A catalyst carrier prepared using natural clay mineral as raw material and a preparation method thereof
By using natural nanoclay minerals, white carbon black and silicon carbide powder and combining pore-forming agents and sintering processes, a catalyst carrier with high porosity and good mechanical strength is prepared, which solves the difficulty of supporting performance in the existing technology to meet the diversity of diversity. The issue of demand has achieved the demand of the chemical and environmental protection industries.
Patent Information
- Application Number
- CN202111012584.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-31
AI Technical Summary
When using natural raw materials, existing catalyst carriers are difficult to meet the requirements of high porosity, mechanical strength and appropriate specific surface area at the same time, and cannot meet the diversified needs of the chemical and environmental protection industries for catalyst carriers.
Natural nanoclay minerals, white carbon black and silicon carbide powder are used as the main raw materials, and combustible pore-making agent is added through specific ratios and processes, and ball milling and sintering processes are used to prepare high porosity, reasonable pore size and good mechanical strength. catalyst support.
The catalyst carrier with high porosity, reasonable pore size and good mechanical strength is achieved, which meets the diversified requirements of the chemical and environmental protection industries for catalyst carriers, reduces manufacturing costs, and improves the performance of the carrier.
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst carrier, and in particular to a catalyst carrier prepared with natural clay mineral as raw material and a preparation method thereof. Background Art
[0002] Catalysis is an important technology that affects our daily lives in many ways. Hydrogenation, oxidation, as well as dehydrogenation, cracking, reforming and other catalytic processes play a vital role in the preparation of important chemicals and intermediates in the current chemical industry. More than 90% of chemical manufacturing is based on or relies on catalytic processes. It is estimated that catalytic reactions account for about 35% of the world's gross domestic product (GDP), and the demand for catalysts has reached $19.5 billion in 2016, and the value of catalysts will be higher in 2021. Among many catalytic reactions, hydrogenation and oxidation play a key role in the current chemical industry. Catalytic hydrogenation, especially the hydrogenation products of olefins, alkynes, aromatics, aldehydes, ketones, esters, carboxylic acids, nitro, nitriles and imines, has attracted great interest as the key to the synthesis and production of petrochemicals and fine chemicals. Oxidation is the second largest process after polymerization, accounting for about 30% of the total output of the chemical industry. A large number of key chemicals and intermediates such as alcohols, aldehydes, ketones, acids and epoxides can be produced by selective oxidation. The increasingly developed nanoparticles (NPs) highly active catalysts have brought a new revolution in the field of catalysis. However, although nanoparticles can provide highly active centers, they are very small in size and thermodynamically unstable. Therefore, nanoparticles are prone to aggregation during the catalytic process and will be poisoned during the reaction, resulting in deactivation and reduced reusability. Highly dispersing nanoparticles and uniformly mixing them with other raw materials and pore-forming agents, and then loading them on a suitable carrier is one of the most effective ways to solve the above problems. Therefore, supported catalysts are widely used in industrial hydrogenation and oxidation reactions. They have good catalytic performance and are easy to separate and recover. Factors that affect the catalytic performance of supported catalysts include: particle size, composition, surface morphology and structure of the catalyst, the properties of the carrier, and the interaction between the nanoparticles and the carrier. By regulating these parameters, the catalytic performance of supported catalysts can be enhanced. However, the design and preparation of catalysts that can simultaneously meet the requirements of high catalytic activity, selectivity and stability remains a long-standing problem for heterogeneous catalysts.
[0003] The catalyst carrier, also known as the support, is one of the components of the supported catalyst. It is the skeleton of the active components of the catalyst, supporting the active components so that the active components can be dispersed, and at the same time it can also increase the strength of the catalyst.
[0004] Natural raw materials are used to replace part of traditional industrial raw materials to save energy, reduce emissions and lower manufacturing costs. However, direct use of natural raw materials will result in carriers with low porosity, insufficient specific surface area and average mechanical strength, which cannot meet diverse requirements. Summary of the invention
[0005] The purpose of the present invention is to provide a catalyst carrier prepared with natural clay minerals as raw materials and a preparation method thereof. The catalyst carrier uses natural raw materials to replace a part of traditional industrial raw materials, and the obtained carrier has high porosity, reasonable pore size, good mechanical strength, and appropriate specific surface area, which meets the diversified requirements of the chemical and environmental protection industries for catalyst carriers.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A catalyst carrier prepared with natural clay mineral as raw material, the carrier comprises natural nano clay mineral, white carbon black and silicon carbide micro powder, and the natural nano clay mineral contains nano particles.
[0008] Preferably, the natural nano clay mineral is one or more of ball clay, bentonite, attapulgite clay and sepiolite clay.
[0009] Preferably, the white carbon black comprises one or both of fumed white carbon black and precipitated white carbon black, and the fumed white carbon black preferably has a specific surface area of 200 to 300 m 2 / g type, the preferred specific surface area of precipitated white carbon is 150-200m 2 / g type
[0010] A method for preparing a catalyst carrier using natural clay minerals as raw materials comprises: mixing natural nanometer clay minerals, white carbon black and silicon carbide micropowder to obtain a primary mixture, adding 0.2-0.4% of ammonium polyacrylate by weight of the primary mixture, adding water in a ball mill, crushing and mixing for 3-4 hours, then adding a combustible pore-forming agent, mixing for 60 minutes before exiting the mill, removing water to form a powder or a mud paste, respectively forming the powder or the mud paste by a rolling granulation process, a hydraulic dry process or a wet plastic extrusion process to form a spherical shape or a Raschig ring shape, and drying the powder and calcining the powder in a kiln at 850-900°C for 2-5 hours.
[0011] Preferably, the premix contains 44-71% natural nano clay minerals, 24-42% white carbon black, and 4-15% silicon carbide powder; and a combustible pore-forming agent is added, and the mass of the combustible pore-forming agent is 5-55% of the premix.
[0012] Preferably, the premix contains 54-70% natural nano clay minerals, 24-42% white carbon black, 4-15% silicon carbide powder, and an additional combustible pore-forming agent, the mass of which accounts for 21-55% of the premix.
[0013] Preferably, the combustible pore-forming agent includes one or more of coke powder, anthracite powder, charcoal powder, flour, rice flour, bran powder, walnut shell powder, starch, wood fiber, polyvinyl alcohol, and methyl cellulose.
[0014] As far as the carrier manufacturing industry is concerned, the use of industrial products such as aluminum hydroxide, pseudo-boehmite, gamma alumina, silica gel, molecular sieves, activated carbon, titanium dioxide, etc. to manufacture carriers still has the disadvantages of high prices and high costs. This patent creatively directly uses natural clay minerals containing nanoparticles (including ball clay, bentonite, attapulgite clay, sepiolite clay) as molding binders, sintering aids and main raw materials, which can solve the above problems to a certain extent, is conducive to the comprehensive utilization and sustainable development of resources, and also helps carrier manufacturing companies reduce costs and improve benefits.
[0015] Alumina, silica, and molecular sieve carriers usually use nanomaterials as sintering aids. For example, the activated alumina carrier uses pseudo-boehmite dissolved in nitric acid to become sol, a liquid nano-alumina material. The high sintering activity of this nano-material is used as a sintering aid (alumina sol can also act as a molding binder) to ensure and improve the mechanical strength of the alumina carrier. For another example, the silica gel carrier uses a certain concentration of silica sol, a liquid nano-silicon dioxide, as a sintering aid to improve the compressive strength of the silica gel carrier (silica sol can also act as a molding binder). Molecular sieve carriers used to mainly use kaolin powder as a molding binder and sintering aid. Generally, 5-10% kaolin is added to the molecular sieve powder. Due to the high refractory point of kaolin, the strength of the molecular sieve carrier made in this way is not high. In practice, we have found that ball clay has a high sintering strength at 700-800°C and is widely used in fixed and unfixed refractory materials. Bentonite begins to have a high strength when calcined at 600°C. When ball clay and bentonite are heated to below 925℃, amorphous metakaolinite (Al2O3·2SiO2) and amorphous SiO2 are generated, both of which have catalytic activity. However, when bentonite and ball clay are heated to above 925℃, aluminum silicon spinel crystals are generated, and at 1050℃, mullite crystals and quartz crystals are generated, which will significantly reduce the activity and specific surface area of the materials. In addition, some scholars have found that when kaolin, ball clay, and bentonite are heated to 950℃, γ-Al2O3 and amorphous SiO2 are generated, both of which are active and are the main materials for preparing carriers. Only at 1100℃, mullite crystals are generated (reference: "Ceramic Technology" compiled by South China Institute of Technology, Nanjing Institute of Chemical Technology, and Wuhan Institute of Building Materials, published by China Building Industry Press in 1981, page 168), at which time the activity begins to decline. This patent uses the above-mentioned natural clay mineral containing nanoparticles as the main raw material and sintering at below 900°C to achieve the effect of improving the carrier strength and ensuring catalytic activity. Since this system is solid-phase sintering and no flux is used, no melt (glass phase) will be produced during sintering, so as not to block the pores, ensuring that the carrier pore volume (porosity) and strength are both achieved, and to a certain extent solving the problem that the porosity and mechanical strength of porous materials are difficult to improve simultaneously.
[0016] The pore volume and specific surface area of the catalyst carrier are important indicators of catalyst performance. The unit of measurement for specific surface area is the internal or external surface area of 1g of catalyst or catalyst carrier. Porous solid particles have a large internal surface area, and these internal surfaces are hidden in the pores of the particles. If they are fine pores, although the surface area is large, when used as a catalyst carrier, it will hinder the diffusion of reactant molecules into the pores and affect the reaction. In this way, not all surfaces play a catalytic role. Therefore, the specific surface area is not the larger the better, but it should be combined with indicators such as pore volume, and can be adjusted and set manually according to needs.
[0017] Due to the solid phase sintering during the calcination of nano mineral materials, the specific surface area of the carrier is reduced, and the adaptability is not wide. However, both fumed silica and precipitated silica have extremely high specific surface areas. For example, the specific surface area of fumed silica can reach 200-400m 2 / g, the particles are mostly in the size of dozens of nanometers, and the specific surface area of precipitated white carbon black is also 100-200m 2 / g (the original particle size is also tens of nanometers, but they are all aggregated into micron-sized particles, which can be dispersed by mechanical methods such as ball milling), so it can be used to adjust the specific surface area of the carrier. At the same time, using combustibles of corresponding particle size and quantity (including coke powder, anthracite powder, charcoal powder, flour, rice flour, bran powder, walnut shell powder, starch, wood fiber, polyvinyl alcohol) as pore-forming agents can control the pore volume, apparent porosity (water absorption rate) and pore size of the carrier, and even produce through-hole carriers; appropriately adding silicon carbide to improve the thermal conductivity and heat resistance of the carrier, thereby preparing aluminum silicate catalyst carriers with adjustable specific surface area, pore volume, etc., to meet the diverse objective needs of the chemical industry and environmental protection fields.
[0018] Beneficial Effects
[0019] The present invention uses natural nano-minerals containing nano-particles to replace some traditional industrial raw materials, including aluminum hydroxide, activated alumina, silica gel powder, etc., to achieve energy conservation and emission reduction and reduce manufacturing costs. At the same time, pore-forming agents are added to adjust the pore size distribution and pore volume, and white carbon black is added to adjust the specific surface area of the carrier. In this way, a carrier with high porosity, reasonable pore size, good mechanical strength and appropriate specific surface area is manufactured to meet the diverse requirements of the chemical and environmental protection industries for catalyst carriers. DETAILED DESCRIPTION
[0020] In order to highlight the implementation purpose, technical solutions and structural advantages of the present invention, the following is a detailed description of the technical solutions in the examples of the present invention. The examples described are part of the examples of the present invention, but not all of the examples. Based on the examples in the present invention, all other examples obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Example 1: 44wt% of Jilin ball clay, 4.5wt% of Guangxi ball clay, 7.5wt% of Liuyang sepiolite, 11wt% of fumed silica, 24wt% of precipitated silica, and 9% of silicon carbide powder were prepared, and 0.2% of ammonium polyacrylate was added. After adding water and wet grinding and mixing in a ball mill for 3-4 hours, 31% of 120-mesh Henan walnut shell powder was added. After mixing for 30 minutes, the mixture was removed from the mill and the water was removed to form a powder. The powder was formed by rolling granulation to form spherical particles with a diameter of 4-5mm. After drying, the particles were calcined in a kiln at 900°C for 5 hours to obtain a carrier. The specific surface area and pore size of the carrier were detected by a Bester specific surface and pore size analyzer 3H-2000PS2. The specific surface area was 44m 2 / g, total pore volume 0.356mL / g, average pore diameter (4V / A by BET, the same below) 30.73nm; the compressive strength of the carrier is greater than 2.4kg / particle.
[0022] Example 2: 54 wt% of Jilin ball clay, 5 wt% of Guangxi ball clay, 4 wt% of fumed silica, 25 wt% of precipitated silica, and 12% of 600 mesh silicon carbide were prepared, and 0.2% of ammonium polyacrylate was added. After adding water and wet grinding and mixing in a ball mill for 3 to 4 hours, 55% of 80 mesh coke powder was added, and mixed for 60 minutes before being milled. After removing the water, the powder was made into a powder, and the powder was formed by rolling granulation to form spherical particles with a diameter of 4 to 5 mm. After drying, the carrier was calcined at 900° C. in a kiln for 5 hours to obtain the carrier. The specific surface area and pore size of the carrier were detected by the Bester specific surface and pore size analyzer 3H-2000PS2, and the specific surface area was 19 m 2 / g, total pore volume 0.361mL / g, average pore diameter 38.87nm; the compressive strength of the carrier is greater than 2.2kg / particle.
[0023] Example 3: According to the proportion of 25wt% Jilin ball clay, 24wt% Anhui attapulgite clay, 8wt% Guangxi ball clay, 5wt% 200-mesh sepiolite, 20wt% precipitated silica, 13wt% fumed silica, and 5% 600-mesh silicon carbide, 0.2% ammonium polyacrylate was added, and after wet grinding and mixing in a ball mill for 3-4 hours, 27% 60-mesh rice bran powder was added, and mixed for 60 minutes. After removing the water, it was made into a powder, and the powder was formed by rolling granulation to form spherical particles with a diameter of 4-5mm. After drying, it was calcined in a kiln at 890°C for 4 hours to obtain a carrier. The specific surface area and pore size of the carrier were detected by the Bester specific surface and pore size analyzer 3H-2000PS2, and the specific surface area was 36m 2 / g, total pore volume 0.31mL / g, average pore diameter 28.77nm; the compressive strength of the carrier is greater than 2.7kg / particle.
[0024] Example 4 The ingredients were prepared according to the ratio of 9wt% Jilin ball clay, 34wt% Anhui attapulgite clay, 6wt% Guangxi ball clay, 5wt% Zhejiang natural sodium bentonite, 4wt% fumed silica, 27wt% precipitated silica, and 15% 600 mesh silicon carbide. After pulverizing and mixing in a ball mill for 3 to 4 hours, 3% polyvinyl alcohol between 30 and 60 mesh, 1% methyl cellulose, and 21% anthracite powder were added. After mixing for 30 minutes, the mixture was discharged from the mill, filtered to remove water, and then made into a mud material. The mixture was extruded into Raschig rings with an outer diameter of 10mm and an inner diameter of 4mm by a vacuum mud kneading machine, and then cut into 10mm high rings. After drying, the mixture was calcined at 900°C in a kiln for 5 hours to obtain a carrier. The specific surface area and pore size of the carrier were detected by a Bester specific surface and pore size analyzer 3H-2000PS2. The specific surface area was 26m 2 / g, total pore volume 0.29mL / g, average pore diameter 45.13nm; the compressive strength of the carrier is greater than 2.1kg / cm.
[0025] Example 5: 39 wt% of Jilin ball clay, 15 wt% of Jiangsu attapulgite clay, 12 wt% of precipitated silica, 30 wt% of fumed silica, and 4% of silicon carbide were prepared, and 0.2% of ammonium polyacrylate was added. After wet grinding and mixing in a ball mill for 3 to 4 hours, 21% of 80-mesh sawdust powder was added. After mixing for 60 minutes, the mixture was removed from the mill and made into a powder. The powder was formed by rolling granulation to form spherical particles with a diameter of 4 to 5 mm. After drying, the particles were calcined in a kiln at 890° C. for 5 hours to obtain a carrier. The specific surface area and pore size of the carrier were detected by a Bester specific surface and pore size analyzer 3H-2000PS2. The specific surface area was 51 m 2 / g, total pore volume 0.41mL / g, average pore diameter 27.13nm; the compressive strength of the carrier is greater than 2.0kg / particle.
[0026] Example 6: 42 wt% of Jilin ball clay, 10 wt% of Guangxi ball clay, 14 wt% of Jiangsu attapulgite clay, 24 wt% of precipitated silica, 4 wt% of fumed silica, and 6% of silicon carbide were prepared, and 0.2% of ammonium polyacrylate was added. After adding water and wet grinding and mixing in a ball mill for 3 to 4 hours, the mixture was taken out of the mill and spray dried to remove moisture to form a powder. Then, 23% of 120 mesh charcoal powder and 0.5% of calcium stearate were mixed for 60 minutes, and then pressed with a hydraulic press to form a Raschig ring with an outer diameter of 8 mm, an inner diameter of 4 mm, and a height of 8 mm. After drying, the mixture was calcined in a kiln at 880°C for 5 hours to obtain a carrier. The specific surface area and pore size of the carrier were detected by a Bester specific surface and pore size analyzer 3H-2000PS2, and the specific surface area was 21 m 2 / g, total pore volume 0.21mL / g, average pore diameter 35.66nm; the compressive strength of the carrier is greater than 3.6kg / cm.
[0027] Implementation Case 7: 39wt% of Jilin ball clay, 10wt% of Guangxi ball clay, 21wt% of Jiangsu attapulgite clay, 4wt% of precipitated silica, 20wt% of fumed silica, and 6% of silicon carbide were prepared, 0.2% of ammonium polyacrylate was added, and the mixture was wet-ground and mixed in a ball mill for 3 to 4 hours with water, 14wt% of 120-mesh rice husk carbon powder and 19wt% of 120-mesh charcoal powder were added, water was added, and the mixture was ground for 1 hour before being removed from the mill, and the mixture was filtered to remove the water and then made into a product. The mud material was formed by a vacuum mud kneading machine to form a Raschig ring with an outer diameter of 10 mm, an inner diameter of 5 mm, and a height of 10 mm. After drying, it was calcined in a kiln at 870°C for 4 hours to obtain a carrier. The specific surface area and pore size of the carrier were detected by the Bester specific surface and pore size analyzer 3H-2000PS2. The specific surface area was 31m2 / g, the total pore volume was 0.24mL / g, and the average pore diameter was 45.66nm; the radial compressive strength of the carrier was greater than 3.2kg / cm. From the carrier properties in Examples 1-7, it can be seen that the catalyst carrier obtained in this application has high porosity, reasonable pore size, good mechanical strength, and suitable specific surface area, which meets the diversified requirements of the chemical and environmental protection industries for catalyst carriers.
[0028] Finally, it is stated that the above detailed description is only for the implementation scheme of the present invention, and is not a limitation on the scope of the patent of the present invention. It should be pointed out that a person of ordinary skill in the art may make several deformations and modifications within the scope of the concept of the present invention, or make relevant replacements to some of the technical features therein, which all belong to the protection scope of the present invention. The above patent protection scope shall be subject to the attached claims. Finally, it should be explained that the above embodiments are only used to illustrate the technical scheme of the present invention, not to limit it; although the present invention is described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that it is still possible to modify the technical schemes recorded in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein; and these modifications or replacements do not make the essence of the corresponding technical scheme deviate from the spirit and scope of the technical schemes of the embodiments of the present invention.
Claims
1. A catalyst carrier prepared from natural clay minerals, It is characterized in that The carrier is made of natural nano clay mineral, white carbon black and silicon carbide powder as raw materials, and the ingredients are prepared according to the following ratio: 44wt% to 71wt% of natural nano clay mineral, 24wt% to 42wt% of white carbon black, and 4wt% to 15wt% of silicon carbide powder; ammonium polyacrylate is added according to 0.2wt% to 0.4wt% of the total amount of the above raw materials, and a combustible pore-forming agent is added according to 5wt% to 55wt% of the total amount of the above raw materials; the above raw materials are wet ball milled, dehydrated, formed, and dried, and then calcined at 850 to 900° C. for 2 to 5 hours to obtain the carrier; The natural nano clay mineral is one or more of ball clay, bentonite, attapulgite clay, and sepiolite clay; the white carbon black includes one or both of fumed white carbon black and precipitated white carbon black, and the specific surface area of the fumed white carbon black is 200 to 300 m 2 / g, the specific surface area of precipitated white carbon is 150~200m 2 / g.
2. The catalyst carrier according to claim 1, It is characterized in that The combustible pore-forming agent includes one or more of coke powder, anthracite powder, charcoal powder, flour, rice flour, bran powder, walnut shell powder, starch, wood fiber, polyvinyl alcohol, and methyl cellulose.
3. The catalyst carrier according to claim 1, It is characterized in that The preparation method of the catalyst carrier comprises the following steps: mixing natural nano clay mineral, white carbon black and silicon carbide powder to obtain a primary mixture, adding ammonium polyacrylate, adding water in a ball mill, crushing and mixing for 3-4 hours, then adding a combustible pore-forming agent, mixing for 60 minutes and then removing the mixture from the mill, removing the water and making the mixture into a powder or a mud paste, respectively forming the mixture by a rolling granulation process, a hydraulic dry process or a wet plastic extrusion process to form a spherical shape or a Raschig ring shape, drying the mixture and then baking the mixture in a kiln.