Positive electrode mixture for lithium ion secondary battery and method for producing the same, and method for producing lithium ion secondary battery
By combining alkali metal salts and alkaline earth metal salts with vinylidene fluoride-based polymers in the positive electrode mixture of lithium-ion secondary batteries, the problems of increasing viscosity and cleaning of the positive electrode mixture of high-nickel active substances are solved, and a simpler Production process and higher stability and performance.
Patent Information
- Application Number
- CN202080030529.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-20
- Filing Date
- 2020-05-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-05-14
AI Technical Summary
In the prior art, the positive electrode mixture of high nickel-based active substances is prone to problems of viscosity increase and gelation during storage, and the cleaning method is complex and costly, which affects the performance and production efficiency of lithium-ion secondary batteries.
The positive electrode mixture formed by mixing and dissolving it in an organic solvent to combine with lithium metal oxide active substances, simplifying the production process and suppressing the viscosity increase. .
It can be made regardless of the type of adhesive, and it can easily suppress the time-lapse viscosity of the high-nickel active substance positive electrode mixture, reduce production costs and complexity, improve the stability of lithium-ion secondary batteries and performance.
Smart Images

Figure GDA0003313179070000161 
Figure GDA0003313179070000171
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode mixture for a lithium ion secondary battery and a method for producing the same, and a method for producing the lithium ion secondary battery. Background Art
[0002] As an active material for the positive electrode of a lithium ion secondary battery, LiCoO is known. 2 、LiNiO 2 , lithium metal oxides such as nickel-cobalt-manganese active materials and nickel-cobalt-aluminum active materials. Among them, the use of Co, which lacks stable supply and is prone to rising resource prices, is being suppressed, and the application of active materials with increased Ni ratios is expanding instead. Active materials with high nickel ratios can increase the charge and discharge capacity of lithium-ion secondary batteries, so their application is also expanding. However, for positive electrode mixtures containing active materials with high nickel ratios, the following problems are known: the viscosity of the slurry-like electrode mixture tends to increase during storage, and sometimes gels depending on the situation. Hereinafter, in this application, active materials with nickel ratios of 55 mol% or more are referred to as high-nickel active materials.
[0003] To address this problem, Patent Document 1 discloses that gelation of the positive electrode mixture can be suppressed by using a vinylidene fluoride polymer containing 70 mol % or more of vinylidene fluoride and 0.5 mol % or more of chlorotrifluoroethylene as a binder.
[0004] Patent Document 2 discloses that high nickel active materials are washed with a lithium carbonate aqueous solution to remove lithium sulfate and lithium hydroxide on the surface of lithium metal oxide particles, or that lithium carbonate is used instead of the lithium hydroxide to suppress gelation of the positive electrode mixture.
[0005] Patent Document 3 discloses that the high nickel active material is washed with an aqueous solution containing a water-soluble lithium salt other than lithium hydroxide, thereby removing impurities such as lithium hydroxide present on the surface of lithium metal oxide particles and suppressing gelation of the positive electrode mixture.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 11-195419
[0009] Patent Document 2: Japanese Patent Application Publication No. 2017-45632
[0010] Patent Document 3: Japanese Patent Application Publication No. 2017-45633 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] As described in Patent Documents 1 to 3, various methods for suppressing the increase in viscosity over time of a positive electrode mixture containing a high-nickel-based active material have been studied.
[0013] However, in crystalline polymers, the crystallinity of copolymers is prone to disorder, so the heat resistance is usually lower than that of homopolymers. Therefore, there is a need to develop a method for suppressing the increase in viscosity over time of a positive electrode mixture containing a high-nickel-based active material even when using a polymer with higher heat resistance such as a polyvinylidene fluoride homopolymer instead of the polyvinylidene fluoride-based copolymer described in Patent Document 1.
[0014] In addition, if an attempt is made to wash the active material as described in Patent Documents 2 and 3, the washing conditions need to be set so that lithium ions from the active material do not elute, or alternatively, since washing and subsequent drying processes are provided during the manufacturing process of the positive electrode mixture, the manufacturing cost increases. Therefore, there is a need to develop a method for suppressing the increase in viscosity over time of a positive electrode mixture containing a high-nickel-based active material by a simpler method.
[0015] The present invention has been completed in view of the above problems, and an object thereof is to provide a positive electrode mixture for a lithium ion secondary battery that can be produced regardless of the type of binder, can be produced more simply than washing the active material, etc., and suppresses the increase in viscosity over time during storage, a method for manufacturing the positive electrode mixture for a lithium ion secondary battery, and a method for manufacturing a lithium ion secondary battery using the positive electrode mixture for a lithium ion secondary battery.
[0016] Technical Solution
[0017] The positive electrode mixture for a lithium ion secondary battery of the present invention for solving the above problems contains: a positive electrode active material containing a lithium metal oxide represented by the formula (1); a polyvinylidene fluoride-based polymer; and an additive selected from the group consisting of an alkali metal salt and an alkaline earth metal salt.
[0018] Li 1+X MO 2 ……(1)
[0019] (In the formula (1), X is a number satisfying -0.15 < X ≤ 0.15, and M is Ni or an atomic group containing two or more atoms containing 55 mol% or more and less than 100 mol% of Ni)
[0020] In addition, the manufacturing method of the positive electrode mixture of the present invention for solving the above problems is a manufacturing method of a positive electrode mixture containing the following substances: a positive electrode active material; a vinylidene fluoride-based polymer; an additive selected from the group consisting of alkali metal salts and alkaline earth metal salts; and optionally an organic solvent. The manufacturing method of the positive electrode mixture includes the following steps: a step of preparing a mixture selected from the group consisting of a mixture of the vinylidene fluoride-based polymer and the additive, a mixture of the organic solvent and the additive, and a mixture of a solution obtained by dissolving the vinylidene fluoride-based polymer in the organic solvent and the additive; and a step of adding the positive electrode active material containing the lithium metal oxide represented by the formula (1) to the mixture and mixing them.
[0021] Li 1+X MO 2 ……(1)
[0022] (In the formula (1), X is a number satisfying -0.15 < X ≤ 0.15, and M is Ni or an atomic group containing two or more atoms containing 55 mol% or more and less than 100 mol% of Ni)
[0023] In addition, the manufacturing method of the lithium ion secondary battery of the present invention for solving the above problems includes the following steps:
[0024] A step of coating the positive electrode mixture for a lithium ion secondary battery or the positive electrode mixture for a lithium ion secondary battery manufactured by the above manufacturing method on the surface of a current collector material and drying it to obtain a positive electrode for a lithium ion secondary battery; and
[0025] A step of combining the positive electrode, the negative electrode for a lithium ion secondary battery, and the electrolyte to obtain a lithium ion secondary battery.
[0026] Advantageous Effects
[0027] According to the present invention, there is provided a positive electrode mixture for a lithium ion secondary battery that can be manufactured regardless of the type of binder, can be manufactured more simply compared to cleaning the active material, etc., and suppresses the increase in viscosity over time during storage, a manufacturing method of the positive electrode mixture for a lithium ion secondary battery, and a manufacturing method of a lithium ion secondary battery using the positive electrode mixture for a lithium ion secondary battery. Detailed Embodiments
[0028] 1. Positive Electrode Mixture for Lithium Ion Secondary Battery
[0029] The first embodiment of the present invention relates to a positive electrode mixture for a lithium ion secondary battery.
[0030] The above positive electrode mixture contains: a positive electrode active material, which is a lithium metal oxide represented by formula (1); a polyvinylidene fluoride-based polymer; and an additive selected from the group consisting of alkali metal salts and alkaline earth metal salts.
[0031] Li 1+X MO 2 ……(1)
[0032] (In formula (1), X is a number satisfying -0.15 < X ≤ 0.15, and M is Ni or an atomic group containing two or more atoms and containing 55 mol% or more and less than 100 mol% of Ni)
[0033] The above positive electrode mixture is usually in the form of a slurry. In addition, the above positive electrode mixture may also contain other substances such as a conductive aid and an organic solvent that are usually contained in the positive electrode mixture.
[0034] 1-1. Positive electrode active material
[0035] The above positive electrode active material contains a lithium metal oxide represented by formula (1).
[0036] Li 1+X MO 2 ……(1)
[0037] In formula (1), X is a number satisfying -0.15 < X ≤ 0.15. X is preferably a number satisfying -0.10 < X ≤ 0.10, and more preferably a number satisfying -0.05 < X ≤ 0.05.
[0038] In addition, in formula (1), M is Ni or an atomic group containing two or more atoms and containing 55 mol% or more and less than 100 mol% of Ni. In addition to Ni, the above atomic group may contain atoms such as Co, Fe, Al, Mn, Cr, and V. When M is the above atomic group, the above atomic group preferably contains 65 mol% or more and less than 98 mol% of Ni, and more preferably contains 75 mol% or more and less than 96 mol% of Ni. The above positive electrode active material is a so-called high-nickel positive electrode active material containing a lithium metal oxide with a relatively large amount of nickel.
[0039] From the viewpoint of further improving the capacity density of the positive electrode, the above positive electrode active material is preferably particles with a smaller particle size. From the above viewpoint, the average particle size of the above positive electrode active material is preferably 30 μm or less, more preferably 1 μm or more and 20 μm or less, and further preferably 2 μm or more and 15 μm or less. It should be noted that the above average particle size is the Dv 50 value (median particle size) obtained by the laser diffraction scattering method.
[0040] In addition, from the viewpoint of suppressing the decrease in energy density and reducing the reaction resistance, the above-mentioned positive electrode active material is preferably a particle with a larger specific surface area. From the above viewpoint, the specific surface area of the above-mentioned positive electrode active material is preferably 0.1 m 2 / g or more and 3m 2 It should be noted that the above-mentioned specific surface area is a value measured by the BET method.
[0041] The above-mentioned positive electrode active material may also include a substance that can function as a positive electrode active material in addition to the lithium metal oxide shown in formula (1). However, according to the viewpoints of the inventors, the increase in the viscosity of the positive electrode mixture over time is significantly observed in the positive electrode mixture containing more of the above-mentioned lithium metal oxide, so the effect of suppressing the above-mentioned increase in viscosity over time is significant in the positive electrode mixture containing more of the above-mentioned lithium metal oxide. From the above-mentioned viewpoint, the content of the lithium metal oxide shown in formula (1) in the above-mentioned positive electrode active material is preferably 10% by mass or more and 95% by mass or less relative to the total mass of the above-mentioned positive electrode active material, and more preferably 50% by mass or more and 90% by mass or less.
[0042] 1-2. Conductive additives
[0043] The conductive additive is typically a carbon material, and graphite including natural graphite and artificial graphite, vapor grown carbon fiber (VGCF), and carbon black including acetylene black, Ketjen black, and furnace black can be used.
[0044] The carbon material may have a spherical shape such as a scale shape, a fiber shape, or a primary particle or a secondary particle formed by an aggregation of the primary particles.
[0045] The content of the conductive aid in the positive electrode mixture is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 0.5 parts by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the positive electrode active material.
[0046] 1-3. Vinylidene fluoride polymers
[0047] The vinylidene fluoride polymer is a resin that functions as a binder for the positive electrode.
[0048] The vinylidene fluoride polymer may be a homopolymer of vinylidene fluoride or a copolymer containing structural units derived from vinylidene fluoride. It should be noted that the copolymer may be a copolymer of vinylidene fluoride and other monomers or a copolymer obtained by grafting a vinylidene fluoride polymer with other monomers.
[0049] Examples of the above-mentioned other monomers include: fluorine-containing alkyl vinyl compounds having one polymerizable group in the molecule (hereinafter referred to as "fluorinated monomers"), cross-linking alkyl vinyl compounds having two or more polymerizable groups in the molecule (hereinafter referred to as "cross-linking monomers"), unsaturated dibasic acids or unsaturated dibasic acid monoesters, and compounds having copolymerizable polar groups (hereinafter referred to as "polar group-containing compounds"), etc.
[0050] The fluorinated monomer can adjust the crystallinity of the vinylidene fluoride polymer. Examples of the fluorinated monomer include vinyl fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene and (per) fluoroalkyl vinyl ether. Among them, from the viewpoint of easier control of crystallinity, tetrafluoroethylene, chlorotrifluoroethylene and hexafluoropropylene are preferred, and hexafluoropropylene is more preferred.
[0051] The content of the structural unit derived from the fluorinated monomer in the vinylidene fluoride polymer is preferably 2 mass % or more and less than 10 mass %, more preferably 3 mass % or more and 9 mass % or less, and further preferably 4 mass % or more and 8 mass % or less, based on the total mass of the vinylidene fluoride polymer.
[0052] The crosslinkable monomer can further improve the bonding strength of the formed positive electrode dry coating to the collector surface, or can inhibit the swelling of the binder when in contact with liquids such as electrolytes. Examples of the crosslinkable monomer include perfluorodivinyl ether and perfluoroalkylene divinyl ether. It should be noted that the perfluoroalkylene divinyl ether can be a compound having the following structure: a structure in which two vinyl ether groups in which all hydrogen atoms are replaced by fluorine atoms are bonded by a linear or branched divalent perfluoroalkylene group having 1 or more and 6 or less carbon atoms.
[0053] The content of the structural unit derived from the crosslinkable monomer in the vinylidene fluoride polymer is preferably more than 0% by mass and less than 5% by mass, more preferably 0.1% by mass to 4% by mass, and further preferably 0.3% by mass to 3% by mass, relative to the total mass of the vinylidene fluoride polymer.
[0054] The above-mentioned unsaturated dibasic acid or unsaturated dibasic acid monoester can further improve the bonding strength of the formed positive electrode dry coating film to the surface of the collector by imparting polarity to the binder. Examples of the above-mentioned unsaturated dibasic acid include: maleic acid, fumaric acid, itaconic acid and citraconic acid. Examples of the above-mentioned unsaturated dibasic acid monoester include: monomethyl maleate, monoethyl maleate, monomethyl citraconic acid and monoethyl citraconic acid.
[0055] The polar group-containing compound can further improve the bonding strength of the formed positive electrode dry coating to the collector surface by imparting polarity to the binder. Examples of the polar group-containing compound include: (meth) acrylic acid, 2-carboxyethyl (meth) acrylic acid, (meth) acryloyloxyethyl succinic acid, (meth) acryloyloxypropyl succinic acid, and (meth) glycidyl acrylate.
[0056] In order to ensure high chemical resistance, heat resistance and electrochemical stability based on vinylidene fluoride, especially high electrochemical stability, the content of structural units derived from vinylidene fluoride in the above-mentioned vinylidene fluoride polymer is preferably 50 mass% or more, more preferably 80 mass% or more, further preferably 85 mass% or more, and particularly preferably 87 mass% or more, relative to the total mass of the above-mentioned vinylidene fluoride polymer.
[0057] In addition, from the perspective of improving the impact resistance of the produced positive electrode or improving the processability of the positive electrode, the logarithmic viscosity (ηinh) of the above-mentioned vinyl fluoride polymer is preferably greater than 0.50 dL / g and less than 5.0 dL / g, more preferably greater than 1.0 dL / g and less than 4.0 dL / g, further preferably greater than 1.0 dL / g and less than 3.5 dL / g, and particularly preferably greater than 1.5 dL / g and less than 3.5 dL / g.
[0058] The inherent viscosity (ηinh) can be obtained by measuring the drop time (t) at 30°C of a solution prepared by dissolving a vinylidene fluoride polymer in N,N-dimethylformamide (DMF) at a concentration of 0.4 g / dL using an Ubbelohde viscometer, the drop time (t 0 ) and the concentration of the vinylidene fluoride copolymer in the above solution (C, here 0.4 g / dL) are calculated by the following formula.
[0059] ηinh=(1 / C)·ln(t / t 0 )
[0060] When the vinylidene fluoride polymer has a carboxyl group derived from the polar group-containing compound, the -1 ~1800cm -1 The maximum peak intensity A1 (absorption originating from the stretching vibration of the carbonyl group) detected is similar to that at 3025 cm -1 The ratio A1 / A2 of the maximum peak intensity A2 (absorption derived from CH stretching vibration) detected nearby, that is, the absorbance ratio AR, is preferably 0.01 to 3, more preferably 0.05 to 1.
[0061] The content of the vinylidene fluoride polymer in the positive electrode mixture is preferably 0.3 parts by mass or more and 10 parts by mass or less, and more preferably 0.5 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the positive electrode active material.
[0062] 1-4. Additives
[0063] The above-mentioned additive is an alkali metal salt or an alkaline earth metal salt.
[0064] When the additive is contained in a positive electrode mixture containing a high-nickel active material, it is possible to suppress an increase in the viscosity of the positive electrode mixture over time.
[0065] Although the reason is not clear, it can be considered that the above-mentioned additives are dissociated and ionized in the organic solvent, and the pH value of the positive electrode mixture is kept low. That is, it can be considered that the reason for the increase in the viscosity of the above-mentioned positive electrode mixture over time is that the vinylidene fluoride polymer dehydrofluorination in the alkaline positive electrode mixture reduces the affinity with the organic solvent and the active material. In particular, the high-nickel active material has a tendency to have a large alkaline impurity content compared with other active materials, which easily dehydrofluorinates the vinylidene fluoride polymer. Therefore, it can be considered that the positive electrode mixture containing high-nickel active materials and vinylidene fluoride polymers is prone to increase in viscosity over time. In contrast, if the above-mentioned additives are added to the positive electrode mixture, the dissociation product of the above-mentioned additives keeps the pH of the positive electrode mixture low by suppressing the dissociation of alkaline impurities from the active material, suppressing the dehydrofluorination reaction of the above-mentioned vinylidene fluoride polymer, thereby suppressing the increase in the viscosity of the above-mentioned positive electrode mixture over time.
[0066] The above-mentioned additive is preferably a lithium metal salt. The cation generated by the lithium metal salt during ionization is lithium, so in addition to effectively suppressing the dissociation of alkaline impurities (lithium hydroxide, lithium carbonate, etc.) present in the positive electrode active material, the above-mentioned cation has little effect on the electrochemical reaction of the lithium ion secondary battery. Therefore, it can be considered that it is not easy to produce a decrease in output density caused by adding lithium metal salt to the positive electrode mixture.
[0067] Examples of additives for the lithium metal salts include: LiCl, LiBr, LiI, LiPF 6 , LiBF 4 、LiAsF 6 、LiSbF 6 、LiClO 4 、LiBrO 4 、LiIO 4 、LiAlCl 4 、LiCF 3 SO 3(LiTf), LiN(FSO 2 ) 2 (LiFSI), LiN(CF 3 SO 2 ) 2 (LiTFSI), LiN(CF 3 CF 2 SO 2 ) 2 (LiBETI), LiN(CF 3 SO 2 )(C 4 F 9 SO 2 ), LiC(CF 3 SO 2 ), LiC 2 BF 2 O 4 (LiDFOB), Li(C 2 O 4 ) 2 B(LiBOB), Li[PF 5 (CF 2 CF 2 CF 3 , Li[PF 4 (CF 2 CF 2 CF 3 ) 2 , Li[PF 3 (CF 2 CF 2 CF 3 ) 3 , Li[PF 5 (CF 2 CF 2 CF 2 CF 3 , Li[PF 4 (CF 2 CF 2 CF 2 CF 3 ) 2 , and Li[PF 3 (CF 2 CF 2 CF 2 CF 3 ) 3 , etc.
[0068] Among them, the above additives are preferably LiPF 6 , LiBF 4 , LiBr, LiBETI, LiAsF6 , LiTf, LiFSI, LiTFSI, LiDFOB or LiBOB.
[0069] Examples of the above additives other than lithium metal salts include: CaCl 2 、NaPF 6 、NaN(CF 3 SO 2 ) 2 (NaTFSI), NaN(FSO 2 ) 2 (NaFSI), potassium perfluorooctanoate, etc.
[0070] The additive is preferably a halogen-containing lithium metal salt. As for the halogen-containing lithium metal salt, the additive has a high oxidation potential and is not easily oxidized even when the potential of the positive electrode rises. Examples of halogens that may be contained in the halogen-containing lithium metal salt include fluorine, chlorine, bromine and iodine.
[0071] Among them, the halogen that the above-mentioned halogen-containing lithium metal salt may contain is preferably fluorine, and the above-mentioned additive is preferably a fluorine-containing lithium metal salt because the halogen-containing anions generated during ionization have high oxidation resistance, are not prone to reduced durability of lithium-ion secondary batteries, and avoid electrochemical side reactions originating from cations generated during ionization.
[0072] In addition, from the viewpoint of making it easier to ionize the above-mentioned additive and making it easier to lower the pH of the positive electrode mixture through the anions generated by the ionization of the above-mentioned additive, the acid dissociation constant (pKa) of the conjugate acid relative to the anion of the above-mentioned additive in water at 25°C is preferably less than 1, more preferably greater than -30 and less than 0, and further preferably greater than -20 and less than -3.
[0073] The content of the above-mentioned additive is preferably an amount of 0.001 parts by mass or more and 1.0 parts by mass or less relative to 100 parts by mass of the above-mentioned positive electrode active material. If the content of the above-mentioned additive is 0.001 parts by mass or more, the viscosity increase over time of the positive electrode mixture can be more effectively suppressed. It should be noted that from the viewpoints of suppressing the reduction in energy density, the reduction in the peel strength of the electrode to the collector, and the increase in the initial (just after manufacturing) viscosity of the positive electrode mixture, the upper limit of the content of the above-mentioned additive is preferably set to 1.0 parts by mass or less. For the same reason, the content of the above-mentioned additive is more preferably an amount of 0.001 parts by mass or more and 0.45 parts by mass or less, and more preferably an amount of 0.01 parts by mass or more and 0.45 parts by mass or less, and particularly preferably an amount of 0.05 parts by mass or more and 0.20 parts by mass or less.
[0074] Furthermore, it is desirable that the additive is contained in a type and amount that satisfactorily suppresses the increase in viscosity of the positive electrode mixture over time by combining with the type and amount of the active material, the vinylidene fluoride polymer, and the organic solvent.
[0075] Specifically, the additive is preferably contained so that the ratio (unit: %) of the viscosity of the positive electrode mixture after 4 days of preparation to the viscosity of the positive electrode mixture just after preparation is 130% or less, more preferably 120% or less, and even more preferably 110% or less.
[0076] Alternatively, the additive is preferably contained in a manner such that the ratio of the viscosity of the positive electrode mixture after 7 days of preparation to the viscosity of the positive electrode mixture just after preparation (unit: %) is 180% or less, more preferably 150% or less, further preferably 130% or less, and particularly preferably 120% or less.
[0077] In addition, it is ideal that the above-mentioned additives are contained in a type and amount such that the initial (immediately after production) viscosity of the positive electrode mixture does not change significantly compared to when the above-mentioned additives are not added, by combining the types or amounts of the above-mentioned positive electrode active material, the above-mentioned vinylidene fluoride copolymer and the organic solvent.
[0078] Specifically, the additive is preferably contained in a manner such that the ratio (unit: %) of the initial viscosity (just after manufacturing) of the positive electrode mixture when the above-mentioned additive is added to the initial viscosity (just after manufacturing) of the positive electrode mixture when the above-mentioned additive is not added is 50% or more and 180% or less, more preferably in a manner such that it is 75% or more and 150% or less, and further preferably in a manner such that it is 85% or more and 125% or less.
[0079] The viscosity of the positive electrode mixture can be a value measured using a known B-type viscometer.
[0080] 1-5. Organic solvents
[0081] The organic solvent may be any organic solvent that can dissolve the vinylidene fluoride polymer.
[0082] Examples of the organic solvent include N-methyl-2-pyrrolidone (NMP), dimethylformamide, N,N-dimethylacetamide, N,N-dimethyl sulfoxide, hexamethylphosphoramide, dioxane, tetrahydrofuran, tetramethylurea, triethyl phosphate, trimethyl phosphate, acetone, methyl ethyl ketone and the like.
[0083] The content of the organic solvent in the positive electrode mixture can be arbitrarily set within a range in which the positive electrode mixture in a slurry state can be applied to the current collector.
[0084] 1-6. Other substances
[0085] The positive electrode mixture may further include other substances that can be included in a positive electrode mixture for a lithium ion secondary battery. For example, the positive electrode mixture may further include a binder other than the vinylidene fluoride polymer.
[0086] 2. Method for producing positive electrode mixture for lithium ion secondary battery
[0087] The positive electrode mixture can be produced by kneading and slurrying the above-mentioned materials.
[0088] At this time, it is preferred to prepare a mixture of the vinylidene fluoride polymer and the additive, a mixture of the organic solvent and the additive, or a mixture of a solution of the vinylidene fluoride polymer dissolved in the organic solvent and the additive, and further mix the mixture with the positive electrode active material.
[0089] The above-mentioned additive is not easily soluble in an organic solvent. Therefore, if the above-mentioned additive and the positive electrode active material are mixed simultaneously in an organic solvent, sometimes the positive electrode active material hinders the dispersion of the above-mentioned additive. In contrast, by separately dispersing the above-mentioned additive in an organic solvent and dispersing the positive electrode active material in an organic solvent, the concentration distribution of the above-mentioned additive in the positive electrode mixture can be made more uniform. Thus, the effect of suppressing the increase in the viscosity of the above-mentioned positive electrode mixture over time brought by the above-mentioned additive is fully utilized.
[0090] As long as the mixture is a mixture obtained by not mixing the positive electrode active material at the same time during preparation, from the viewpoint of making the additive more uniformly dispersed, it is preferred to prepare a mixture of the organic solvent and the additive and mix it with other materials. Specifically, the method for manufacturing the positive electrode mixture preferably includes the following steps: preparing a mixture of the organic solvent and the additive (additive dispersion); preparing a solution (binder solution) in which the vinylidene fluoride polymer is dissolved in the organic solvent; and mixing the additive dispersion, the binder solution and the positive electrode active material.
[0091] When preparing the positive electrode mixture containing the conductive auxiliary agent, the conductive auxiliary agent is preferably mixed with the positive electrode active material in advance.
[0092] 3. Method for manufacturing lithium-ion secondary battery
[0093] The positive electrode mixture can be applied to the surface of a current collector and dried to produce a positive electrode for a lithium ion secondary battery.
[0094] The above-mentioned current collecting material can be any known current collecting material used for the positive electrode of a lithium ion secondary battery. Examples of the material of the above-mentioned current collecting material include: iron, copper, aluminum, nickel, titanium and alloys thereof (including stainless steel and steel). The above-mentioned current collecting material can be any shape such as foil or mesh, and its thickness is preferably 3 μm or more and 100 μm or less, and can also be 5 μm or more and 20 μm or less.
[0095] The coating can be performed on one side or both sides of the collector material. The coating can be performed in the following manner: after drying at a temperature of 50°C to 170°C, the coating weight is 50 to 1000 g / m2 per side. 2 , preferably 100 to 650 g / m 2 , a positive electrode mixture layer with a thickness of 10μm to 1000μm.
[0096] The positive electrode produced in this way can be combined with a negative electrode for a lithium ion secondary battery, an electrolyte, and an optional separator to produce a lithium ion secondary battery.
[0097] The negative electrode may be a known negative electrode in which a negative electrode mixture layer including a negative electrode active material, an optional negative electrode conductive aid, and a negative electrode binder is formed on a current collector.
[0098] Examples of the current collector include aluminum, nickel, copper, iron, and alloys thereof (including stainless steel and steel).
[0099] Examples of the negative electrode active material include carbon materials, silicon materials, metal oxides, and lithium alloys.
[0100] Examples of the above-mentioned conductive auxiliary agent for the negative electrode include carbon fibers and the like.
[0101] Examples of the above-mentioned negative electrode binder include: thermoplastic resins such as vinylidene fluoride polymers, vinyl acetate polymers, thermoplastic polyimide and thermoplastic urethane resins; thermosetting resins such as epoxy resins, thermosetting polyimide, urea resin and thermosetting urethane resins; and rubber polymers such as butyl rubber and styrene rubber.
[0102] The electrolyte solution may be any known electrolyte solution used for lithium ion secondary batteries, and may be any known electrolyte solution in which a lithium metal salt serving as an electrolyte is dissolved in a non-aqueous solvent.
[0103] Examples of the non-aqueous solvent include ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethyl butyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, methyl propionate, ethyl propionate, and the like.
[0104] Examples of the electrolyte of the lithium metal salt include: LiCl, LiBr, LiI, LiPF 6 , LiBF 4 、LiBETI、LiAsF 6 、LiSbF 6 、LiClO 4 、LiBrO 4 、LiIO 4 、LiAlCl 4 , LiTf, LiFSI, LiTFSI, LiBETI, LiN(CF 3 SO 2 )(C 4 F 9 SO 2 )、LiC(CF 3 SO 2 )、LiDFOB、LiBOB、Li[PF 5 (CF 2 CF 2 CF 3 )]、Li[PF 4 (CF 2 CF 2 CF 3 ) 2 ]、Li[PF 3 (CF 2 CF 2 CF 3 ) 3 ]、Li[PF 5 (CF 2 CF 2 CF 2 CF 3 )]、Li[PF 4 (CF 2 CF 2 CF 2 CF 3 ) 2 ] and Li[PF 3 (CF 2 CF 2 CF 2 CF 3 ) 3 ]wait.
[0105] Among them, the electrolyte is preferably LiPF 6 , LiBF 4 、LiBr、LiBETI、LiAsF 6 , LiTf, LiFSI, LiTFSI, LiDFOB or LiBOB.
[0106] Examples of the separator include olefin resins such as polyethylene and polypropylene, fluorine resins such as vinylidene fluoride polymers, cellulose resins, polyimides, and polyamides.
[0107] The lithium ion secondary battery may be in a known shape such as a cylindrical shape, a needle shape, a coin shape, or a laminate shape.
[0108] Example
[0109] Hereinafter, specific examples of the present invention will be described together with comparative examples, but the present invention is not limited thereto.
[0110] 1. Materials
[0111] The following materials were used to prepare a positive electrode mixture for a lithium ion secondary battery, and the positive electrode mixture was used to make a positive electrode for a lithium ion secondary battery.
[0112] 1-1. Positive electrode active material
[0113] As the positive electrode active material, any of the following was used.
[0114] NCA-1: Made by Nippon Chemical Industry Co., Ltd., NC-01 (Li 1.05 Ni 0.85 Co 0.13 Al 0.02 O 2 , composed of analytical values based on ICP).
[0115] LCO-1: CELLSEED C-10N (LiCoO 2 ).
[0116] 1-2. Conductive additives
[0117] As the conductive aid, any of the following was used.
[0118] CB: manufactured by Timcal Corporation, SuperP (conductive carbon black).
[0119] 1-3. Adhesive
[0120] As the binder, any one obtained in the following synthesis examples was used.
[0121] 1-3-1. Modified PVDF
[0122] A powdery modified PVDF (hereinafter referred to as "Mod-1") was obtained by the following steps.
[0123] Into an autoclave having an internal capacity of 2 liters, 1000 g of ion exchange water as a dispersion medium, 0.4 g of Metolose SM-100 (manufactured by Shin-Etsu Chemical Co., Ltd.) as a cellulose-based suspending agent, 2.0 g of a 50 wt% diisopropyl peroxydicarbonate-Freon 225cb solution as a polymerization initiator, 1.1 g of ethyl acetate as a chain transfer agent, 400 g of vinylidene fluoride, and 0.2 g of acryloxypropylsuccinic acid as a monomer were charged, and the temperature was raised to 25°C over 1 hour.
[0124] Next, while maintaining the temperature at 25°C, a 5 wt% aqueous solution of acryloyloxypropyl succinic acid was slowly added at a rate of 0.068 g / min over 20 hours. Including the amount added initially, a total of 5.2 g of acryloyloxypropyl succinic acid was added. After the addition of the aqueous solution of acryloyloxypropyl succinic acid was completed, the temperature was raised to 40°C, and the polymerization was stopped when the internal pressure reached 1.5 MPa-G.
[0125] After the polymerization, the polymer slurry was heat treated at 95°C for 60 minutes, dehydrated, washed with water, and dried at 80°C for 20 hours to obtain Mod-1. The yield of the obtained polymer was 92%, the inherent viscosity ηinh was 2.50 dL / g, and the absorbance ratio AR was 0.57.
[0126] (Calculation of absorbance ratio AR)
[0127] Mod-1 was pressed at 230°C and measured using an FT-730 infrared spectrophotometer manufactured by Horiba, Ltd. at a wavelength of 1500 cm -1 ~4000cm -1 Find the FT-IR spectrum within the range of 1700cm -1 ~1800cm -1 The maximum peak intensity detected was taken as the absorption A1 derived from the stretching vibration of the carbonyl group, and the peak intensity at 3025 cm -1 The maximum peak intensity detected in the vicinity was taken as absorption A2 derived from CH stretching vibration, and the ratio A1 / A2 thereof was taken as absorbance ratio AR.
[0128] (Calculation of inherent viscosity ηinh)
[0129] In order to calculate the inherent viscosity ηinh, a polymer solution was prepared by dissolving 80 mg of the polymer in 20 mL of N,N-dimethylformamide (DMF). The flow time t of the polymer solution was measured in a 30°C constant temperature bath using an Ubbelohde viscometer. Similarly, the flow time t of DMF was also measured. 0 Then, the inherent viscosity ηinh is calculated according to the following formula.
[0130] ηinh=(1 / C)·ln(t / t 0 )
[0131] In the above formula, C is 0.4 g / dL.
[0132] 1-3-2.PVDF homopolymer
[0133] A powdery PVDF homopolymer (hereinafter referred to as "Homo-1") was obtained by the following steps.
[0134] Into a 2-liter autoclave, 1024 g of ion exchange water, 0.2 g of methylcellulose, 400 g of vinylidene fluoride monomer, 0.6 g of diisopropyl peroxydicarbonate, and 1.9 g of ethyl acetate were charged, and suspension polymerization was performed at 26° C. for 20 hours. After the polymerization was completed, the obtained polymer slurry was heat-treated at 95° C. for 30 minutes, dehydrated, washed with water, and further dried at 80° C. for 20 hours to obtain Homo-1. The yield of the obtained polymer was 92%, and the logarithmic viscosity ηinh was 3.10 dL / g.
[0135] 1-4. Additives
[0136] Using LiCl, LiBr, LiTFSI, CaCl 2 , LiFSI and LiBETI as an additive.
[0137] 1-5. Organic solvents
[0138] N-methyl-2-pyrrolidone (hereinafter, referred to as "NMP") was used as an organic solvent.
[0139] 2. Preparation of positive electrode mixture
[0140] 2-1. Preparation of binder solution
[0141] 94 g of NMP adjusted to 25° C. was accurately weighed into a conical flask, and 6 g of the above binder (either Mod-1 or Homo-1) was added while stirring with a magnetic stirrer to obtain a mixture. Then, the above mixture was heated to 60° C. and maintained at 60° C. for 5 hours to obtain each binder solution. Each binder solution was stored at room temperature overnight and then used to prepare a positive electrode mixture.
[0142] 2-2. Preparation of additive dispersion
[0143] 9.4 g of NMP adjusted to 25° C. was accurately weighed into a conical flask, and 0.6 g of LiCl powder was added while stirring with a magnetic stirrer to obtain a mixture. The mixture was then heated to 60° C. and maintained at 60° C. for 5 hours to obtain an additive dispersion.
[0144] The type of additive was changed to obtain various additive dispersions, and each additive dispersion was used to prepare a positive electrode mixture immediately after preparation.
[0145] 2-3. Preparation of positive electrode mixture
[0146] An electrode mixture in the form of a slurry was prepared using AWATORI Rentaro MODEL: ARE-310 manufactured by THINKY CO., LTD.
[0147] First, weigh 30g of the positive electrode active material (either NCA-1 or LCO-1) and 0.6g of the conductive aid (CB), and stir and mix at a rotation speed of 320rpm and a revolution speed of 800rpm for 1 minute. Then, add 1.3g of the binder solution, add a specified amount of the additive dispersion, and further dilute with NMP in a manner that the solid content concentration becomes 84.2%. Then, mix for 2 minutes at a rotation speed of 800rpm and a revolution speed of 2000rpm. Then, add 3.7g of the binder solution, mix for 2 minutes at a rotation speed of 800rpm and a revolution speed of 2000rpm, and prepare a slurry electrode mixture.
[0148] Each electrode mixture was obtained in the same manner except that the type and amount of the additive dispersion were changed.
[0149] 3. Evaluation
[0150] 3-1. Thickening test
[0151] Prepare two PP test tubes were prepared, and the slurry electrode mixture was dispensed into each test tube in a manner such that the height was 5 cm. The viscosity was measured using a B-type viscometer (manufactured by Eikon Seiki Co., Ltd., DV-E VISCOMETER) with rotor No. 64 and a rotation speed of 6 rpm. The viscosity values after 2 minutes were recorded from the electrode mixture dispensed into each test tube, and their average value was set as the initial viscosity value of the dispensed electrode mixture.
[0152] Then, each test tube was sealed with a cap, and the positive electrode mixture dispensed into one test tube was allowed to stand at room temperature for 4 days and then the viscosity was measured in the same manner, and the positive electrode mixture dispensed into the other test tube was allowed to stand at room temperature for 7 days and then the viscosity was measured in the same manner.
[0153] For each combination of positive electrode active material and binder, the ratio of the initial viscosity value of the positive electrode mixture with the additive added to the initial viscosity value of the positive electrode mixture without the additive added was calculated as the "initial viscosity ratio". In addition, for each positive electrode active material, the ratio of the viscosity after 4 days to the initial viscosity value was calculated as the "viscosity ratio after 4 days". In addition, for each positive electrode active material, the ratio of the viscosity after 7 days to the initial viscosity value was calculated as the "viscosity ratio after 7 days".
[0154] 3-2. Peel strength of electrode
[0155] The electrode mixture was applied to one side of a 15 μm thick aluminum collector foil using a bar coater, and dried at 110°C for 30 minutes and then at 130°C for 2 hours to produce an electrode mixture with a unit area weight of about 250 g / m2 in a dry state. 2 of electrodes.
[0156] The surface of the electrode produced above on which the positive electrode mixture was applied was bonded to a thick plastic plate (made of acrylic resin, 5 mm thick) using a double-sided tape, and the 90° peel strength was measured in accordance with JIS K6854-1.
[0157] For each combination of the positive electrode active material and the binder, the ratio of the peel strength of the positive electrode mixture to which the additive was added to the peel strength of the positive electrode mixture to which the additive was not added was calculated as the “peel strength ratio”.
[0158] Table 1 shows the initial viscosity ratio, viscosity ratio after 4 days, viscosity ratio after 7 days, and peel strength ratio of the experiments performed by changing the types of positive electrode active materials and binders and the types and addition amounts of additives.
[0159] [Table 1]
[0160]
[0161]
[0162] As shown in Table 1, the viscosity increase over time of the positive electrode mixture containing a high nickel positive electrode active material, a vinylidene fluoride polymer, and an additive selected from the group consisting of an alkali metal salt and an alkaline earth metal salt is suppressed. In contrast, the viscosity increase over time of the positive electrode mixture containing a high nickel positive electrode active material and a vinylidene fluoride polymer but not containing the above additives is significant.
[0163] It should be noted that the positive electrode mixture including the non-high nickel positive electrode active material and the vinylidene fluoride polymer is unlikely to increase in viscosity over time even without adding an additive selected from the group consisting of alkali metal salts and alkaline earth metal salts.
[0164] This application is a patent application claiming priority based on Japanese Patent Application No. 2019-094638 filed on May 20, 2019, and the contents described in the specification and claims involved in that application are incorporated herein by reference.
[0165] Industrial Applicability
[0166] The positive electrode mixture for lithium ion secondary battery of the present invention can suppress the viscosity increase of the positive electrode mixture containing high nickel active material over time by a method that can be implemented more easily. Therefore, according to the present invention, the process of making lithium ion secondary battery can be changed more freely and cheaply, and it can be expected to contribute to the progress and popularization of technology in the same field.
Claims
1. A positive electrode mixture for a lithium ion secondary battery, comprising: a positive electrode active material, the positive electrode active material comprising a lithium metal oxide represented by formula (1); a binder; and an additive selected from the group consisting of LiBr, LiCl, CaCl2, LiAsF6, LiTf, LiDFOB, and LiBOB, wherein the binder is composed of a vinylidene fluoride-based polymer, That 1+X MO2……(1) in formula (1), X is a number satisfying -0.15 < X ≤ 0.15, and M is Ni or an atomic group containing two or more atoms containing 55 mol% or more and less than 100 mol% of Ni.
2. The positive electrode mixture for a lithium ion secondary battery according to claim 1, wherein the content of the additive is in an amount of 0.001 parts by mass or more and 1 part by mass or less with respect to 100 parts by mass of the positive electrode active material.
3. A method for manufacturing a positive electrode mixture for a lithium ion secondary battery, which is a method for manufacturing a positive electrode mixture for a lithium ion secondary battery containing the following substances: a positive electrode active material; a binder; an additive selected from the group consisting of LiBr, LiCl, CaCl2, LiAsF6, LiTf, LiDFOB, and LiBOB; and optionally contained organic solvent, the method for manufacturing the positive electrode mixture for a lithium ion secondary battery includes the following steps: a step of preparing a mixture selected from the group consisting of a mixture of the binder and the additive, a mixture of the organic solvent and the additive, and a mixture of a solution obtained by dissolving the binder in the organic solvent and the additive; and a step of adding a positive electrode active material containing a lithium metal oxide represented by formula (1) to the mixture and mixing, That 1+X MO2……(1) in formula (1), X is a number satisfying -0.15 < X ≤ 0.15, and M is Ni or an atomic group containing two or more atoms containing 55 mol% or more and less than 100 mol% of Ni, wherein the binder is composed of a vinylidene fluoride-based polymer.
4. A method for manufacturing a lithium ion secondary battery, which includes the following steps: a step of coating the positive electrode mixture for a lithium ion secondary battery according to claim 1 or 2 or the positive electrode mixture for a lithium ion secondary battery manufactured by the manufacturing method according to claim 3 on the surface of a current collector material and drying it to obtain a positive electrode for a lithium ion secondary battery; and a step of combining the positive electrode, a negative electrode for a lithium ion secondary battery, and an electrolyte to obtain a lithium ion secondary battery.