A MOF-derived composite absorbing material and its preparation method and application

Through the MOF-derived preparation method, the porous structure and magnetic properties of FeNi-MIL-101 and FeNiC-X composite materials are used to solve the problems of large density and narrow absorption bandwidth of existing wave absorbing materials, and lightweight and efficient electromagnetic wave absorption is achieved Performance improves the attenuation capability of electromagnetic waves.

CN113840528BActive Publication Date: 2024-11-05ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111018699.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-01
Publication Date
2024-11-05
Estimated Expiration
2041-09-01

AI Technical Summary

Technical Problem

The existing composite wave absorbing materials are complex in synthesis, have large density and narrow effective absorption bandwidth, making it difficult to achieve excellent electromagnetic wave absorption performance.

Method used

Using the MOF-derived preparation method, FeNiC-X composite absorbing material is prepared by hydrothermal reaction and calcination of FeNi-MIL-101. The porous structure of MOF and the magnetic properties of metal/metal oxide are used to achieve dielectric loss and magnetic loss. The balance of the material enhances the impedance matching and absorption bandwidth.

Benefits of technology

The prepared FeNiC-X composite absorbing material has a lightweight, porous structure, wide effective absorption bandwidth and strong reflection loss value, which significantly improves the attenuation ability of electromagnetic waves, realizes impedance matching and multiple reflection scattering, and improves the attenuation of electromagnetic waves. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113840528B_ABST
    Figure CN113840528B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a composite wave absorbing material derived from MOF. The present invention has a simple preparation process and low cost, and can realize large-scale mass production. The prepared wave absorbing material has good impedance matching, a wide effective absorption bandwidth, and a strong reflection loss value. The present invention uses MOFs as a template to synthesize an ordered porous wave absorbing material. The magnetic metal, alloy, or metal oxide produced after calcination will bring excellent magnetic loss, which will be beneficial to impedance matching and a wider effective absorption bandwidth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to a MOF-derived composite absorbing material and a preparation method and application thereof. Background Art

[0002] At present, people are increasingly relying on the great convenience brought by electronic products, but it also causes many electromagnetic wave interference problems. Studies have shown that for people who are in an electromagnetic radiation environment for a long time, the central nervous system, reproductive system and immune system will be damaged to varying degrees. In recent years, nanomagnetic metals, alloys or metal oxides have been synthesized one after another. Absorbing materials mainly use the interaction between materials and electromagnetic waves to achieve electromagnetic wave absorption. "Strong, wide, light and thin" is the development goal of absorbing materials. To achieve this goal, researchers have developed various composite structures, such as graphene / alloy composites and carbon nanotube / ferrite composites. However, to achieve the excellent absorption capacity of composites, the following two key scientific problems must be solved: first, understand the growth mechanism of different nanostructures and realize the construction and regulation of nano ordered structures; second, optimize the functional structure design of materials, realize the superposition of multiple losses of electromagnetic waves, expand the absorption bandwidth and increase the reflection loss. Therefore, it is urgent to manufacture new electromagnetic wave absorbers to attenuate or even eliminate the radiation of electromagnetic waves. Summary of the invention

[0003] The present invention provides a method for preparing a composite absorbing material derived from MOF to solve the problems of complex synthesis, high density, and narrow effective absorption bandwidth of composite absorbing materials in the prior art. The preparation process of the present invention is simple, the cost is low, and large-scale mass production can be achieved. The prepared absorbing material has good impedance matching, a wide effective absorption bandwidth, and a strong reflection loss value.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] A MOF-derived composite absorbing material, wherein the MOF-derived composite absorbing material is prepared by the following method:

[0006] (1) Preparation of FeNi-MIL-101:

[0007] Dissolve H2BDC (terephthalic acid) in DMF (N, N-dimethylformamide), stir, add FeCl3·6H2O and Ni(acac)2, mix by ultrasonication, transfer the obtained mixture to a stainless steel autoclave for hydrothermal reaction at 110-130°C (preferably 120°C) for 1-32h (preferably 8h), cool to room temperature, centrifuge to obtain a brown precipitate, wash the brown precipitate with DMF or ethanol, dry overnight to obtain FeNi-MIL-101; the molar ratio of Ni(acac)2, FeCl3·6H2O to H2BDC is 1:1-3:1-3 (preferably 1:2:2);

[0008] (2) Preparation of FeNiC-X composite absorbing materials:

[0009] The FeNi-MIL-101 prepared in step (1) is placed in a tubular furnace, heated to 600-800°C (preferably 700°C) at a rate of 1-10°C / min (preferably 5°C / min) under a protective atmosphere (such as an inert gas or nitrogen, preferably nitrogen), and calcined for 1-4h (preferably 2h) to obtain the MOF-derived composite absorbing material, i.e., a black FeNiC-X composite absorbing material.

[0010] Furthermore, in step (1), the volume of DMF is 0.1 to 0.5 mL / mg (0.1 L / g) based on the mass of H2BDC.

[0011] Preferably, in step (1), the stirring time of dissolving H2BDC in DMF is 10 to 60 minutes.

[0012] Preferably, in step (1), the ultrasonic mixing time is 10 to 60 minutes.

[0013] Preferably, in step (1), the washing is performed 1 to 10 times.

[0014] Preferably, in step (1), the drying is carried out at a temperature of 60 to 80°C.

[0015] A heating rate of 5°C / min is more conducive to maintaining the original microstructure and significantly improving the wave absorption effect.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. Compared with most existing absorber material preparation technologies, the absorber synthesized by the MOF derivative method has light weight, large specific surface area, porous structure, and diverse structure. In particular, by achieving a proper balance between dielectric loss and magnetic loss, effective impedance matching, i.e., a suitable loss tangent value, can be obtained to obtain excellent electromagnetic wave attenuation capability. MOF is an ideal sacrificial precursor for synthesizing highly dispersed metal / metal compound / carbon materials or their composites through a calcination-thermal decomposition strategy. There are many advantages in using MOF as a precursor for preparing absorber materials: 1) the sample preparation is relatively simple and convenient; 2) the pore structure and diameter of MOF can be adjusted; 3) the porous structure of MOF allows other substances in the pores to enter and polymerize; 4) there are a large number of MOFs with different compositions and multiple topological structures, which can be further converted into target MOF derivative materials; 5) the carbon substrate derived from the decomposition of organic ligands can prevent the aggregation of metal / metal compound particles or the collapse of the integrated structure during calcination; 6) MOF-derived materials can maintain the original form of MOF under appropriate conditions. In addition, the present invention uses MOFs as a template to synthesize an ordered porous absorbing material, and the magnetic metal, alloy or metal oxide produced after calcination will bring excellent magnetic loss, which will be beneficial to impedance matching and a wider effective absorption bandwidth.

[0018] 2. The FeNiC-X composite absorbing material prepared by the present invention has a unique microstructure. The hollow spindle structure not only greatly reduces the weight and density, but also can cause multiple reflections and scattering of electromagnetic waves to dissipate energy. In addition, the porous structure also reduces the dielectric constant, so that the material obtains better impedance matching and enhances the attenuation of electromagnetic waves.

[0019] 3. The FeNiC-X composite absorber prepared by the present invention has excellent electromagnetic absorption performance. Through the dielectric loss derived from the conductivity loss and polarization loss and the high magnetic loss generated by the natural resonance and exchange resonance, the reflection loss value of the FeNiC-X composite absorber reaches -62.7

[0020] dB. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the XRD pattern of the FeNiC-X composite absorbing material prepared in Example 1.

[0022] Figure 2 This is the SEM image of the FeNiC-X composite absorbing material prepared in Example 1.

[0023] Figure 3 This is a Raman graph of the FeNiC-X composite absorbing material prepared in Example 1 of the present invention.

[0024] Figure 4This is a reflection loss (RL) curve of the FeNiC-X composite absorbing material prepared in Example 1 of the present invention.

[0025] Figure 5 This is a reflection loss (RL) curve of the FeNiC-X composite absorbing material prepared in Example 2 of the present invention.

[0026] Figure 6 This is a reflection loss (RL) curve of the FeNiC-X composite absorbing material prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0027] To facilitate those skilled in the art to understand the present invention, the specific implementation of the present invention is described below in conjunction with the accompanying drawings. It should be understood that the following text is only used to describe one or several specific implementations of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention.

[0028] XRD (PANalytical X'Pert PRO) analysis was used to determine the physical phase and crystal structure of the absorbing material. The morphology and microstructure of the absorbing material were analyzed by TEM (JEOL JEM-2100). The Raman spectrometer (Raman WITec Alpha300R) system with an excitation wavelength of 532nm was used to measure the graphitization degree of the absorbing material by Raman spectroscopy. The dielectric constant and magnetic permeability of the material in the frequency range of 2-18GHz were measured using a vector network analyzer (Agilent PNA N5234A), and the test step was 0.08GHz. The test sample preparation process is as follows: First, 0.03g of the material to be tested and 0.07g of paraffin were weighed and added to a beaker pre-filled with 2mL of n-hexane. Ultrasonication for 5min was performed to completely dissolve the paraffin in the n-hexane, and the test powder was also evenly dispersed. Then the beaker was placed in a water bath at 70°C, and the n-hexane was evaporated while stirring to obtain a uniform paraffin-coated powder. Finally, the powder is placed in a mold and a certain pressure is applied to press it into a ring-shaped test sample. The outer diameter of the test sample is 7mm and the inner diameter is 3.04mm. The reflection loss caused by the electromagnetic wave entering the absorbing coating can be calculated by the following equation:

[0029]

[0030]

[0031] Where z0 is the free space wave impedance, μ r is the magnetic permeability, ε r is the dielectric constant, f is the frequency of the electromagnetic wave, d is the coating thickness, and c is the speed of light in a vacuum.

[0032] Example 1

[0033] A method for preparing a MOF-derived composite absorbing material comprises the following steps:

[0034] (1): 166 mg (1 mmol) of H2BDC powder was dissolved in 16.6 mL of DMF solution, and then the mixed solution was stirred on a magnetic stirrer at 1000 rpm for 10 min. After stirring, 270 mg (1 mmol) of FeCl3·6H2O and 128 mg (0.5 mmol) of Ni(acac)2 powder were added. After ultrasonic mixing for 20 min, the mixture was transferred to a stainless steel autoclave for hydrothermal reaction at 120 ° C for 12 h. After the hydrothermal reaction was completed, it was cooled to room temperature and centrifuged to obtain a brown precipitate, which was then washed with DMF and ethanol for 6 times. Finally, the brown product was dried in an oven at 70 ° C overnight.

[0035] (2) The FeNi-MIL-101 prepared in step 1 is placed in a tubular furnace and calcined at 700°C at a heating rate of 5°C / min for 2 h in a nitrogen atmosphere. After calcination, a black FeNiC-X composite absorbing material is obtained.

[0036] The FeNiC-X composite absorbing material prepared in Example 1 was subjected to XRD test. The test results are shown in FIG. Figure 1 As shown in the figure, the diffraction peaks indicate that NiFe alloy and NiFe2O4 ferrite have been successfully synthesized. The diffraction peaks at 2θ=35.5, 44.7 and 45.6, 50.7 and 74.9 are respectively directed to NiFe2O4 (JCPDS No.10-0325) and Fe 0.64 Ni 0.36 Alloy (JCPDS No.47-1405).

[0037] The FeNiC-X composite absorbing material prepared in Example 1 was subjected to SEM testing. The test results are shown in FIG. Figure 2 As shown, FeNiC-X is a spindle-shaped composite material with a length of about 2.5 μm and a width of 0.5 μm. Many magnetic nanoparticles are evenly dispersed on the carbon skeleton with an average diameter of about 70 nm. In addition, Figure 1 The cracked samples in the sample confirmed that the calcined sample has a hollow structure. This special structure not only greatly reduces the weight and density, but also can cause multiple reflections and scattering of electromagnetic waves to enhance attenuation.

[0038] The FeNiC-X composite absorbing material prepared in Example 1 was subjected to Raman testing. The test results are shown in FIG. Figure 3 As shown. ~1330cm -1 and ~1590cm -1 The two peaks at 1 and 2 correspond to the D band and G band of carbon, respectively, and the intensity ratio of the D band to the G band (I D / I G ) reveals the degree of graphitization. D / I G The value is 0.78, indicating a high degree of graphitization, which provides the possibility for the attenuation of electromagnetic waves.

[0039] The electromagnetic absorbing performance of the FeNiC-X composite absorbing material prepared in Example 1 is calculated. The reflection loss (RL) curve of the absorber with a thickness of 1.6 to 5.5 mm is as follows: Figure 4 As shown. Effective absorption bandwidth and minimum reflection loss value (RL) are usually used as parameters to evaluate the wave absorption performance of materials. When the RL value is less than -10B, it means that 90% of the electromagnetic wave energy is absorbed, and the bandwidth less than -10dB is called the effective absorption bandwidth. Figure 4 We can see that the FeNiC-X composite absorber exhibits excellent electromagnetic wave absorption performance. At a frequency of 17.6GHz, the RL value reaches -62.7dB and the effective absorption bandwidth reaches 7.5GHz. The excellent electromagnetic wave absorption performance of the material is mainly attributed to the hollow structure, strong dielectric loss and magnetic loss of the material. First, the hollow porous structure not only significantly reduces the weight and density, but also causes multiple reflections and scattering to dissipate energy. In addition, the porous structure significantly reduces the dielectric constant and obtains a better impedance matching value. Second, the presence of a large number of small-sized nanoparticles in the carbon layer causes dipole polarization, resulting in strong dielectric loss. Finally, a large number of NiFe and NiFe2O4 nanoparticles provide high magnetic losses derived from magnetic resonance. Therefore, the FeNiC-X composite absorber has a strong electromagnetic wave attenuation performance.

[0040] Example 2

[0041] A method for preparing a MOF-derived composite absorbing material comprises the following steps:

[0042] (1): 166 mg (1 mmol) of H2BDC powder was dissolved in 16.6 mL of DMF solution, and then the mixed solution was stirred on a magnetic stirrer at 1000 rpm for 10 min. After stirring, 270 mg (1 mmol) of FeCl3·6H2O and 128 mg (0.5 mmol) of Ni(acac)2 powder were added. After ultrasonic mixing for 20 min, the mixture was transferred to a stainless steel autoclave for hydrothermal reaction at 120 ° C for 12 h. After the hydrothermal reaction was completed, it was cooled to room temperature and centrifuged to obtain a brown precipitate, which was then washed with DMF and ethanol for 6 times. Finally, the brown product was dried in an oven at 70 ° C overnight.

[0043] (2): The FeNi-MIL-101 prepared in step 1 is placed in a tubular furnace and calcined at 600°C at a heating rate of 5°C / min for 2 hours in a nitrogen atmosphere. After the calcination, the final black FeNiC-X composite absorbing material is obtained.

[0044] The electromagnetic absorbing performance of the FeNiC-X composite absorbing material prepared in Example 2 is calculated. The reflection loss (RL) curve of the absorber with a thickness of 1.6 to 5.5 mm is as follows: Figure 5 As shown in the figure, compared with the material prepared in Example 1, the overall effective absorption bandwidth of the FeNiC-X material prepared in Example 2 is increased, but the wave absorption performance is slightly reduced, wherein the effective absorption bandwidth of the material is 7.6 GHz, and the minimum reflection loss value is -40.9 dB. This is because the values ​​of the complex dielectric constant and complex magnetic permeability of the composite material are small, resulting in a decrease in the dielectric loss and magnetic loss of the material, thereby causing a decrease in the wave absorption performance.

[0045] Example 3

[0046] A method for preparing a MOF-derived composite absorbing material comprises the following steps:

[0047] (1): 166 mg (1 mmol) of H2BDC powder was dissolved in 16.6 mL of DMF solution, and then the mixed solution was stirred on a magnetic stirrer at 1000 rpm for 10 min. After stirring, 270 mg (1 mmol) of FeCl3·6H2O and 128 mg (0.5 mmol) of Ni(acac)2 powder were added. After ultrasonic mixing for 20 min, the mixture was transferred to a stainless steel autoclave for hydrothermal reaction at 120 ° C for 12 h. After the hydrothermal reaction was completed, it was cooled to room temperature and centrifuged to obtain a brown precipitate, which was then washed 6 times with DMF and ethanol. Finally, the brown product was dried in an oven at 70 ° C overnight.

[0048] (2): The FeNi-MIL-101 prepared in step 1 is placed in a tubular furnace and calcined at 800°C at a heating rate of 5°C / min for 2 hours in a nitrogen atmosphere. After the calcination, the final black FeNiC-X composite absorbing material is obtained.

[0049] The electromagnetic absorbing performance of the FeNiC-X composite absorbing material prepared in Example 3 was calculated. The reflection loss (RL) curve of the absorber with a thickness of 1.6 to 5.5 mm is as follows: Figure 6As shown, compared with the materials prepared in Examples 1 and 2, the overall wave absorption performance of the FeNiC-X material prepared in Example 3 is greatly reduced, the effective absorption bandwidth of the material is 4.6 GHz, and the minimum reflection loss value is -18.6 dB. This is because when the calcination temperature is increased to 800°C, the conductivity of the composite material is enhanced, resulting in material impedance mismatch, causing a large amount of electromagnetic waves to be reflected, and thus reducing the wave absorption performance.

[0050] The above is a detailed description of the implementation mode of the present invention in conjunction with the embodiments, which does not limit the present invention in any form. For those skilled in the art, after knowing the contents recorded in the present invention, they can make several improvements and substitutions without departing from the principle of the present invention, and these equivalent improvements and substitutions should also be regarded as belonging to the protection scope of the present invention.

Claims

1. A MOF-derived composite absorbing material, characterized in that The MOF-derived composite absorbing material is prepared by the following method: (1) Preparation of FeNi-MIL-101: Dissolve H2BDC in DMF, stir, add FeCl3·6H2O and Ni(acac)2, mix by ultrasonic, transfer the obtained mixture to a stainless steel autoclave for hydrothermal reaction at 110-130°C for 1-32h, cool to room temperature, centrifuge to obtain a brown precipitate, wash the brown precipitate with DMF or ethanol, dry overnight to obtain FeNi-MIL-101; the molar ratio of Ni(acac)2, FeCl3·6H2O and H2BDC is 1:1-3:1-3; (2) Preparation of FeNiC-X composite absorbing materials: The FeNi-MIL-101 prepared in step (1) is placed in a tubular furnace, heated to 600-800° C. at a rate of 1-10° C. / min under a protective atmosphere, and calcined for 1-4 hours to obtain the MOF-derived composite absorbing material; the protective atmosphere is an inert gas or nitrogen.

2. The MOF-derived composite absorbing material according to claim 1, characterized in that: In step (1), the volume of DMF is 0.1-0.5 mL / mg based on the mass of H2BDC powder.

3. The MOF-derived composite absorbing material according to claim 1, characterized in that: In step (1), the stirring time of the H2BDC dissolved in DMF is 10 to 60 minutes.

4. The MOF-derived composite absorbing material according to claim 1, characterized in that: In step (1), the ultrasonic mixing time is 10 to 60 minutes.

5. The MOF-derived composite absorbing material according to claim 1, characterized in that: In step (1), the washing is performed 1 to 10 times.

6. The MOF-derived composite absorbing material according to claim 1, characterized in that: In step (1), the drying is carried out at a temperature of 60 to 80°C.

7. The MOF-derived composite absorbing material according to claim 1, characterized in that: In step (1), the temperature of the hydrothermal reaction is 120° C. and the time is 8 hours.

8. The MOF-derived composite absorbing material according to claim 1, characterized in that: In step (1), the molar ratio of Ni(acac)2, FeCl3·6H2O and H2BDC is 1:2:

2.

9. The MOF-derived composite absorbing material according to claim 1, characterized in that: The heating rate in step (2) is 5°C / min.

10. The MOF-derived composite absorbing material according to claim 1, characterized in that: The calcination temperature in step (2) is 700°C.