Method for producing modified vinyl alcohol polymer particles and particles obtained by the same

By using an transesterification reaction of unsaturated carboxylic acid and an acid catalyst in vinyl alcohol polymer particles, the problems of particle shape and residual sulfur components are solved, and efficient manufacturing and excellent performance of modified vinyl alcohol polymer particles are achieved.

CN113728016BActive Publication Date: 2024-10-29KURARAY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202080028776.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-03-12
Publication Date
2024-10-29
Estimated Expiration
2040-03-12

AI Technical Summary

Technical Problem

When manufacturing unsaturated hydrocarbon-based modified vinyl alcohol polymer particles using the existing technology, it is difficult to control the particle shape and separate the particles, and there are problems such as residual sulfur components and poor seepage, which affects its application performance.

Method used

Using a mixed medium containing unsaturated carboxylic acid, acid catalyst and water to react with vinyl alcohol polymer particles, modified vinyl alcohol polymer particles with specific structure and particle size are generated through transesterification reaction to avoid the precipitation of poor solvents and reduce the Sulfur content.

Benefits of technology

It achieves control of particle shape and reduction of sulfur content, improves the high-energy ray reactivity and liquid seepage performance of the particles, is suitable for use as a column filler, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113728016B_ABST
    Figure CN113728016B_ABST
Patent Text Reader

Abstract

A method for producing modified vinyl alcohol polymer particles, which comprises mixing a mixed medium containing an unsaturated carboxylic acid, an acid catalyst and water with vinyl alcohol polymer particles, wherein the mixed medium is mixed with the vinyl alcohol polymer particles, and the unsaturated carboxylic acid is reacted with the vinyl alcohol polymer, thereby obtaining modified vinyl alcohol polymer particles containing a vinyl ester unit represented by the following formula (2), a vinyl alcohol unit having a content of 95 to 99.99 mol % relative to all structural units, and an average particle size of 50 to 2000 μm. This production method does not have the problem of residual sulfur components from the liquid medium used in the reaction, and can modify the vinyl alcohol polymer particles while maintaining the particle shape, so there is no need for a step of precipitating the polymer in a large amount of a poor solvent, and is therefore simple and economically excellent. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing modified vinyl alcohol polymer particles having an unsaturated hydrocarbon group in a side chain and particles obtained by the method. Background Art

[0002] Vinyl alcohol polymers represented by polyvinyl alcohol have excellent interface characteristics and strength characteristics as a small number of crystalline water-soluble polymers, and are therefore used in paper processing, fiber processing, and stabilizers for emulsions. In addition, vinyl alcohol polymer gels cross-linked by various methods are used for super absorbent polymers (Super Absorbent Polymer), contact lenses, and fillers for water-based / organic solvent-based SEC columns due to their hydrophilicity and safety. In particular, vinyl alcohol polymers with a vinyl alcohol unit content of more than 95 mol% show high hydrophilicity as column fillers, and the membranes and fibers obtained using aqueous solutions of such vinyl alcohol polymers have excellent strength. In addition, in order to improve specific functions, attempts have been made to introduce functional groups into vinyl alcohol polymers, and various modified vinyl alcohol copolymers are being developed.

[0003] Among them, the modified vinyl alcohol polymers with unsaturated hydrocarbon groups introduced into the side chains can be cross-linked and water-resistant by high-energy ray irradiation, modified by graft polymerization, etc. As a method for introducing unsaturated hydrocarbon groups into the side chains, a method of reacting the hydroxyl groups possessed by the vinyl alcohol polymers with various compounds is common. For example, Patent Document 1 discloses a method for synthesizing vinyl alcohol polymers containing unsaturated hydrocarbon groups by acetalization using aldehydes having unsaturated hydrocarbon groups. Patent Document 2 discloses a method for synthesizing vinyl alcohol polymers containing unsaturated hydrocarbon groups by etherification using epoxy compounds having unsaturated hydrocarbon groups. However, it is believed that there are compounds with mutagenicity in aldehyde and epoxy compounds, so a method that does not use these compounds is needed.

[0004] On the other hand, a method for synthesizing a vinyl alcohol polymer containing an unsaturated hydrocarbon group by esterification using an unsaturated carboxylic acid or an unsaturated carboxylic acid ester with higher safety is also disclosed. For example, Patent Documents 3 and 4 disclose the following method: a vinyl alcohol polymer is dissolved in dimethyl sulfoxide (DMSO), then an unsaturated carboxylic acid ester is used for esterification, and then the polymer is precipitated in a poor solvent to obtain a modified vinyl alcohol polymer. Patent Document 5 describes the following method: a vinyl alcohol polymer is dissolved in water, then an unsaturated carboxylic acid and an acid catalyst are used to esterify the polymer, thereby producing a solution containing a modified vinyl alcohol polymer. Non-Patent Document 1 discloses the following method: a vinyl alcohol polymer is dissolved in water, then an unsaturated carboxylic acid, acetic acid and an acid catalyst are used to esterify the polymer, and then the polymer is precipitated in a poor solvent to obtain a modified vinyl alcohol polymer.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-108305

[0008] Patent Document 2: Japanese Patent Application Publication No. 2003-231715

[0009] Patent Document 3: WO2018 / 124015

[0010] Patent Document 4: WO2018 / 124014

[0011] Patent Document 5: Japanese Patent Application Publication No. 2007-321099

[0012] Non-patent literature

[0013] Non-patent document 1: Journal of Polymer Science: Series A: Polymer Chemistry, 1997, Vol. 35, pp. 3603-3611 Summary of the invention

[0014] Problems to be solved by the invention

[0015] However, in the methods for producing modified vinyl alcohol polymers described in Patent Documents 3 and 4, the ester exchange reaction is carried out in a state where the vinyl alcohol polymer is dissolved in DMSO. In order to isolate the modified vinyl alcohol polymer, it is necessary to precipitate the polymer in a large amount of poor solvent after the reaction, which is extremely complicated and economically disadvantageous. In addition, it is also clear that when the polymer is precipitated by such a method, it is difficult to control the particle shape, and when the obtained polymer is used as a column filler, problems such as poor liquid permeation occur.

[0016] In addition, the present inventors have found the following problem: DMSO has a very high affinity for vinyl alcohol polymers and is likely to remain in the resin even when precipitated in a poor solvent. Therefore, when the obtained vinyl alcohol polymer is used as a column filler, there is a problem of sulfur components eluting over time and causing pollution. In addition, when the modified vinyl alcohol polymer obtained by the production method described in Patent Documents 3 and 4 is stored in the form of an aqueous solution, there is also a problem of a significant odor caused by the residual sulfur components.

[0017] With regard to the manufacture method of the modified vinyl alcohol polymer of recording in patent documentation 5 and non-patent documentation 1, owing to reacting with water as solvent instead of DMSO, although the problem of the residual sulfur component can be eliminated, in order to isolate the modified vinyl alcohol polymer, it is necessary to make the above-mentioned polymer precipitate in a large amount of poor solvents after the reaction, which is extremely numerous and economically disadvantageous. In addition, it is also clear that, when utilizing such a method to precipitate polymer, it is difficult to control particle shape, and when the obtained polymer is used as the filler of column, problems such as causing the infiltration are bad are generated. In addition, only the solution comprising the modified vinyl alcohol polymer is disclosed in patent documentation 5, and particle shape is not disclosed at all.

[0018] The present invention has been made to solve the above-mentioned problems, and its object is to provide a method for producing modified vinyl alcohol polymer particles having an unsaturated hydrocarbon group, which can control the particle shape and is excellent in cost. Another object is to provide modified vinyl alcohol polymer particles having an unsaturated hydrocarbon group, which have a low sulfur content and an average particle size within a predetermined range.

[0019] Methods used to solve problems

[0020] The inventors of the present invention have conducted in-depth research to solve the above-mentioned problems, and have found the following points as a result. That is, it has been found that by mixing a mixed medium containing an unsaturated carboxylic acid, an acid catalyst and water with vinyl alcohol polymer particles to react the unsaturated carboxylic acid with the vinyl alcohol polymer particles, not only does it not need to precipitate into a large amount of poor solvents during the separation of the reaction product, but it is also possible to control the particle shape of the obtained modified vinyl alcohol polymer. In addition, it has been found that by reducing the content of sulfur components, the odor when the modified vinyl alcohol polymer particles are made into an aqueous solution for use is reduced. In addition, by making the average particle size of the modified vinyl alcohol polymer particles within a specific range and reducing the content of sulfur components, the problems of liquid permeability and contamination when the modified vinyl alcohol polymer particles are used as a column filler can be eliminated, thereby completing the present invention.

[0021] That is, the above-mentioned problem can be solved by providing a method for producing modified vinyl alcohol polymer particles, which comprises mixing a mixed medium containing an unsaturated carboxylic acid, an acid catalyst and water with vinyl alcohol polymer particles, wherein the unsaturated carboxylic acid is represented by the following formula (1), mixing the mixed medium with the vinyl alcohol polymer particles, and reacting the unsaturated carboxylic acid with the vinyl alcohol polymer particles, thereby obtaining modified vinyl alcohol polymer particles comprising a vinyl ester unit represented by the following formula (2), a vinyl alcohol unit content of 95 to 99.99 mol % relative to all structural units, and an average particle size of 50 to 2000 μm.

[0022]

[0023] [In formula (1), X represents a carbon-carbon bond or a divalent saturated hydrocarbon group having 1 to 10 carbon atoms which may have a branched structure, Y represents a hydrogen atom or a saturated hydrocarbon group having 1 to 6 carbon atoms which may have a branched structure, and Z represents a hydrogen atom or a methyl group.]

[0024]

[0025] [X, Y, and Z in formula (2) have the same meanings as in formula (1).]

[0026] In this case, it is preferred that the specific surface area of ​​the modified vinyl alcohol polymer particles is 0.01 to 1.0 m 2 / g. It is also preferred that the content of water in the mixed medium is 1 to 30% by mass. It is also preferred that the mixed medium further contains acetic acid. It is also preferred that Y is a hydrogen atom. It is also preferred that X is a carbon-carbon bond.

[0027] In the above production method, it is preferred that the modified vinyl alcohol polymer particles are further washed.

[0028] The above problems can also be solved by providing modified vinyl alcohol polymer particles, which are modified vinyl alcohol polymer particles comprising vinyl ester units represented by the following formula (2), wherein the content of vinyl alcohol units relative to all structural units is 95 to 99.99 mol%, the content of sulfur components is 0.01 to 20000 ppm, and the average particle size is 50 to 2000 μm.

[0029]

[0030] [In formula (2), X represents a carbon-carbon bond or a divalent saturated hydrocarbon group having 1 to 10 carbon atoms which may have a branched structure, Y represents a hydrogen atom or a saturated hydrocarbon group having 1 to 6 carbon atoms which may have a branched structure, and Z represents a hydrogen atom or a methyl group.]

[0031] At this time, it is preferred that the ratio of the vinyl ester units present in triads or more in the modified vinyl alcohol polymer relative to the total vinyl ester units is 10 mol% or less. It is also preferred that the yellow index (YI) of the modified vinyl alcohol polymer particles measured in accordance with ASTM D1925 is 50 or less. It is also preferred that the content of the vinyl ester units represented by the above formula (2) in the modified vinyl alcohol polymer particles relative to the total structural units is 0.01 to 5 mol%. It is also preferred that Y is a hydrogen atom. It is also preferred that X is a carbon-carbon bond.

[0032] Effects of the Invention

[0033] The method for producing modified vinyl alcohol polymer particles of the present invention not only does not have the problem of residual sulfur components from the liquid medium used in the reaction, but also can modify the vinyl alcohol polymer particles while maintaining the particle shape, so there is no need for a step of precipitating the polymer in a large amount of poor solvent, so it is simple and economically excellent. In addition, the modified vinyl alcohol polymer particles of the present invention have a low content of sulfur components, excellent high-energy ray reactivity, and an average particle size within a specified range, so they are suitable for use as column fillers, etc. In addition, when manufacturing a film or fiber, the modified vinyl alcohol polymer particles of the present invention have less odor when used as an aqueous solution. DETAILED DESCRIPTION

[0034] The present invention is a method for producing modified vinyl alcohol polymer particles by mixing a mixed medium containing an unsaturated carboxylic acid, an acid catalyst and water with vinyl alcohol polymer particles, wherein the unsaturated carboxylic acid is represented by the following formula (1), the mixed medium and the vinyl alcohol polymer particles are mixed, and the unsaturated carboxylic acid and the vinyl alcohol polymer particles are reacted to obtain modified vinyl alcohol polymer particles containing vinyl ester units represented by the following formula (2), a vinyl alcohol unit content of 95 to 99.99 mol% relative to all structural units, and an average particle size of 50 to 2000 μm.

[0035]

[0036] [In formula (1), X represents a carbon-carbon bond or a divalent saturated hydrocarbon group having 1 to 10 carbon atoms which may have a branched structure, Y represents a hydrogen atom or a saturated hydrocarbon group having 1 to 6 carbon atoms which may have a branched structure, and Z represents a hydrogen atom or a methyl group.]

[0037]

[0038] [X, Y, and Z in formula (2) have the same meanings as in formula (1).]

[0039] In the production method of the present invention, as the unsaturated carboxylic acid to be reacted with the above-mentioned vinyl alcohol polymer particles, a substance represented by formula (1) is used. X in formula (1) represents a carbon-carbon bond or a divalent saturated hydrocarbon group having 1 to 10 carbon atoms and may have a branched structure. From the viewpoint of high-energy ray reactivity, X is preferably a carbon-carbon bond. Specific examples of unsaturated carboxylic acids when X is a carbon-carbon bond include methacrylic acid, acrylic acid, crotonic acid, and the like.

[0040] The carbon number of the saturated hydrocarbon group used as X is 1 to 10. When the carbon number exceeds 10, the water solubility is poor. The carbon number is preferably 5 or less, more preferably 3 or less, and further preferably 2 or less.

[0041] Examples of the divalent saturated hydrocarbon group used as X include alkylene and cycloalkylene. Examples of the alkylene include methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, and decylene. Examples of the cycloalkylene include cyclopropylene, cyclobutylene, cyclopentylene, and cyclohexylene. The alkylene and cycloalkylene used as X may have an alkyl group such as a methyl group or an ethyl group as a branched structure.

[0042] Y in formula (1) represents a hydrogen atom or an optionally branched saturated hydrocarbon group having 1 to 6 carbon atoms. Y is preferably a hydrogen atom.

[0043] The carbon number of the saturated hydrocarbon group used as Y is 1 to 6. When the carbon number exceeds 6, water solubility may be poor. The carbon number is preferably 5 or less, more preferably 3 or less, and further preferably 2 or less.

[0044] As the saturated hydrocarbon group used as Y, alkyl groups, cycloalkyl groups, etc. can be cited. As the alkyl group, methyl groups, ethyl groups, propyl groups, isopropyl groups, butyl groups, isobutyl groups, sec-butyl groups, tert-butyl groups, pentyl groups, isopentyl groups, neopentyl groups, and hexyl groups can be cited. As the cycloalkyl group, cyclopropyl groups, cyclobutyl groups, cyclopentyl groups, and cyclohexyl groups can be cited. The alkyl group and cycloalkyl group used as Y can have alkyl groups such as methyl groups and ethyl groups as branched structures.

[0045] Specific examples of the unsaturated carboxylic acid represented by formula (1) include methacrylic acid, acrylic acid, crotonic acid, 3-methyl-3-butenoic acid, 4-pentenoic acid, 2-methyl-4-pentenoic acid, 5-hexenoic acid, 3,3-dimethyl-4-pentenoic acid, 7-octenoic acid, trans-3-pentenoic acid, trans-4-decenoic acid, 10-undecenoic acid, etc. Among them, methacrylic acid, acrylic acid, 4-pentenoic acid, and 10-undecenoic acid are preferred from the viewpoint of industrial availability and reactivity.

[0046] In the manufacturing method of the present invention, an acid catalyst is used as a catalyst for the reaction between the unsaturated carboxylic acid and the vinyl alcohol polymer particles. Thus, the reaction between the unsaturated carboxylic acid and the vinyl alcohol polymer particles is promoted. The acid catalyst can be any one of an organic acid and an inorganic acid as long as it catalyzes the dehydration esterification reaction between the unsaturated carboxylic acid represented by formula (1) and the hydroxyl group of the vinyl alcohol polymer particles. Examples of organic acids include methanesulfonic acid, benzenesulfonic acid, trifluoromethanesulfonic acid, and p-toluenesulfonic acid, and examples of inorganic acids include sulfuric acid, hydrochloric acid, and nitric acid. Among them, methanesulfonic acid, p-toluenesulfonic acid and sulfuric acid are preferred, and p-toluenesulfonic acid is particularly preferred.

[0047] The saponification degree of the vinyl alcohol polymer constituting the vinyl alcohol polymer particles used in the present invention is preferably 95 to 99.99 mol%. In addition, the viscosity average polymerization degree of the above-mentioned vinyl alcohol polymer is preferably 100 to 5000, and more preferably 200 to 4000. When the viscosity average polymerization degree is less than 100, the mechanical strength of the obtained modified vinyl alcohol polymer may be reduced. On the other hand, when the viscosity average polymerization degree exceeds 5000, the industrial production of vinyl alcohol polymer particles may become difficult. The saponification degree and viscosity average polymerization degree of the vinyl alcohol polymer are measured according to JIS K6726.

[0048] The vinyl alcohol units in the above-mentioned vinyl alcohol polymers can be derived from vinyl ester units by hydrolysis, alcoholysis, etc. Therefore, depending on the conditions when converting the vinyl ester units to the vinyl alcohol units, the vinyl ester units may remain in the vinyl alcohol polymer.

[0049] Examples of the vinyl ester of the vinyl ester unit include vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl versatate, vinyl caproate, vinyl octanoate, vinyl laurate, vinyl palmitate, vinyl stearate, vinyl oleate, vinyl benzoate, etc. Among them, vinyl acetate is preferred from an industrial point of view.

[0050] The vinyl alcohol polymer may contain other monomer units in addition to the vinyl alcohol unit and the vinyl ester unit as long as the effects of the present invention are not impaired. Examples of such other monomer units include monomer units derived from ethylenically unsaturated monomers copolymerizable with vinyl esters. Examples of such ethylenically unsaturated monomers include α-olefins such as ethylene, propylene, n-butene, isobutylene, and 1-hexene; acrylic acid and its salts; acrylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate; methacrylic acid and its salts; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, and octadecyl methacrylate; acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidopropanesulfonic acid and its salts, acrylamidopropyldimethylamine, and salts thereof (e.g., quaternary salts); methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidepropanesulfonic acid and its salts, methacrylamidepropyldimethylamine and its salts (e.g., quaternary salts); vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether, 2,3-diacetoxy-1-vinyloxypropane; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride and vinyl fluoride; vinyl halides such as vinylidene chloride and vinylidene fluoride; allyl compounds such as allyl acetate, 2,3-diacetoxy-1-allyloxypropane, and allyl chloride; unsaturated dicarboxylic acids such as maleic acid, itaconic acid, and fumaric acid, and their salts or esters; vinyl silyl compounds such as vinyltrimethoxysilane; isopropenyl acetate, etc.

[0051] The content of monomer units other than the vinyl alcohol unit and the vinyl ester unit in the vinyl alcohol polymer is usually 10 mol% or less, preferably 5 mol% or less, and more preferably 1 mol% or less.

[0052] The average particle size of the vinyl alcohol polymer particles used in the present invention is preferably 50 to 2000 μm. When the above average particle size is less than 50 μm, when the obtained modified vinyl alcohol polymer particles are used as a column filler, the liquid permeability may become insufficient. The above average particle size is more preferably 100 μm or more, further preferably 200 μm or more, particularly preferably 300 μm or more, and most preferably 500 μm or more. On the other hand, when the above average particle size exceeds 2000 μm, it is possible that the reaction cannot be carried out uniformly inside and outside the particles. The above average particle size is more preferably 900 μm or less, and further preferably 800 μm or less.

[0053] Modified vinyl alcohol polymer particles are obtained by mixing a mixed medium containing an unsaturated carboxylic acid represented by formula (1), the acid catalyst and water with vinyl alcohol polymer particles to react the unsaturated carboxylic acid with the vinyl alcohol polymer particles. In this way, by reacting the vinyl alcohol polymer particles with the unsaturated carboxylic acid, that is, reacting while maintaining the particle shape of the vinyl alcohol polymer particles as a raw material, not only is it not necessary to precipitate the reaction product into a large amount of poor solvent during separation, but also the particle shape of the modified vinyl alcohol polymer particles can be controlled. In addition, there is no problem that sulfur components from the liquid medium used during the reaction remain in the modified vinyl alcohol polymer particles. In addition, in the obtained modified vinyl alcohol polymer particles, since the proportion of vinyl ester units present in triads or more is reduced, the viscosity stability is improved when an aqueous solution is prepared. As a method for reacting the unsaturated carboxylic acid with the vinyl alcohol polymer particles, the following method is preferred: by mixing the mixed medium with the vinyl alcohol polymer particles, the vinyl alcohol polymer particles are dispersed in the mixed medium, and the unsaturated carboxylic acid is reacted with the vinyl alcohol polymer particles. Specifically, the following method can be cited: the above-mentioned mixed medium and the above-mentioned vinyl alcohol polymer particles are mixed to form a slurry or a dispersion, and the above-mentioned unsaturated carboxylic acid and the above-mentioned vinyl alcohol polymer particles are reacted. In addition, the following method can be cited: the above-mentioned mixed medium and the above-mentioned vinyl alcohol polymer particles are uniformly mixed, and the above-mentioned unsaturated carboxylic acid and the above-mentioned vinyl alcohol polymer particles are reacted.

[0054] The method for mixing the mixed medium and the vinyl alcohol polymer particles is not particularly limited as long as the two can be uniformly mixed. Specifically, the following methods can be mentioned: (1) preparing the mixed medium and then mixing the mixed medium with the vinyl alcohol polymer particles; (2) mixing the vinyl alcohol polymer with a part of the mixed medium and then mixing the obtained mixture with the remaining components of the mixed medium; (3) mixing the components of the mixed medium and the vinyl alcohol polymer particles at the same time, among which (1) is preferred.

[0055] When the mixed medium and the vinyl alcohol polymer particles are mixed, the mass ratio of the vinyl alcohol polymer particles to the mixed medium [polymer particles / mixed medium] is preferably 3 / 97 to 90 / 10. When the mass ratio [polymer particles / mixed medium] is less than 3 / 97, the reactivity may be significantly reduced. The mass ratio [polymer particles / mixed medium] is more preferably 10 / 90 or more. On the other hand, when the mass ratio [polymer particles / mixed medium] exceeds 90 / 10, the mixed medium and the vinyl alcohol polymer particles may not be uniformly mixed, and the reactivity may be significantly reduced. The mass ratio [polymer particles / mixed medium] is more preferably 80 / 20 or less, and further preferably 50 / 50 or less.

[0056] The water content in the mixed medium is preferably 1 to 30% by mass. When the water content is less than 1% by mass, the obtained modified vinyl alcohol polymer particles may be easily colored. The water content is more preferably 3% by mass or more, more preferably 5% by mass or more, and particularly preferably 8% by mass or more. On the other hand, when the water content exceeds 30% by mass, the vinyl alcohol polymer dissolves during the reaction, and it may be difficult to modify the vinyl alcohol polymer particles while maintaining the particle shape. The water content is more preferably 20% by mass or less, and more preferably 18% by mass or less.

[0057] When the unsaturated carboxylic acid is reacted with the vinyl alcohol polymer particles, the amount of the acid catalyst added is preferably 0.0001 to 0.1 mol per 1 mol of the hydroxyl group in the vinyl alcohol polymer. The amount added is more preferably 0.0005 mol or more. On the other hand, the amount added is more preferably 0.08 mol or less.

[0058] The content of the unsaturated carboxylic acid in the mixed medium is preferably 5 to 2000 parts by mass relative to 100 parts by mass of the vinyl alcohol polymer particles. When the amount of the unsaturated carboxylic acid added is less than 5 parts by mass, the reactivity may be reduced. The content of the unsaturated carboxylic acid is more preferably 10 parts by mass or more, further preferably 20 parts by mass or more, and particularly preferably 30 parts by mass or more. On the other hand, when the content of the unsaturated carboxylic acid exceeds 2000 parts by mass, it is possible that the unreacted unsaturated carboxylic acid increases, thereby increasing the cost. The content of the unsaturated carboxylic acid is more preferably 1500 parts by mass or less, further preferably 1000 parts by mass or less, and particularly preferably 700 parts by mass or less.

[0059] From the viewpoint of controlling the content of the vinyl acetate unit of the modified vinyl alcohol polymer, the mixed medium preferably further contains acetic acid. The content of acetic acid in the mixed medium is preferably 1 to 1000 parts by mass relative to 100 parts by mass of water in the mixed medium. The content of acetic acid is more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more. On the other hand, the content of acetic acid is more preferably 800 parts by mass or less, and even more preferably 600 parts by mass or less.

[0060] The mixed medium may contain other additives besides the unsaturated carboxylic acid represented by formula (1), the acid catalyst, water and acetic acid. Examples of other additives include surfactants and organic solvents. Examples of surfactants include: nonionic surfactants such as polyoxyethylene-alkyl ether type, polyoxyethylene-alkylphenol type, polyoxyethylene-polyol ester type, esters of polyols and fatty acids, and oxyethylene-oxypropylene block polymers; anionic surfactants and reactive surfactants such as higher alcohol sulfates, higher fatty acid alkali salts, polyoxyethylene alkylphenol ether sulfates, alkylbenzene sulfonates, naphthalene sulfonate formalin condensates, alkyl diphenyl ether sulfonates, dialkyl sulfosuccinates, and higher alcohol phosphate esters. Examples of organic solvents include: alcohols such as methanol, ethanol, propanol, and butanol; aliphatic or alicyclic hydrocarbons such as n-hexane, n-pentane, and cyclohexane; aromatic hydrocarbons such as benzene and toluene; nitriles such as acetonitrile and benzonitrile; ether, diphenyl ether, anisole, 1,2-dimethoxyethane, 1,4-dimethoxyethane, and 1,4-dimethoxyethane. Ethers such as alkanes; ketones such as acetone, methyl ethyl ketone, methyl isopropyl ketone, methyl isobutyl ketone; esters such as methyl acetate, ethyl acetate, ethyl propionate, etc. Other additives may also include ultraviolet absorbers, light stabilizers, antioxidants, plasticizers, and defoamers. The content of other additives in the mixed medium is preferably 50% by mass or less, more preferably 35% by mass or less. In addition, the mixed medium preferably does not contain a sulfur-containing liquid medium.

[0061] The temperature when the unsaturated carboxylic acid and the vinyl alcohol polymer particles are reacted is preferably 10 to 120° C. The temperature is more preferably 30° C. or higher, and further preferably 50° C. or higher. On the other hand, the temperature is more preferably 100° C. or lower, and further preferably 90° C. or lower. The reaction time when the unsaturated carboxylic acid and the vinyl alcohol polymer particles are reacted is usually 0.5 to 72 hours.

[0062] It is preferred that the modified vinyl alcohol polymer particles after the reaction are further washed. As a specific washing method, a method of washing the particles with a solvent can be cited. Specifically, a method of immersing the particles in a solvent and then removing the liquid, a method of washing by circulating a solvent in a washing tower while bringing the solvent into contact with the particles, a method of spraying a washing solvent while flowing the particles, etc. can be cited. Examples of the solvent used include: alcohols such as methanol, ethanol, propanol, and butanol; aliphatic or alicyclic hydrocarbons such as n-hexane, n-pentane, and cyclohexane; aromatic hydrocarbons such as benzene and toluene; nitriles such as acetonitrile and benzonitrile; diethyl ether, diphenyl ether, anisole, 1,2-dimethoxyethane, 1,4-dimethoxyethane, etc. Ethers such as alkane; ketones such as acetone, methyl ethyl ketone, methyl isopropyl ketone, methyl isobutyl ketone; esters such as methyl acetate, ethyl acetate, ethyl propionate, etc. Among them, alcohols, ethers, ketones, and esters are more preferred, and methanol, ethanol, propanol, ethyl ether, 1,2-dimethoxyethane, acetone, methyl ethyl ketone, methyl acetate, and ethyl acetate are further preferred, and methanol, propanol, acetone, methyl ethyl ketone, methyl acetate, and ethyl acetate are particularly preferred. These organic solvents may be used alone or in combination of two or more.

[0063] It is preferred that the modified vinyl alcohol polymer particles after the reaction are washed as needed and then dried. In this case, the drying temperature is usually 20 to 150° C. and the drying time is 1 to 72 hours. In addition, the drying of the modified vinyl alcohol polymer particles can be carried out under atmospheric pressure or under reduced pressure.

[0064] The average particle size of the modified vinyl alcohol polymer particles thus obtained needs to be 50 to 2000 μm. The modified vinyl alcohol polymer particles of such an average particle size are excellent in terms of liquid permeability when used as a column filler. Moreover, according to the manufacturing method of the present invention, it is easy to control the particle shape of the modified vinyl alcohol polymer, so it is possible to simply manufacture modified vinyl alcohol polymer particles of such an average particle size. In the case where the above-mentioned average particle size is less than 50 μm, when the obtained modified vinyl alcohol polymer particles are used as a column filler, the liquid permeability becomes insufficient. The above-mentioned average particle size is preferably 100 μm or more, more preferably 200 μm or more, further preferably 300 μm or more, and particularly preferably 500 μm or more. On the other hand, when the above-mentioned average particle size exceeds 2000 μm, when manufacturing the modified vinyl alcohol polymer particles, the reaction cannot be carried out uniformly inside and outside the particles. The above-mentioned average particle size is preferably 900 μm or less, and more preferably 800 μm or less.

[0065] The specific surface area of ​​the obtained modified vinyl alcohol polymer particles is preferably 0.01 to 1.0 m 2 / g. The above specific surface area is less than 0.01m 2 / g, when used as a column filler, the separation performance may be deteriorated. The above specific surface area is more preferably 0.1m 2 On the other hand, the above specific surface area exceeds 1.0 m 2 / g, when used as a column filler, the particles may be compacted and filtration failure may occur.

[0066] From the viewpoint of improving the viscosity stability when an aqueous solution is prepared, in the obtained modified vinyl alcohol polymer particles, the proportion of vinyl ester units present in triads or more relative to all vinyl ester units is preferably 10 mol% or less. The above proportion is more preferably 9 mol% or less, further preferably 8 mol% or less, and particularly preferably 7 mol% or less. On the other hand, the proportion of vinyl ester units present in triads or more is usually 0.1 mol% or more. The proportion of vinyl ester units present in triads or more can be determined by using the method described in the examples below. 1 It was determined by the method of H-NMR measurement.

[0067] The content of the vinyl alcohol unit in the modified vinyl alcohol polymer obtained relative to the total structural units needs to be 95 to 99.99 mol%. When the content of the vinyl alcohol unit is less than 95 mol%, the crystallinity of the modified vinyl alcohol polymer is significantly reduced, and the mechanical strength is likely to be reduced. The content of the vinyl alcohol unit is more preferably 95.5 mol% or more. On the other hand, when the content of the vinyl alcohol unit exceeds 99.99 mol%, it is likely to be difficult to manufacture the modified vinyl alcohol polymer industrially. The content of the vinyl alcohol unit is preferably 99.9 mol% or less.

[0068] The content of the vinyl ester unit represented by formula (2) in the obtained modified vinyl alcohol polymer particles relative to the total structural units is preferably 0.01 to 5 mol%. When the content of the above-mentioned vinyl ester unit is less than 0.01 mol%, when the cross-linking reaction of the modified vinyl alcohol polymer particles is carried out, the cross-linking reaction may not proceed sufficiently. The content of the above-mentioned vinyl ester unit is more preferably 0.05 mol% or more, further preferably 0.3 mol% or more, and particularly preferably 0.5 mol% or more. On the other hand, when the content of the above-mentioned vinyl ester unit exceeds 5 mol%, the water solubility of the modified vinyl alcohol polymer particles may deteriorate. The content of the vinyl ester unit represented by formula (2) can be determined by using the method described in the examples described later. 1 It was determined by the method of H-NMR measurement.

[0069] The obtained modified vinyl alcohol polymer particles may contain other monomer units other than vinyl alcohol units and vinyl ester units as long as the effect of the present invention is not impaired. As such other monomer units, the monomer units described above as monomer units other than vinyl alcohol units and vinyl ester units contained in the vinyl alcohol polymer particles used in the production of modified vinyl alcohol polymer particles can be cited. The content of other monomer units other than vinyl alcohol units and vinyl ester units in the above-mentioned modified vinyl alcohol polymer particles is usually 10 mol% or less, preferably 5 mol% or less, and more preferably 1 mol% or less.

[0070] The viscosity average degree of polymerization of the modified vinyl alcohol polymer particles obtained is preferably 100 to 5000, more preferably 200 to 4000. When the viscosity average degree of polymerization is less than 100, the mechanical strength of the modified vinyl alcohol polymer particles obtained may be reduced. On the other hand, when the viscosity average degree of polymerization exceeds 5000, industrial production of the vinyl alcohol polymer particles may become difficult. The viscosity average degree of polymerization of the modified vinyl alcohol polymer particles is measured in accordance with JIS K6726.

[0071] The content of sulfur in the obtained modified vinyl alcohol polymer particles is preferably 0.01 to 20,000 ppm. Such modified vinyl alcohol polymer particles with a low content of sulfur are less likely to cause the problem of contamination caused by the dissolution of sulfur when used as a column filler. In addition, there is less odor when the modified vinyl alcohol polymer particles are made into an aqueous solution. The content of sulfur is more preferably 10,000 ppm or less, further preferably 5,000 ppm or less, and particularly preferably 3,000 ppm or less. On the other hand, when the content of sulfur is less than 0-01 ppm, the industrial production of modified vinyl alcohol polymer particles may become difficult. The content of sulfur is more preferably 0.1 ppm or more, and further preferably 1 ppm or more.

[0072] The yellow index (YI) of the obtained modified vinyl alcohol polymer particles measured according to ASTM D1925 is preferably 50 or less. By using such modified vinyl alcohol polymer particles, a molded product such as a film and a fiber with good appearance can be obtained. In addition, when using modified vinyl alcohol polymer particles with good hue as a filler for a column, the change in hue can be used as an indicator to judge the deterioration of the column. The YI is more preferably 40 or less, further preferably 30 or less, and particularly preferably 20 or less.

[0073] The modified vinyl alcohol polymer particles of the present invention are modified vinyl alcohol polymer particles comprising vinyl ester units represented by the following formula (2), wherein the content of the vinyl alcohol units relative to all structural units is 95 to 99.99 mol%, the content of the sulfur component is 0.01 to 20000 ppm, and the average particle size is 50 to 2000 μm.

[0074]

[0075] [In formula (2), X represents a carbon-carbon bond or a divalent saturated hydrocarbon group having 1 to 10 carbon atoms which may have a branched structure, Y represents a hydrogen atom or a saturated hydrocarbon group having 1 to 6 carbon atoms which may have a branched structure, and Z represents a hydrogen atom or a methyl group.]

[0076] The vinyl ester unit represented by the formula (2) in the modified vinyl alcohol polymer particles of the present invention is the same as the vinyl ester unit represented by the formula (2) in the modified vinyl alcohol polymer particles obtained by the above-mentioned production method.

[0077] The ratio of the vinyl ester units present in triads or more in the modified vinyl alcohol polymer particles of the present invention to the total vinyl ester units is preferably 10 mol% or less. It is also preferred that the yellowness index (YI) of the modified vinyl alcohol polymer particles measured in accordance with ASTM D1925 is 50 or less. It is also preferred that the content of the vinyl ester units represented by the above formula (2) in the modified vinyl alcohol polymer particles is 0.01 to 5 mol% relative to the total structural units.

[0078] Such modified vinyl alcohol polymer particles are suitable for use as column fillers because they have a low content of sulfur components, excellent high-energy ray reactivity, and an average particle size within a specified range. The modified vinyl alcohol polymer particles of the present invention have a good hue, high viscosity stability when made into an aqueous solution, and little odor, so they are also suitable for molded products such as membranes and fibers. Since the modified vinyl alcohol polymer particles of the present invention with an average particle size within a specified range can be efficiently transported, it is possible to expect cost reduction. In addition, in the modified vinyl alcohol polymer particles of the present invention, since the content of sulfur-containing micropowder is low, it is also possible to prevent health damage to operators due to their attraction.

[0079] [Example]

[0080] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples. It should be noted that, unless otherwise specified, "%" and "part" in the examples and comparative examples represent "mass %" and "mass part", respectively.

[0081] [Calculation of Vinyl Alcohol Unit Content]

[0082] The modified vinyl alcohol polymer particles were measured at room temperature using a nuclear magnetic resonance device "LAMBDA 500" manufactured by JEOL Ltd. using DMSO-d6 solvent. 1 The content of vinyl alcohol units in the polymer particles was calculated from the integrated value of the peak (3.4 to 4.0 ppm) attributed to methine protons bonded to the hydroxyl group and the integrated value of the peak (4.7 to 5.3 ppm) attributed to methine protons of the vinyl ester group by H-NMR.

[0083] [Calculation of modification rate]

[0084] The modified vinyl alcohol polymer particles were measured at room temperature using a nuclear magnetic resonance device "LAMBDA 500" manufactured by JEOL Ltd. 1H-NMR, the modification rate of the polymer particles [the content (mol %) of the vinyl ester unit represented by the above formula (2) relative to all structural units] was calculated from the integrated value of the peak (5.0 to 7.5 ppm) attributed to the olefin protons. For example, in Example 1, the modification rate was calculated from the integrated value of the peaks attributed to the olefin protons appearing at 5.6 ppm and 6.0 ppm.

[0085] [Calculation based on the ratio of vinyl ester groups present in triads or more]

[0086] The modified vinyl alcohol polymer particles were measured at 80°C using a nuclear magnetic resonance device "LAMBDA 500" manufactured by JEOL Ltd. using a DMSO-d6 solvent. 1 H-NMR. The ratio of vinyl ester groups present in triads or more to all vinyl ester units is calculated from the integrated values ​​of (a) 4.7 to 4.9 ppm (hydroxy-vinyl ester group-hydroxyl group's middle methine proton), (b) 4.9 to 5.05 ppm (hydroxy-vinyl ester group-vinyl ester group's middle methine proton), and (c) 5.05 to 5.25 ppm (vinyl ester group's middle methine proton).

[0087] The ratio of vinyl ester groups present in triads or more (%) = (c) / {(a)+(b)+(c)}×100

[0088] [Measurement of average particle size]

[0089] The modified vinyl alcohol polymer particles were dispersed in methanol, and the volume average particle size (μm) was measured using a laser diffraction apparatus "LA-950V2" manufactured by Horiba, Ltd.

[0090] [Measurement of specific surface area]

[0091] The specific surface area (m2) of the modified vinyl alcohol polymer particles was derived by the BET single-point method using a specific surface area measuring device "MONOSORB" manufactured by Yuasi Ionics Co., Ltd. 2 / g).

[0092] [Measurement of hue (yellow index; YI)]

[0093] The YI (ASTM D1925) of the modified vinyl alcohol polymer particles obtained in the examples or comparative examples was measured using a spectrophotometer "CM-8500d" manufactured by Konica Minolta, Inc. by the following method (light source: D65, CM-A120 white calibration plate, using CM-A126 Petri dish set, regular reflection measurement of SCE, measurement diameter φ30 mm). 5 g of the sample was added to the Petri dish, the side was gently tapped without compacting the powder, and the Petri dish was shaken to evenly spread the powder. In this state, a total of 10 measurements were performed (each time the Petri dish was shaken and then measured), and the average value was taken as the YI of the polymer particles.

[0094] [Evaluation of photosensitivity]

[0095] In an aqueous solution (concentration of 5% by mass) in which the modified vinyl alcohol polymer particles obtained in the examples or comparative examples are dissolved, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone as a photoinitiator is added so that 1 part by mass is added to 100 parts by mass of the particles, and then dissolved to prepare a coating liquid. The coating liquid is cast on a 15 cm × 15 cm mold frame made by bending the edge of a polyethylene terephthalate film, and the solvent is fully volatilized at room temperature and atmospheric pressure to obtain a film with a thickness of about 100 μm. Here, the coating liquid is cast on a 10 J / cm 2 The film for evaluation is prepared by irradiating ultraviolet rays with an intensity of , and then the mass (W2) is measured. The obtained evaluation film is immersed in boiling water for 1 hour, taken out of the water, vacuum dried at 40°C for 12 hours, and then the mass (W1) is measured. The dissolution rate under boiling conditions is calculated according to the following formula from the obtained mass (W1) and the mass of the film before immersion (W2), and the dissolution rate is used as an index of photosensitivity (the lower the dissolution rate, the higher the photosensitivity). It should be noted that when the evaluation film dissolves during the immersion in water, it is evaluated as "cannot be measured" and recorded as "-" in Table 1.

[0096] Dissolution rate (mass %) = 100 × ([W2] - [W1]) / [W2]

[0097] [Viscosity stability]

[0098] The viscosity η0 of the aqueous solution (concentration 15 mass %) in which the particles obtained in the examples or comparative examples were dissolved was measured using a viscometer "LVDV-2+PRO" manufactured by Brookfield. The viscosity η7 immediately after preparation and the viscosity η0 7 days after preparation were measured. The viscosity ratio η7 / η0 was calculated and the viscosity stability was evaluated according to the following criteria. The larger the value of the viscosity ratio η7 / η0, the greater the increase in the viscosity of the solution and the worse the viscosity stability.

[0099] A: η7 / η0 is less than 1.3

[0100] B: η7 / η0 is 1.3 or more and less than 1.6

[0101] C: η7 / η0 is 1.6 or more

[0102] [Evaluation of liquid permeability]

[0103] The modified vinyl alcohol polymer particles obtained in the examples or comparative examples are irradiated with 150 kGy of electron beams to make them cross-linked and water-resistant. 100 parts by mass of the cross-linked modified vinyl alcohol polymer particles are filled into a chromatographic column (a glass filter with an inner diameter of 50 mm and an opening diameter of 40 to 50 μm and a stopcock). 130 parts by mass of a mixture of methanol / water = 9 / 1 (mass ratio) are filled therein, and then the stopcock is opened to start filtering. The filtrate is recovered, and the time when 90% (i.e., 117 parts by mass) of the added mixture is collected as the filtrate is recorded as "end of filtration", and the permeability is evaluated based on the time required from the start of filtration to the end of filtration.

[0104] A: When filtering ends in less than 150 seconds

[0105] B: If the time is more than 150 seconds and less than 300 seconds, the

[0106] C: When it takes more than 300 seconds to complete filtering

[0107] [Evaluation of sulfur content]

[0108] The modified vinyl alcohol polymer particles obtained in Examples or Comparative Examples were dried at 80° C. for 12 hours, and then the content of sulfur components in the modified vinyl alcohol polymer particles was measured using an organic element analyzer 2400II manufactured by PerkinElmer.

[0109] [Example 1]

[0110] Into a reactor equipped with a stirrer, a reflux pipe, and an addition port, 482.0 parts by mass of methacrylic acid, 85.1 parts by mass of ion exchange water, 1.3 parts by mass of p-methoxyphenol, and 4.5 parts by mass of 47% sulfuric acid were sequentially added, and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 500, saponification degree 98.5 mol%, average particle size 723 μm) was added while stirring at room temperature, and the temperature was raised to 80°C while stirring, and the mixture was reacted in a slurry state for 5 hours. Then, the mixture was cooled to room temperature, the contents were filtered, and the modified vinyl alcohol polymer was recovered, washed with a large amount of methanol, and dried at 40°C and 1.3 Pa for 20 hours to obtain the target particles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0111] [Example 2]

[0112] Into a reactor equipped with a stirrer, a reflux pipe, and an addition port, 510.3 parts by mass of 4-pentenoic acid, 56.7 parts by mass of ion exchange water, 1.3 parts by mass of p-methoxyphenol, and 4.2 parts by mass of p-toluenesulfonic acid monohydrate were sequentially added, and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 1700, saponification degree 98.5 mol%, average particle size 698 μm) was added while stirring at room temperature, and the temperature was raised to 60° C. while stirring, and the mixture was reacted in a slurry state for 3 hours. Then, the post-treatment was performed in the same manner as in Example 1 to obtain the target particles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0113] It should be noted that the obtained modified vinyl alcohol polymer particles are 1 The result of H-NMR measurement is that the proportion of vinyl ester groups existing in triads or more cannot be calculated because the olefin proton peaks belonging to the unsaturated hydrocarbon group and the methine proton peaks of the vinyl ester group overlap. Therefore, modified vinyl alcohol polymer particles (the content of the modified vinyl alcohol polymer is 5% by mass) are dissolved in water, and then 1 mol of propanethiol is added to 1 mol of the above-mentioned olefin, and further, 1 mol of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone as a photoinitiator is added to 1 mol of propanethiol. At 3000mJ / cm 2 The solution thus prepared was irradiated with ultraviolet light of a certain intensity. The obtained solution was added to a large amount of methanol to precipitate polymer particles, and then 1 The particles were analyzed by H-NMR. As a result, the olefin proton peak disappeared due to the addition of mercaptan, and thus the ratio of the vinyl ester groups present in triads or more could be calculated.

[0114] [Example 3]

[0115] Into a reactor equipped with a stirrer, a reflux pipe, and an addition port, 454.2 parts by mass of methacrylic acid, 5.7 parts by mass of acetic acid, 56.7 parts by mass of ion exchange water, 1.3 parts by mass of p-methoxyphenol, and 4.2 parts by mass of p-toluenesulfonic acid monohydrate were sequentially added, and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 1700, saponification degree 99.5 mol%, average particle size 128 μm) was added while stirring at room temperature, and the temperature was raised to 90° C. while stirring, and the mixture was reacted in a slurry state for 3 hours. Then, the post-treatment was performed in the same manner as in Example 1 to obtain the target particles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0116] [Example 4]

[0117] Into a reactor equipped with a stirrer, a reflux pipe, and an addition port, 510.3 parts by mass of methacrylic acid, 28.4 parts by mass of acetic acid, 28.4 parts by mass of ion exchange water, 1.3 parts by mass of p-methoxyphenol, and 8.1 parts by mass of p-toluenesulfonic acid monohydrate were sequentially added, and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 1700, saponification degree 95 mol%, average particle size 730 μm) was added while stirring at room temperature, and the temperature was raised to 65° C. while stirring, and the mixture was reacted in a slurry state for 5 hours. Then, the post-treatment was performed in the same manner as in Example 1 to obtain the target particles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0118] [Example 5]

[0119] Into a reactor equipped with a stirrer, a reflux pipe, and an addition port, 493.3 parts by mass of acrylic acid, 17.0 parts by mass of acetic acid, 56.7 parts by mass of ion exchange water, 1.3 parts by mass of p-methoxyphenol, and 4.2 parts by mass of p-toluenesulfonic acid monohydrate were sequentially added, and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity polymerization degree 1000, saponification degree 98.5 mol%, average particle size 725 μm) was added while stirring at room temperature, and the temperature was raised to 65° C. while stirring, and the reaction was carried out in a slurry state for 5 hours. Then, the post-treatment was carried out in the same manner as in Example 1 to obtain the target particles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0120] [Example 6]

[0121] 100 parts by mass of commercially available polyvinyl alcohol resin (viscosity average polymerization degree 1700, saponification degree 98.5 mol%, average particle size 698 μm) was added to a reactor equipped with a stirrer, a reflux pipe, and an addition port. A mixed solution of 58.0 parts by mass of methacrylic acid, 2.0 parts by mass of acetic acid, 6.7 parts by mass of ion exchange water, 0.3 parts by mass of p-methoxyphenol, and 12.6 parts by mass of p-toluenesulfonic acid monohydrate, which had been mixed in advance, was added in small amounts at a time while stirring at room temperature. The mixed solution was stirred fully to uniformly mix the entire polyvinyl alcohol resin, and then the temperature was raised to 70°C while stirring, and the mixture was reacted in a powder state for 5 hours. Then, the powder was washed with a large amount of methanol, and then dried at 40°C and 1.3 Pa for 12 hours to obtain the target particles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0122] [Example 7]

[0123] Into a reactor equipped with a stirrer, a reflux pipe, and an addition port, 564.2 parts by mass of methacrylic acid, 2.8 parts by mass of ion exchange water, 1.3 parts by mass of p-methoxyphenol, and 4.2 parts by mass of p-toluenesulfonic acid monohydrate were sequentially added, and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 500, saponification degree 98.5 mol%, average particle size 720 μm) was added while stirring at room temperature, and the temperature was raised to 80° C. while stirring, and the mixture was reacted in a slurry state for 5 hours. Then, the post-treatment was performed in the same manner as in Example 1 to obtain the target particles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0124] [Comparative Example 1]

[0125] Evaluation was performed on a commercially available polyvinyl alcohol resin (viscosity average degree of polymerization: 1700, saponification degree: 98.5 mol %, average particle size: 698 μm). Table 1 shows the results of structural analysis and physical property evaluation.

[0126] [Comparative Example 2]

[0127] 400.0 parts by mass of dimethyl sulfoxide and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 1700, saponification degree 98.5 mol%, average particle size 698 μm) which had been vacuum dried at 80°C for 24 hours were added to a reactor equipped with a stirrer, a reflux tube, and an addition port, and the temperature was raised to 100°C while stirring to obtain a uniform solution. 33.4 parts by mass of methyl methacrylate and 1.1 parts by mass of phenothiazine were added to the solution, and the mixture was stirred until uniform. 1.9 parts by mass of sodium acetate as an ester exchange catalyst was added to the obtained solution, the mixture was reacted for 5 hours, and then naturally cooled to room temperature. After DMSO was added to the reaction solution to dilute it, it was added dropwise to methanol to separate the polymer, and dried at 40°C and 1.3 Pa for 12 hours. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0128] [Comparative Example 3]

[0129] 400.0 parts by mass of dimethyl sulfoxide and 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 500, saponification degree 98.5 mol%, average particle size 723 μm) which had been vacuum dried at 80°C for 24 hours were added to a reactor equipped with a stirrer, a reflux pipe, and an addition port, and the temperature was raised to 100°C while stirring to obtain a uniform solution. 40.0 parts by mass of 3,3-dimethylpentenoic acid methyl ester (MPM) was added to the solution and stirred until uniform. 0.4 parts by mass of tetramethylammonium methyl carbonate as an ester exchange catalyst was added to the obtained solution, reacted for 5 hours, and then naturally cooled to room temperature. After adding DMSO to the reaction solution to dilute it, it was added dropwise to methanol to separate the polymer, and dried at 40°C and 1.3 Pa for 12 hours. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0130] [Comparative Example 4]

[0131] 288.0 parts by mass of ion exchange water were added to a reactor equipped with a stirrer, a reflux pipe, and an addition port. 100 parts by mass of a commercially available polyvinyl alcohol resin (viscosity average polymerization degree 500, saponification degree 98.5 mol%, average particle size 723 μm) was added while stirring, and the temperature was raised to 95°C and heated and stirred for 3 hours to obtain a uniform solution. The solution was cooled to room temperature, and 558.0 parts by mass of methacrylic acid, 2 parts by mass of p-methoxyphenol, and 27.0 parts by mass of a 36% aqueous solution of hydrochloric acid were added in sequence while stirring. The temperature was raised to 80°C while stirring, and the mixture was reacted in a uniform solution state for 2 hours, and then cooled to room temperature. The obtained solution was diluted, and a large amount of methanol was added in small amounts to the place where the stirring was strong, so that modified vinyl alcohol polymer microparticles were precipitated. The precipitate was recovered, washed with a large amount of methanol, and then dried at 40°C and 1.3 Pa for 12 hours to obtain the target microparticles. The structural analysis results and physical property evaluation results of the obtained modified vinyl alcohol polymer particles are shown in Table 1.

[0132]

[0133] As can be seen from Examples 1 to 7, in the manufacturing method of the present invention, since the modification is directly carried out in the particle shape, the modified vinyl alcohol polymer particles can be easily separated without performing an operation of precipitating the reaction product in a poor solvent. The modified vinyl alcohol polymer particles of the present invention show high viscosity stability when made into an aqueous solution, and there is little odor caused by the sulfur component. In addition, the modified vinyl alcohol polymer particles have excellent high-energy ray reactivity and have excellent liquid permeability when used as a column filler after cross-linking. In addition, in the manufacturing method of the present invention, since DMSO is not used, it is also possible to suppress contamination by the sulfur component.

[0134] As in Comparative Examples 2 to 4, when the vinyl alcohol polymer particles are dissolved in a solvent and reacted, in order to separate the modified vinyl alcohol polymer particles as the reaction product, it is necessary to precipitate them in a poor solvent, which is not only complicated but also difficult to control the particle shape. In addition, the unmodified vinyl alcohol polymer particles of Comparative Example 1 do not show photosensitivity. The viscosity stability of the vinyl alcohol polymer particles in Comparative Examples 1 and 2, in which the proportion of vinyl ester groups present in triads or more exceeds 10%, is low when made into aqueous solutions. As in Comparative Examples 2 to 4, the average particle size of the modified vinyl alcohol polymer particles obtained by the reaction in a state where the vinyl alcohol polymer particles are dissolved is less than 50 μm, and the liquid permeability is poor. As in Comparative Examples 2 and 3, when DMSO is used in the reaction, the content of sulfur components in the modified vinyl alcohol polymer particles is extremely high.

[0135] [Example 8]

[0136] The modified vinyl alcohol polymer particles obtained in Example 6 were evaluated as column fillers. The particles were irradiated with 150 kGy of electron beams to crosslink and make them water-resistant. 100 parts by mass of the crosslinked modified vinyl alcohol polymer particles were filled into a chromatographic column (a glass filter with an inner diameter of 50 mm and an opening diameter of 40 to 50 μm and a stopcock), and 1000 parts by mass of super-dehydrated methanol as an eluent was passed to wet the polymer particles. Super-dehydrated methanol containing 5% by mass of ion exchange water was adsorbed on the polymer particles at the top of the column, and then 100 parts by mass of super-dehydrated methanol as an eluent was passed. The liquid was recovered from the column outlet for analysis.

[0137] During the above test period, good liquid permeability was maintained. 1 The recovered liquid was analyzed by H-NMR, and the results confirmed that the recovered liquid did not contain water, and therefore water was retained in the modified vinyl alcohol polymer particles. In addition, the recovered liquid was subjected to elemental analysis, and the sulfur content in the recovered liquid was 18 ppm.

Claims

1. A method for producing modified vinyl alcohol polymer particles, comprising mixing a mixed medium containing an unsaturated carboxylic acid, an acid catalyst and water with the vinyl alcohol polymer particles, wherein: The unsaturated carboxylic acid is represented by the following formula (1): The mixed medium and the vinyl alcohol polymer particles are mixed, and the unsaturated carboxylic acid and the vinyl alcohol polymer particles are reacted while maintaining the particle shape of the vinyl alcohol polymer particles, thereby obtaining modified vinyl alcohol polymer particles comprising a vinyl ester unit represented by the following formula (2), a vinyl alcohol unit content of 95 to 99.99 mol % relative to all structural units, and an average particle size of 50 to 2000 μm. In formula (1), X represents a carbon-carbon bond or a divalent saturated hydrocarbon group having 1 to 10 carbon atoms which may have a branched structure, Y represents a hydrogen atom or a saturated hydrocarbon group having 1 to 6 carbon atoms which may have a branched structure, and Z represents a hydrogen atom or a methyl group. X, Y, and Z in formula (2) have the same meanings as in formula (1).

2. The manufacturing method according to claim 1, wherein: The specific surface area of ​​the modified vinyl alcohol polymer particles is 0.01 to 1.0 m 2 / g.

3. The manufacturing method according to claim 1 or 2, wherein: The content of water in the mixed medium is 1 to 30% by mass.

4. The manufacturing method according to claim 1 or 2, wherein: The mixed medium also contains acetic acid.

5. The manufacturing method according to claim 1 or 2, wherein: Y is a hydrogen atom.

6. The manufacturing method according to claim 1 or 2, wherein: X is a carbon-carbon bond.

7. The manufacturing method according to claim 1 or 2, wherein: The modified vinyl alcohol polymer particles are further washed.

8. A modified vinyl alcohol polymer particle comprising a vinyl ester unit represented by the following formula (2), wherein: The content of vinyl alcohol units relative to all structural units is 95 to 99.99 mol%, the content of sulfur components is 0.01 to 20000 ppm, and the average particle size is 50 to 2000 μm. In formula (2), X represents a carbon-carbon bond or a divalent saturated hydrocarbon group having 1 to 10 carbon atoms which may have a branched structure, Y represents a hydrogen atom or a saturated hydrocarbon group having 1 to 6 carbon atoms which may have a branched structure, and Z represents a hydrogen atom or a methyl group.

9. The particle according to claim 8, wherein The ratio of the vinyl ester units present in triads or more in the modified vinyl alcohol polymer to all the vinyl ester units is 10 mol% or less.

10. The particle according to claim 8 or 9, wherein The yellowness index (YI) measured in accordance with ASTM D1925 is 50 or less.

11. The particle according to claim 8 or 9, wherein The content of the vinyl ester unit represented by the formula (2) is 0.01 to 5 mol% based on the total structural units.

12. The particle according to claim 8 or 9, wherein Y is a hydrogen atom.

13. The particle according to claim 8 or 9, wherein X is a carbon-carbon bond.

Citation Information

Patent Citations

  • Modified ethylene - vinyl alcohol copolymer and method for producing the same

    JP2003231715A

  • Method for producing unsaturated carboxylic acid-modified vinyl alcohol-based polymer and gas barrier membrane or gas barrier laminate using the same

    JP2007321099A

  • Polyvinyl acetal

    JP2009108305A

  • Side-chain-olefin-containing vinyl alcohol polymer and method of producing same

    WO2018124014A1

  • Method for producing modified polymer polyol

    WO2018124015A1