tetraethylphosphonium chloride, 1-ethyl-3-methylimidazolium dihexyl phosphate, 1-butyl-3-methylimidazolium methanesulfonate, 1-ethyl-3-methylimidazolium toluenesulfonate, and 1-ethylpyridine thiocyanate.
5. The high specific energy lithium battery for electric tools according to claim 1, characterized in that: The organic solvent is selected from at least one of acetone, DMF, tetrahydrofuran, dimethyl sulfoxide, dimethylacetamide, dichloromethane, acetonitrile, N-methylpyrrolidone and butyrolactone.
6. The high specific energy lithium battery for electric tools according to claim 1, characterized in that: The concentration of the metal salt is 0.1-0.8 mol / L; the concentration of the organic ligand is 0.1-0.5 mol / L.
Citation Information
Patent Citations
Lithium battery anode material, lithium battery anode, preparing method of lithium battery anode, and lithium battery
CN107732201A
NCM (Nickel Cobalt Manganese)-lithium iron phosphate anode material, lithium ion battery and preparation method of lithium ion battery
CN107946586A
Modified lithium iron phosphate material and preparation method thereof
CN111916732A
Cathode active material added with fluorine compound for lithium secondary batteries and method of producing thereof
WO2006137673A1
Electrodes having electrode additive for high performance batteries and applications of same
WO2020167725A1