Semiconductor photoresist composition and method for forming pattern using the same
By using a combination of an organic metal compound and a specific organic acid in the photoresist, the problem of insufficient resolution and roughness of the existing photoresist in extreme ultraviolet lithography is solved, and high resolution and low roughness are achieved. Pattern formation.
Patent Information
- Application Number
- CN202110510318.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-12
- Filing Date
- 2021-05-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-05-11
AI Technical Summary
Existing chemically amplified photoresists have deficiencies in resolution, photosensitivity speed and line edge roughness in extreme ultraviolet lithography, making it difficult to meet the needs of next-generation semiconductor devices.
A semiconductor photoresist composition containing an organometallic compound and an organic acid with a specific vapor pressure and pKa value is used to improve the resolution, sensitivity and etching resistance of the photoresist by adjusting the ratio of ligands and additives.
Achieving high resolution, low line edge roughness and improved patterning capabilities in extreme ultraviolet lithography, providing high aspect ratio photoresist patterns without pattern collapse.
Smart Images

Figure CN113655689B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2020-0056720 filed in the Korean Intellectual Property Office on May 12, 2020, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present disclosure relates to a semiconductor photoresist composition and a method of forming a pattern using the same. Background Art
[0004] Extreme ultraviolet (EUV) lithography has attracted attention as a basic technology for manufacturing next-generation semiconductor devices. EUV lithography is a pattern forming technology that uses EUV rays having a wavelength of about 13.5 nanometers as an exposure light source. According to EUV lithography, it is known that extremely fine patterns (e.g., less than or equal to about 20 nanometers) can be formed in an exposure process during the manufacture of semiconductor devices.
[0005] Extreme ultraviolet (EUV) lithography is achieved through the development of compatible photoresists that can be performed at a spatial resolution of less than or equal to about 16 nanometers. Currently, efforts are underway to meet the inadequate specifications of conventional chemically amplified (CA) photoresists for next-generation devices, such as resolution, photospeed, and feature roughness (or also known as line edge roughness or LER).
[0006] Intrinsic image blurring due to acid-catalyzed reactions in these polymer-based photoresists limits resolution in small feature sizes, which has long been known in electron beam (e-beam) lithography. Chemically amplified (CA) photoresists are designed for high sensitivity, but may have more difficulty under EUV exposure in part because their typical elemental composition reduces the photoresist's light absorption at wavelengths of about 13.5 nanometers and thus reduces its sensitivity.
[0007] In addition, CA photoresists may have difficulty with small feature sizes due to roughness issues, and experimentally, the line edge roughness (LER) of CA photoresists increases because the photospeed is reduced in part due to the nature of the acid catalyst process. Therefore, due to these defects and problems of CA photoresists, new high performance photoresists are needed in the semiconductor industry.
[0008] Inorganic photoresists based on peroxopolyacids of tungsten mixed with tungsten, niobium, titanium and / or tantalum have been reported as radiation-sensitive materials for patterning ( US 5061599 ; H. Okamoto, T. Iwayanagi, K. Mochiji, H. Umezaki, T. Kudo, Applied Physics Letters, 495, 298-300, 1986 ).
[0009] These materials are effective for patterning large features for dual layer configurations, such as extreme ultraviolet (deep UV), X-ray, and electron beam sources. Recently, impressive performance has been achieved in the case of using cationic metal oxide hafnium sulfate (HfSOx) materials with peroxide complexing agents for imaging 15 nanometer half-pitch (HP) by projection EUV exposure (US2011-0045406; JK Stowers, A. Telecky, M. Kocsis, BL Clark, DA Keszler, A. Grenville, CN Anderson, PP Naulleau, Proc. SPIE, 7969, 796915, 2011). This system presents the highest performance of non-CA photoresists and has a feasible photosensitivity close to the requirements of EUV photoresists. However, metal oxide hafnium sulfate materials with peroxo complexing agents have several practical disadvantages. First, these materials are coated in a corrosive sulfuric acid / hydrogen peroxide mixture and have insufficient shelf life stability. Second, as a complex mixture, it is not easy to change the structure for performance improvement. Third, it should be developed in tetramethylammonium hydroxide (TMAH) solutions at very high concentrations of about 25 wt% and the like.
[0010] In order to overcome the aforementioned disadvantages of chemically amplified (CA) organic photosensitive compositions, inorganic photosensitive compositions have been studied. Inorganic photosensitive compositions are mainly used for negative patterning, which has resistance to removal by a developer composition due to chemical modification by a non-chemical amplification mechanism. The inorganic composition contains an inorganic element having a higher EUV absorption rate than hydrocarbons, and thus can ensure sensitivity by a non-chemical amplification mechanism, and in addition, is less sensitive to stochastic effects, and thus is known to have low line edge roughness and a small number of defects.
[0011] In recent years, since molecules containing tin are known to have excellent extreme ultraviolet absorption, active research has been conducted. For organotin polymers therein, alkyl ligands are dissociated by light absorption or secondary electrons generated thereby, and cross-linked with adjacent chains by oxo bonds, and thus negative patterning that can be removed without organic developer is achieved. Such organotin polymers exhibit greatly improved sensitivity and maintain resolution and line edge roughness, but additional improvement in patterning characteristics is required for commercial availability. Summary of the invention
[0012] Embodiments provide a semiconductor photoresist composition having improved resolution, sensitivity, etching resistance, and pattern forming capability.
[0013] Another embodiment provides a method of forming a pattern using a semiconductor photoresist composition.
[0014] A semiconductor photoresist composition according to an embodiment includes (A) an organic metal compound, (B) an organic acid having a vapor pressure of less than or equal to about 1.0 mmHg at 25° C. and a pKa of about 3 to about 5, and (C) a solvent.
[0015] The (B) organic acid may have a vapor pressure of about 0.01 mmHg to about 0.5 mmHg at 25° C. and a pKa of about 3 to about 4.3.
[0016] The (B) organic acid may be included in an amount of about 0.1 parts by weight to about 15 parts by weight based on 100 parts by weight of the (A) organic metal compound.
[0017] The semiconductor photoresist composition may include about 0.01 wt % to about 2 wt % of the organic acid based on the total mass of the semiconductor photoresist composition.
[0018] The (A) organic metal compound may be a compound containing tin (Sn).
[0019] (A) The organic metal compound may be an organic metal compound represented by Chemical Formula 1.
[0020] [Chemical formula 1]
[0021]
[0022] In Chemical Formula 1,
[0023] R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethoxy group, a propoxy group, or a combination thereof,
[0024] X, Y and Z are each independently -OR 1 or -OC(=O)R 2 ,
[0025] R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and
[0026] R 2 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.
[0027] The semiconductor photoresist composition may further include, in addition to the compound represented by Chemical Formula 1, an organic metal compound represented by Chemical Formula 2, an organic metal compound represented by Chemical Formula 3, or a combination thereof.
[0028] [Chemical formula 2]
[0029]
[0030] In chemical formula 2,
[0031] X' is -OR 3 or -OC(=O)R 4 ,
[0032] R 3 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and
[0033] R 4 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof;
[0034] [Chemical formula 3]
[0035]
[0036] Among them, in chemical formula 3,
[0037] X" is -OR 5 or -OC(=O)R 6 ,
[0038] R 5 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof,
[0039] R 6 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and
[0040] L is a single bond, a substituted or unsubstituted divalent C1 to C20 saturated aliphatic hydrocarbon group, a substituted or unsubstituted divalent C3 to C20 saturated or unsaturated alicyclic hydrocarbon group, a substituted or unsubstituted divalent C2 to C20 unsaturated aliphatic hydrocarbon group containing at least one double bond or triple bond, a substituted or unsubstituted divalent C6 to C20 aromatic hydrocarbon group, -O-, -C(=O)-, or a combination thereof.
[0041] The total of the compound represented by Chemical Formula 2 and the compound represented by Chemical Formula 3 and the organic metal compound represented by Chemical Formula 1 may be included in a weight ratio of about 1:1 to about 1:20.
[0042] The compound represented by Chemical Formula 1 may include a compound represented by Chemical Formula 4, a compound represented by Chemical Formula 5, a compound represented by Chemical Formula 6, a compound represented by Chemical Formula 7, or a combination thereof.
[0043] [Chemical formula 4]
[0044]
[0045] [Chemical formula 5]
[0046]
[0047] [Chemical formula 6]
[0048]
[0049] [Chemical formula 7]
[0050]
[0051] In Chemical Formula 4 to Chemical Formula 7,
[0052] R a , R b , R c , R i , Rk and R l Independently with R 1 The definition of is the same as
[0053] R d , R e , R f , R g , R h and R j Independently with R 2 The definition is the same.
[0054] The semiconductor photoresist composition may further include an additive of a surfactant, a cross-linking agent, a leveler, a quencher, or a combination thereof.
[0055] The method of forming a pattern according to an embodiment includes: forming an etch target layer on a substrate; coating a semiconductor photoresist composition on the etch target layer to form a photoresist layer; patterning the photoresist layer to form a photoresist pattern; and etching the etch target layer using the photoresist pattern as an etch mask.
[0056] The photoresist pattern may be formed using light having a wavelength of about 5 nanometers to about 150 nanometers.
[0057] The method of forming a pattern may further include providing a resist bottom layer formed between the substrate and the photoresist layer.
[0058] The photoresist pattern may have a width of about 5 nanometers to about 100 nanometers.
[0059] The semiconductor photoresist composition according to the embodiment has relatively improved etching resistance, sensitivity, resolution, and pattern forming ability, and thus can provide a photoresist pattern having improved sensitivity and a high aspect ratio without pattern collapse. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figures 1 to 5 is a cross-sectional view for explaining a method of forming a pattern using a semiconductor photoresist composition according to an embodiment.
[0061] Description of Figure Numbers
[0062] 100: substrate;
[0063] 102: Film;
[0064] 104: resist bottom layer;
[0065] 106: photoresist layer;
[0066] 106a: non-exposed area;
[0067] 106b: exposure area;
[0068] 108: photoresist pattern;
[0069] 112: organic layer pattern;
[0070] 114: Thin film pattern. DETAILED DESCRIPTION
[0071] Hereinafter, with reference to the accompanying drawings, embodiments of the present disclosure are described in detail. In the following description of the present disclosure, well-known functions or constructions will not be described in order to clarify the present disclosure.
[0072] In order to clearly illustrate the present disclosure, description and relationship are omitted, and throughout the present disclosure, the same or similar configuration elements are designated by the same reference numerals. In addition, since the size and thickness of each configuration shown in the drawings are arbitrarily shown for better understanding and ease of description, the present disclosure is not necessarily limited thereto.
[0073] In the drawings, thicknesses are exaggerated to clearly indicate various layers and regions. In the drawings, thicknesses of portions of layers or regions, etc., are exaggerated for clarity. It should be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it can be directly on the other element, or intervening elements may also be present.
[0074] As used herein, "substituted" refers to replacement of a hydrogen atom by: deuterium, halogen, hydroxyl, cyano, nitro, -NRR' (wherein, R and R' are independently hydrogen, substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or substituted or unsubstituted C6 to C30 aromatic hydrocarbon group), -SiRR'R" (wherein, R, R' and R" are independently hydrogen, substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or substituted or unsubstituted C6 to C30 aromatic hydrocarbon group), C1 to C30 alkyl, C1 to C10 haloalkyl, C1 to C10 alkylsilanyl, C3 to C30 cycloalkyl, C6 to C30 aryl, C1 to C20 alkoxy or a combination thereof. "Unsubstituted" means that a hydrogen atom is not replaced by another substituent and that a hydrogen atom remains.
[0075] As used herein, when no definition is otherwise provided, "alkyl" refers to a straight or branched aliphatic hydrocarbon group. The alkyl group may be a "saturated alkyl group" not having any double or triple bonds.
[0076] The alkyl group may be a C1 to C8 alkyl group. For example, the alkyl group may be a C1 to C7 alkyl group, a C1 to C6 alkyl group, a C1 to C5 alkyl group, or a C1 to C4 alkyl group. For example, the C1 to C4 alkyl group may be a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, or a 2,2-dimethylpropyl group.
[0077] As used herein, when a definition is not otherwise provided, "cycloalkyl" refers to a monovalent cyclic aliphatic hydrocarbon group.
[0078] The cycloalkyl group may be a C3 to C8 cycloalkyl group, such as a C3 to C7 cycloalkyl group, a C3 to C6 cycloalkyl group, a C3 to C5 cycloalkyl group, or a C3 to C4 cycloalkyl group. For example, the cycloalkyl group may be a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, or a cyclohexyl group, but is not limited thereto.
[0079] As used herein, "aliphatic unsaturated organic group" refers to a hydrocarbon group containing bonds, wherein the bonds between carbon and carbon atoms in the molecule are double bonds, triple bonds, or a combination thereof.
[0080] The aliphatic unsaturated organic group can be a C2 to C8 aliphatic unsaturated organic group. For example, the aliphatic unsaturated organic group can be a C2 to C7 aliphatic unsaturated organic group, a C2 to C6 aliphatic unsaturated organic group, a C2 to C5 aliphatic unsaturated organic group or a C2 to C4 aliphatic unsaturated organic group. For example, the C2 to C4 aliphatic unsaturated organic group can be vinyl, ethynyl, allyl, 1-propenyl, 1-methyl-1-propenyl, 2-propenyl, 2-methyl-2-propenyl, 1-propynyl, 1-methyl-1-propynyl, 2-propynyl, 2-methyl-2-propynyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-butynyl, 2-butynyl or 3-butynyl.
[0081] As used herein, "aryl" refers to a substituent in which all atoms in the cyclic substituent have p-orbitals and these p-orbitals are conjugated and may contain monocyclic or fused-ring polycyclic functional groups (ie, rings that share adjacent pairs of carbon atoms) functional groups.
[0082] As used herein, unless otherwise defined, "alkenyl" refers to an aliphatically unsaturated alkenyl group containing at least one double bond as a straight or branched aliphatic hydrocarbon group.
[0083] As used herein, unless otherwise defined, "alkynyl" refers to an aliphatic unsaturated alkynyl group containing at least one triple bond as a straight or branched aliphatic hydrocarbon group.
[0084] Hereinafter, a semiconductor photoresist composition according to an embodiment is described.
[0085] A semiconductor photoresist composition according to an embodiment of the present disclosure includes (A) an organometallic compound, (B) an organic acid having a vapor pressure of less than or equal to about 1.0 mmHg at 25° C. and a pKa of about 3 to about 5, and (C) a solvent.
[0086] Meanwhile, the (A) organic metal compound may include tin (Sn), and specifically, the (A) organic metal compound may be represented by Chemical Formula 1.
[0087] [Chemical formula 1]
[0088]
[0089] In Chemical Formula 1,
[0090] R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethoxy group, a propoxy group, or a combination thereof,
[0091] X, Y and Z are each independently -OR 1 or -OC(=O)R 2 ,
[0092] R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and
[0093] R 2 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.
[0094] The organometallic compound represented by Chemical Formula 1 has a structure in which the tin atom is composed of one R group and three -OR 1 or -OC(=O)R 2 Replaced structure.
[0095] The compound represented by Chemical Formula 1 is an organic tin compound, wherein tin can strongly absorb extreme ultraviolet (EUV) light at 13.5 nanometers and thus has excellent sensitivity with respect to light having high energy, and R of Chemical Formula 1 can give photosensitivity to the compound represented by Chemical Formula 1 and further, can bond to tin and form a Sn—R bond, and thus impart solubility to an organic solvent to the organic tin compound.
[0096] Regarding R of Chemical Formula 1, when an organic tin copolymer having a structural unit represented by Chemical Formula 1 and formed by copolymerization of an organic metal compound is exposed to extreme ultraviolet rays, the R functional group dissociates from the Sn-R bond and forms a free radical, and this free radical forms an additional -Sn-O-Sn- bond and initiates a condensation polymerization reaction between the organic tin copolymers, and thus facilitates the formation of a semiconductor photoresist from the composition according to an embodiment.
[0097] In the organometallic compound represented by Chemical Formula 1, the substituent represented by R may be a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethoxy group, a propoxy group, or a combination thereof.
[0098] The organometallic compound represented by Chemical Formula 1 further includes three organic ligands X, Y, and Z, each of which is hydrolyzed to form a Sn-O bond. X, Y, and Z are heat-treated under an acidic catalyst or an alkaline catalyst, or hydrolyzed and dehydrated by non-thermal treatment to form a Sn-O-Sn bond between the organotin compounds, thereby forming an organotin copolymer including the organometallic compound represented by Chemical Formula 1.
[0099] In addition, X, Y, and Z determine the solubility of the organometallic compound represented by Chemical Formula 1 in a solvent.
[0100] In addition to the organic metal compound represented by Chemical Formula 1 and the solvent, the semiconductor photoresist composition according to an embodiment of the present disclosure further includes an organic acid, wherein the organic acid has a vapor pressure of less than or equal to about 1.0 mmHg at 25° C. When the semiconductor photoresist composition includes an organic acid satisfying the vapor pressure and pKa conditions, it is possible to improve pattern forming characteristics of the semiconductor photoresist composition, such as resolution, sensitivity, and line edge roughness (LER) characteristics.
[0101] The organic acid may have a vapor pressure of less than or equal to about 1.0 mmHg at 25° C., for example, less than or equal to about 0.9 mmHg, less than or equal to about 0.8 mmHg, less than or equal to about 0.7 mmHg, less than or equal to about 0.6 mmHg, less than or equal to about 0.5 mmHg, less than or equal to about 0.4 mmHg, less than or equal to about 0.3 mmHg, less than or equal to about 0.2 mmHg, less than or equal to about 0.1 mmHg, less than or equal to about 0.09 mmHg, less than or equal to about 0.08 mmHg, less than or equal to about 0.07 mmHg, less than or equal to about 0.06 mmHg, less than or equal to about 0.05 mmHg, less than or equal to about 0.04 mmHg, less than or equal to about 0.03 mmHg, less than or equal to about 0.02 mmHg, or less than or equal to about 0.01 mmHg, but is not limited thereto. When the organic acid has a vapor pressure greater than about 1.0 mmHg at about 25° C., the organic acid is easily evaporated on the wafer, and the effect of improving the pattern forming characteristics of the semiconductor photoresist composition such as resolution, sensitivity, line edge roughness (LER) characteristics, and the like is not achieved when the semiconductor photoresist composition is coated on the wafer.
[0102] When the acid (HA) dissociates into H + When A-, pKa is obtained by taking the negative logarithm (-logarithm) of the acid dissociation constant Ka, wherein the larger the pKa, the weaker the acid. The organic acid included in the semiconductor photoresist composition according to an embodiment of the present disclosure may have a pKa of about 3 to about 5, for example, about 3 to about 4.9, about 3 to about 4.8, about 3 to about 4.7, about 3 to about 4.6, about 3 to about 4.5, about 3 to about 4.4, about 3 to about 4.3, about 3 to about 4.2, about 3 to about 4.1 or about 3 to about 4. When two or more than two acid dissociation functional groups are present in one organic acid molecule, the pKa of the molecule is determined by the functional group with the lowest pKa. When the semiconductor photoresist composition also includes an organic acid with a pKa of about 3 to about 5, the resolution, sensitivity and line edge roughness (LER) characteristics can be improved more than when the semiconductor photoresist composition includes an organic acid with a pKa less than about 3 or greater than about 5 or no organic acid.
[0103] The organic acid may contain two or more different types of organic acids at the same time.
[0104] The organic acid may be, for example, citric acid, glycolic acid, lactic acid, succinic acid, etc., but is not limited thereto.
[0105] (B) organic acid may be included in an amount of about 0.1 parts by weight or more, about 0.2 parts by weight or more, about 0.3 parts by weight or more, about 0.4 parts by weight or more, about 0.5 parts by weight or more, about 0.6 parts by weight or more, about 0.7 parts by weight or more, about 0.8 parts by weight or more, about 0.9 parts by weight or more, about 1.0 parts by weight or less, about 15 parts by weight or less, about 14 parts by weight or less, about 13 parts by weight or less, about 12 parts by weight or less, about 11 parts by weight or less, or about 10 parts by weight or less, based on 100 parts by weight of (A) organometallic compound. When the organic acid is included in the semiconductor photoresist composition in the above content range, the resolution, sensitivity, and line edge roughness (LER) characteristics may be improved at the same time.
[0106] The semiconductor photoresist composition may include an organic acid in an amount of about 0.01 wt % to about 2 wt %, based on the total mass of the semiconductor photoresist composition, such as about 0.01 wt % to about 1.9 wt %, about 0.01 wt % to about 1.8 wt %, about 0.01 wt % to about 1.7 wt %, about 0.01 wt % to about 1.6 wt %, about 0.01 wt % to about 1.5 wt %, about 0.01 wt % to about 1.4 wt %, about 0.01 wt % to about 1.3 wt %, about 0.01 wt % to about 1.2 wt %. %, about 0.01 wt % to about 1.1 wt %, about 0.01 wt % to about 1.0 wt %, about 0.01 wt % to about 0.9 wt %, about 0.01 wt % to about 0.8 wt %, about 0.01 wt % to about 0.7 wt %, about 0.01 wt % to about 0.6 wt %, about 0.01 wt % to about 0.5 wt %, about 0.01 wt % to about 0.4 wt %, about 0.01 wt % to about 0.3 wt %, about 0.01 wt % to about 0.2 wt %, about 0.01 wt % to about 0.1 wt %. When the organic acid is included in an amount of less than about 0.01 wt %, the pattern forming ability of the semiconductor photoresist composition is not sufficiently improved, and when the organic acid is included in an amount exceeding 2 wt %, development may not occur due to excessive thermal reaction.
[0107] The semiconductor photoresist composition according to an embodiment may further include an organic metal compound represented by Chemical Formula 2, an organic metal compound represented by Chemical Formula 3, or a combination thereof in addition to the compound represented by Chemical Formula 1.
[0108] [Chemical formula 2]
[0109]
[0110] In chemical formula 2,
[0111] X' is -OR 3 or -OC(=O)R 4 ,
[0112] R 3 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and
[0113] R 4 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof;
[0114] [Chemical formula 3]
[0115]
[0116] Among them, in chemical formula 3,
[0117] X" is -OR 5 or -OC(=O)R 6 ,
[0118] R 5 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof,
[0119] R 6 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and
[0120] L is a single bond, a substituted or unsubstituted divalent C1 to C20 saturated aliphatic hydrocarbon group, a substituted or unsubstituted divalent C3 to C20 saturated or unsaturated alicyclic hydrocarbon group, a substituted or unsubstituted divalent C2 to C20 unsaturated aliphatic hydrocarbon group containing at least one double bond or triple bond, a substituted or unsubstituted divalent C6 to C20 aromatic hydrocarbon group, -O-, -C(=O)-, or a combination thereof.
[0121] The semiconductor photoresist composition according to an embodiment of the present disclosure includes both an organic metal compound and an organic acid as well as the organic metal compound represented by Chemical Formula 2 and / or the organic metal compound represented by Chemical Formula 3, and thus may provide a semiconductor photoresist composition having excellent sensitivity and pattern formability.
[0122] By appropriately adjusting the ratio of the organic metal compound represented by Chemical Formula 2 or the organic metal compound represented by Chemical Formula 3 contained in the organic metal copolymer, the degree of dissociation of the ligand represented by R from the copolymer can be controlled, and thus, a semiconductor photoresist having excellent sensitivity and low line edge roughness and excellent resolution can be provided, while the degree of cross-linking with the surrounding chains through oxo group bonding is controlled by the free radicals generated when the ligand is dissociated. That is, by simultaneously containing the organic metal compound represented by Chemical Formula 1 and the organic metal compound represented by Chemical Formula 2 or the organic metal compound represented by Chemical Formula 3, a semiconductor photoresist having excellent sensitivity, line edge roughness and resolution can be provided.
[0123] The sum of the compound represented by Chemical Formula 2 and the compound represented by Chemical Formula 3 and the organometallic compound represented by Chemical Formula 1 may be included in a weight ratio of about 1:1 to about 1:20, for example, about 1:1 to about 1:19, for example, about 1:1 to about 1:18, for example, about 1:1 to about 1:17, for example, about 1:1 to about 1:16, for example, about 1:1 to about 1:15, for example, about 1:1 to about 1:14, for example, about 1:1 to about 1:15 When the weight ratio of the organic metal compound represented by Chemical Formula 1 to the compound represented by Chemical Formula 2, the organic metal compound represented by Chemical Formula 3, or a combination thereof satisfies the above range, a semiconductor photoresist composition having excellent sensitivity and resolution can be provided.
[0124] R of the compound represented by Chemical Formula 1 can be, for example, a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C20 aryl group, an ethoxy group, a propoxy group or a combination thereof, for example, a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, a 2,2-dimethylpropyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a vinyl group, a propenyl group, a butenyl group, an ethynyl group, a propynyl group, a butynyl group, a phenyl group, a tolyl group, a xylene group, a benzyl group, an ethoxy group, a propoxy group or a combination thereof.
[0125] R of the compound represented by Chemical Formula 1 1 It can be a substituted or unsubstituted C1 to C8 alkyl, a substituted or unsubstituted C3 to C8 cycloalkyl, a substituted or unsubstituted C2 to C8 alkenyl, a substituted or unsubstituted C2 to C8 alkynyl, a substituted or unsubstituted C6 to C20 aryl or a combination thereof, for example, methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylene, benzyl or a combination thereof.
[0126] R of the compound represented by Chemical Formula 1 2It can be hydrogen, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl or a combination thereof, for example, hydrogen, methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylene, benzyl or a combination thereof.
[0127] The compound represented by Chemical Formula 1 may include a compound represented by Chemical Formula 4, a compound represented by Chemical Formula 5, a compound represented by Chemical Formula 6, a compound represented by Chemical Formula 7, or a combination thereof.
[0128] [Chemical formula 4]
[0129]
[0130] [Chemical formula 5]
[0131]
[0132] [Chemical formula 6]
[0133]
[0134] [Chemical formula 7]
[0135]
[0136] In Chemical Formula 4 to Chemical Formula 7,
[0137] R a , R b , R c , R i , R k and R l Independently with R 1 The definition of is the same as
[0138] R d , R e , R f , R g , R h and R j Independently with R 2 The definition is the same.
[0139] The solvent included in the semiconductor photoresist composition according to the embodiment may be an organic solvent. The solvent may be, for example, an aromatic compound (e.g., xylene, toluene, etc.), an alcohol (e.g., 4-methyl-2-pentanol, 4-methyl-2-propanol, 1-butanol, methanol, isopropanol, 1-propanol, propylene glycol monomethyl ether), an ether (e.g., anisole, tetrahydrofuran), an ester (n-butyl acetate, propylene glycol monomethyl ether acetate, ethyl acetate, ethyl lactate), a ketone (e.g., methyl ethyl ketone, 2-heptanone) or a mixture thereof, but is not limited thereto.
[0140] In one embodiment, the semiconductor photoresist composition may further include a resin in addition to the aforementioned organometallic compound and solvent.
[0141] The resin may be a phenolic resin comprising at least one or more aromatic moieties in Group 1.
[0142] [Group 1]
[0143]
[0144] The resin may have a weight average molecular weight of about 500 to about 20,000.
[0145] The resin may be included in an amount of about 0.1 wt % to about 50 wt % based on the total amount of the semiconductor photoresist composition.
[0146] When the resin is included within the amount range, it may have excellent etching resistance and heat resistance.
[0147] On the other hand, the semiconductor photoresist composition according to the embodiment is ideally composed of an organic metal compound, a solvent and a resin. However, the semiconductor photoresist composition according to the above-mentioned embodiment may further include additives as needed. Examples of additives may include surfactants, crosslinking agents, leveling agents, quenchers or combinations thereof.
[0148] The surfactant may include, for example, alkylbenzene sulfonate, alkylpyridinium salt, polyethylene glycol, quaternary ammonium salt, or a combination thereof, but is not limited thereto.
[0149] The crosslinking agent may be, for example, a melamine-based crosslinking agent, a substituted urea-based crosslinking agent, an acryl-based crosslinking agent, an epoxy-based crosslinking agent or a polymer-based crosslinking agent, but is not limited thereto. It may be a crosslinking agent having at least two crosslinking-forming substituents, for example, a compound such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, 4-hydroxybutyl acrylate, acrylic acid, urethane acrylate, methacrylate, 1,4-butanediol diglycidyl ether, glycidol, diglycidyl 1,2-cyclohexane dicarboxylate, trimethylpropane triglycidyl ether, 1,3-bis(glycidyloxypropyl)tetramethyldisiloxane, methoxymethylated urea, butoxymethylated urea or methoxymethylated thiourea and the like.
[0150] The leveling agent may be used to improve the flatness of the coating during printing, and may be a known leveling agent that is commercially available.
[0151] The quencher may be tri-p-toluidine, methyldiphenylamine, triphenylamine, phenylenediamine, naphthylamine, diaminonaphthalene, or a combination thereof.
[0152] The amount of additive used can be controlled depending on the desired properties.
[0153] In addition, the semiconductor photoresist composition may further include a silane coupling agent as an adhesion enhancer to improve the close contact force with the substrate (for example, to improve the adhesion of the semiconductor photoresist composition to the substrate). The silane coupling agent may be, for example, a silane compound containing a carbon-carbon unsaturated bond, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrichlorosilane, vinyltri(β-methoxyethoxy)silane; or 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, p-phenylyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane; trimethoxy[3-(phenylamino)propyl]silane and the like, but is not limited thereto.
[0154] Semiconductor photoresist composition can be formed into a pattern with high aspect ratio without collapse. Therefore, in order to form a fine pattern with a width of, for example, about 5 nanometers to about 100 nanometers, about 5 nanometers to about 80 nanometers, about 5 nanometers to about 70 nanometers, about 5 nanometers to about 50 nanometers, about 5 nanometers to about 40 nanometers, about 5 nanometers to about 30 nanometers or about 5 nanometers to about 20 nanometers, semiconductor photoresist composition can be used for using a photoresist process of light with a wavelength range of about 5 nanometers to about 150 nanometers (for example, about 5 nanometers to about 100 nanometers, about 5 nanometers to about 80 nanometers, about 5 nanometers to about 50 nanometers, about 5 nanometers to about 30 nanometers or about 5 nanometers to about 20 nanometers). Therefore, semiconductor photoresist composition according to an embodiment can be used for using an EUV light source with a wavelength of about 13.5 nanometers to realize extreme ultraviolet lithography.
[0155] According to another embodiment, a method for forming a pattern using the semiconductor photoresist composition is provided. For example, the pattern formed can be a photoresist pattern.
[0156] The method of forming a pattern according to an embodiment includes forming an etch target layer on a substrate, coating a semiconductor photoresist composition on the etch target layer to form a photoresist layer, patterning the photoresist layer to form a photoresist pattern, and etching the etch target layer using the photoresist pattern as an etch mask.
[0157] In the following, reference Figures 1 to 5 Methods of forming patterns using semiconductor photoresist compositions are described. Figures 1 to 5 is a cross-sectional view for explaining a method of forming a pattern using a semiconductor photoresist composition according to an embodiment.
[0158] refer to Figure 1 , an object for etching is prepared. The object for etching may be a thin film 102 formed on a semiconductor substrate 100. Hereinafter, the object for etching is limited to the thin film 102. The entire surface of the thin film 102 is washed to remove impurities and the like remaining thereon. The thin film 102 may be, for example, a silicon nitride layer, a polysilicon layer, or a silicon oxide layer.
[0159] Subsequently, a resist base layer composition for forming a resist base layer 104 is spin-coated on the surface of the washed thin film 102. However, the embodiment is not limited thereto, and known various coating methods such as spray coating, dip coating, knife edge coating, printing methods (e.g., inkjet printing and screen printing), and the like may be used.
[0160] The coating process of the resist underlayer may be omitted, and hereinafter, a process including coating of the resist underlayer is described.
[0161] Subsequently, the applied composition is dried and baked to form a resist bottom layer 104 on the thin film 102. The baking may be performed at about 100°C to about 500°C, for example, about 100°C to about 300°C.
[0162] The resist bottom layer 104 is formed between the substrate 100 and the photoresist layer 106 and thus prevents non-uniformity of photoresist line width and patterning capability when radiation reflected from the interface between the substrate 100 and the photoresist layer 106 or from a hard mask between layers is scattered into unintended photoresist areas.
[0163] refer to Figure 2 , a photoresist layer 106 is formed by coating a semiconductor photoresist composition on the resist bottom layer 104. The photoresist layer 106 is obtained by coating the aforementioned semiconductor photoresist composition on the thin film 102 formed on the substrate 100, and then curing the photoresist layer 106 by heat treatment.
[0164] More specifically, forming a pattern by using a semiconductor photoresist composition may include coating the semiconductor photoresist composition on the substrate 100 having the thin film 102 by spin coating, slit coating, inkjet printing, and the like, and then drying the semiconductor photoresist composition to form a photoresist layer 106 .
[0165] The semiconductor photoresist composition has been described in detail and will not be described again.
[0166] Subsequently, the substrate 100 having the photoresist layer 106 is subjected to a first baking process. The first baking process may be performed at about 80°C to about 120°C.
[0167] refer to Figure 3 , the photoresist layer 106 can be selectively exposed.
[0168] For example, exposure can use activating radiation having a high energy wavelength such as extreme ultraviolet (EUV; wavelength of about 13.5 nanometers), E beam (electron beam), and the like, and short wavelength light such as i line (wavelength of about 365 nanometers), KrF excimer laser (wavelength of about 248 nanometers), ArF excimer laser (wavelength of about 193 nanometers), and the like.
[0169] More specifically, light for exposure according to an embodiment may have a short wavelength and a high energy wavelength in a range of about 5 nm to about 150 nm, such as extreme ultraviolet (EUV; wavelength of about 13.5 nm), E beam (electron beam), and the like.
[0170] The exposed region 106 b of the photoresist layer 106 has a different solubility from the non-exposed region 106 a of the photoresist layer 106 by forming a polymer through a cross-linking reaction such as condensation between organic metal compounds.
[0171] Subsequently, the substrate 100 is subjected to a second baking process. The second baking process may be performed at a temperature of about 90° C. to about 200° C. The exposed region 106 b of the photoresist layer 106 becomes less soluble with respect to a developing solution due to the second baking process.
[0172] exist Figure 4 In the process, the non-exposed area 106a of the photoresist layer is dissolved and removed using a developer to form a photoresist pattern 108. Specifically, the non-exposed area 106a of the photoresist layer is dissolved and removed using an organic solvent such as 2-heptanone and the like to complete the photoresist pattern 108 corresponding to the negative image.
[0173] As described above, the developer used in the method for forming a pattern according to the embodiment may be an organic solvent. The organic solvent used in the method for forming a pattern according to the embodiment may be, for example, ketones such as methyl ethyl ketone, acetone, cyclohexanone, 2-heptanone, and the like; alcohols such as 4-methyl-2-propanol, 1-butanol, isopropanol, 1-propanol, methanol, and the like; esters such as propylene glycol monomethyl ether acetate, ethyl acetate, ethyl lactate, n-butyl acetate, butyrolactone, and the like; aromatic compounds such as benzene, xylene, toluene, and the like, or a combination thereof.
[0174] However, the photoresist pattern according to the embodiment is not necessarily limited to a negative image, but may be formed to have a positive image. Herein, the developer for forming the positive image may be a quaternary ammonium hydroxide composition, such as tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, or a combination thereof.
[0175] As described above, exposure to light having high energy such as extreme ultraviolet (EUV; wavelength of about 13.5 nanometers), E-beam (electron beam), and the like, and light having a wavelength such as i-line (wavelength of about 365 nanometers), KrF excimer laser (wavelength of about 248 nanometers), ArF excimer laser (wavelength of about 193 nanometers), and the like can provide a photoresist pattern 108 having a width of about 5 nanometers to about 100 nanometers in thickness. For example, the photoresist pattern 108 may have a width of about 5 nanometers to about 90 nanometers, about 5 nanometers to about 80 nanometers, about 5 nanometers to about 70 nanometers, about 5 nanometers to about 60 nanometers, about 10 nanometers to about 50 nanometers, about 10 nanometers to about 40 nanometers, about 10 nanometers to about 30 nanometers, or about 10 nanometers to about 20 nanometers in thickness.
[0176] On the other hand, the photoresist pattern 108 may have a pitch with a half pitch less than or equal to about 50 nanometers (e.g., less than or equal to about 40 nanometers, less than or equal to about 30 nanometers, or less than or equal to about 25 nanometers) and a line width roughness less than or equal to about 10 nanometers or less than or equal to about 5 nanometers.
[0177] Subsequently, the resist bottom layer 104 is etched using the photoresist pattern 108 as an etching mask. Through this etching process, an organic layer pattern 112 is formed. The organic layer pattern 112 may also have a width corresponding to the width of the photoresist pattern 108.
[0178] refer to Figure 5 , the photoresist pattern 108 is used as an etching mask to etch the exposed thin film 102. Thus, the thin film is formed into a thin film pattern 114.
[0179] The etching of the thin film 102 may be, for example, dry etching using an etching gas, and the etching gas may be, for example, CHF 3 , CF 4 , Cl 2 , BCl 3 , and a mixed gas thereof.
[0180] In the exposure process, the thin film pattern 114 formed by using the photoresist pattern 108 formed by the exposure process performed by using the EUV light source may have a width corresponding to the width of the photoresist pattern 108. For example, the thin film pattern 114 may have a width of about 5 nanometers to about 100 nanometers, which is equal to the width of the photoresist pattern 108. For example, the thin film pattern 114 formed by using the photoresist pattern 108 formed by the exposure process performed by using the EUV light source may have a width of about 5 nanometers to about 90 nanometers, about 5 nanometers to about 80 nanometers, about 5 nanometers to about 70 nanometers, about 5 nanometers to about 60 nanometers, about 10 nanometers to about 50 nanometers, about 10 nanometers to about 40 nanometers, about 10 nanometers to about 30 nanometers, and about 10 nanometers to about 20 nanometers, or specifically, less than or equal to about 20 nanometers, which is like the width of the photoresist pattern 108.
[0181] Hereinafter, the present disclosure will be described in more detail by way of an example of the preparation of the aforementioned semiconductor photoresist composition. However, the present disclosure is not technically limited by the following examples.
[0182] Examples
[0183] Synthesis Example 1
[0184] 20 g (51.9 mmol) of Ph3SnCl was dissolved in 70 ml of THF in a 250 ml 2-neck round bottom flask and then cooled to 0°C in an ice bath. Subsequently, 1M butylmagnesium chloride (BuMgCl) THF solution (62.3 mmol) was slowly added thereto in a dropwise manner. When the dropwise addition was completed, the obtained mixture was stirred at 25°C for 12 hours to obtain a compound represented by Chemical Formula 8a.
[0185] [Chemical formula 8a]
[0186]
[0187] Subsequently, the compound represented by Chemical Formula 8a (10 g, 24.6 mmol) was dissolved in 50 ml of CH2Cl2, and 3 equivalents of 2M HCl diethyl ether solution (73.7 mmol) were slowly added thereto in a dropwise manner over 30 minutes at -78°C. Subsequently, the obtained mixture was stirred at 25°C for 12 hours, and then, the compound represented by Chemical Formula 8b was obtained by concentrating the solvent and performing vacuum distillation.
[0188] [Chemical formula 8b]
[0189]
[0190] Subsequently, 25 ml of acetic acid was slowly added dropwise to 10 g (25.6 mmol) of the compound represented by Chemical Formula 8b according to Synthesis Example 4 at 25° C., and then heated and refluxed for 12 hours. And then, the acetic acid was vacuum distilled to obtain the compound represented by Chemical Formula 8.
[0191] [Chemical formula 8]
[0192]
[0193] Synthesis Example 2
[0194] 20 g (51.9 mmol) of Ph3SnCl was dissolved in 70 ml of THF in a 250 ml two-necked round-bottom flask, and the temperature was lowered to 0° C. in an ice bath. Subsequently, 2M isopropylmagnesium chloride (iPrMgCl) THF solution (62.3 mmol) was slowly added thereto in a dropwise manner. When the dropwise addition was completed, the obtained mixture was stirred at 25° C. for 12 hours to obtain the compound represented by Chemical Formula 9a.
[0195] [Chemical formula 9a]
[0196]
[0197] Subsequently, the compound represented by Chemical Formula 9a (10 g, 24.6 mmol) was dissolved in 50 ml of CH2Cl2, and 3 equivalents of 2M HCl diethyl ether solution (73.7 mmol) were slowly added thereto in a dropwise manner over 30 minutes at -78°C. Subsequently, the obtained mixture was stirred at 25°C for 12 hours, and then, the compound represented by Chemical Formula 9b was obtained by concentrating the solvent and performing vacuum distillation.
[0198] [Chemical formula 9b]
[0199]
[0200] 25 ml of acrylic acid was slowly added dropwise to 10 g (25.4 mmol) of the compound represented by Chemical Formula 9b at 25° C., and then heated and refluxed at 80° C. for 6 hours. The temperature was reduced to 25° C., and then, the acrylic acid was vacuum distilled to obtain the compound represented by Chemical Formula 9.
[0201] [Chemical formula 9]
[0202]
[0203] Synthesis Example 3
[0204] 20 g (51.9 mmol) of Ph3SnCl was dissolved in 70 ml of THF in a 250 ml two-necked round-bottom flask, and the temperature was lowered to 0° C. in an ice bath. Subsequently, 1 M neopentylmagnesium chloride THF solution (62.3 mmol) was slowly added dropwise. When the dropwise addition was completed, the obtained mixture was stirred at 25° C. for 12 hours to obtain the compound represented by Chemical Formula 10a.
[0205] [Chemical formula 10a]
[0206]
[0207] Subsequently, the compound represented by Chemical Formula 10a (10 g, 24.6 mmol) was dissolved in 50 ml of CH2Cl2, and 3 equivalents of 2M HCl diethyl ether solution (73.7 mmol) were slowly added thereto in a dropwise manner over 30 minutes at -78°C. Subsequently, the obtained mixture was stirred at 25°C for 12 hours, and then, the compound represented by Chemical Formula 10b was obtained by concentrating the solvent and performing vacuum distillation.
[0208] [Chemical formula 10b]
[0209]
[0210] 25 ml of propionic acid was slowly added dropwise to 10 g (23.7 mmol) of the compound represented by Chemical Formula 10b at 25° C., and then heated and refluxed at 110° C. for 12 hours. The temperature was reduced to 25° C., and then, propionic acid was vacuum distilled to obtain the compound represented by Chemical Formula 10.
[0211] [Chemical formula 10]
[0212]
[0213] Synthesis Example 4
[0214] 10 g (25.4 mmol) of the compound represented by Chemical Formula 9a was put into a 100 ml round-bottom flask, and 25 ml of formic acid was slowly added thereto in a dropwise manner at 25°C, and then heated and refluxed at 100°C for 24 hours.
[0215] Subsequently, the temperature was lowered to 25° C., and then formic acid was vacuum distilled to obtain the compound represented by Chemical Formula 11.
[0216] [Chemical formula 11]
[0217]
[0218] Instance 1 to Instance 32
[0219] Each of the compounds represented by Chemical Formula 8 to Chemical Formula 11 obtained in Synthesis Examples 1 to Synthesis Examples 4 and citric acid (Sigma-Aldrich Corporation) and succinic acid (Sigma-Aldrich Corporation) as organic acids were dissolved in 1-methyl-2-propyl acetate at the weight ratios shown in Tables 1 to 4 at each concentration of 3 wt %, and filtered with a 0.1 μm polytetrafluoroethylene (PTFE) syringe filter to prepare each of the semiconductor photoresist compositions according to Examples 1 to 32.
[0220] A disk-shaped silicon wafer having an intrinsic oxide surface and a diameter of 4 inches was used as a substrate for thin film coating, and was treated in a UV ozone cleaning system for 10 minutes before coating the composition. On the treated substrate, the semiconductor photoresist compositions according to Examples 1 to 32 were spin-coated at 1500 rpm for 30 seconds, respectively, and then baked (baked after coating, post-apply bake (PAB)) at 100° C. for 120 seconds to form a photoresist film.
[0221] After coating and baking, the thickness of the film was measured by ellipsometry and was about 27 nanometers.
[0222] (Table 1) (Unit: parts by weight)
[0223]
[0224] (Table 2) (Unit: parts by weight)
[0225]
[0226] (Table 3) (Unit: parts by weight)
[0227]
[0228] (Table 4) (Unit: parts by weight)
[0229]
[0230] Comparative Example 1
[0231] 6 parts by weight of acetic acid based on 100 parts by weight of the compound represented by Chemical Formula 8 obtained in Synthesis Example 1 was dissolved in 4-methyl-2-pentanol at a concentration of 3 wt % and filtered with a 0.1 μm polytetrafluoroethylene (PTFE) syringe filter to prepare a semiconductor photoresist composition according to Comparative Example 1.
[0232] A photoresist film including the semiconductor photoresist composition according to Comparative Example 1 was prepared in the same manner as in Example 1. After coating and baking, the thickness of the film was about 25 nm.
[0233] Comparative Example 2
[0234] A semiconductor photoresist composition according to Comparative Example 2 and a photoresist thin film including the same were manufactured according to the same method as Comparative Example 1, except that propionic acid was used instead of acetic acid. After coating and baking, the thickness of the film was about 24 nm.
[0235] Comparative Example 3
[0236] A semiconductor photoresist composition according to Comparative Example 3 and a photoresist thin film including the same were manufactured according to the same method as Comparative Example 1, except that cyanoacetic acid was used instead of acetic acid. After coating and baking, the thickness of the film was about 23 nm.
[0237] Comparative Example 4
[0238] A semiconductor photoresist composition according to Comparative Example 4 and a photoresist thin film including the same were manufactured according to the same method as Comparative Example 1, except that malonic acid was used instead of acetic acid. After coating and baking, the thickness of the film was about 23 nm.
[0239] Comparative Example 5
[0240] A semiconductor photoresist composition according to Comparative Example 5 and a photoresist thin film including the same were manufactured according to the same method as Comparative Example 1, except that oxalic acid was used instead of acetic acid. After coating and baking, the thickness of the film was about 22 nm.
[0241] Comparative Example 6
[0242] A semiconductor photoresist composition according to Comparative Example 6 and a photoresist thin film including the same were manufactured according to the same method as Comparative Example 1, except that acetic acid (organic acid) was not used. After coating and baking, the thickness of the film was about 27 nm.
[0243] Evaluate
[0244] The films according to Examples 1 to 32, Comparative Examples 1 to 6 formed on a disk-shaped silicon wafer in a coating method were exposed to extreme ultraviolet light (EUV) to form a 16-nanometer line / space pattern by changing energy and focus. After exposure, the film was baked at 180° C. for 120 seconds, then immersed in a Petri dish containing 2-heptanone for 60 seconds and taken out, and washed with the same solvent for 10 seconds. Finally, the film was baked at 150° C. for 5 minutes, and then its pattern image was obtained by scanning electron microscopy (SEM). From the SEM image, Table 5 provides the ideal energy and line edge roughness (LER).
[0245] (Table 5)
[0246] Energy (mJ / cm2) LER(Nano) Example 1 300 1.8 Example 2 250 1.8 Example 3 200 1.9 Example 4 160 2.0 Example 5 310 1.6 Example 6 290 1.8 Example 7 250 1.7 Example 8 230 1.9 Example 9 260 1.8 Example 10 220 1.8 Example 11 180 1.7 Example 12 140 2.0 Example 13 280 1.8 Example 14 250 1.8 Example 15 230 1.9 Example 16 200 1.8 Example 17 270 1.8 Example 18 230 1.8 Example 19 180 2.0 Example 20 140 2.2 Example 21 280 1.8 Example 22 260 1.6 Example 23 230 1.9 Example 24 220 2.0 Example 25 280 1.8 Example 26 240 1.9 Example 27 180 1.9 Example 28 160 2.0 Example 29 290 1.6 Example 30 260 1.6 Example 31 250 1.8 Example 32 230 1.9 Comparative Example 1 360 1.6 Comparative Example 2 380 1.7 Comparative Example 3 160 5.5 Comparative Example 4 180 3.0 Comparative Example 5 Impossible to develop Impossible to develop Comparative Example 6 320 1.8
[0247] Referring to Table 5, the photoresist films using the semiconductor photoresist compositions according to Examples 1 to 32 exhibited excellent sensitivity and line edge roughness (LER).
[0248] In contrast, the photoresist films using the semiconductor photoresist compositions according to Comparative Examples 1 to 5 containing an organic acid that does not satisfy the conditions and content of a vapor pressure of less than or equal to about 1.0 mmHg at 25° C. and a pKa of about 3 to about 5 and according to Comparative Example 6 containing no organic acid exhibited higher ideal energy or were impossible to develop than the photoresist films using the semiconductor photoresist compositions according to Examples 1 to 32, thereby causing insufficient sensitivity or line edge roughness characteristics.
[0249] In the above, certain embodiments of the present disclosure have been described and illustrated, however, it is obvious to those skilled in the art that the present disclosure is not limited to the embodiments as described, and various modifications and conversions may be made without departing from the spirit and scope of the present disclosure. Therefore, the modified or converted embodiments may not be understood solely from the technical concepts and aspects of the present disclosure, and the modified embodiments are within the scope of the claims of the present disclosure.
Claims
1. A semiconductor photoresist composition comprising: an organometallic compound represented by Chemical Formula 1; an organic acid having a vapor pressure less than or equal to 1.0 mmHg at 25°C and a pKa of 3 to 4.3; as well as solvents, [Chemical Formula 1] Wherein, in Chemical Formula 1, R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethoxy group, a propoxy group, or a combination thereof, X, Y and Z are each independently -OR 1 or -OC(=O)R 2 , R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and R 2 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof. 2 . The semiconductor photoresist composition according to claim 1 , wherein the organic acid is present in an amount of 0.1 to 15 parts by weight based on 100 parts by weight of the organometallic compound. 3 . The semiconductor photoresist composition according to claim 1 , wherein the semiconductor photoresist composition comprises 0.01 wt % to 2 wt % of the organic acid based on the total mass of the semiconductor photoresist composition.
4. The semiconductor photoresist composition according to claim 1, wherein R is a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C20 aryl group, an ethoxy group, a propoxy group, or a combination thereof, R 1 is a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 alkenyl group, a substituted or unsubstituted C2 to C8 alkynyl group, a substituted or unsubstituted C6 to C20 aryl group, or a combination thereof, and R 2 is hydrogen, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl, or a combination thereof.
5. The semiconductor photoresist composition according to claim 1, wherein R is methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, ethoxy, propoxy, or a combination thereof, R 1 is methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, or a combination thereof, and R 2 is hydrogen, methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, or a combination thereof.
6. The semiconductor photoresist composition according to claim 1, wherein the semiconductor photoresist composition further comprises an organometallic compound represented by Chemical Formula 2, an organometallic compound represented by Chemical Formula 3, or a combination thereof in addition to the organometallic compound represented by Chemical Formula 1: [Chemical Formula 2] in, In Chemical Formula 2, X' is -OR 3 or -OC(=O)R 4 , R 3 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and R 4 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof; [Chemical Formula 3] Wherein, in Chemical Formula 3, X" is -OR 5 or -OC(=O)R 6 , R 5 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, R 6 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and L is a single bond, a substituted or unsubstituted divalent C1 to C20 saturated aliphatic hydrocarbon group, a substituted or unsubstituted divalent C3 to C20 saturated or unsaturated alicyclic hydrocarbon group, a substituted or unsubstituted divalent C2 to C20 unsaturated aliphatic hydrocarbon group containing at least one double bond or triple bond, a substituted or unsubstituted divalent C6 to C20 aromatic hydrocarbon group, -O-, -C(=O)-, or a combination thereof. 7 . The semiconductor photoresist composition according to claim 6 , wherein the total of the organometallic compound represented by Chemical Formula 2 and the organometallic compound represented by Chemical Formula 3 and the organometallic compound represented by Chemical Formula 1 are included in a weight ratio of 1:1 to 1:
20.
8. The semiconductor photoresist composition according to claim 1, wherein the organometallic compound represented by Chemical Formula 1 comprises a compound represented by Chemical Formula 4, a compound represented by Chemical Formula 5, a compound represented by Chemical Formula 6, a compound represented by Chemical Formula 7, or a combination thereof: [Chemical Formula 4] [Chemical Formula 5] [Chemical Formula 6] [Chemical Formula 7] in, In Chemical Formulas 4 to 7, R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethoxy group, a propoxy group, or a combination thereof, R a 、R b 、R c 、R i 、R k and R l are each independently a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and R d 、R e 、R f 、R g 、R h and R j and each is independently hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof. 9 . The semiconductor photoresist composition according to claim 1 , wherein the semiconductor photoresist composition further comprises an additive, wherein the additive comprises a surfactant, a cross-linking agent, a leveler, a quencher, or a combination thereof.
10. A method for forming a pattern, comprising: forming an etching target layer on a substrate; applying the semiconductor photoresist composition according to any one of claims 1 to 9 on the etching target layer to form a photoresist layer; patterning the photoresist layer to form a photoresist pattern; as well as The etch target layer is etched using the photoresist pattern as an etch mask. 11 . The method of forming a pattern according to claim 10 , wherein the photoresist pattern is formed using light having a wavelength of 5 nm to 150 nm.
12. The method of forming a pattern according to claim 10, further comprising providing a resist bottom layer formed between the substrate and the photoresist layer. 13 . The method of forming a pattern according to claim 10 , wherein the photoresist pattern has a width of 5 nm to 100 nm.