Method for manufacturing a piston

By using traditional casting or forging on the upper part of the piston and using the superposition method to manufacture the lower part of the piston, combined with laser melting and finishing technology, the low strength of the existing piston under high thermal mechanical load conditions is solved, and the high strength and lightness of the piston is achieved Quantification, improving heat transfer and cooling effects.

CN113798419BActive Publication Date: 2024-12-03MAHLE INT GMBH
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202110645286.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-17
Filing Date
2021-06-10
Publication Date
2024-12-03
Estimated Expiration
2041-06-10

AI Technical Summary

Technical Problem

The existing pistons have increased fuel consumption and weight due to low strength problems caused by superposition manufacturing under high heat and mechanical load conditions.

Method used

The upper part of the piston is made by traditional casting or forging, the lower part of the piston is made by superposition, and the cooling channel is closed by laser melting or laser sintering, and the annular groove is finished to improve the heat transfer and cooling effect of the piston, while saving material in the lower part of the piston to reduce weight.

Benefits of technology

The high strength of the upper part of the piston under high thermal mechanical load conditions and the lightweight of the lower part of the piston under low thermal mechanical load conditions are achieved, which improves the heat transfer and cooling effect of the piston, and reduces fuel consumption and weight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113798419B_ABST
    Figure CN113798419B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a piston (1) for an internal combustion engine from an upper piston portion (2) and a lower piston portion (3), the method comprising the steps of: manufacturing the upper piston portion (2) by, for example, forging or casting, the upper piston portion (2) having a piston crown (6), at least a portion of an annular portion (12) and an upper portion (7) of a cooling channel (8); manufacturing the lower piston portion (3) by a stacking method and closing the upper portion (7) of the cooling channel (8) arranged in the upper piston portion (2); and finishing the piston (1) including creating at least one annular groove (4) in an annular support (5) for receiving piston rings. The piston (1) manufactured based on the above method has greater strength in the upper piston portion (2) subjected to high thermal and mechanical loads than in the lower piston portion (3) subjected to low thermal and mechanical loads, and allows for greater manufacturing freedom in terms of the shape of the lower piston portion (3).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing a piston for an internal combustion engine from a piston upper part and a piston lower part. The invention also relates to a piston manufactured by the method. Background Art

[0002] WO 2014 / 165734 A1 discloses a method for producing a piston of the type in question, in which a piston lower part having a piston skirt and a piston pin bore boss is cast or forged, and a piston upper part is subsequently produced therefrom by a stack hardening method.

[0003] WO2015 / 134424A1 discloses a method for manufacturing a piston, wherein a piston body having an annular portion, a piston skirt and a cooling channel opening toward a piston top are cast or forged. In a subsequent method step, the cooling channel initially opening toward the piston top is closed by a superposition method.

[0004] WO 2018 / 063863 A1 again discloses a method for manufacturing a piston, in which an initially open cooling channel is closed by a superposition method.

[0005] However, a disadvantage of the known pistons is that, in particular, the regions of the piston which are subject to high thermal and mechanical loads during subsequent operation are produced by the additive process, which can lead to problems in the long term due to the lower strengths that can be achieved by the additive process. To compensate for these disadvantages, the piston is usually designed to be stronger in the additively produced parts, but this leads to an increase in weight and therefore also to an increase in fuel consumption during subsequent operation. Summary of the invention

[0006] The present invention is therefore based on the problem of proposing an improved or at least alternative embodiment for a method for producing a piston which in particular no longer has the disadvantages known from the prior art.

[0007] The invention is based on the following main idea: essentially, the piston is manufactured from a piston upper part (especially a forged or cast piston upper part) and a superimposed piston lower part. The advantage of this process is that, in the case of a superimposed combination, a relatively free shaping can be achieved, which is possible but with great difficulty, if this is done by conventional manufacturing methods, such as casting or forging. In addition, such a method provides the following great advantages: the area of ​​the piston that is subjected to high thermal and mechanical loads (i.e., the piston upper part) is manufactured in a conventional manner (especially casting or forging), while the area subjected to lower loads in the piston lower part is manufactured by a superimposed method. The method according to the invention has the following method steps: First, the piston upper part having a piston crown, at least a part of the annular part and the upper part of the cooling channel is manufactured, for example, in the form of a disk, wherein an annular support can be forged or cast and the material of the piston upper part is firmly embedded therein. Subsequently, the piston lower part is manufactured by a superimposed method, for example by laser melting or laser sintering, and the upper part arranged in the piston upper part is closed, which is closed by the cooling channel. Finally, the piston is subjected to a finishing process including the production of at least one annular groove, in particular in the annular support, for the subsequent reception of the piston ring, wherein such finishing can be accomplished, for example, by turning, grinding, grinding and / or polishing. By means of the method according to the invention, for the first time, the regions of the piston which are subject to high thermal and mechanical loads can be manufactured in a conventional manner, for example by forging or casting, while the regions which are subject to lower thermal and mechanical loads, in this case the piston lower part, can be manufactured by means of a superposition method. A further advantage of the method according to the invention is, for example, that the upper part of the cooling channel can be located in the piston upper part, and the lower part of the cooling channel can also be located in the piston lower part, thereby enabling, for example, a waist shape which is difficult to realize, although possible, to be manufactured by means of salt cores or the like (usually by means of cast cores). Due to the upper part of the initial opening of the cooling channel in the piston upper part, the inner surface of the upper part of the cooling channel can be additionally roughened, thereby resulting in an increase in the surface area and, as a result, enabling a better heat transfer to be achieved. Closing the cooling channels by the additive method also enables the production of different components, such as jet splitters or cooling fins, which can be produced but with great difficulty and significantly improve cooling, if this is done by conventional production methods such as casting cores. In addition, in the additively produced piston lower part, material can be saved in the piston skirt and in the boss area of ​​the less stressed points, as a result of which the piston can be designed to be lighter overall, which is not achievable in this way by conventional casting or forging processes.

[0008] In an advantageous development, the annular support forming the annular groove is forged or cast into the piston upper part. As a result, the annular groove can be made of a material different from that of the piston upper part.

[0009] In an advantageous development of the technical solution according to the invention, the upper part of the cooling channel located in the piston upper part is introduced by forging, casting cores or chip removal. Thus, if the piston upper part is cast, for example, a corresponding casting core, such as a salt core, can be used to form the cooling channel. If the piston upper part is forged, the upper part of the cooling channel located in the piston upper part is forged by a correspondingly shaped forging punch. Of course, a chip removal method is also conceivable, in which the upper part of the cooling channel located in the piston upper part is introduced into the piston upper part after the forging or casting process is completed. In particular, the chip removal method provides the following great advantages: the piston upper part can be pre-manufactured in the form of a disk and only has an inserted annular support, and the introduction of the cooling channel only occurs in a subsequent method step, for example by grinding, grinding or chip removal.

[0010] In an advantageous development of the technical solution according to the invention, the piston upper part is surface turned at least on the side facing the piston lower part before the superimposed production of the piston lower part, that is to say before the piston lower part is superimposedly assembled on the piston upper part. In this context, such surface turning or faceting, and in particular surface grinding, is preferably carried out before the upper part of the cooling channel located in the piston upper part is introduced, until it is introduced after forging or casting. Such a faceted side makes it significantly easier to assemble the piston lower part. In the superimposed assembly of the piston lower part, the piston upper part is turned upside down, so that the superimposed assembly of the piston lower part can be carried out from above. By surface turning, a flat base or joining surface can be produced, so that an AM process (superimposed process) can be carried out on it without problems. In addition, the surface quality can be influenced in a way that is beneficial to the AM process via processing parameters, such as the setting of certain roughness.

[0011] In a further advantageous development of the technical solution according to the invention, the lower part of the cooling channel in the region of the piston lower part has a rougher surface than the upper part of the cooling channel in the piston upper part, which surface is produced by a superposition method. By the superposition production of the piston lower part and the closing of the cooling channel by the superposition method, the inner surface of the cooling channel can be made rougher, as a result of which the surface area itself can be enlarged and the heat transfer and thus the cooling of the piston can be improved. In this case, the closing of the upper part of the cooling channel in the piston upper part by the superposition combination of the piston lower part can optionally entail closing only the cooling channel in the piston upper part or forming a separate part of the cooling channel in the piston lower part. By the superposition process, an almost unlimited choice of cross-sectional shapes of the cooling channel is conceivable, in particular, for example, also waist-shaped cross-sections are conceivable, which can be produced but only with difficulty, if this is done, by salt cores due to the fragility of the salt cores.

[0012] It is convenient if the lower part of the cooling channel in the area of ​​the lower part of the piston has at least one of the following components manufactured by the superposition method: an oil-conducting structure, such as an injection splitter, a ramp, a cooling fin or a compression piece. In general, a good structure can be manufactured by such a superposition process, which can be selected almost arbitrarily with respect to its shape and cannot be turned, forged or manufactured by salt core in terms of geometry. In particular, reference can be made at these points to the possibility of providing more than two cooling channels and connecting cavities at the weak load points in the lower part of the piston, which helps to save mass and thus reduce weight, and makes the operation of an internal combustion engine equipped with such a piston more economical. Such closed cavities can also be arranged in such a way that they behave as heat-conducting obstacles and thus guide heat conduction in a specific direction in the piston. It is thus possible to achieve particularly targeted heat dissipation of such a piston and therefore particularly targeted cooling.

[0013] It is advantageous if the piston top is made of a steel alloy or of an aluminum alloy. For example, the piston top can thus be designed with relatively high strength, for example as an aluminum piston with an embedded annular support. As a result, the areas subject to the greatest mechanical and thermal loads can be embedded with appropriate strength.

[0014] In a further advantageous development of the technical solution according to the invention, the piston lower part is produced by laser melting. Laser melting belongs to the group of beam melting processes and is an additive production method in which the material to be processed, for example metal, in particular aluminum, is applied to the piston upper part in the form of powder in a thin layer and is locally completely remelted by laser radiation. After the remelted material has solidified, it forms a solid material layer. Subsequently, the piston upper part is lowered by the amount of the layer thickness previously applied, and the material to be processed is applied again in the form of powder (for example, aluminum powder). This will continue until all layers have been remelted and the piston lower part has been completely assembled. Cleaning or finishing is then carried out. The great advantage of such laser melting is the inexpensive and high-quality structure of the piston lower part, while at the same time, an almost unlimited choice of shapes and even the formation of cavities can be achieved without problems.

[0015] In a further advantageous embodiment of the solution according to the invention, the piston upper part is cast, in particular by gravity chill casting, wherein the annular support is previously aluminized in an aluminum melt, for example in an aluminum-silicon melt. By such aluminizing, a particularly good connection between the annular support and the base material of the piston upper part can be achieved. This is a great advantage, in particular if the material used for the piston upper part is a ferrous material.

[0016] In a further advantageous embodiment of the technical solution according to the invention, the piston lower part has at least a part of the piston pin bore boss and / or the piston skirt produced by the superposition method. In purely theoretical terms, the piston upper part can therefore have not only the piston crown, at least a part of the ring part and the upper part of the cooling channel, but can also, for example, have a part of the piston skirt or a part of the piston pin bore boss. There is almost no limit to the choice of dividing the piston lower part, which usually has at least a part of the piston skirt and a part of the piston pin bore boss, among the ring part, the cooling channel, the piston pin bore boss and the piston skirt. However, the piston lower part can also have a part of the ring part, in particular the part below the annular support of the ring part. The great advantage therefore lies in the fact that the division of the regions between the piston upper part and the piston lower part can be freely selected and suitable production processes can be adapted on a conventional basis.

[0017] It is advantageous if the cooling channel has a non-rotationally symmetrical shape relative to the piston vertical axis 14 and / or the piston transverse axis. This allows a customized cooling effect to be achieved, for example increased cooling at certain points due to a corresponding cooling channel geometry. The cooling channel can branch or a plurality of cooling channels can be introduced into the piston, which is not achievable by conventional production methods such as forging or casting.

[0018] In an advantageous development according to the invention, provision is made for the piston consisting of the piston upper part and the piston lower part to be subjected to a heat treatment before finishing. This tempering is used for stress reduction. During this process, the hardness decreases and the roughness increases.

[0019] The invention is also based on the main idea of ​​proposing a piston manufactured by the above method. This type of piston provides the following great advantages: the upper part of the piston that absorbs high mechanical and thermal loads has high strength because it is manufactured in a traditional way, for example by traditional forging or casting, while the lower part of the piston that absorbs low thermal and mechanical loads can be manufactured by a superposition method. The superposition manufacturing of the lower part of the piston also provides the following great advantages: the inner surface of the cooling channel located in the lower part of the piston is made rougher and therefore has a larger surface area, and the entire lower part of the piston is also made thinner, thereby making it possible to save weight. Even the cavity can be set without problems, because a plurality of cooling channels or a plurality of cooling channels with complex cross-sectional shapes (for example, waist-shaped, which can be realized, but with great difficulty) are provided, if this is done, by traditional manufacturing methods, such as casting cores. In addition, the manufacture of the cavity makes it possible to guide the outflow of heat in the lower part of the piston.

[0020] Further important features and advantages of the invention will be found in the accompanying drawings and in the associated description of the drawings with reference to the drawings.

[0021] It goes without saying that the features mentioned above and those yet to be explained below can be used not only in the respectively specified combination but also in other combinations or on their own, without departing from the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Preferred exemplary embodiments of the invention are illustrated in the drawings and will be explained in more detail in the following description, wherein the same reference numerals refer to the same or similar or functionally identical components.

[0023] The following drawings are schematic,

[0024] Figure 1 shows a section through a piston produced by the method according to the invention,

[0025] Figure 2 The first method step of the method according to the invention for producing a piston upper part is shown.

[0026] Figure 3 Shown as Figure 2 , but with additional cooling channels,

[0027] Figure 4 The additive method according to the invention for producing a piston lower part on a cast or forged piston upper part is shown. DETAILED DESCRIPTION

[0028] according to Figure 1 , by the method according to the present invention (comparison Figure 2 and Figure 4 ) according to the invention for an internal combustion engine (not shown) has a piston top 2 and a piston bottom 3. At least one annular groove 4 formed or reinforced by an annular support 5 is provided in the piston top 2, for example. In addition, the piston top 2 has a piston top 6 facing the combustion chamber (not shown) and an upper part 7 of the cooling channel 8. For the sake of simplicity, according to Figure 1 The piston crown 6 is depicted in a rectilinear manner, but can of course also have a combustion chamber depression as an alternative.

[0029] The piston lower part 3 usually has at least a portion of a piston skirt 9 for guiding the piston 1 in the cylinder and a piston pin bore boss (not shown in detail) for receiving a piston pin, via which the piston 1 is connected to a connecting rod of the internal combustion engine. Likewise, a lower portion 10 of the cooling channel 8 can be arranged in the piston lower part 3. Figure 1 , the upper part 7 of the cooling channel 8 is located above the dividing plane in the piston upper part 2 , while the lower part 10 is arranged below the dividing plane 11 in the piston lower part 3 .

[0030] Here, the piston upper part 2 is manufactured in a conventional manner, more specifically, for example, by a forging method or a casting method, while according to the invention, the piston lower part 3 is manufactured by an additive method (for example, a laser melting method). This offers the following great advantage: the area that is subject to high mechanical and thermal loads during operation (in this case, the piston upper part 2) can be formed from a harder material, while the piston lower part 3 that is subject to lower thermal and mechanical loads can be manufactured by an additive method.

[0031] Typically, the piston 1 according to the invention is manufactured as follows:

[0032] First, the piston upper part 2 is manufactured, for example by forging or casting, wherein the annular support 5 can be forged or cast into the material 13 of the piston upper part 2. The piston upper part 2 has a piston crown 6 and at least a part of the annular part 12 and an upper part 7 of the cooling channel 8 (see Figure 2 ).

[0033] In this case, the upper part 7 of the cooling channel 8 located above the dividing plane 11 (i.e. in the piston upper part 2) can be produced during forging by a corresponding punching machine or during casting of the piston upper part 2 by a corresponding casting core. As an alternative, it is of course also conceivable to introduce the upper part 7 of the cooling channel 8 located in the piston upper part 2 into the material 13 of the piston upper part 2 by a chip removal method or by grinding or grinding after production (in particular casting or forging of the piston upper part 2). This can be illustrated, for example, in Figure 3 In the method steps shown, Figure 2 The cast or forged upper portion 7 of the piston upper part 2 is shown without the cooling channel 8 appearing therein.

[0034] The piston upper part 2 is then turned over and the piston lower part 3 is manufactured thereon by means of a superposition method (see Figure 4 ), and at the same time, the cooling channel 8 can be closed during the process. In the additive manufacturing method, of course, the cooling channel 8 can be closed directly and horizontally along the subsequent dividing plane 11, or the lower part 10 of the cooling channel 8 is arranged in the piston lower part 3.

[0035] A great advantage of a piston 1 produced in this way is that the region of the piston 1 that is subject to the highest thermal and mechanical loads, namely the piston upper part 2, can be cast or forged from a stronger material, such as an aluminum alloy or a steel alloy, while the piston lower part 3 that is exposed to lower thermal and mechanical loads is produced by an additive process. The additive process offers the following great advantages: In particular, at locations that are subject to low mechanical loads, for example, cavities (not shown) can be produced, by means of which cavities in the piston lower part 3 not only a weight reduction can be achieved, but also a targeted heat dissipation can be achieved, since such cavities serve as heat-conducting barriers.

[0036] Before the piston lower part 3 is produced by stacking, the piston upper part 2 can be turned over, in particular, surface turned at least on the side facing the piston lower part 3 .

[0037] The lower part 10 of the cooling channel 8 in the region of the piston lower part 3 can have a rougher surface than the upper part 7 of the cooling channel 8 in the piston upper part 2, which is produced by the above-mentioned superposition method. Such a rougher surface can only be produced very expensively, if it is produced in this way, for example by casting cores or in the casting process. With such a rough surface, a larger surface area can be achieved and thus an improved heat exchange and improved cooling of the piston 1 can be achieved.

[0038] Furthermore, it is conceivable that the lower part 10 of the cooling channel 8, which is located in the region of the piston lower part 3, has at least one of the following components, which are also manufactured by the additive method: an oil guide structure, such as a jet splitter, a ramp, a cooling fin or a compression piece. By means of such a compression piece, in particular, a plurality of cooling channels 8 (in particular cooling channels 8 separated from each other) can be created, which can only be manufactured with difficulty if this is done by conventional manufacturing methods, such as casting. When casting by casting cores (due to the fragility of salt cores, for example, salt cores are used), this also involves specific cross-sectional shapes, for example, such as kidney-shaped cross-sections of the cooling channel 8, which can only be manufactured with great difficulty if this is done. However, by means of the additive method according to the invention, the above-mentioned components can be manufactured without problems, which provides a major advantage compared to the conventional production of such a piston.

[0039] For example, the piston upper part 2 can be cast, in particular by gravity chill casting, wherein the annular support 5 is previously aluminized in an aluminum melt, for example an aluminum-silicon melt, so that a reliable bond with the material 13 of the piston upper part 2 can be achieved.

[0040] In this case, Figure 1 The depicted dividing plane 11 can of course also be located further up or further down, and the piston lower part 3 can therefore also include a part of the ring section 12 , for example.

[0041] After production of the piston lower part 3 and closing of the upper part 7 of the cooling channel 8 arranged in the piston upper part 2 by the additive process, the piston 1 is finished, for example by turning, grinding and / or polishing, wherein the annular groove 4 is introduced into the annular support 5 .

[0042] according to Figure 2 , similarly as in Figure 4As in the drawing, the subsequent contour of the piston upper part 2 or the piston 1 is illustrated by dashed lines. In the finishing of the piston 1, the dashed lines are therefore removed outside the material and the piston 1 is reduced to its outer contour indicated by the dashed lines. In this step, machining of the piston lower part 3 can of course also be carried out, for example grinding or turning.

[0043] By combining conventional manufacturing methods according to the invention, in particular casting or forging of the piston upper part 2 and superposition of the piston lower part 3, it is possible to create a combined piston 1 according to the invention which has considerable degrees of freedom, in particular in the design of the piston lower part 3. It is also particularly advantageous here that, for example, due to the manufacturing method, the piston lower part 3 produced by the additive method can be thinned in areas that cannot be thinned in the legacy casting or forging processes. These are, for example, the areas of the attachment between the piston pin bore boss and the piston crown (currently solid line), or the piston skirt and the ring part (see monsterm®). In principle, a significant degree of freedom is also obtained in the design (shape, location, position) of the cooling channels.

Claims

1. A method for producing a piston (1) for an internal combustion engine from a piston upper part (2) and a piston lower part (3), It is characterized in that The following steps are involved: The piston upper part (2) is manufactured by forging or casting, and comprises a piston crown (6), at least a part of an annular part (12) and an upper part (7) of a cooling channel (8), The piston lower part (3) is manufactured by an additive method and the upper part (7) arranged in the piston upper part (2) closes the cooling channel (8), wherein, before the additive manufacturing of the piston lower part (3), the piston upper part (2) is surface turned at least on the side facing the piston lower part (3) to form a flat base or a joint surface; the surface turning is performed before the upper part of the cooling channel located in the piston upper part is introduced; the lower part (10) of the cooling channel (8) located in the area of ​​the piston lower part (3) has a surface rougher than the upper part (7) of the cooling channel (8) located in the piston upper part (2), the surface being manufactured by the additive method; The piston (1) is finished, including producing at least one annular groove (4) in the annular support (5) for receiving a piston ring.

2. The method according to claim 1, Features: Forging or casting an annular support (5) into the piston upper part (2) and forming the annular groove (4), and / or The upper part (7) of the cooling channel (8) located in the piston upper part (2) is introduced by forging, core casting or chip removal.

3. The method according to claim 1, Features: The cooling channel (8) has a rotationally non-symmetrical shape relative to the piston vertical axis (14) and / or the piston transverse axis, and / or The cooling channel (8) can be branched, or a plurality of cooling channels (8) can be introduced into the piston (1).

4. The method according to any one of claims 1 to 3, Features: The lower part (10) of the cooling channel (8) in the region of the piston lower part (3) has at least one oil-conducting structure produced by an additive process, the oil-conducting structure being a jet splitter, a ramp, a cooling fin or a compression element.

5. The method according to any one of claims 1 to 3, Features: The piston upper part (2) is made of a steel alloy or an aluminum alloy.

6. The method according to any one of claims 1 to 3, Features: The piston (1) consisting of the piston upper part (2) and the piston lower part (3) is subjected to a heat treatment before finishing.

7. The method according to any one of claims 1 to 3, Features: The piston lower part (3) is produced by laser melting.

8. The method according to any one of claims 1 to 3, Features: The piston upper part (2) is cast, wherein the annular support (5) is previously aluminized in an aluminum melt.

9. The method according to claim 8, Features: The piston upper part (2) is cold cast by gravity.

10. The method according to claim 8, Features: The annular support member (5) is aluminized in aluminum silicon melt in advance.

11. The method according to any one of claims 1 to 3, Features: The piston lower part (3) has at least a portion of a piston pin hole boss and / or a piston skirt (9) manufactured by a superposition method, The piston lower part (3) has at least a portion of the annular portion (12) produced by an additive process.

12. A piston (1) for an internal combustion engine, produced by the method according to any of the preceding claims.

Citation Information

Patent Citations

  • Piston made using additive manufacturing techniques

    WO2014165734A1

  • One-piece piston featuring additive machining produced combustion bowl rim and cooling gallery

    WO2015134424A1

  • Piston ring-belt structural reinforcement via additive machining

    WO2018063863A1

  • Method for producing a piston for an internal combustion engine