Carbon-coated graphene / metal oxide composite material and preparation method thereof
The preparation of carbon-coated graphene/metal oxide composite materials through shear-assisted continuous sand grinding method has solved the problems of complex preparation process, high cost and environmental pollution in the existing technology, and achieved high efficiency , low-cost graphene preparation and improved electrochemical performance, suitable for industrial applications.
Patent Information
- Application Number
- CN202110970789.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-08-23
AI Technical Summary
The preparation method of existing graphene/metal oxide composite materials is complex, has high cost, and has serious environmental pollution problems. It is difficult to achieve industrial mass production, resulting in low conductivity of graphene, which limits the power density and magnification of energy storage devices. performance.
Using shear-assisted continuous sand grinding method, graphite is pre-stripped through a shear emulsifier and stabilizer and metal salt are added to the reaction system, and grinding is combined with a sand mill to form graphene/metal oxide precursor and thermal annealing. The carbon-coated graphene/metal oxide composite was obtained, and continuous production was achieved.
It improves the peeling efficiency and electrochemical performance of graphene, reduces production costs, avoids environmental pollution, and achieves the integrity of graphene structure and excellent electrochemical performance, which is suitable for industrial applications.
Smart Images

Figure CN113690429B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy materials, and specifically relates to a carbon-coated graphene / transition metal compound composite material and a preparation method thereof. Background Art
[0002] Graphene / metal oxide composites can be used as electrode materials for energy storage devices such as lithium-ion batteries or supercapacitors. They can combine the excellent conductivity of graphene and the high energy density of transition metal oxides to exert the synergistic effect of the two components and improve the energy density, power density, rate performance and cycle life of energy storage devices.
[0003] Since the discovery of graphene in 2004, it has shown great application prospects in various fields such as new materials and electronic information. The preparation methods of graphene mainly include: chemical oxidation-reduction method, chemical vapor deposition method, mechanical exfoliation method, etc. Among them, the chemical oxidation-reduction method requires the use of sulfuric acid and potassium permanganate to treat natural graphite, and then ultrasonic exfoliation to obtain graphene oxide, and finally reduction with reducing agents such as hydrazine hydrate to obtain graphene. This method is helpful for the grafting modification of graphene, but it is easy to cause environmental pollution; chemical vapor deposition method can obtain a few-layer graphene with a complete structure, but the yield is low and the cost is high, which is only suitable for high-end application fields such as optoelectronics; mechanical exfoliation method can also obtain graphene with a complete lattice structure, and the equipment requirements are low, and it can be prepared in large quantities, which can meet the needs of the energy and composite materials industry. For example: exfoliation of graphite by ultrasound, ball milling, etc. can obtain a few-layer (<10) graphene, but the energy utilization efficiency and graphene yield of ultrasonic exfoliation method are low. For example, the yield of single-layer graphene obtained by ultrasonic stripping is 1wt% in Nat.Nanotechnol., 2008, 3(9): 563, and the yield after repeated ultrasonic stripping is expected to reach 7-12wt%, but it is time-consuming and energy-consuming, and has low efficiency. Ball milling stripping method takes a long time to prepare, and the quality of graphene sheets is difficult to control. For example, Chinese invention patent CN105084374A proposes a surfactant-assisted ball milling of graphite, wherein the grinding liquid is left to stand to obtain a first supernatant, the first supernatant is centrifuged to obtain a second supernatant, and the second supernatant is filtered and dried to obtain graphene. It can be seen that this method obtains graphene from the second supernatant, which is less efficient, time-consuming, and cannot achieve continuous production, which is not conducive to its market application. In addition, in addition to being affected by van der Waals forces, graphene sheets are also affected by hydrophobic effects, etc., and are easily aggregated, resulting in poor stability of graphene prepared by the stripping method, and it is also difficult to functionalize or composite with other materials.
[0004] At present, the preparation of graphene / metal oxide composite materials is mostly based on graphene oxide as a precursor, mixed with transition metal compounds, and then in situ generated on the surface of graphene oxide by coprecipitation, hydrothermal, solvent thermal and other methods. Transition metal oxides are finally obtained by thermal annealing or chemical reduction (for example: Chinese invention patents CN 104701035 A, CN 106829927 A, CN 102757041 A, CN102185144, etc.). However, the above method is complex, costly, and prone to environmental problems; at the same time, graphene oxide is difficult to be 100% reduced, and the resulting graphene conductivity is not high, resulting in limited improvement in the power density and rate performance of the device; in addition, the above method is more suitable for laboratory preparation of composite materials, and is difficult to industrialize and mass produce, which restricts the commercial application of graphene. Summary of the invention
[0005] The present invention is made to solve the above problems and aims to provide a shear-assisted continuous sand milling method for preparing carbon-coated graphene / metal oxide composite materials. Shear emulsifier Pre-stripped graphite, and at the same time, stabilizers and metal salts are added to the reaction system to improve the graphite stripping efficiency and dispersion stability; then the sand mill feed pipe is placed in the above reaction system for synchronous grinding treatment to induce a mechanochemical reaction to obtain a graphene / metal oxide precursor; finally, a carbon-coated graphene / metal oxide composite material is obtained after thermal annealing. The present invention organically combines the three by shearing and stripping graphite to prepare graphene, sand milling to promote mechanochemical reaction to generate metal oxide precursors, and thermal annealing to produce carbon coating, which can realize continuous production and processing, with low production costs and no environmental pollution problems. The graphene structure is complete and the electrochemical performance is excellent.
[0006] In order to achieve the above object, the present invention adopts the following scheme:
[0007] <Preparation method>
[0008] The present invention provides a method for preparing a carbon-coated graphene / metal oxide composite material, which is characterized by comprising the following steps: step 1. dispersing graphite powder and a stabilizer in a solvent, and then using a shear emulsifier to perform shear emulsification treatment for 10-30 minutes; step 2. adding a metal salt and an auxiliary agent to the mixed solution obtained in step 1, and continuing the shear emulsification treatment for 10-30 minutes; step 3. placing a sand mill feed pipe in the dispersion liquid in step 2, performing continuous sand milling treatment while shearing emulsification for 30-60 minutes, and then filtering and drying to obtain graphene / metal oxide precursor powder; step 4. performing thermal annealing treatment on the powder sample obtained in step 3, The stabilizer is converted into porous carbon encapsulated in graphite during thermal annealing. olefin / metal oxide surfaces,A carbon-coated graphene / metal oxide composite material is obtained.
[0009] Preferably, the graphite powder includes at least one of flake graphene, expanded graphite, fluorinated graphite, and thermal cracked graphite.
[0010] Preferably, the stabilizer includes at least one of urea, glucose, melamine, proanthocyanidin, tannic acid, methylimidazole, tetrakis(4-aminophenyl)methane, di(1H-pyrrol-2-yl)methane, tribenzoate, biphenyl-4,4′-dicarboxylic acid, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene alkylamine, and polyoxyethylene-polyoxypropylene ether triblock copolymer (F127).
[0011] Preferably, the solvent includes at least one of deionized water, ethanol, methanol, N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dibasic acid ester mixture (DBE).
[0012] Preferably, the metal salt includes at least one of nickel nitrate, manganese sulfate, cobalt acetate, ferric chloride, titanium orthosulfate, and zinc chloride.
[0013] Preferably, the auxiliary agent includes at least one of ammonium carbonate, ammonium bicarbonate, sodium hydroxide, ammonium chloride, ammonia water, and sodium carbonate.
[0014] Preferably, the concentration of graphite powder in the solvent is 0.2-5 g / L, the mass ratio of graphite to stabilizer is 1:0.5-1:5, the mass ratio of graphite to metal salt is 1:0.2-1:10, and the mass ratio of metal salt to additive is 1:0.5-1:2.
[0015] Preferably, the shear emulsification speed is 5000-30000 rpm and the temperature is 20-70°C.
[0016] Preferably, Sand grinder A horizontal sand mill or a vertical sand mill is selected, and at least one of glass beads, zirconium silicate beads or zirconium oxide beads is used as grinding beads. The size of the grinding beads is 0.4 to 3.0 mm, the mass ratio of the sand milling medium to the formula material is 1:0.5 to 1:2, and the grinding speed is 300 to 1000 rpm.
[0017] Preferably, in step 4, the thermal annealing temperature is 200-600° C., the thermal annealing atmosphere is at least one of an air atmosphere and a nitrogen atmosphere, and the thermal annealing time is 0.5-6 hours.
[0018] <Carbon-coated graphene / metal oxide composites>
[0019] Furthermore, the present invention also provides a carbon-coated graphene / metal oxide composite material prepared by the method described in the above <Preparation method>.
[0020] <Application>
[0021] Furthermore, the present invention also provides the use of the carbon-coated graphene / metal oxide composite material as an active electrode material for supercapacitors, lithium-ion batteries, and sodium-ion batteries.
[0022] Functions and Effects of the Invention
[0023] Compared with the prior art, the carbon-coated graphene / metal oxide composite material and the preparation method thereof of the present invention have the following outstanding features and excellent effects:
[0024] 1. The present invention adopts a shear emulsification method to pre-strip graphite to obtain graphene sheets, and adopts a stabilizer to be adsorbed on the surface of the newly generated graphene sheets to prevent self-aggregation, thereby greatly improving the efficiency of graphite stripping, and also ensuring the integrity of the graphene lattice structure, which is beneficial to improving the conductivity and electrochemical properties.
[0025] 2. On the one hand, metal salts and additives can act as ion intercalants, which can be intercalated into the graphite layers during the shear emulsification process to increase the interlayer spacing and improve the graphite exfoliation efficiency; on the other hand, they can undergo mechanochemical reactions during the grinding process of the sand mill to generate metal oxide precursors, which are loaded on the surface of the graphene sheets.
[0026] 3. The combination of shear pre-stripping and sand grinding stripping improves the efficiency of graphite stripping into graphene. The efficiency of graphite conversion into graphene can reach more than 80wt%, which is much higher than the 7-12wt% of the traditional ultrasonic stripping method (Nat. Nanotechnol., 2008, 3(9): 563), and is also significantly better than the small amount of graphene in the secondary supernatant of the ball milling-centrifugation method (Chinese invention patent CN105084374A).
[0027] 4. The present invention uses a continuous sand milling method to achieve continuous production operations, and directly obtains a graphene / metal oxide precursor, which is then subjected to thermal annealing to obtain a carbon-coated graphene / metal oxide composite material. The method has simple process, low cost, no pollution, and excellent electrochemical performance, which helps promote downstream industrial applications and development.
[0028] 5. In the method provided by the present invention, the stabilizer is converted into porous carbon during the thermal annealing process and coated on the graphene / metal oxide surface, thereby enhancing the interfacial bonding force between graphene and metal oxide nanoparticles, improving the conductivity and structural stability, and as an electrode material for supercapacitors or lithium-ion batteries, the energy density, power density and service life can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1This is a transmission electron microscope photo of the carbon-coated graphene / manganese dioxide composite material prepared in Example 1;
[0030] Figure 2 This is a high-resolution transmission electron micrograph of the carbon-coated graphene / manganese dioxide composite material prepared in Example 1;
[0031] Figure 3 1 is the cyclic voltammetry curve of the carbon-coated graphene / manganese dioxide composite material prepared in Example 1;
[0032] Figure 4 This is the constant current charge and discharge curve of the nitrogen-doped porous carbon-coated graphene / cobalt oxide composite material prepared in Example 2. DETAILED DESCRIPTION
[0033] The specific implementation scheme of the carbon-coated graphene / metal oxide composite material and the preparation method thereof according to the present invention is described in detail below with reference to the accompanying drawings.
[0034] <Example 1>
[0035] In the first embodiment, graphite is exfoliated by a shear-assisted continuous sand milling method, and then subjected to a thermal annealing treatment to obtain a carbon-coated graphene / manganese dioxide composite material.
[0036] Preparation method:
[0037] (1) 1000 mg of expanded graphite, 600 mg of F127 and 1000 mg of tannic acid were weighed and added to 1000 mL of a mixed solvent of deionized water / ethanol (volume ratio 4:1), and treated with a shear emulsifier for 20 minutes at a stirring speed of 20,000 rpm;
[0038] (2) Weigh 3200 mg of manganese sulfate and 2000 mg of ammonium carbonate and add them to the dispersion in step 1, and continue the shear emulsification treatment for 20 minutes;
[0039] (3) placing the feed pipe of the sand mill into the dispersion of step (2), using two diameters of grinding beads (0.5 mm and 1.0 mm) in a mass ratio of 2:1 as the sand milling medium, adjusting the grinding speed to 500 rpm, and continuously performing sand milling for 60 minutes while maintaining shear emulsification. During this process, the graphene sheet is sheared and thinned, and the metal salt, auxiliary agent, and stabilizer undergo a mechanochemical reaction, and a manganese dioxide precursor (manganese carbonate) is in situ grown on the surface of the graphene sheet. Finally, the product is filtered, washed, and dried to obtain a graphene / metal oxide precursor powder. After weighing, the yield is calculated to be 82wt%, which is much higher than the traditional ultrasonic exfoliation method (Nat. Nanotechnol., 2008, 3 (9): 563) and the direct ball milling-centrifugal method (Chinese invention patent CN105084374A).
[0040] (4) The powder sample obtained in step (3) is transferred to an atmosphere furnace and annealed at 450° C. in a nitrogen atmosphere for 4 hours. During this process, manganese carbonate is converted into manganese dioxide, and F127 and tannic acid are converted into porous carbon, thereby obtaining a carbon-coated graphene / manganese dioxide composite material.
[0041] Performance characterization:
[0042] Carbon-coated graphene / manganese dioxide composites
[0043] The obtained carbon-coated graphene / manganese dioxide composite material was photographed using a transmission electron microscope, and its morphology is as follows Figure 1 As shown, it can be observed that the material contains a two-dimensional sheet structure, and it can be seen that the sheet thickness is very thin, which is a few-layer graphene sheet, and its surface is loaded with a large number of granular structures. Figure 2 The high-resolution transmission electron microscope observation shows that the material exhibits three different crystalline states, representing MnO2 crystals, amorphous porous carbon, and regular graphene sheets. The above results confirm that Example 1 successfully prepared a carbon-coated graphene / manganese dioxide composite material, wherein the MnO2 crystal size is about 10nm, which is coated with porous carbon and uniformly loaded on the surface of the few-layer graphene.
[0044] The carbon-coated graphene / manganese dioxide composite material was used as the electrode of the supercapacitor to test the electrochemical performance of the supercapacitor. The cyclic voltammetry curve is shown in Figure 3As shown in the figure, the energy storage device exhibits typical electrochemical properties of manganese dioxide, with specific capacitances of 338 F / g and 242 F / g at 5 mV / s and 100 mV / s, respectively. When the scanning speed is increased by 20 times, the capacitance retention rate reaches 71.6%, indicating that the energy storage device has excellent specific capacitance and rate performance, which is significantly better than graphene / manganese dioxide composites prepared by other methods, such as: Electrochimica Acta, 2016, 222, 1393–1401 (5 mV / s—270 F / g, 100 mV / s—131.5 F / g, 48.7%); Composites Part B, 2019, 161, 37–43 (5mV / s—292.9F / g, 100mV / s—156.1F / g, 53.3%); Literature EnergyE nviron. Sci., 2014, 7, 3709-3719 (10mV / s—215F / g, 100mV / s—106F / g, 49.3%).
[0045] The excellent electrochemical performance is derived from the structure of the carbon-coated graphene / manganese dioxide composite material. The porous carbon-coated MnO2 nanocrystals are loaded on the surface of few-layer graphene. The MnO2 nanocrystals have small particle size and large specific surface area, which is beneficial to the diffusion of electrolyte ions and improves the utilization efficiency of active materials, thereby improving its specific capacitance. At the same time, the few-layer graphene has a regular graphitized structure, and the porous carbon-coated MnO2 nanocrystals enhance the interfacial interaction between it and the graphene sheets, which is beneficial to the conduction of electrons, thereby improving its rate performance. In addition, the porous carbon coating can also inhibit the dissociation of MnO2 nanocrystals during the electrochemical reaction, thereby ensuring that the supercapacitor has a long service life.
[0046] This method has simple procedures, cheap raw materials, continuous production, large-scale preparation, low cost and no pollution, which is very consistent with the requirements of industrial production. At the same time, the obtained product has good conductivity and high quality. As a supercapacitor electrode material, its specific capacitance and rate performance are far superior to conventional methods.
[0047] <Example 2>
[0048] In the second embodiment, graphite is exfoliated by a shear-assisted continuous sand milling method, and then subjected to a thermal annealing treatment to obtain a nitrogen-doped porous carbon-coated graphene / cobalt tetroxide composite material.
[0049] Preparation method:
[0050] (1) Weigh 2000 mg of expanded graphite and 1500 mg of N-methylimidazole and add them to 1000 mL of a mixed solvent of deionized water / methanol (volume ratio 1:9), and treat with a shear emulsifier for 20 minutes at a stirring speed of 30,000 rpm;
[0051] (2) Weighing 1000 mg of cobalt nitrate, adding it to the dispersion in step 1, and continuing the shear emulsification treatment for 10 minutes;
[0052] (3) placing the feed pipe of the sand mill into the dispersion of step (2), using three diameters of grinding beads (0.5 mm, 1.0 mm and 2.0 mm) in a mass ratio of 1:1:1 as sand milling media, adjusting the grinding speed to 800 rpm, and continuously performing sand milling for 30 minutes while maintaining shear emulsification, during which the cobalt ions interact with N-methylimidazole to in-situ grow a cobalt-based organic covalent polymer (MOF: ZIF-67) on the surface of the graphene sheet. Finally, filtering, washing and drying the product to obtain a precursor powder.
[0053] (4) The powder sample obtained in step (3) is transferred to an atmosphere furnace, and first annealed in a nitrogen atmosphere at 600°C for 2 hours to convert the organic ligand into porous carbon; then the temperature is reduced to 250°C, and heat treated in an air atmosphere for 2 hours, during which cobalt tetroxide is generated, thereby obtaining a nitrogen-doped porous carbon-coated graphene / cobalt tetroxide composite material.
[0054] Performance characterization:
[0055] The nitrogen-doped porous carbon-coated graphene / cobalt oxide composite material was used as the electrode of the supercapacitor. The electrochemical performance of the supercapacitor was tested. Its constant current charge and discharge curve is shown in Figure 4 As shown, the energy storage device exhibits typical pseudocapacitive electrochemical characteristics, with specific capacitances of up to 1025 F / g and 800 F / g at 1 A / g and 8 A / g, respectively. The retention rate reaches 78% when the scan speed is increased by 8 times, indicating that the energy storage device has excellent specific capacitance and rate performance.
[0056] <Example 3>
[0057] In the third embodiment, graphite is exfoliated by a shear-assisted continuous sanding method, and then a thermal annealing treatment is performed to obtain a porous carbon-coated graphene / NiCo2O4 composite material.
[0058] Preparation method:
[0059] (1) Weigh 1000 mg of expanded graphite and 1000 mg of biphenyl-4,4′-dicarboxylic acid (stabilizer) and add them to 1000 mL of N-methylpyrrolidone solvent, and treat them with a shear emulsifier for 30 minutes at a stirring speed of 10,000 rpm;
[0060] (2) Weigh 728 mg of cobalt nitrate, 352 mg of nickel acetate and 240 mg of sodium hydroxide and add them to the dispersion in step 1, and continue the shear emulsification treatment for 30 minutes;
[0061] (3) placing the feed pipe of the sand mill into the dispersion of step (2), using grinding beads with a diameter of 0.5 mm as the sand milling medium, adjusting the grinding speed to 300 rpm, and continuously performing sand milling for 60 minutes while maintaining shear emulsification. During this process, cobalt and nickel ions react with the additives to produce a mechanochemical reaction, and cobalt / nickel hydroxide is in situ grown on the surface of the graphene sheet. The product is then filtered, washed, and dried to obtain a precursor powder.
[0062] (4) The powder sample obtained in step (3) is transferred to an atmosphere furnace, and is first annealed in a nitrogen atmosphere at 500°C for 1 hour to convert the stabilizer into porous carbon; then the temperature is reduced to 280°C and heat treated in an air atmosphere for 2 hours. During this process, cobalt / nickel hydroxide is converted into NiCo2O4, thereby obtaining a porous carbon-coated graphene / NiCo2O4 composite material.
[0063] Performance characterization:
[0064] The porous carbon-coated graphene / NiCo2O4 composite material was used as the electrode material of the lithium-ion battery, and the electrochemical performance of the lithium-ion battery was tested. The specific capacity at 0.1C and 2C was as high as 1225mAh / g and 800mAh / g, respectively, and the capacity retention rate after 500 charge and discharge cycles at 0.5C could reach 82%, indicating that the energy storage device has excellent specific capacity, rate performance and cycle life.
[0065] The above embodiments are merely examples of the technical solutions of the present invention. The carbon-coated graphene / metal oxide composite material and its preparation method and application involved in the present invention are not limited to the contents described in the above embodiments, but are subject to the scope defined by the claims. Any modification, supplement or equivalent replacement made by a technician in the field of the present invention based on the embodiment is within the scope of protection required by the claims of the present invention.
Claims
1. A method for preparing a carbon-coated graphene / metal oxide composite material, characterized in that: The steps include: Step 1. Disperse graphite powder and stabilizer in solvent, then use shear Emulsifier Performing shear emulsification treatment for 10-30 minutes to obtain a mixed solution; Step 2. Add metal salt and additives to the mixed solution, and continue shearing and emulsification treatment for 10-30 minutes to obtain a dispersion; Step 3. placing a sand mill feed pipe in the dispersion, performing continuous sand milling treatment while shearing and emulsifying for 30 to 60 minutes, and then filtering and drying to obtain graphene / metal oxide precursor powder; Step 4. thermally annealing the graphene / metal oxide precursor powder, wherein the stabilizer is converted into porous carbon and coated on the surface of the graphene / metal oxide during the thermal annealing process to obtain a carbon-coated graphene / metal oxide composite material; Wherein, in step 1, the stabilizer includes at least one of urea, glucose, melamine, proanthocyanidin, tannic acid, methylimidazole, tetrakis(4-aminophenyl)methane, di(1H-pyrrol-2-yl)methane, tribenzoate, biphenyl-4,4′-dicarboxylic acid, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene alkylamine, and polyoxyethylene-polyoxypropylene ether triblock copolymer; Wherein, in step 2, the auxiliary agent includes at least one of ammonium carbonate, ammonium bicarbonate, sodium hydroxide, ammonium chloride, ammonia water, and sodium carbonate; The concentration of graphite powder in the solvent is 0.2-5 g / L, the mass ratio of graphite to stabilizer is 1:0.5-1:5, the mass ratio of graphite to metal salt is 1:0.2-1:10, and the mass ratio of metal salt to additive is 1:0.5-1:
2.
2. The method for preparing the carbon-coated graphene / metal oxide composite material according to claim 1, characterized in that: in, In step 1, the graphite powder includes at least one of flake graphene, expanded graphite, fluorinated graphite, and thermal cracked graphite.
3. The method for preparing the carbon-coated graphene / metal oxide composite material according to claim 1, characterized in that: in, In step 1, the solvent includes at least one of deionized water, ethanol, methanol, N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dibasic acid ester mixture (DBE).
4. The method for preparing the carbon-coated graphene / metal oxide composite material according to claim 1, characterized in that: in, In step 2, the metal salt includes at least one of nickel nitrate, manganese sulfate, cobalt acetate, ferric chloride, titanium orthosulfate, and zinc chloride.
5. The method for preparing the carbon-coated graphene / metal oxide composite material according to claim 1, characterized in that: in, The shear emulsification speed is 5000-30000 rpm, and the temperature is 20-70°C. Sand grinder A horizontal sand mill or a vertical sand mill is selected, and at least one of glass beads, zirconium silicate beads or zirconium oxide beads is used as grinding beads. The size of the grinding beads is 0.4 to 3.0 mm, the mass ratio of the sand milling medium to the formula material is 1:0.5 to 1:2, and the grinding speed is 300 to 1000 rpm.
6. The method for preparing the carbon-coated graphene / metal oxide composite material according to claim 1, characterized in that: in, In step 4, the thermal annealing temperature is 200-600° C., the thermal annealing atmosphere is at least one of an air atmosphere and a nitrogen atmosphere, and the thermal annealing time is 0.5-6 hours.
7. A carbon-coated graphene / metal oxide composite material, characterized in that: Prepared by the preparation method described in any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method of graphene / metal oxide nanocomposite powder
CN102757041A
Preparation method of metal oxide / graphene or multi-metal oxide / graphene composite electrode material
CN104701035A
Preparation method for colored silicon oxide aerogel
CN105084374A
Metal oxide graphene composite material and preparation method thereof
CN106829927A
Preparation method and application of carbon-coated grapheme-based metal oxide composite