A method for preparing high-purity quartz sand

By combining low-temperature and high-temperature roasting-water quenching technology in the preparation process of quartz sand, the roasting temperature problem in the existing technology is solved, and the preparation of high-purity quartz sand is realized, and the product quality and added value are improved.

CN113735128BActive Publication Date: 2024-11-15WUHAN UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110938039.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-16
Publication Date
2024-11-15
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

In the purification process of low-quality gangue quartz ore, the high calcination temperature leads to the mineral inclusion being re-encapsulated, impurities are difficult to clean, and the low calcination temperature leads to insufficient cracks, affecting the quality and added value of quartz sand.

Method used

The combination of low-temperature roasting-water quenching and high-temperature roasting-water quenching is adopted. The first low-temperature roasting-water quenching is carried out after grinding, and the temperature is controlled to retain the inclusions. The subsequent acid leaching is carried out to remove impurities, and the second high temperature is high. Roasting-removing the inclusions during water quenching to improve the purity and added value of quartz sand.

Benefits of technology

Effectively remove gangue minerals, improve the purity and added value of quartz sand, ensure the impurity cleaning effect during subsequent processing, and meet the energy needs of phase change during roasting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113735128B_ABST
    Figure CN113735128B_ABST
Patent Text Reader

Abstract

A method for preparing high-purity quartz sand comprises the following steps: S1, crushing low-grade vein quartz ore; S2, color sorting the crushed sample to select heterochromatic particles; S3, wet grinding and grading the color sorted sample; S4, magnetically separating the ground sample to remove magnetic impurities to obtain a quartz coarse concentrate; S5, roasting the quartz coarse concentrate at 400-800°C for 1-3h, and water quenching the quartz coarse concentrate after roasting; S6, performing multiple reverse flotation on the quartz coarse concentrate to remove gangue minerals to obtain a flotation concentrate; S7, placing the flotation concentrate and mixed acid in a high-pressure acid leaching device to react to obtain acid-leached quartz; S8, roasting the acid-leached quartz at 800-1200°C for 1-3h, and water quenching the quartz after roasting, and then drying to obtain high-purity quartz; S9, inspecting and screening the high-purity quartz to remove fine powder. This design can significantly improve product quality and added value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quartz processing, and in particular to a method for preparing high-purity quartz sand, which is mainly suitable for improving product quality and product added value. Background Art

[0002] Vein quartz is a collection of silicon dioxide formed by underground magma secretion. It has a relatively pure chemical composition, with a silicon dioxide content of more than 98%. The associated minerals include aluminum silicate minerals such as mica and feldspar, iron-containing minerals, fluorite, etc. At present, my country's high-tech fields such as semiconductors, photovoltaic power generation, communications, electrical and electronics, and national defense and military industries are developing rapidly. High-purity quartz sand is an indispensable key material and has an important strategic position in my country's high-end manufacturing. Refining, upgrading and improving the production technology of quartz raw materials is indispensable for the sustainable development of my country's high-tech industry.

[0003] As a high-quality raw material for producing high-purity quartz, vein quartz has been studied in depth by many scholars and has achieved rich results. However, due to the limitation of quartz resource quality, low-quality vein quartz cannot be effectively purified according to existing technologies and methods. In the existing secondary roasting and water quenching purification technology, a purification process of crushing, roasting and water quenching, grinding, magnetic separation, flotation, acid leaching, and secondary roasting and water quenching is adopted. The first roasting and water quenching temperature of this process is too high. For low-grade vein quartz ore, the content of gangue minerals is large, and the content of mineral inclusions is high. The roasting temperature is too high, and the mineral inclusions are re-wrapped by softened quartz and gangue minerals. The internal cracks generated by water quenching penetrate into impurities in the subsequent grinding and acid leaching processes, and the impurities are not easy to be cleaned; and the expansion rate of quartz is reduced when the temperature is too high, so that the phase change of quartz sand in the secondary roasting process is inhibited to a certain extent, affecting the effect of secondary roasting and water quenching. If the roasting temperature is too low, the cracks will be insufficient. Therefore, a purification method that is conducive to the removal of gangue minerals should be designed to improve the quality of quartz products and their added value. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects and problems of poor product quality and low product added value in the prior art, and to provide a method for preparing high-purity quartz sand with good product quality and high product added value.

[0005] To achieve the above purpose, the technical solution of the present invention is: a method for preparing high-purity quartz sand, the preparation method comprising the following steps:

[0006] S1. crushing low-grade vein quartz ore to obtain a crushed sample;

[0007] S2. Color sorting the crushed samples to separate particles of different colors and obtain color sorted samples;

[0008] S3, subjecting the color sorted samples to wet grinding and classification to obtain grinding samples;

[0009] S4, using a magnetic separator to magnetically separate the ground ore sample to remove magnetic impurities and obtain a rough quartz concentrate;

[0010] S5, placing the quartz rough concentrate into a high temperature furnace, and roasting it at a low temperature in an air atmosphere, the roasting temperature is 400-800° C., and the roasting time is 1-3 hours. After the roasting is completed, the quartz rough concentrate is taken out from the high temperature furnace and directly poured into deionized water at room temperature to complete water quenching;

[0011] S6, repeatedly reverse-floating the roasted and water-quenched quartz coarse concentrate to remove gangue minerals and obtain a flotation concentrate;

[0012] S7, firstly placing the flotation concentrate and the mixed acid in a high-pressure acid leaching device for hot-pressing reaction, then repeatedly washing with deionized water until the solution is neutral, filtering and dehydrating, and then drying to obtain acid-leached quartz;

[0013] S8, firstly put the acid-leached quartz into a high temperature furnace, and calcine it at a high temperature in an air atmosphere, the calcination temperature is 800-1200° C., and the calcination time is 1-3 hours. After the calcination is completed, take out the quartz from the high temperature furnace and directly pour it into deionized water at room temperature to complete water quenching, wash it several times, and then dry it at 40-110° C. to obtain high-purity quartz;

[0014] S9. Inspect and screen high-purity quartz to remove fine powder with a particle size smaller than 0.106 mm.

[0015] In step S1, the particle size of the crushed sample is less than or equal to 20 mm.

[0016] In step S3, the particle size of the ground sample is -0.18 mm + 0.106 mm.

[0017] In step S4, the magnetic separation intensity of the magnetic separation is 1 to 1.6 T, and the pulsation frequency is 100 to 200 r / min.

[0018] In step S6, 1-2 mol / L sulfuric acid is used as a pH regulator, dodecylamine, octadecylamine, coconut amine or a mixed amine is used as a collector, and mica is removed by reverse flotation multiple times at a pH of 2-3. Then, 1-2 mol / L sulfuric acid is used as a pH regulator, an anion-cation mixed collector is used, and feldspar impurities are removed by reverse flotation multiple times at a pH of 1.5-2.

[0019] In step S6, the total amount of collector used to remove mica is 100-200 g / t, wherein the amount ratio of collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., the nth reverse flotation is 4:3:2:1:...:1.

[0020] In step S6, the anionic and cationic mixed collector includes propylene diamine + sodium dodecyl sulfate, sodium oleate + dodecylamine, octadecylamine + sodium dodecyl sulfate, propylene diamine + sodium petroleum sulfonate, wherein the ratio of the anionic collector to the cationic collector is 3:1 to 7:1.

[0021] In step S6, the total dosage of the anion and cation mixed collector is 800-1800 g / t, wherein the dosage ratio of the collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., the nth reverse flotation is 5:5:2:1:...:1.

[0022] In step S7, the mixed acid includes 1.5-4.5 mol / L hydrochloric acid, 0.5-1.5 mol / L nitric acid and 0.5-1.5 mol / L hydrofluoric acid.

[0023] In step S7, the flotation concentrate and mixed acid in a ratio of 1:1 to 1:8 are first subjected to hot pressing reaction at a temperature of 150 to 300° C. for 3 to 6 hours, then repeatedly washed with deionized water for 5 to 10 times until the solution is neutral, filtered and dehydrated, and then dried at 40 to 110° C. to obtain acid-leached quartz.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. In a method for preparing high-purity quartz sand of the present invention, the first roasting-water quenching is performed after grinding. This is because the roasting-water quenching effect of coarse particles is not as good as that of roasting-water quenching after grinding. Due to the limitation of thermal reaction dynamics, the mineral interface inside the coarse particles is not fully dissociated during the roasting-water quenching of coarse particles, and the effect of roasting-water quenching cannot be fully exerted. Roasting-water quenching is performed after grinding, the particle size becomes smaller, the roasting-water quenching dissociation effect is more sufficient, the cracks generated by roasting-water quenching expose the gangue minerals inside the particles, and the flotation behavior of the gangue minerals and the intergrowth is directly affected. At the same time, the mineral inclusions inside the quartz are connected to the outside world, which is conducive to subsequent acid leaching removal.

[0026] 2. In a method for preparing high-purity quartz sand of the present invention, low-temperature roasting is used for the first roasting-water quenching. By controlling the temperature, some inclusions can be retained, and no inclusion vacancy defects will be generated. Fine impurities and ionic impurities will not be adsorbed into internal vacancies during subsequent processing, which is not conducive to washing and removal. At the same time, the precisely controlled low-temperature roasting can produce sufficient mineral interface cracks to dissociate or expose the gangue minerals, which is conducive to subsequent removal. In addition, the precisely controlled low-temperature roasting has little effect on the phase change process during the second roasting of quartz, so that the secondary roasting-water quenching can fully play its role.

[0027] 3. In the preparation method of high-purity quartz sand of the present invention, a mixed acid solution is used to acid-leach the flotation concentrate during the acid leaching process, which can effectively remove gangue minerals; the second roasting-water quenching adopts high-temperature roasting, which can remove a large number of inclusions, reduce the impurity content, improve the purity, increase its added value, and can meet the more heat required in the second roasting process. Therefore, the present invention improves product quality and product added value. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart of a method for preparing high-purity quartz sand.

[0029] Figure 1 In the figure, +0.18mm means that particles with a size of 0.18mm or above are returned to the mill for regrinding, particles with a size of -0.18mm+0.106mm are test samples, and particles with a size of -0.106mm are particles that pass the mill sieve as by-products.

[0030] Figure 2 It is the TG-DSC curve of vein quartz sample. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0032] See also Figure 1 , a method for preparing high-purity quartz sand, the preparation method comprising the following steps:

[0033] S1. crushing low-grade vein quartz ore to obtain a crushed sample;

[0034] S2. Color sorting the crushed samples to separate particles of different colors and obtain color sorted samples;

[0035] S3, subjecting the color sorted samples to wet grinding and classification to obtain grinding samples;

[0036] S4, using a magnetic separator to magnetically separate the ground ore sample to remove magnetic impurities and obtain a rough quartz concentrate;

[0037] S5, placing the quartz rough concentrate into a high temperature furnace, and roasting it at a low temperature in an air atmosphere, the roasting temperature is 400-800° C., and the roasting time is 1-3 hours. After the roasting is completed, the quartz rough concentrate is taken out from the high temperature furnace and directly poured into deionized water at room temperature to complete water quenching;

[0038] S6, repeatedly reverse-floating the roasted and water-quenched quartz coarse concentrate to remove gangue minerals and obtain a flotation concentrate;

[0039] S7, firstly placing the flotation concentrate and the mixed acid in a high-pressure acid leaching device for hot-pressing reaction, then repeatedly washing with deionized water until the solution is neutral, filtering and dehydrating, and then drying to obtain acid-leached quartz;

[0040] S8, firstly put the acid-leached quartz into a high temperature furnace, and calcine it at a high temperature in an air atmosphere, the calcination temperature is 800-1200° C., and the calcination time is 1-3 hours. After the calcination is completed, take out the quartz from the high temperature furnace and directly pour it into deionized water at room temperature to complete water quenching, wash it several times, and then dry it at 40-110° C. to obtain high-purity quartz;

[0041] S9. Inspect and screen high-purity quartz to remove fine powder with a particle size smaller than 0.106 mm.

[0042] In step S1, the particle size of the crushed sample is less than or equal to 20 mm.

[0043] In step S3, the particle size of the ground sample is -0.18 mm + 0.106 mm.

[0044] In step S4, the magnetic separation intensity of the magnetic separation is 1 to 1.6 T, and the pulsation frequency is 100 to 200 r / min.

[0045] In step S6, 1-2 mol / L sulfuric acid is used as a pH regulator, dodecylamine, octadecylamine, coconut amine or a mixed amine is used as a collector, and mica is removed by reverse flotation multiple times at a pH of 2-3. Then, 1-2 mol / L sulfuric acid is used as a pH regulator, an anion-cation mixed collector is used, and feldspar impurities are removed by reverse flotation multiple times at a pH of 1.5-2.

[0046] In step S6, the total amount of collector used to remove mica is 100-200 g / t, wherein the amount ratio of collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., the nth reverse flotation is 4:3:2:1:...:1.

[0047] In step S6, the anionic and cationic mixed collector includes propylene diamine + sodium dodecyl sulfate, sodium oleate + dodecylamine, octadecylamine + sodium dodecyl sulfate, propylene diamine + sodium petroleum sulfonate, wherein the ratio of the anionic collector to the cationic collector is 3:1 to 7:1.

[0048] In step S6, the total dosage of the anion and cation mixed collector is 800-1800 g / t, wherein the dosage ratio of the collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., the nth reverse flotation is 5:5:2:1:...:1.

[0049] In step S7, the mixed acid includes 1.5-4.5 mol / L hydrochloric acid, 0.5-1.5 mol / L nitric acid and 0.5-1.5 mol / L hydrofluoric acid.

[0050] In step S7, the flotation concentrate and mixed acid in a ratio of 1:1 to 1:8 are first subjected to hot pressing reaction at a temperature of 150 to 300° C. for 3 to 6 hours, then repeatedly washed with deionized water for 5 to 10 times until the solution is neutral, filtered and dehydrated, and then dried at 40 to 110° C. to obtain acid-leached quartz.

[0051] The principle of the present invention is described as follows:

[0052] In the process of quartz purification, roasting-water quenching utilizes the difference in phase change and expansion rate between quartz and gangue minerals during heating-cooling, thereby generating cracks between the interfaces of quartz and gangue minerals. However, the prior art mainly considers this factor when performing roasting-water quenching, thereby ignoring that after a phase change, the expansion rate and phase change of quartz will change. The expansion rate of roasted quartz sand is significantly lower than that of unroasted sand. The prior art performs high-temperature roasting and water quenching before impurity removal, which will remove gas-liquid inclusions. The resulting inclusion vacancies will absorb fine particles and ionic impurities during subsequent processing, which are not easy to wash and remove, resulting in low product quality. In addition, the prior art does not take into account that when the first roasting temperature is too high, the quartz may be overheated and softened, and the internal gangue minerals and inclusions may be re-wrapped.

[0053] The position of roasting and water quenching in the quartz purification process has an important influence on the purification of quartz. In the existing technology, the effect of roasting and water quenching on grinding is mainly considered, while the effect of roasting and water quenching on ore dressing and purification is ignored, and the gain effects of the two are not compared. Roasting and water quenching is located before grinding, which is limited by the thermal reaction dynamics of coarse particles. The mineral interface dissociation inside the coarse particles is not sufficient. After grinding, the gain effect of roasting and water quenching cannot be fully exerted. Roasting and water quenching after grinding will reduce the particle size, and the dissociation effect of roasting and water quenching will be more sufficient. The cracks caused by roasting and water quenching will expose the gangue minerals inside the particles, and the flotation behavior of gangue minerals and intergrowths will be directly affected. At the same time, the mineral inclusions inside the quartz are connected to the outside world, which is conducive to the subsequent acid leaching removal, and can better meet the subsequent processes for effective ore dressing and purification. Figure 2As shown in the figure, quartz will undergo phase change at 572.1℃ and 862.5℃. Due to the different phase change temperatures and expansion rates of quartz and gangue minerals, cracks are generated between the interfaces of quartz and gangue minerals by controlling the temperature, which is conducive to the monomer dissociation of quartz and gangue minerals during the grinding process. At the same time, the cracks generated are conducive to the mixed acid entering the interior of quartz through the cracks during the acid leaching process, thereby achieving the purpose of removing impurities inside the quartz. Therefore, the first roasting-water quenching is at a low temperature, which is beneficial to the subsequent acid leaching. The energy absorbed by the phase change of quartz sand during heating is greater than the heat released by the phase change during cooling, and the phase change of the roasted quartz sand requires more energy. The first roasting-water quenching uses a relatively low temperature, and the second roasting-water quenching uses a relatively high temperature, which can better meet the more energy required for the phase change of the roasted quartz sand. Therefore, the first roasting-water quenching has little effect on the second roasting-water quenching. In addition, during the heating process, the expansion rate of quartz sand increases with the increase of temperature. The expansion rate of quartz sand after roasting is significantly lower than that of new sand. The first roasting adopts a relatively low temperature, which has not yet reached the temperature of the second phase change of quartz, and has little effect on the relatively high temperature phase change and expansion rate in the second roasting.

[0054] The second roasting adopts a relatively high temperature, and the changes inside the crystal are drastic, which can cause the fluid inclusions to break and the gangue mineral monomers to dissociate; in the process of the second roasting-water quenching, the first roasting-water quenching adopts 400℃, 600℃, and 800℃ respectively, and the second roasting-water quenching adopts 1000℃. When the first roasting temperature is 600℃, the lowest Al and Fe elements are 216.16μg / g and 3.73μg / g respectively, and both are lower than the quartz concentrate purified by the single roasting-water quenching process, thereby further improving its added value. Since the roasted quartz sand requires more energy, if the same temperature or a lower temperature is used, it is difficult to meet the higher energy required for the phase change of the roasted quartz sand. Therefore, the second roasting-water quenching adopts a relatively high temperature, which is much higher than the temperature of the phase change produced by the first relatively low temperature roasting water quenching, and also higher than the temperature of the second phase change of quartz, which can meet the higher energy required for the phase change of the roasted quartz sand.

[0055] Embodiment 1:

[0056] See also Figure 1 , a method for preparing high-purity quartz sand, the preparation method comprising the following steps:

[0057] S1. Crushing low-grade vein quartz ore (from a place in Gansu, with a silicon dioxide content of 98.96%) to obtain a crushed sample, wherein the particle size of the crushed sample is less than or equal to 20 mm;

[0058] S2. Color sorting the crushed samples to separate particles of different colors and obtain color sorted samples;

[0059] S3, wet grinding and classification of the color selected samples to obtain grinding samples, the particle size of the grinding samples is -0.18mm+0.106mm;

[0060] S4. Use a magnetic separator to magnetically separate the ground ore sample, with a magnetic separation intensity of 1 to 1.6 T and a pulsation frequency of 100 to 200 r / min, to remove magnetic impurities and obtain a rough quartz concentrate, which is then dried at 40 to 110°C for sample preparation;

[0061] S5, placing the quartz rough concentrate in a high temperature furnace, and roasting it at a low temperature in an air atmosphere, the roasting temperature is 400° C., and the roasting time is 1 to 3 hours. After the roasting is completed, the quartz rough concentrate is taken out from the high temperature furnace and directly poured into deionized water at room temperature to complete water quenching;

[0062] S6, repeatedly reverse-floating the roasted and water-quenched quartz coarse concentrate to remove gangue minerals and obtain a flotation concentrate;

[0063] First, 1-2 mol / L sulfuric acid is used as a pH regulator, dodecylamine, octadecylamine, coconut amine or mixed amines are used as collectors, and under the condition of pH 2-3, reverse flotation is used to remove mica for multiple times, and the total amount of the collector used is 100-200 g / t, wherein the amount ratio of the collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., the nth reverse flotation is 4:3:2:1:...:1 (all after the third stage are 1); then, 1-2 mol / L sulfuric acid is used as a pH regulator, an anion-cation mixed collector is used, and under the condition of pH 1.5-2 Under the condition, reverse flotation is repeated to remove feldspar impurities, the anion and cation mixed collector includes propylene diamine + sodium dodecyl sulfonate, sodium oleate + dodecylamine, octadecylamine + sodium dodecyl sulfonate, propylene diamine + sodium petroleum sulfonate, wherein the ratio of the anion collector to the cationic collector is 3:1-7:1, and the total amount of the anion and cation mixed collector is 800-1800 g / t, wherein the amount ratio of the collector in the first stage of reverse flotation, the second stage of reverse flotation, the third stage of reverse flotation, the fourth stage of reverse flotation, ..., the nth stage of reverse flotation is 5:5:2:1:...:1 (all 1 after the third stage);

[0064] S7, firstly placing the flotation concentrate and mixed acid in a ratio of 1:1 to 1:8 in a high-pressure acid leaching device, hot pressing and reacting at a temperature of 150 to 300°C for 3 to 6 hours, then repeatedly washing with deionized water for 5 to 10 times until the solution is neutral, filtering and dehydrating, and then drying at 40 to 110°C to obtain acid-leached quartz; the mixed acid comprises 1.5 to 4.5 mol / L hydrochloric acid, 0.5 to 1.5 mol / L nitric acid and 0.5 to 1.5 mol / L hydrofluoric acid;

[0065] S8, firstly put the acid-leached quartz into a high temperature furnace, and calcine it at a high temperature in an air atmosphere, the calcination temperature is 800°C, and the calcination time is 1 to 3 hours. After the calcination is completed, take out the quartz from the high temperature furnace and directly pour it into deionized water at room temperature to complete water quenching, wash it several times, and then dry it at 40 to 110°C to obtain high-purity quartz;

[0066] S9. Inspect and screen high-purity quartz to remove fine powder with a particle size smaller than 0.106 mm.

[0067] Using ICP detection, the purity of high-purity quartz is greater than 99.95%.

[0068] Embodiment 2:

[0069] The basic content is the same as that of Example 1, except that:

[0070] In step S8, the calcination temperature is 1000°C.

[0071] Embodiment 3:

[0072] The basic content is the same as that of Example 1, except that:

[0073] In step S8, the calcination temperature is 1200°C.

[0074] Embodiment 4:

[0075] The basic content is the same as that of Example 1, except that:

[0076] In step S5, the calcination temperature is 600°C.

[0077] Embodiment 5:

[0078] The basic content is the same as that of Example 1, except that:

[0079] In step S5, the calcination temperature is 600°C; in step S8, the calcination temperature is 1000°C.

[0080] Embodiment 6:

[0081] The basic content is the same as that of Example 1, except that:

[0082] In step S5, the calcination temperature is 600°C; in step S8, the calcination temperature is 1200°C.

[0083] Embodiment 7:

[0084] The basic content is the same as that of Example 1, except that:

[0085] In step S5, the calcination temperature is 800°C.

[0086] Embodiment 8:

[0087] The basic content is the same as that of Example 1, except that:

[0088] In step S5, the calcination temperature is 800°C; in step S8, the calcination temperature is 1000°C.

[0089] Embodiment 9:

[0090] The basic content is the same as that of Example 1, except that:

[0091] In step S5, the calcination temperature is 800°C; in step S8, the calcination temperature is 1200°C.

[0092] In step S5, the calcination and water quenching are performed at 400°C, 600°C and 800°C respectively, and in step S8, the calcination and water quenching are performed at 800°C. The results are shown in Table 1.

[0093] Table 1 Al and Fe contents of the final concentrate after secondary roasting and water quenching (μg / g)

[0094]

[0095] In step S5, the calcination and water quenching are performed at 400°C, 600°C, and 800°C respectively, and in step S8, the calcination and water quenching are performed at 1000°C. The results are shown in Table 2.

[0096] Table 2 Al and Fe contents of the final concentrate after secondary roasting and water quenching (μg / g)

[0097]

[0098] In step S5, the calcination and water quenching are performed at 400°C, 600°C, and 800°C respectively, and in step S8, the calcination and water quenching are performed at 1200°C. The results are shown in Table 3.

[0099] Table 3 Al and Fe contents of the final concentrate after secondary roasting and water quenching (μg / g)

[0100]

[0101]

[0102] Embodiment 10:

[0103] A method for preparing high-purity quartz sand, the preparation method comprising the following steps:

[0104] S1. Crushing low-grade vein quartz ore (from a place in Gansu, with a silicon dioxide content of 98.96%) to obtain a crushed sample, wherein the particle size of the crushed sample is less than or equal to 20 mm;

[0105] S2. Color sorting the crushed samples to separate particles of different colors and obtain color sorted samples;

[0106] S3, placing the color sorted sample into a high temperature furnace, and roasting it at a low temperature in an air atmosphere, the roasting temperature is 600°C, and the roasting time is 1 to 3 hours. After the roasting is completed, the quartz rough concentrate is taken out from the high temperature furnace and directly poured into deionized water at room temperature to complete water quenching;

[0107] S4, wet grinding and classifying the water-quenched sample to obtain a grinding sample, the particle size of the grinding sample is -0.18mm+0.106mm;

[0108] S5. Use a magnetic separator to magnetically separate the ground ore sample, with a magnetic separation intensity of 1 to 1.6 T and a pulsation frequency of 100 to 200 r / min, to remove magnetic impurities and obtain a rough quartz concentrate, which is then dried at 40 to 110°C for sample preparation;

[0109] S6, repeatedly reverse-floating the roasted and water-quenched quartz coarse concentrate to remove gangue minerals and obtain a flotation concentrate;

[0110] First, 1-2 mol / L sulfuric acid is used as a pH regulator, dodecylamine, octadecylamine, coconut amine or mixed amines are used as collectors, and under the condition of pH 2-3, reverse flotation is used to remove mica for multiple times, and the total amount of the collector used is 100-200 g / t, wherein the amount ratio of the collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., the nth reverse flotation is 4:3:2:1:...:1 (all after the third stage are 1); then, 1-2 mol / L sulfuric acid is used as a pH regulator, an anion-cation mixed collector is used, and under the condition of pH 1.5-2 Under the condition, reverse flotation is repeated to remove feldspar impurities, the anion and cation mixed collector includes propylene diamine + sodium dodecyl sulfonate, sodium oleate + dodecylamine, octadecylamine + sodium dodecyl sulfonate, propylene diamine + sodium petroleum sulfonate, wherein the ratio of the anion collector to the cationic collector is 3:1-7:1, and the total amount of the anion and cation mixed collector is 800-1800 g / t, wherein the amount ratio of the collector in the first stage of reverse flotation, the second stage of reverse flotation, the third stage of reverse flotation, the fourth stage of reverse flotation, ..., the nth stage of reverse flotation is 5:5:2:1:...:1 (all 1 after the third stage);

[0111] S7, firstly placing the flotation concentrate and mixed acid in a ratio of 1:1 to 1:8 in a high-pressure acid leaching device, hot pressing and reacting at a temperature of 150 to 300°C for 3 to 6 hours, then repeatedly washing with deionized water for 5 to 10 times until the solution is neutral, filtering and dehydrating, and then drying at 40 to 110°C to obtain acid-leached quartz; the mixed acid comprises 1.5 to 4.5 mol / L hydrochloric acid, 0.5 to 1.5 mol / L nitric acid and 0.5 to 1.5 mol / L hydrofluoric acid;

[0112] S8, firstly put the acid-leached quartz into a high temperature furnace, and calcine it at a high temperature in an air atmosphere, the calcination temperature is 1000° C., and the calcination time is 1 to 3 hours. After the calcination is completed, take out the quartz from the high temperature furnace and directly pour it into deionized water at room temperature to complete water quenching, wash it several times, and then dry it at 40 to 110° C. to obtain high-purity quartz;

[0113] S9. Inspect and screen high-purity quartz to remove fine powder with a particle size smaller than 0.106 mm.

[0114] In this embodiment, the first roasting-water quenching is located before grinding, the first roasting-water quenching is at 600°C, and the second roasting-water quenching is at 1000°C. The results are shown in Table 4.

[0115] Table 4 Al and Fe contents of the final concentrate after secondary roasting and water quenching (μg / g)

[0116]

Claims

1. A method for preparing high-purity quartz sand, characterized in that: The preparation method comprises the following steps: S1. crushing low-grade vein quartz ore to obtain a crushed sample; S2. Color sorting the crushed samples to separate the particles of different colors and obtain color sorted samples; S3, wet grinding and classification of the color sorted sample to obtain a grinding sample; the particle size of the grinding sample is -0.18mm+0.106mm; S4, using a magnetic separator to magnetically separate the ground ore sample to remove magnetic impurities and obtain a rough quartz concentrate; S5, placing the quartz rough concentrate in a high temperature furnace, and roasting it at a low temperature in an air atmosphere, the roasting temperature is 400° C., and the roasting time is 1 to 3 hours. After the roasting is completed, the quartz rough concentrate is taken out from the high temperature furnace and directly poured into deionized water at room temperature to complete water quenching; S6, performing multiple reverse flotation on the roasted and water-quenched quartz rough concentrate to remove gangue minerals, thereby obtaining a flotation concentrate; First, using 1-2 mol / L sulfuric acid as a pH regulator and dodecylamine, octadecylamine, coconut amine or mixed amines as collectors, at a pH of 2-3, reverse flotation is performed to remove mica for multiple times, and then using 1-2 mol / L sulfuric acid as a pH regulator and anion and cation mixed collectors, at a pH of 1.5-2, reverse flotation is performed to remove feldspar impurities for multiple times; The total amount of collector used to remove mica is 100-200 g / t, wherein the amount ratio of collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., and the nth reverse flotation is 4:3:2:1:...:1; The anionic and cationic mixed collectors include propylene diamine + sodium dodecyl sulfonate, sodium oleate + dodecyl amine, octadecyl amine + sodium dodecyl sulfonate, propylene diamine + sodium petroleum sulfonate, wherein the ratio of the anionic collector to the cationic collector is 3:1 to 7:1; The total dosage of the anion and cation mixed collector is 800-1800 g / t, wherein the dosage ratio of the collector in the first reverse flotation, the second reverse flotation, the third reverse flotation, the fourth reverse flotation, ..., the nth reverse flotation is 5:5:2:1:...:1; S7, first placing the flotation concentrate and the mixed acid in a high-pressure acid leaching device for hot-pressing reaction, then repeatedly washing with deionized water until the solution is neutral, filtering and dehydrating, and then drying to obtain acid-leached quartz; The mixed acid includes 1.5-4.5 mol / L hydrochloric acid, 0.5-1.5 mol / L nitric acid and 0.5-1.5 mol / L hydrofluoric acid; First, the flotation concentrate and mixed acid in a ratio of 1:1 to 1:8 are hot-pressed at a temperature of 150 to 300°C for 3 to 6 hours, then repeatedly washed with deionized water for 5 to 10 times until the solution is neutral, filtered and dehydrated, and then dried at 40 to 110°C to obtain acid-leached quartz; S8, firstly put the acid-leached quartz into a high temperature furnace, and calcine it at a high temperature in an air atmosphere, the calcination temperature is 800°C, and the calcination time is 1 to 3 hours. After the calcination is completed, take out the quartz from the high temperature furnace and directly pour it into deionized water at room temperature to complete water quenching, wash it several times, and then dry it at 40 to 110°C to obtain high-purity quartz; S9. Inspect and screen high-purity quartz to remove fine powder with a particle size smaller than 0.106 mm.

2. The method for preparing high-purity quartz sand according to claim 1, characterized in that: In step S1, the particle size of the crushed sample is less than or equal to 20 mm.

3. The method for preparing high-purity quartz sand according to claim 1, characterized in that: In step S4, the magnetic separation intensity of the magnetic separation is 1 to 1.6 T, and the pulsation frequency is 100 to 200 r / min.

Citation Information

Patent Citations

  • Method for preparing ultralow-metallic-element ultrahigh-purity quartz through mixed acid hot-pressing leaching reaction

    CN103539133A

  • Purifying method of ultralow-metal element highly pure quartz

    CN105936509A

  • Method for preparing high-purity quartz sand from vein quartz ore

    CN106064819A

  • Method for purifying quartz by chloridizing roasting

    CN111874913A

  • Method for preparing high-purity quartz sand with vein quartz as raw material

    CN111874915A