A polyvinylidene fluoride-based composite material with high dielectric constant, low loss and high breakdown strength and its preparation method and application

By adding nanometer sodium bismuth titanate modified with silane coupling agent to polyvinylidene fluoride, a polyvinylidene fluoride-based composite material with high dielectric, low loss and high breakdown strength was prepared, which solved the problem of PVDF dielectric constant shortage. problem, it is suitable for high-performance capacitors and energy storage devices, achieving performance improvement and cost reduction.

CN113773536BActive Publication Date: 2024-10-22HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111055221.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-09
Publication Date
2024-10-22
Estimated Expiration
2041-09-09

AI Technical Summary

Technical Problem

Polyvinylidene fluoride (PVDF) has a limited dielectric constant, making it difficult to meet the high dielectric performance requirements of high-performance capacitors and energy storage devices.

Method used

Nano-sodium bismuth titanate modified with silane coupling agent and polyvinylidene fluoride are used as the doping phase of the composite material. Nano-sodium bismuth titanate powder is prepared by hydrothermal method, and heated on a film spreading machine and a flat vulcanizer. Pressure treatment to form polyvinylidene fluoride-based composite materials with high dielectric, low loss and high breakdown strength.

Benefits of technology

It significantly improves the dielectric constant and breakdown field strength of the composite material, maintains low dielectric loss, is suitable for use in modern high-performance capacitors and energy storage devices, achieves lightweight and miniaturization, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113773536B_ABST
    Figure CN113773536B_ABST
Patent Text Reader

Abstract

The present invention discloses a polyvinylidene fluoride-based composite material with high dielectric, low loss and high breakdown strength, and a preparation method and application thereof, which belong to the application fields of high-performance capacitors and energy storage devices. The present invention aims to solve the technical problem that the PVDF dielectric constant is limited and it is difficult to meet the high dielectric performance requirements of capacitors and energy storage devices. The present invention is a nano-sodium bismuth titanate modified with a silane coupling agent, the morphology of the nano-sodium bismuth titanate is spherical, and polyvinylidene fluoride is used as a matrix; the method is: adding the nano-sodium bismuth titanate modified with a silane coupling agent to N,N-dimethylformamide, ultrasonically stirring for 2 hours, adding polyvinylidene fluoride powder, ultrasonically stirring and reacting for 2 hours; laying a film, drying; hot pressing. The present invention is used to make capacitors and energy storage devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the application fields of high-performance capacitors and energy storage devices, and specifically relates to a polyvinylidene fluoride (PVDF)-based composite material with high dielectric, low loss and high breakdown strength, and a preparation method and application thereof. Background Art

[0002] Dielectric capacitors are expected to become the most promising devices in energy storage capacitors due to their ultra-fast charge and discharge speed, high power density, and low loss. At present, dielectric capacitors have been widely used in new energy power generation systems, hybrid vehicles, aerospace equipment, and electromagnetic pulse systems. With the rapid advancement of science and technology, the demand for further flexibility, miniaturization, and low cost of high-performance electronic components has become more urgent.

[0003] Most dielectric polymers, although they have the advantages of high breakdown field strength, low cost, easy processing, good flexibility and light weight, often have low dielectric constants and are difficult to meet higher performance requirements, thus limiting the development and application of high energy density dielectrics. Traditional inorganic dielectrics, such as ceramic particles such as barium titanate, lead zirconate titanate, and calcium copper titanate, have high relative dielectric constants, but their breakdown field strength is low and it is not easy to form films on a large area. Therefore, the research turned to polymer-based dielectric composites, using polymers that are easy to process, have good flexibility and high breakdown field strength as the matrix, and adding dielectric ceramics with ultra-high dielectric constants as the filling phase. Ultimately, the prepared polymer-based composites have the advantages of both, and ultimately the dielectric properties and breakdown field strength of the material are improved at the same time.

[0004] However, due to the large difference in properties between the two phases, the compatibility is not good enough, and the high content of ceramic powder is very easy to agglomerate, forming a large number of pores inside the composite material, which will reduce the dielectric constant and breakdown field strength of the composite material. In order to overcome these problems, an effective method is to use a suitable coupling agent to modify the surface of the inorganic filler, thereby improving the compatibility between the filler and the polymer matrix and making the filler evenly dispersed. In this way, a polymer-based composite material with high dielectric constant, low dielectric loss and high breakdown strength is obtained.

[0005] Polyvinylidene fluoride (PVDF) has good dielectric properties due to its unique crystal structure and is one of the most widely used polymers in the field of polymer energy storage. PVDF also has excellent properties such as good flexibility and thermal stability, but polyvinylidene fluoride is a thermoplastic polymer and its limited dielectric constant cannot meet the requirements of high-performance capacitors and energy storage devices for high dielectric properties of materials. Summary of the invention

[0006] The present invention aims to solve the technical problem that PVDF has a limited dielectric constant and cannot meet the high dielectric performance requirements of capacitors and energy storage devices; and proposes a polyvinylidene fluoride based composite material with high dielectric, low loss and high breakdown strength, and a preparation method and application thereof.

[0007] In order to solve the above technical problems, the doped phase of the polyvinylidene fluoride based composite material with high dielectric, low loss and high breakdown strength of the present invention is nano-sodium bismuth titanate modified with a silane coupling agent, the morphology of the nano-sodium bismuth titanate is spherical, and polyvinylidene fluoride is used as a matrix; the preparation method thereof is specifically carried out according to the following steps: step 1, adding the nano-sodium bismuth titanate modified by a silane coupling agent to N,N-dimethylformamide, ultrasonically stirring for 2 hours, adding polyvinylidene fluoride powder, ultrasonically stirring and reacting for 2 hours to obtain a glue solution; step 2, laying the obtained glue solution on a film laying machine and drying; step 3, hot pressing the obtained film on a flat vulcanizer to obtain the composite material.

[0008] It is further defined that the content of the doped phase is 15%-30% of the mass of the polyvinylidene fluoride.

[0009] It is further defined that the diameter of the sodium bismuth titanate is 150nm to 200nm;

[0010] It is further defined that the sodium bismuth titanate is prepared by a hydrothermal method using bismuth nitrate pentahydrate as a bismuth source, tetrabutyl titanate as a titanium source, and sodium hydroxide as a sodium source and a mineralizer; wherein the hydrothermal reaction temperature is 150°C-180°C, and the hydrothermal reaction time is 20h-24h.

[0011] It is further defined that the doped phase is prepared by ultrasonically stirring the nano-sodium bismuth titanate in a 95% (volume) ethanol solution for 2 hours, then adding a silane coupling agent dropwise at 50°C-80°C, heating and stirring for 6h-8h, and then repeatedly washing with ethanol or deionized water and drying to obtain coupling agent-modified sodium bismuth titanate, wherein the amount of the silane coupling agent used is 1%-3% of the mass fraction of the nano-sodium bismuth titanate.

[0012] It is further defined that step 2 is drying at 80° C. for 2 h.

[0013] It is further defined that in step three, hot pressing is performed at a temperature of 160-190° C. and a pressure of 10 MPa for 30 minutes.

[0014] The composite material or the composite material prepared by the method is used to make capacitors and energy storage devices.

[0015] The spherical sodium bismuth titanate (Na 0.5 Bi 0.5TiO3, NBT), the preparation process is conducive to saving resources and reducing costs, and the preparation process has little pollution. The powder is obtained directly from the liquid phase, eliminating high-temperature calcination and ball milling, and avoiding the appearance of impurities and structural defects.

[0016] The polyvinylidene fluoride based composite material with high dielectric, low loss and high breakdown strength prepared by the present invention will be applied to modern high-performance capacitors and energy storage devices, can effectively realize the lightweight and miniaturization of energy storage devices, improve the energy storage capacity of capacitors, and can maintain low dielectric loss.

[0017] The polyvinylidene fluoride-based composite material with high dielectric, low loss and high breakdown strength prepared by the present invention is doped with polyvinylidene fluoride by sodium bismuth titanate ceramic modified by a coupling agent, thereby improving the compatibility between the filler and the matrix, and greatly improving the dielectric constant of the composite material while maintaining the low dielectric loss of the polyvinylidene fluoride itself.

[0018] The polyvinylidene fluoride-based composite material with high dielectric, low loss and high breakdown strength prepared by the present invention has a doped sodium bismuth titanate particle size as small as nanometer level and a regular spherical morphology, and is well dispersed in the polyvinylidene fluoride matrix without excessive agglomeration, thereby avoiding the formation of a conductive path and achieving low dielectric loss and high breakdown field strength.

[0019] The polyvinylidene fluoride based composite material with high dielectric, low loss and high breakdown strength prepared by the present invention has a simple preparation process, a simple preparation method, no pollution emission during the preparation process, low cost and high safety factor, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron microscope image of spherical sodium bismuth titanate;

[0021] Figure 2 It is the dielectric constant diagram under different addition amounts;

[0022] Figure 3 It is the dielectric loss diagram under different addition amounts;

[0023] Figure 4 It is the conductivity graph under different addition amounts;

[0024] Figure 5 is the Weibull distribution diagram of breakdown strength at different addition amounts;

[0025] Figure 6 It is the hysteresis loop diagram under different addition amounts;

[0026] Figure 7 It is the energy storage density diagram under different addition amounts. DETAILED DESCRIPTION

[0027] Embodiment 1:

[0028] The sodium bismuth titanate used in this embodiment is prepared by a hydrothermal method using bismuth nitrate pentahydrate as a bismuth source, tetrabutyl titanate as a titanium source, and sodium hydroxide as a sodium source and a mineralizer. The specific steps are as follows:

[0029] S1: Dissolve 0.003 mol of bismuth nitrate pentahydrate and 0.006 mol of tetrabutyl titanate in 15 mL of deionized water and stir evenly.

[0030] S2: Slowly titrate a sodium hydroxide solution with a concentration of 12 mol / L into the mixed solution obtained in step S1, and then place it on a magnetic stirrer and stir for 30 minutes until the precipitation is complete to obtain a hydrothermal reaction precursor.

[0031] S3: The precursor obtained in S2 is transferred to a high-pressure reactor, the filling degree of the high-pressure reactor is maintained at 60%, and the high-pressure reactor is reacted in a vacuum oven at 180° C. for 24 hours.

[0032] S4: After the reaction is completed, the reaction vessel is naturally cooled to room temperature, and then the hydrothermal synthesized product is taken out and repeatedly centrifuged and washed with distilled water until the pH value of the washed solution reaches 7-8, and then the obtained powder is placed in a vacuum drying oven at 80°C and dried for about 24 hours to obtain spherical sodium bismuth titanate powder.

[0033] In this embodiment, the coupling agent-modified sodium bismuth titanate is prepared by ultrasonically stirring spherical sodium bismuth titanate powder in a 95% ethanol solution for 2 hours, then dropping a silane coupling agent KH550 having a mass fraction of 1% of the sodium bismuth titanate at 80° C., heating and stirring for 8 hours, and then repeatedly centrifugally washing with ethanol or deionized water, and drying to obtain the coupling agent-modified sodium bismuth titanate.

[0034] The polyvinylidene fluoride composite material with high dielectric constant, low loss and high breakdown strength is prepared by the following steps:

[0035] Step 1: Dissolve the coupling agent-modified sodium bismuth titanate in 65 mL of N,N-dimethylformamide and stir for 2 h, add 5 g of polyvinylidene fluoride powder, stir for 2 h, and obtain a glue solution. The doping amount of the coupling agent-modified sodium bismuth titanate is 15%, 20%, 25% or 30% of the mass of the polyvinylidene fluoride.

[0036] Step 2: After the bubbles are removed by vacuum evacuation, the adhesive obtained in step 1 is laid on a film laying machine and dried at 80°C for 4 hours. The obtained film is hot-pressed on a flat vulcanizer at a temperature of 180°C and a pressure of 10 MPa for 30 minutes, and the thickness of the obtained composite material is 80 μm.

[0037] The performance effect of this embodiment is as follows Figure 1-Figure 7 shown.

[0038] Depend on Figure 1 It can be seen that the sodium bismuth titanate powder synthesized by the hydrothermal method is a regular spherical particle, and the size can be observed to be 150nm to 200nm, indicating that NBT nanoparticles with high sphericity and good dispersion can be obtained under the reaction conditions.

[0039] Depend on Figure 2 It can be seen that the NBT / PVDF composite material has similar frequency-dependent dielectric properties as pure PVDF membrane, and in the entire test frequency range, with the increase of NBT filling amount, the relative dielectric constant of the NBT / PVDF composite medium gradually increases, especially when the mass fraction of NBT filler is 30wt.%, the dielectric constant of the NBT / PVDF composite material reaches 1.6 times that of pure PVDF. The increase in the relative dielectric constant is due to the Maxwell-Wagner effect between the ceramic powder particles and the polymer matrix as the doping concentration of sodium bismuth titanate powder increases. Therefore, under the action of the external electric field, a large amount of charge will accumulate at the interface between the particles and the matrix and polarization will occur. In addition, it can be seen from the figure that with the increase of frequency, the dielectric constant of the composite medium slowly decreases and then drops rapidly, which is normal for dielectrics. This is because the response frequency range of different polarization modes is different. When the frequency is at a relatively low level, all polarization mechanisms are involved. With the increase of frequency, the interface polarization cannot keep up with the change of frequency, resulting in the inability to reverse the dipole moment, thereby causing the dielectric constant of the NBT / PVDF composite material to slowly decrease. As the frequency continues to increase, the rotation speed of some dipoles gradually cannot keep up with the change in frequency, and they lose their effect on the overall polarization of the composite material, causing the dielectric constant of the composite material to drop rapidly.

[0040] Depend on Figure 3 It can be seen that with the increase of frequency, the loss factor of the composite material shows a change pattern of first decreasing and then increasing, showing the typical low-frequency Maxwell-Wagner (MW) and high-frequency phase relaxation characteristics of polymer composites, which corresponds to the low-frequency and high-frequency changes in the relationship between the relative dielectric constant and frequency, proving the existence of different relaxation polarization processes, and the dielectric loss of the overall NBT / PVDF composite material is maintained at a low level, especially at a frequency of 10 2 Hz-10 4 In the Hz range, the dielectric loss of all composite materials is less than 0.027, showing stability with frequency, which will enhance their applicability in electronic products.

[0041] Depend on Figure 4It can be seen that the conductivity is highly dependent on the frequency of the electric field. In the entire frequency range, the conductivity of the composite medium increases with the increase of frequency. It can also be seen that with the increase of the filler amount, the conductivity of the composite material increases. At a frequency of 100 Hz, the conductivity of 30 wt.% filled NBT / PVDF is about 2.47×10 -11 S / cm, although slightly higher than that of pure PVDF (1.08×10 -11 S / cm, but it still remains at a low order of magnitude, indicating that the composite material has good insulation properties.

[0042] Depend on Figure 5 It can be seen that with the increase of filling amount, the breakdown field strength of the composite material shows a trend of gradually decreasing. When the addition amount is 15wt.%, the breakdown field strength of the NBT / PVDF composite medium decreases slowly. This may be because the NBT particles with a small filling amount are more evenly dispersed in the PVDF matrix and have good interface compatibility, so the breakdown field strength of the composite medium decreases slowly; however, as the NBT content in the composite medium further increases, E b The value decreases faster. This may be because as the number of ceramic particles increases, the distance between the particles becomes smaller, which makes it easy for the inorganic filler phase to agglomerate, and the contact probability of the conductive phase increases, so it is easy to form a conductive path inside the composite material. At the same time, the shape parameter β value in the Weibull distribution diagram is high, indicating that the data obeys the Weibull distribution and the data distribution is relatively concentrated.

[0043] Depend on Figure 6 It can be seen that under the same electric field, the composite membrane has a higher maximum potential transfer than the pure PVDF membrane. When the mass fraction of the filler increases, the maximum polarization value of the composite membrane increases, but the residual polarization also increases. When the filler content is 0wt.%, 15wt.%, 20wt.%, 25wt.% and 30wt.%, the maximum potential shift of the composite medium is about 2.26μC / cm 2 , 3.51μC / cm2, 3.49μC / cm 2 、3.69μC / cm 2 、3.16μC / cm 2 .according to Figure 6 Based on the DE curve data in , the relationship between the energy storage density and electric field strength of composite materials with different filler contents at a frequency of 100Hz was calculated. Figure 7 It can be seen that with the increase of filling amount, the energy storage density of the composite material increases first and then decreases. Under the electric field strength of 220KV / mm, the maximum energy storage density of 15wt.%NBT / PVDF is about 2.58J / cm 3, which is 23.4% higher than pure PVDF. However, as the filler mass fraction continues to increase, the energy storage efficiency of the film decreases. This phenomenon is caused by the increase in structural defects and conductive losses in the composite film caused by the increase in filler content. Therefore, a lower filler addition is more beneficial to improving the energy storage density of PVDF composite membranes.

Claims

1. A polyvinylidene fluoride based composite material with high dielectric, low loss and high breakdown strength, It is characterized in that The doped phase of the composite material is nano-sodium bismuth titanate modified with silane coupling agent KH550, the morphology of the nano-sodium bismuth titanate is a regular sphere, and polyvinylidene fluoride is used as a matrix; the diameter of the nano-sodium bismuth titanate is 150nm-200nm; the nano-sodium bismuth titanate is prepared according to the following steps: S1: Dissolve 0.003 mol of bismuth nitrate pentahydrate and 0.006 mol of tetrabutyl titanate in 15 mL of deionized water and stir evenly; S2: Slowly titrate a 12 mol / L sodium hydroxide solution into the mixed solution obtained in step S1, and then stir the mixture on a magnetic stirrer for 30 min until the precipitation is complete to obtain a hydrothermal reaction precursor; S3: The precursor obtained in S2 is transferred to an autoclave, the filling degree in the autoclave is maintained at 60%, and the autoclave is reacted in a vacuum oven at 180° C. for 24 h; S4: After the reaction is completed, the reaction vessel is naturally cooled to room temperature, and then the hydrothermal synthesized product is taken out and repeatedly centrifuged and washed with distilled water until the pH value of the washed solution reaches 7-8, and then the obtained powder is placed in a vacuum drying oven at 80° C. and dried for 24 hours to obtain spherical sodium bismuth titanate powder; The content of the doped phase is 15%-30% of the mass of the polyvinylidene fluoride.

2. The composite material according to claim 1, It is characterized in that The doping phase is prepared by ultrasonically stirring nano-sodium bismuth titanate for 2 hours in an ethanol solution with a volume concentration of 95%, then dropping a silane coupling agent at 50° C.-80° C., heating and stirring for 6 hours-8 hours, and then repeatedly washing with ethanol or deionized water and drying to obtain sodium bismuth titanate modified with a silane coupling agent. The amount of the silane coupling agent used is 1%-3% of the mass fraction of the nano-sodium bismuth titanate.

3. A method for preparing a composite material according to claim 1 or 2, Features The preparation method is carried out according to the following steps: step 1, adding nano-sodium bismuth titanate modified by silane coupling agent into N,N-dimethylformamide, ultrasonically stirring for 2 hours, adding polyvinylidene fluoride powder, ultrasonically stirring and reacting for 2 hours to obtain a glue solution; step 2, laying a film on a film laying machine and drying; step 3, hot pressing the obtained film on a flat vulcanizer to obtain the composite material.

4. The preparation method according to claim 3, Features Step 2: Dry at 80°C for 2h.

5. The preparation method according to claim 3, Features In step 3, hot pressing is performed at a temperature of 160-190° C. and a pressure of 10 MPa for 30 minutes.

6. The composite material according to claim 1 or 2 or the composite material prepared by the method according to any one of claims 3 to 5 is used for making capacitors and energy storage devices.