Method for manufacturing single crystal silicon wafer and single crystal silicon wafer
Patent Information
- Application Number
- CN202080028464.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-02-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-02-05
AI Technical Summary
然而,若以高浓度掺杂氮、碳、硼,则会于表层形成氧析出物,存在电特性发生恶化的问题
[0028] As described above, according to the manufacturing method of a single crystal silicon wafer of the present invention, a single crystal silicon wafer suitable for a multi-layer structure device can be manufactured, which can improve the strength of the device formation region and suppress dislocations in the surface layer The production and elongation. In addition, the single crystal silicon wafer according to the present invention is a single crystal silicon wafer suitable for multi-layer structure devices, which can improve the strength of the device formation area and suppress the generation and elongation of dislocations in the surface layer. .
Smart Images

Figure CN113906171B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a single crystal silicon wafer suitable for a multi-layer structure device and the single crystal silicon wafer. Background Art
[0002] The latest memory (3D Xpoint) requires higher strength of the silicon substrate in the device area (range of about 0.5 μm in depth from the surface) and improved strength of the substrate surface layer formed by stacking 3D NAND.
[0003] Usually, nitrogen, carbon, and boron are doped into single crystal silicon for the purpose of imparting gettering properties and improving the strength of the surface body. However, if nitrogen, carbon, and boron are doped at high concentrations, oxygen precipitates will be formed on the surface layer, and there is a problem of deterioration of electrical properties. In response to this problem, a countermeasure is taken to diffuse impurities outward through heat treatment. At this time, a DZ layer is formed on the surface layer. The DZ layer becomes hypoxic due to the outward diffusion of oxygen, and is prone to slip due to the stress received when forming the device.
[0004] Furthermore, Patent Documents 1, 2, and 3 disclose techniques for controlling BMD density so as not to excessively form oxygen precipitates, and Patent Document 4 discloses a single crystal wafer that is in contact with a defect-free region and has close-range gettering performance.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-100542
[0008] Patent Document 2: Japanese Patent No. 4055343
[0009] Patent Document 3: Japanese Patent No. 4794137
[0010] Patent Document 4: Japanese Patent Application Publication No. 2015-216375
[0011] Patent Document 5: Japanese Patent Application Publication No. 2016-111044 Summary of the invention
[0012] Technical Problems to be Solved by the Invention
[0013] However, even with the single crystal wafer described in Patent Documents 1 to 4, there is still the problem of slippage in the device formation area when a multi-layer structure device is formed on the single crystal wafer, so a single crystal silicon wafer is sought that will not slip in the device formation area even when a multi-layer structure device is formed.
[0014] The present invention is completed in order to solve the above-mentioned problems, and its purpose is to provide a manufacturing method and a single crystal silicon wafer suitable for multi-layer structure devices. The single crystal silicon wafer can use the BMD layer just below the surface part to absorb defects caused by strain caused by the stress on the surface of the silicon wafer when forming the device, thereby improving the strength of the device formation area and suppressing the generation and elongation of dislocations in the surface layer.
[0015] Technical means to solve technical problems
[0016] The present invention is completed in order to achieve the above-mentioned object, and provides a method for manufacturing a single crystal silicon wafer, which is a method for manufacturing a single crystal silicon wafer suitable for a multilayer structure device, wherein N having an oxygen concentration of 12 ppma (JEITA) or more is used. V A single crystal silicon wafer having a thickness of at least 5 to 12.5 μm and a BMD density of 1×10 11 / cm 3 The BMD layer above the single crystal silicon wafer.
[0017] By using this method for manufacturing a single crystal silicon wafer, a single crystal silicon wafer suitable for a multi-layer structure device can be obtained, which can improve the strength of the device forming area and inhibit the generation and elongation of dislocations in the surface layer.
[0018] In this case, the RTA treatment can be performed under heat treatment conditions of less than 10 seconds and a temperature drop rate of 30° C. / second or more.
[0019] This can enhance the effect of suppressing the outward diffusion of vacancies, make the vacancy distribution in the depth direction steeper, and obtain a steeper BMD density distribution.
[0020] At this time, the BMD forming heat treatment may be performed under heat treatment conditions of an argon atmosphere at a temperature of 870 to 950° C. for 2 hours or more.
[0021] This allows the precipitation nuclei to grow only to a certain extent in size, and thus allows the BMD distribution to be made steeper.
[0022] The present invention is completed in order to achieve the above-mentioned purpose, and provides a single crystal silicon wafer, which is a single crystal silicon wafer suitable for multi-layer structure devices, and the single crystal silicon wafer is N V The single crystal silicon wafer of the region comprises at least a DZ layer and a BMD layer located directly below the DZ layer in sequence from the surface of the single crystal silicon wafer, wherein the thickness of the DZ layer is 5 to 12.5 μm, and the BMD density of the BMD layer is 1×10 11 / cm3 above.
[0023] This single crystal silicon wafer is suitable for multi-layer structure devices, which can improve the strength of the device formation area and inhibit the generation and extension of dislocations in the surface layer.
[0024] At this time, to satisfy the relationship Depth = 3 × Fz 0.6 When a pressing pressure Fz is applied to form an indentation with an indentation depth Depth on the surface of the single crystal silicon wafer in a manner, the single crystal silicon wafer is a stacked structure having at least three layers of a strained layer, a DZ layer, and a BMD layer in sequence from the surface, wherein Depth is the indentation depth (unit: μm), Fz is the pressing pressure (unit: N), and is set to Depth=0.01 μm or more and less than 5.00 μm,
[0025] When the single crystal silicon wafer having the indentation formed therein is subjected to a heat treatment at a temperature of 900° C. for 1 hour, a rosette length of a dislocation in the DZ layer after the heat treatment is shorter than a rosette length of a dislocation in the DZ layer before the heat treatment.
[0026] This further improves the performance of suppressing the extension of dislocations.
[0027] Effects of the Invention
[0028] As described above, according to the method for manufacturing a single crystal silicon wafer of the present invention, a single crystal silicon wafer suitable for a multi-layer structure device can be manufactured, which can improve the strength of the device formation area and suppress the generation and elongation of dislocations in the surface layer. In addition, according to the single crystal silicon wafer of the present invention, it is a single crystal silicon wafer suitable for a multi-layer structure device, which can improve the strength of the device formation area and suppress the generation and elongation of dislocations in the surface layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The single crystal silicon wafer of the present invention is shown.
[0030] Figure 2 An explanatory diagram of the Rost test is shown.
[0031] Figure 3 The relationship between the DZ layer thickness, BMD density, and the difference in Rost length is shown.
[0032] Figure 4 A cross-sectional observation photograph of a single crystal silicon wafer of the present invention is shown.
[0033] Figure 5 The relationship among the DZ layer thickness, BMD density, and Rost difference of Example 2 and Comparative Example 2 is shown.
[0034] Figure 6 The relationship among the DZ layer thickness, BMD density, and Rost length difference of Comparative Example 3 is shown. DETAILED DESCRIPTION
[0035] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0036] As described above, a method for manufacturing a single crystal silicon wafer and a single crystal silicon wafer suitable for a multi-layer structure device are sought, wherein the single crystal silicon wafer can use a BMD layer directly below the surface portion to absorb defects caused by strain due to stress on the surface of the silicon wafer when forming a device, thereby improving the strength of the device formation area and inhibiting the generation and elongation of dislocations in the surface layer.
[0037] The inventors of the present application have repeatedly conducted in-depth research on the above technical problems, and as a result, have found that a single crystal silicon wafer suitable for multilayer structure devices that can improve the strength of the device formation area and suppress the generation and elongation of dislocations in the surface layer can be manufactured by the following single crystal silicon wafer manufacturing method, thereby completing the present invention. The single crystal silicon wafer manufacturing method is a single crystal silicon wafer manufacturing method suitable for multilayer structure devices, wherein N with an oxygen concentration of 12 ppma (JEITA) or more is used. V A single crystal silicon wafer having a thickness of at least 5 to 12.5 μm and a BMD density of 1×10 11 / cm 3 The BMD layer above the single crystal silicon wafer.
[0038] In addition, the following single crystal silicon wafer was found to be a single crystal silicon wafer suitable for multilayer structure devices, which can improve the strength of the device formation area and suppress the generation and elongation of dislocations in the surface layer of the wafer, thereby completing the present invention. The single crystal silicon wafer is a single crystal silicon wafer suitable for multilayer structure devices, and the single crystal silicon wafer is N V The single crystal silicon wafer of the region comprises at least a DZ layer and a BMD layer located directly below the DZ layer in sequence from the surface of the single crystal silicon wafer, wherein the thickness of the DZ layer is 5 to 12.5 μm, and the BMD density of the BMD layer is 1×10 11 / cm 3 above.
[0039] Hereinafter, description will be given with reference to the accompanying drawings.
[0040] The inventors of this application focus on Figure 1An investigation was conducted on the thickness of the DZ layer 1 and the BMD density of the BMD layer 2 of the single crystal silicon wafer 100 shown, which has at least a DZ layer 1 and a BMD layer 2 located directly below the DZ layer 1. It was found that when the thickness of the DZ layer 1 and the BMD density of the BMD layer 2 satisfy a specific relationship, the strength of the device formation area can be improved and the generation and elongation of dislocations in the surface layer can be suppressed.
[0041] First, prepare the defect area to be N V The single crystal silicon CW (Chemical Etched Wafer) wafers with different oxygen concentrations in different regions were used to produce single crystal silicon PW (Polished Wafer) wafers with various DZ layer thicknesses and BMD layer BMD densities by changing the conditions of RTA treatment and BMD formation heat treatment, and the effect of suppressing the generation and extension of dislocations (dislocation absorption effect) was investigated. The following is an explanation of the investigation content and results.
[0042] Prepare a 300mm diameter, <100>, P type, 10Ωcm, oxygen concentration 14ppma (JEITA), and N defect area on the entire surface V A single crystal silicon CW wafer with a defect-free region (a region where vacancies below the saturation concentration are dominant). The CW wafer was subjected to a heat treatment at a temperature of 1150-1300°C for 9 seconds in an NH3+Ar atmosphere as an RTA treatment. Thereafter, the target processing amount was set to 6μm and PW processing was performed. Thus, the nitride film formed in the RTA treatment was removed. Finally, a heat treatment at a temperature of 1200°C for 2 hours in an Ar atmosphere was performed as a BMD formation heat treatment. The DZ layer thickness and BMD density of the obtained single crystal silicon PW wafer were measured, and the results showed that the DZ layer thickness was 0.5-19.4μm and the BMD density was 3.5×10 9 / cm 3 ~4.9×10 11 / cm 3 of the sample.
[0043] The effect of suppressing the generation and elongation of dislocations is evaluated by the Rost test (measurement and comparison of the Rost length). Specifically, for the single crystal silicon PW wafer with a DZ layer and a BMD layer produced as described above, an indentation with a depth of more than 0.01 μm and less than 5.00 μm is formed with an indentation pressure of 0.24 to 2.9 N, and the Rost length is measured. In addition, after the indentation is formed, a heat treatment at 900°C for 1 hour is further performed, and then the Rost length is measured. In addition, the Rost lengths before and after the above-mentioned heat treatment are compared.
[0044] Here, the Rost test is described. The dislocation suppression effect of the single crystal silicon wafer of the present invention can be evaluated by the length of the dislocation (Rost length). The Rost test is an evaluation method described in Patent Document 5. This evaluation method applies strain to the surface layer of the wafer by forming an indentation on the surface of the wafer to be evaluated. Then, a heat treatment is performed to elongate the dislocation, and the length of the dislocation (Rost length) is measured. The shorter the length of the dislocation, the higher the performance of suppressing the generation and elongation of dislocations.
[0045] Below, refer to Figure 2 The specific evaluation method is described with reference to the illustration of the Rost test. First, a pressing pressure is applied to the surface layer of the prepared single crystal silicon wafer 100 using, for example, a Vickers hardness tester to form an indentation 3. In addition, as long as a pressing pressure can be applied to the surface layer of the wafer to form an indentation, the instrument used is not particularly limited.
[0046] In the process of forming the indentation, it is preferred to satisfy the relationship Depth = 3 × Fz 0.6 In the manner of (where Depth is the indentation depth (unit: μm), Fz is the pressing pressure (unit: N), Depth = 0.01 μm or more and less than 5.00 μm), a pressing pressure Fz is applied to form an indentation 3 with an indentation depth Depth on the wafer surface. When the indentation is formed in this way, a stacked structure of at least three layers including a strained layer 4, a DZ layer 1, and a BMD layer 2 is formed in order from the surface. As long as the indentation 3 is formed under such conditions, the effect of suppressing the generation and elongation of dislocations can be evaluated with high accuracy.
[0047] After the indentation is formed, in order to fully extend the Rost length, the silicon wafer is preferably subjected to heat treatment. By performing the heat treatment, the dislocation extension region 5 ( Figure 2 ). As the heat treatment here, for example, the heat treatment temperature can be set to 850°C or more and 1200°C or less. As long as it is set to 850°C or more, the temperature is above the ductile-brittle transition temperature of silicon, and the dislocation can be fully elongated during the evaluation. In addition, as long as it is set to 1200°C or less, the treatment can be performed in a vertical heat treatment furnace.
[0048] The heat treatment time can be set to, for example, more than 30 minutes and less than 1 hour. As long as the time is within this range, it is sufficient to elongate the dislocation. Further, it can be set to an Ar atmosphere. This is because Ar has no effect of hindering the movement of dislocations, so the strength of the wafer itself can be evaluated more accurately. In particular, when the heat treatment conditions are set to 900°C and 1 hour, the dislocations in the DZ layer can be efficiently elongated, and the absorption effect of the BMD layer after the heat treatment on the dislocations can be more accurately confirmed. As a result, a higher performance of suppressing the generation and elongation of dislocations can be obtained.
[0049] Next, in order to measure the length of the dislocation, selective etching is performed to make the dislocation prominent. The selective etching method is not particularly limited as long as it can make the dislocation prominent. For example, wet etching using an etching solution (liquid C in JIS H0609-199) mixed with hydrofluoric acid, nitric acid, acetic acid and water can be performed. In addition, dry etching such as reactive ion etching (RIE: Reactive Ion Etching) can also be performed.
[0050] After the dislocation extending from the indentation is made prominent in this manner, the length of the dislocation (Rost length) is measured.
[0051] The results of the investigation conducted by the inventors of the present application to achieve the above-mentioned object are shown in Figure 3 . Figure 3 The relationship between the Rost length, DZ layer thickness, and BMD density is shown. Figure 3 The horizontal axis of the graph shown is the difference between the Rost length of the single crystal silicon PW wafer before the heat treatment at 900°C for 1 hour as the reference value (reference) and the Rost length of each sample after the heat treatment at 900°C for 1 hour (hereinafter referred to as "the difference in Rost length"). That is, Figure 3 The range in which the difference in the Rost length on the horizontal axis is a positive value means that the Rost length after the heat treatment at 900°C for 1 hour is shorter than that of the single crystal silicon PW wafer before the heat treatment at 900°C for 1 hour, and means that the effect of suppressing the generation of dislocations and elongation is high. On the contrary, Figure 3 The range in which the difference in the Rost length on the horizontal axis is a negative value means that the Rost length after the heat treatment at 900°C for 1 hour is longer than that of the single crystal silicon PW wafer before the heat treatment at 900°C for 1 hour, and means that there is no effect of suppressing the generation and elongation of dislocations.
[0052] also, Figure 3 The first axis of the vertical axis (the vertical axis on the left) shows the DZ layer thickness of the single crystal silicon wafer that has undergone RTA treatment and BMD formation heat treatment, and the second axis of the vertical axis (the vertical axis on the right) shows the BMD density of the BMD layer of the single crystal silicon wafer that has undergone RTA treatment and BMD formation heat treatment.
[0053] like Figure 3 As shown in Figure 2, it was found that the thickness of the DZ layer was less than 12.5 μm and the BMD density of the BMD layer was 1×10 11 / cm 3The above range is the range in which the difference in Rost length is positive, that is, the effect of suppressing the generation of dislocations and the elongation is improved, forming a wafer suitable for multilayer structure devices. As long as the thickness of the DZ layer is less than 10μm, the above effect can be obtained more stably. In addition, the range condition in which the difference in Rost length is positive is the range in which the RTA treatment temperature is above 1225°C, which will be specifically described in the comparison of Example 1 and Comparative Example 1 described later. In addition, the thickness of the DZ layer is set to 5μm or more to ensure the device manufacturing area.
[0054] The single crystal silicon wafer 100 of the present invention is N V area of single crystal silicon wafers. And, Figure 1 As shown, from the surface of the wafer, there are at least a DZ layer 1 and a BMD layer 2 located directly below the DZ layer 1 in sequence. Here, "located directly below" has the same meaning as "adjacent contact". In addition, regarding the BMD layer 2, the portion of the single crystal silicon wafer 100 excluding the DZ layer 1 may be the BMD layer 2, or only a portion of the portion of the single crystal silicon wafer 100 excluding the DZ layer 1 may be the BMD layer 2.
[0055] In addition, the monocrystalline silicon wafer of the present invention has the following characteristics: the thickness of the DZ layer is 5 to 12.5 μm, and preferably 5 to 10 μm, and the BMD density of the BMD layer is 1×10 11 / cm 3 By making the thickness of the DZ layer and the BMD density of the BMD layer within the above range, a single crystal silicon wafer with a very high dislocation absorption effect is formed. When such a single crystal silicon wafer is used to form a multi-layer structure device, the generation and extension of dislocations generated in the device formation area can be suppressed, and the generation of defects such as slip can be suppressed.
[0056] In addition, for the single crystal silicon wafer of the present invention, when the indentation is formed as described above and the heat treatment is performed at a temperature of 900° C. for 1 hour, the Rost length of the dislocation of the DZ layer after the heat treatment is shorter than the Rost length of the dislocation of the DZ layer of the single crystal silicon wafer (PW) without forming the BMD layer. Such a single crystal silicon wafer has a higher performance in suppressing the generation and elongation of dislocations.
[0057] Next, the method for producing a single crystal silicon wafer of the present invention will be described in detail.
[0058] In order to manufacture a DZ layer having at least a thickness of 5 to 12.5 μm and a BMD density of 1×10 11 / cm 3 Single crystal silicon wafers with BMD layers above 12 ppma (JEITA) are used. Vregion. The upper limit of oxygen concentration is not particularly limited, and can be set, for example, to 17 ppma (JEITA) or less. To prepare a CW wafer that meets this specification, first, an RTA treatment is performed in a nitrogen-containing atmosphere at a temperature of 1225°C or more. The heat treatment conditions for the RTA treatment are preferably set to less than 10 seconds and a cooling rate of 30°C / second or more. There is no particular limit to the lower limit of the heat treatment time for the RTA treatment, and can be set, for example, to more than 1 second. There is no particular limit to the upper limit of the cooling rate, and can be set, for example, to less than 100°C / second. In this way, when the temperature is rapidly lowered from the high temperature heat treatment temperature, the effect of suppressing the outward diffusion of vacancies can be enhanced, and the vacancy distribution in the depth direction can be made steeper. As a result, the BMD density distribution can be made steeper. In addition, there is no particular limit to the upper limit of the BMD density, and can be set, for example, to 1×10 12 / cm 3 the following.
[0059] After the RTA treatment, mirror polishing is performed. The mirror polishing conditions are not particularly limited, as long as mirror polishing that meets the usual specifications is performed.
[0060] The BMD density is 1×10 11 / cm 3 The BMD layer is preferably formed at an argon atmosphere, 870 to 950°C, and 2 hours or more. As long as the heat treatment conditions are such, only crystals with a certain size of precipitation nuclei will grow, so the BMD distribution can be made steeper. In addition, as for the heat treatment time, since the change in BMD density distribution cannot be observed even if it is set to a too long time, it is preferably set to, for example, 8 hours or less in terms of efficiency.
[0061] Example
[0062] Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited thereto.
[0063] (Example 1)
[0064] First, prepare a 300mm diameter, <100>, P type, 10Ωcm, oxygen concentration 14ppma (JEITA), and N defect area on the entire surface. VThe CW wafer is heat treated at 1225-1300°C for 9 seconds in an NH3+Ar atmosphere as an RTA process. Afterwards, the target processing amount is set to 6μm and PW processing is performed. Thus, the nitride film formed in the RTA process is removed. Finally, a heat treatment at 1200°C for 2 hours in an Ar atmosphere is performed as a BMD formation heat treatment. The DZ layer thickness and BMD density of the obtained single crystal silicon wafer are measured. The DZ layer thickness is 6.7-10.5μm, and the BMD density is 1.8×10 11 ~4.9×10 11 / cm 3 .also, Figure 4 The RTA treatment temperature is 1300°C, the DZ layer thickness is 6.7 μm, and the BMD density is 4.9×10 11 / cm 3 Cross-sectional TEM image.
[0065] In addition, the same CW was used to perform RTA treatment and BMD formation heat treatment, and then the wafer surface was pressed with a pressure of 0.24 to 2.9 N to form an indentation with a depth of 1 to 5 μm, and then the Rost length before and after the heat treatment at 900° C. for 1 hour was measured by the Rost test. The difference in the Rost length obtained in this way was calculated as the difference in the Rost length.
[0066] (Comparative Example 1)
[0067] The treatment and evaluation were performed in the same manner as in Example 1 except that the RTA treatment temperature was set to 1150°C to 1200°C. The DZ layer thickness was 14.7 to 19.4 μm, and the BMD density was 3.5×10 9 ~6.6×10 10 / cm 3 .
[0068] The difference in Rost length of Example 1 is 2 to 13 μm. On the other hand, the difference in Rost length of Comparative Example 1 is -3 to -12 μm. Thus, it can be seen that in the single crystal silicon wafer of the embodiment, the generation and elongation of dislocations can be effectively suppressed. This shows that after the heat treatment that causes the dislocations to elongate (grow) and when the Rost length of the dislocations is short, the effect of absorbing dislocations is obtained by forming a high-density BMD layer directly below the DZ layer.
[0069] (Example 2)
[0070] The samples were prepared under the same conditions as in Example 1 except that a single crystal silicon CW wafer with an oxygen concentration of 12 ppma (JEITA) was used and the RTA treatment temperature was set to 1225-1250°C. The DZ layer thickness of the obtained single crystal silicon wafer was 10.3-12.3 μm, and the BMD density was 1.3×10 11 ~1.7×10 11 / cm 3 The difference in the Rost length is 0.5 to 6.0 μm.
[0071] (Comparative Example 2)
[0072] The samples were prepared under the same conditions as in Example 1 except that a silicon single crystal CW wafer with an oxygen concentration of 12 ppma (JEITA) was used and the RTA treatment temperature was set to 1175-1200°C. The DZ layer thickness of the obtained single crystal silicon wafer was 15.7-18.7 μm, and the BMD density was 5.4×10 9 ~7.1×10 10 / cm 3 The difference in the Rost length is -2.0 to -5.5 μm.
[0073] The results of Example 2 and Comparative Example 2 are shown in Figure 5 In Example 2, a single crystal silicon wafer having a difference in the Rost length in a positive range is obtained.
[0074] (Comparative Example 3)
[0075] The samples were prepared under the same conditions as in Example 1 except that a silicon single crystal CW wafer with an oxygen concentration of 11 ppma (JEITA) was used and the RTA treatment temperature was set to 1225-1300°C. The DZ layer thickness of the obtained single crystal silicon wafer was 21.5-33.0 μm, and the BMD density was 1.0×10 9 ~4.6×10 9 / cm 3 The difference in the Rost length is -5.0 to -12.0 μm.
[0076] The results of Comparative Example 3 are shown in Figure 6 When the oxygen concentration is less than 12 ppma (JEITA), even if the RTA treatment temperature is increased, a single crystal silicon wafer having a positive difference in the Rost length cannot be obtained.
[0077] In addition, the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and technical solutions having substantially the same structure as the technical concept described in the claims of the present invention and having the same effects are all included in the protection scope of the present invention.
Claims
1. A single crystal silicon wafer, which is suitable for a multi-layer structure device, characterized in that: The single crystal silicon wafer is N V area of single crystal silicon wafers, The single crystal silicon wafer has at least a DZ layer and a BMD layer located directly below the DZ layer in order from the surface of the single crystal silicon wafer. The thickness of the DZ layer is 5 to 12.5 μm, and the BMD density of the BMD layer is 1×10 11 / cm 3 above, To satisfy the relationship Depth = 3 × Fz 0.6 In a manner, when a pressing pressure Fz is applied to form an indentation with an indentation depth Depth on the surface of the single crystal silicon wafer, the single crystal silicon wafer is a stacked structure of at least three layers including a strained layer, a DZ layer, and a BMD layer in order from the surface, Wherein, Depth is the indentation depth, and its unit is μm; Fz is the pressing pressure, and its unit is N, and Depth is set to be greater than 0.01 μm and less than 5.00 μm. When the single crystal silicon wafer having the indentation formed therein is subjected to a heat treatment at 900° C. for 1 hour, the Rostol length of the dislocation of the DZ layer after the heat treatment is shorter than the Rostol length of the dislocation of the DZ layer before the heat treatment.
Citation Information
Patent Citations
Semiconductor wafer of silicon, and production method thereof
JP2015216375A
Thermal treatment method of silicon single crystal wafer
JP2016100542A
Evaluation method for silicon wafer
JP2016111044A
Method For Manufacturing Silicon Single Crystal Wafer
US20090000535A1
Silicon single crystal wafer production method, silicon epitaxial wafer production method, silicon single crystal wafer, and silicon epitaxial wafer
WO2018037755A1