Random copolymer, method for producing pellets, and pneumatic tire

Through random copolymers and process optimization of specific structures, the problems of poor processability and high moisture content of hydrogenated polymers in tire composites are solved, and the dehydration efficiency and productivity are improved.

CN113943403BActive Publication Date: 2024-11-15ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110798173.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-05-12
Filing Date
2021-07-14
Publication Date
2024-11-15
Estimated Expiration
2041-07-14

AI Technical Summary

Technical Problem

The existing hydrogenated polymers have poor processability and high moisture content when making tire composites, resulting in a reduced dehydration efficiency, and it is difficult to effectively solve the moisture content problem by blending polymers with low molecules.

Method used

Using random copolymers with specific structures, the molecular weight distribution is unimodal, including aromatic vinyl monomers, conjugated diene monomers and ethylene structures, the continuous polymerization process is used by controlling the particle size and moisture content of the particles. and hydrogenation process optimize the performance of the polymer.

Benefits of technology

Moderate hypertrophy of the agglomerate particle size is achieved, dehydration efficiency and productivity are improved, moisture content of the hydrogenated polymer is reduced, and processability is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003162223570000321
    Figure BDA0003162223570000321
  • Figure BDA0003162223570000331
    Figure BDA0003162223570000331
  • Figure BDA0003162223570000341
    Figure BDA0003162223570000341
Patent Text Reader

Abstract

The present invention relates to a random copolymer, a method for producing pellets and a pneumatic tire, and provides a random copolymer capable of properly controlling the particle size and water content of pellets. A random copolymer comprises an aromatic vinyl monomer unit, a conjugated diene monomer unit and an ethylene structure, and has a unimodal molecular weight distribution based on GPC, and a molecular weight distribution of 1.30 to 1.75.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a random copolymer, a method for producing pellets and a pneumatic tire. Background Art

[0002] In the past, it was predicted that the spread of autonomous driving technology would increase the demand for reducing the frequency of tire replacement, that is, improving the durability of tires. In particular, regarding the performance of the braking device, it is required to maintain high performance for a longer period of time than before in order to ensure the safety of the passengers.

[0003] In order to improve the durability of a tire, it is essential to improve the wear resistance of the tire. Conventionally, a technology for improving the wear resistance by using a polymer containing an ethylene structure in a tire tread has been disclosed (for example, see Patent Document 1).

[0004] As a method for producing a polymer containing an ethylene structure, for example, a method of producing by hydrogenating a conjugated diene polymer having a structural unit of butadiene in the chain can be cited. For example, Patent Document 1 discloses a method of obtaining a copolymer having an ethylene structure by hydrogenating a styrene-butadiene copolymer.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 6004081 Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, the hydrogenated polymer described in Patent Document 1 has a problem of poor processability when made into a tire compound. Patent Document 1 uses adhesion to a roller as an indicator to evaluate processability when made into a tire compound, but generally the evaluation of polymer adhesion to a roller is also related to the evaluation of productivity when manufacturing the polymer. Specifically, for hydrogenated polymers with low adhesion, the adhesion of the pellets obtained by the steam stripping process during production is also low, and the pellets tend to become fine. Fine pellets tend to cause a decrease in dehydration efficiency in the dehydration process after the above-mentioned steam stripping process, resulting in a problem of increased water content in the finally obtained hydrogenated polymer product.

[0010] Therefore, when the hydrogenated polymer described in Patent Document 1 is used as a tire compound, the problems of poor processability and increased water content of the hydrogenated polymer product should be solved.

[0011] In the technology disclosed in Patent Document 1, the poor processability of a tire compound is improved by blending a high molecular weight hydrogenated polymer and a low molecular weight hydrogenated polymer. However, since the high molecular weight hydrogenated polymer and the low molecular weight hydrogenated polymer are manufactured separately, the problem of excessively high water content of the high molecular weight hydrogenated polymer has not been solved.

[0012] Therefore, in order to improve the productivity when producing a hydrogenated polymer, a technology that can appropriately control the particle size of pellets obtained in the stripping step and appropriately control the water content of the hydrogenated polymer is desired.

[0013] Therefore, in view of the above-mentioned problems of the prior art, an object of the present invention is to provide a random copolymer which can appropriately control the particle size and water content of pellets and has excellent productivity.

[0014] Means for solving problems

[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems of the prior art and, as a result, have found that a random copolymer having a specific structure can solve the above-mentioned problems of the prior art, thereby completing the present invention.

[0016] That is, the present invention is as follows. [1]

[0018] A random copolymer comprising an aromatic vinyl monomer unit, a conjugated diene monomer unit and an ethylene structure,

[0019] The molecular weight distribution based on GPC is unimodal.

[0020] The molecular weight distribution is 1.30-1.75. [2]

[0022] The random copolymer as described in the above-mentioned [1] has an iodine value of 14 or more and 200 or less. [3]

[0024] The random copolymer as described in [1] or [2] above has a weight average molecular weight of 300,000 to 800,000. [4]

[0026] The random copolymer as described in any one of [1] to [3] above, wherein the glass transition temperature is -70°C to -50°C. [5]

[0028] A method for producing pellets, which is a method for producing pellets of the random copolymer described in any one of [1] to [4] above, comprising the following steps:

[0029] a step of polymerizing an aromatic vinyl compound and a conjugated diene compound in a solution, and

[0030] A step of obtaining pellets by removing the solvent from a solution containing a polymer,

[0031] This production method can obtain pellets having a median diameter (D50) of 6.0 mm or more and 12.0 mm or less. [6]

[0033] A pneumatic tire comprising:

[0034] The random copolymer described in any one of [1] to [4] above;

[0035] Rubber components other than the above-mentioned random copolymers;

[0036] Plasticizer ingredients; and

[0037] Filler ingredients.

[0038] Effects of the Invention

[0039] According to the present invention, a random copolymer in which the particle size and water content of aggregates can be appropriately controlled can be provided. DETAILED DESCRIPTION

[0040] A specific embodiment of the present invention (hereinafter referred to as "this embodiment") is described in detail below.

[0041] It should be noted that the following embodiments are examples for explaining the present invention, and the present invention is not limited to the following embodiments. The present invention can be implemented by appropriately modifying the present invention within the scope of the gist thereof.

[0042] [Random copolymer]

[0043] The random copolymer of the present embodiment has an aromatic vinyl monomer unit, a conjugated diene monomer unit, and an ethylene structure, and has a unimodal molecular weight distribution based on GPC (gel permeation chromatography), and the molecular weight distribution is 1.30 to 1.75.

[0044] The random copolymer of the present embodiment has the above-mentioned configuration, and in particular, has a molecular weight distribution within the above-mentioned range. Therefore, when a random copolymer having a weight average molecular weight suitable for a tire composition is prepared, the pellet size does not become too small, thereby achieving excellent pellet dehydration efficiency.

[0045] By setting the molecular weight distribution to the above-mentioned specific range, the abundance ratio of the low molecular weight component effective for enlarging the aggregate particle size can be increased, and the aggregates can be appropriately enlarged, thereby preventing the aggregate particle size from becoming too fine.

[0046] (GPC curve shape of random copolymer)

[0047] The GPC curve of the random copolymer of the present embodiment is unimodal.

[0048] The fact that the GPC curve is unimodal means that when the amount of change is the dissolution time, the slope of the tangent line of the dissolution curve shows 0° only once.

[0049] In the case of batch polymerization for coupling reaction, as long as the modification rate is not 100%, more than two peaks will be shown by the polymer before coupling and the coupling, and no unimodality will be constituted. On the other hand, in the polymer manufactured by continuous polymerization, the peak of the GPC curve is one. In the case of coupling reaction, although a shoulder peak may appear on the low molecular side, multiple peaks will not be formed. Therefore, for the polymer manufactured by continuous polymerization, as long as the polymers in different molecular weight regions are not blended, the GPC curve of the random copolymer can be made unimodal.

[0050] The molecular weight distribution of the random copolymer can be controlled by adjusting the ratio of the height (L) to the diameter (D) inside the polymerization reactor.

[0051] (Composition of random copolymer)

[0052] The random copolymer of the present embodiment has an aromatic vinyl monomer unit, a conjugated diene monomer unit, and an ethylene structure.

[0053] Here, the "ethylene structure" is a structure having an ethylene monomer as a repeating unit, and is a structure in which carbon atoms are linked to each other by single bonds.

[0054] It should be noted that the “ethylene structure” is not limited to the case where an ethylene monomer is polymerized, and includes the case where an ethylene structure is formed by hydrogenating a conjugated diene part as described below.

[0055] Among the random copolymers of this embodiment, from the perspective of commercial production, it is preferably a hydrogenated copolymer having an ethylene structure formed by adding hydrogen to a copolymer having an aromatic portion as an aromatic vinyl monomer unit and a conjugated diene portion as a conjugated diene monomer unit, but it may also be a random copolymer formed by copolymerizing an aromatic vinyl compound, a conjugated diene compound and ethylene.

[0056] The hydrogenated copolymer is a copolymer in which a part or all of the double bonds in the conjugated diene part are converted into an ethylene structure by partially hydrogenating the double bonds in the conjugated diene part. By increasing the hydrogenation rate, the content of the ethylene structure can be increased.

[0057] It should be noted that when the random copolymer of the present embodiment is a hydrogenated copolymer, the structure obtained by hydrogenating the polymer chain formed by both ends of the main chain of the conjugated diene compound (for example, 1,4-bonding of a polymer with 1,3-butadiene as a monomer) is regarded as an ethylene structure, and the structure obtained by hydrogenating other forms (for example, 1,2-bonding (vinyl bonding) of a polymer with 1,3-butadiene as a monomer) is not included in the ethylene structure.

[0058] It should be noted that the ethylene structure can be determined by 1 The spectrum obtained by H-NMR was calculated from the spectrum reduction rate derived from the 1,4-linked unsaturated bond portion of the conjugated diene compound.

[0059] As aromatic vinyl compounds for forming aromatic vinyl monomer units, for example, styrene, 4-methylstyrene, α-methylstyrene, 1-vinylnaphthalene, 3-vinyltoluene, ethylvinylbenzene, divinylbenzene, 4-cyclohexylstyrene, 2,4,6-trimethylstyrene, etc. can be cited but are not limited thereto. These compounds can be used alone or in combination of two or more. Among these, styrene is particularly preferred from the practical aspects such as the ease of obtaining the monomer.

[0060] As the conjugated diene compound for forming the conjugated diene monomer unit, for example, 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethylbutadiene, 2-phenyl-1,3-butadiene, 1,3-hexadiene, etc. can be cited but not limited to. These compounds can be used alone or in combination of two or more. Among these, from the practical aspects such as the ease of obtaining the monomer, 1,3-butadiene and isoprene are preferred, and 1,3-butadiene is more preferred.

[0061] In the random copolymer of the present embodiment, when the content of a chain consisting of eight or more consecutive aromatic vinyl monomer units is defined as a long chain ratio, the long chain ratio is preferably 10% by mass or less based on the total aromatic vinyl monomer units.

[0062] When the long chain ratio is 10% by mass or less, excellent fuel efficiency tends to be obtained.

[0063] Here, the content of long chains consisting of eight or more aromatic vinyl monomer units in a row (long chain ratio) is determined by measuring the random copolymer using deuterated chloroform as a solvent. 1 The long chain ratio is obtained by calculating the ratio of the integrated value in the following range (a) to the total integrated value of each chemical shift range in the following ranges (a) to (c) in the H-NMR spectrum.

[0064] For example, when the aromatic vinyl group is styrene, the ratio of the integral value of the range (a) to the total integral value of each range (a) to (c) is calculated and the value is multiplied by 2.5 to calculate the ratio of styrene. This allows the chain state of the aromatic vinyl monomer unit to be understood.

[0065] (a) Aromatic vinyl compound with 8 or more chains: 6.00≦S<6.68

[0066] (b) Aromatic vinyl compound chains 2 to 7: 6.68 ≦ S < 6.89

[0067] (c) Short chain aromatic vinyl compounds: 6.89≦S≦8.00

[0068] The random copolymer of the present embodiment may be a modified or unmodified copolymer, but is preferably a hydrogenated modified random copolymer from the viewpoint of braking performance and wear resistance.

[0069] The modification mentioned above refers to functionalizing the random copolymer with a compound containing nitrogen. The type of modification may be either a chain end modification in which the polymer chain end is modified or a main chain modification in which a compound containing nitrogen is copolymerized during polymerization.

[0070] (Iodine value of random copolymer)

[0071] In the random copolymer, the iodine value is preferably 14 or more, more preferably 30 or more, further preferably 70 or more, and still more preferably 100 or more, from the viewpoint of crosslinking properties.

[0072] Moreover, from the viewpoint of crosslinking density, it is preferably 200 or less, more preferably 180 or less, and further preferably 160 or less.

[0073] It should be noted that the iodine value can be measured by the method described in Examples below.

[0074] The iodine value of the random copolymer of the present embodiment can be controlled within the above range by adjusting the mass ratio of the conjugated diene compound to the aromatic vinyl monomer in the random copolymer and the hydrogen conversion rate.

[0075] Specifically, when the mass ratio of the aromatic vinyl monomer in the random copolymer is 30 mass %, the iodine value can be controlled to be 100 or more by setting the hydrogen conversion rate to 69% or less.

[0076] Furthermore, when the hydrogen conversion rate is set to 70%, the iodine value can be controlled to be 100 or more by setting the ratio of the aromatic vinyl monomer in the random copolymer to 29 mass % or less.

[0077] (Hydrogenation rate of random copolymer)

[0078] The hydrogenation rate (ratio of hydrogenating the conjugated diene portion) of the random copolymer of the present embodiment is preferably 50 mol% or more, more preferably 60 mol% or more, and further preferably 70 mol% or more from the aspect of crosslinking. In addition, it is preferably 95 mol% or less, more preferably 90 mol% or less, and further preferably 85 mol% or less from the aspect of crosslinking.

[0079] It should be noted that the hydrogenation rate can be determined according to 1 The spectral reduction rate of the unsaturated bond portion in the spectrum obtained by H-NMR was calculated.

[0080] (Content of aromatic vinyl monomer units in random copolymer)

[0081] Regarding the content of the aromatic vinyl monomer unit in 100% by mass of the random copolymer of this embodiment, from the perspective of wet grip performance when processed into a tire, it is preferably 10% by mass or more, more preferably 20% by mass or more, and further preferably 30% by mass or more, and from the perspective of low fuel consumption, it is preferably 60% by mass or less, and more preferably 50% by mass or less.

[0082] In addition, the content of the aromatic vinyl monomer unit can be measured by the method described in the examples described later.

[0083] (Weight average molecular weight of random copolymer)

[0084] The weight average molecular weight (Mw) of the random copolymer according to the present embodiment is preferably 300,000 to 800,000.

[0085] From the perspective of wear resistance when the random copolymer of this embodiment is used in a tire composition, the weight average molecular weight is preferably 300,000 or more, more preferably 400,000 or more, and further preferably 450,000 or more. From the perspective of Mooney viscosity, it is preferably 800,000 or less, more preferably 700,000 or less, further preferably 600,000 or less, and further preferably 550,000 or less.

[0086] The weight average molecular weight of the random copolymer can be controlled within the above numerical range by adjusting polymerization conditions such as the amount of monomer added, polymerization time, and polymerization temperature in the polymerization step.

[0087] (Molecular weight distribution of random copolymer)

[0088] The molecular weight distribution (Mw / Mn) of the random copolymer of the present embodiment is 1.30 or more and 1.75 or less.

[0089] The molecular weight distribution of the random copolymer affects the size of the aggregates produced when the polymerization solution of the random copolymer is stripped.

[0090] In the case of narrow molecular weight distribution, the proportion of low molecular weight components with strong adhesion is small, so the pellets become thinner, and in the dehydration process based on the extruder after the stripping process, sufficient shear pressure cannot be applied, and the dehydration efficiency is reduced. In addition, in the case of too wide molecular weight distribution, the proportion of low molecular weight components with strong adhesion increases, and the pellets become too large as a result. In the case of too large pellets, the drying efficiency in the oven deteriorates, and the drying efficiency of the pellets deteriorates as a result. It should be noted that if only the low molecular weight components with strong adhesion are focused on, the amount of low molecular weight components also increases when the average molecular weight is small. In this case, although the pellets increase, the dehydration efficiency still tends to decrease. Therefore, from the perspective of improving production efficiency, it is more appropriate to control the molecular weight distribution than to reduce the overall molecular weight.

[0091] Based on the above reasons, the molecular weight distribution of the random copolymer of the present embodiment is 1.30 or more, preferably 1.40 or more, and more preferably 1.50 or more, from the viewpoint of increasing the average particle size of the aggregates generated during stripping.

[0092] In order to prevent the average particle size of the aggregates from becoming too large, the molecular weight distribution of the random copolymer of the present embodiment is 1.75 or less, preferably 1.70 or less, and more preferably 1.65 or less.

[0093] In the continuous polymerization process, as a means of controlling the molecular weight distribution of the random copolymer, there are a method of adjusting the aspect ratio (L / D) of the polymerization reactor and a method of adjusting the polymerization temperature.

[0094] In order to control the molecular weight distribution to 1.75 or less, the L / D of the polymerization reactor is preferably 4.0 or more, more preferably 6.0 or more, and even more preferably 7.0 or more.

[0095] From the viewpoint of controlling the molecular weight distribution to be 1.75 or less, the temperature of the polymerization reactor is preferably 80° C. or less, more preferably 75° C. or less, and even more preferably 72° C. or less.

[0096] On the other hand, from the viewpoint of controlling the molecular weight distribution to 1.3 or more, in the continuous polymerization process, L / D is preferably 1.0 or more, more preferably 2.0 or more, and even more preferably 3.0 or more.

[0097] In order to control the molecular weight distribution, it is preferred to select a monomer that undergoes quantitative polymerization and is less likely to cause side reactions. From the perspective of quantitative anionic polymerization without causing side reactions and controlling the molecular weight distribution, the conjugated diene compound is preferably 1,3-butadiene or isoprene.

[0098] From the viewpoint of controlling the molecular weight distribution, the aromatic vinyl compound is preferably styrene or 4-methylstyrene.

[0099] In addition, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are measured by the method described in the Examples mentioned later.

[0100] (Glass transition temperature of random copolymer)

[0101] The glass transition temperature (Tg) of the random copolymer of the present embodiment is preferably -70°C or higher, more preferably -50°C or higher, further preferably -40°C or higher, and still more preferably -30°C or higher from the perspective of braking performance. In addition, from the perspective of low-temperature characteristics of the tire, it is preferably -10°C or lower, more preferably -15°C or lower, further preferably -20°C or lower, and still more preferably -50°C or lower.

[0102] The Tg of the random copolymer can be controlled by adjusting the composition ratio of the aromatic vinyl monomer unit to the conjugated diene monomer unit and the iodine value.

[0103] Specifically, the Tg of the random copolymer can be increased by increasing the composition ratio of the aromatic vinyl monomer unit, and the Tg of the random copolymer can be increased by increasing the 1,2-bonding amount in the conjugated diene monomer unit. More specifically, when the content of the aromatic vinyl monomer unit in the random copolymer is 20% by mass, the Tg can be made above -50°C by setting the iodine value to about 38 to 94. On the other hand, when the iodine value is set to 110, the Tg can be made above -50°C by setting the content of the aromatic vinyl monomer unit to 20% by mass or more.

[0104] In addition, the glass transition temperature (Tg) can be measured by the method described in the examples mentioned later.

[0105] [Method for producing random copolymer]

[0106] The random copolymer of the present embodiment can be produced through a polymerization step, a modification step, and a hydrogenation step.

[0107] (Polymerization process)

[0108] There is no particular limitation on the polymerization method for the random copolymer, and solution polymerization, gas phase polymerization, and bulk polymerization can all be used. From the perspective of commercial production, solution polymerization is particularly preferred.

[0109] In addition, regarding the polymerization form, a continuous form is preferred in the present embodiment.

[0110] When using a solution polymerization method, the monomer concentration in the solution is preferably 5% by mass or more, more preferably 10% by mass or more. By making the monomer concentration in the solution 5% by mass or more, the amount of the obtained random copolymer is sufficient, which is preferred from the perspective of cost. In addition, the monomer concentration in the solution is preferably 50% by mass or less, more preferably 30% by mass or less. When the monomer concentration in the solution is 50% by mass or less, it is possible to prevent the solution viscosity from being too high, and it is easy to stir, which has a tendency to easily implement the polymerization process.

[0111] <Polymerization Initiator>

[0112] When anionic polymerization is performed in the polymerization step, the polymerization initiator is not particularly limited, but an organic lithium compound is preferably used.

[0113] As the organic lithium compound, an organic lithium compound having an alkyl group having 2 to 20 carbon atoms is preferred, and examples thereof include ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, tert-octyl lithium, n-decyl lithium, phenyl lithium, 2-naphthyl lithium, 2-butylphenyl lithium, 4-phenylbutyl lithium, cyclohexyl lithium, cyclopentyl lithium, and a reaction product of diisopropenylbenzene and butyl lithium, etc. Among these, n-butyl lithium and sec-butyl lithium are preferred from the perspectives of availability, safety, etc.

[0114] When coordination polymerization is performed in the polymerization step, it is preferable to use a polymerization catalyst composition described in JP-A-2020-45500 as a polymerization initiator, for example.

[0115] <Aggregation method>

[0116] The method for producing the random copolymer by anionic polymerization or coordination polymerization using a polymerization initiator is not particularly limited, and a conventionally known method can be used.

[0117] Specifically, in an organic solvent inert to the reaction, for example, a hydrocarbon solvent such as an aliphatic, alicyclic, or aromatic hydrocarbon compound, butyl lithium is used as a polymerization initiator, and if necessary, styrene, 1,3-butadiene, ethylene, etc. are polymerized in the presence of a randomizer to be described later, thereby obtaining the target random copolymer.

[0118] <Hydrocarbon Solvent>

[0119] As the hydrocarbon solvent, preferably a hydrocarbon solvent having 3 to 8 carbon atoms, for example, propane, n-butane, isobutane, n-pentane, isopentane, n-hexane, cyclohexane, propylene, 1-butene, isobutylene, trans-2-butene, cis-2-butene, 1-pentene, 2-pentene, 1-hexene, 2-hexene, benzene, toluene, xylene, ethylbenzene and the like can be mentioned but are not limited thereto.

[0120] These solvents may be used alone or in combination of two or more.

[0121] <Randomizer in Anionic Polymerization>

[0122] The randomizer mentioned above refers to a compound having the following effects: controlling the microstructure of the conjugated diene part in the copolymer, such as increasing the 1,2-bonding in butadiene and the 3,4-bonding in isoprene; or controlling the composition distribution of the monomer units in the copolymer, such as the randomization of the styrene unit and the butadiene unit in the styrene butadiene copolymer.

[0123] There is no particular limitation on the randomizer, and any substance among the known compounds commonly used as randomizers can be used. Examples include, but are not limited to, ethers and tertiary amines such as dimethoxybenzene, tetrahydrofuran, dimethoxyethane, diethylene glycol dibutyl ether, diethylene glycol dimethyl ether, 2,2-bis(2-tetrahydrofuranyl)propane, triethylamine, pyridine, N-methylmorpholine, N,N,N',N'-tetramethylethylenediamine, and 1,2-dipiperidylethane. In addition, potassium salts such as potassium tert-amylate and potassium tert-butoxide, and sodium salts such as sodium tert-amylate can also be used.

[0124] These randomizers may be used alone or in combination of two or more.

[0125] In addition, the amount of the randomizer is preferably 0.01 molar equivalent or more, more preferably 0.05 molar equivalent or more, per 1 mole of the organic lithium compound as the polymerization initiator. By making the amount of the randomizer 0.01 molar equivalent or more, an addition effect can be obtained, and there is a tendency to easily randomize. In addition, the amount of the randomizer is preferably 1000 molar equivalent or less, more preferably 500 molar equivalent or less, per 1 mole of the organic lithium compound. By making the amount of the randomizer 1000 molar equivalent or less, it is possible to prevent the reaction rate of the monomer from changing significantly, and there is a tendency to easily randomize.

[0126] <Reaction Temperature>

[0127] The reaction temperature during polymerization is not particularly limited as long as the reaction can proceed appropriately, but is preferably -10°C to 100°C, more preferably 25°C to 70°C.

[0128] (Modification process)

[0129] A functional group that interacts with silicon oxide can be introduced into the polymerization terminal of the random copolymer by reacting the active terminal of the random copolymer obtained in the polymerization step with a compound having a functional group that interacts with silicon oxide. Thus, a random copolymer with a modified polymerization terminal can be obtained.

[0130] The random copolymer used for the modification reaction (hereinafter also referred to as terminal modification reaction) only needs to have an active terminal, and the polymerization start terminal may be unmodified or modified.

[0131] The compound used in the modification step is not particularly limited as long as it has a functional group that interacts with silicon oxide and can react with the polymerization active terminal. For example, it is preferred to use a terminal modifier containing a tin atom or a nitrogen atom, and it is more preferred to use a terminal modifier containing a nitrogen atom.

[0132] The modification step also includes a coupling step that is accompanied by an increase in molecular weight. Specifically, a random copolymer having a branched structure can be obtained by reacting a coupling agent having two or more reaction points with an active terminal.

[0133] A coupling agent having nitrogen is called a modifier. Thus, by selecting a compound having a coupling function as a modifier, a coupling effect can be obtained through the modification process.

[0134] In the modification reaction accompanied by an increase in molecular weight, the modification rate (coupling rate) affects the molecular weight distribution. Therefore, from the perspective of controlling the molecular weight distribution to 1.75 or less, the modification rate is preferably 60% or more, more preferably 70% or more, and even more preferably 75% or more.

[0135] When a modifier having two or more functional groups is used, a multi-branched polymer is generated by coupling, and regardless of the number of functional groups, the molecular weight distribution tends to shift while maintaining a narrowness as long as the modification rate is high.

[0136] Since the structure of the modifier has little influence on the molecular weight distribution, it can be selected according to the desired function of the random copolymer to be produced.

[0137] In addition, the modification rate can be measured by the method described in the Examples mentioned later.

[0138] As terminal modifiers containing nitrogen atoms, preferred ones include isocyanate compounds, isothiocyanate compounds, isocyanuric acid derivatives, nitrogen-containing carbonyl compounds, nitrogen-containing vinyl compounds, nitrogen-containing epoxides, and nitrogen-containing alkoxysilane compounds from the perspective of polymerization productivity and high modification rate.

[0139] As these terminal modifiers containing nitrogen atoms, nitrogen group-containing alkoxysilane compounds are more preferred from the viewpoints of polymerization productivity, high modification rate, and tensile strength when used as tires.

[0140] Examples of nitrogen-containing alkoxysilane compounds include, but are not limited to, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclohexane, 2,2-dimethoxy-1-(5-trimethoxysilylpropyl)-1-aza-2-silacyclohexane, 2-(3-(trimethoxy)silyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-diethoxyethylsilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-ethyl-1-(3-triethoxymethyl)-1-aza-2-silacyclopentane 2-methoxy-2-methyl-1-(3-dimethoxymethylsilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-ethyl-1-(3-diethoxyethylsilylpropyl)-1-aza-2-silacyclopentane, tris(3-trimethoxysilylpropyl)amine, tris(3-methyldimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-tri ... 3-methyldiethoxysilylpropyl)amine, tris(trimethoxysilylmethyl)amine, tris(2-trimethoxysilylethyl)amine, and tris(4-trimethoxysilylbutyl)amine, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propylenediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-propylenediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, and N 1 -(3-(Bis(3-(trimethoxysilyl)propyl)amino)propyl)-N 1 -Methyl-N 3 -(3-(methyl(3-(trimethoxysilyl)propyl)amino)propyl)-N 3 -(3-(Trimethoxysilyl)propyl)-1,3-propanediamine.

[0141] The terminal modification reaction can be carried out in the form of a solution reaction, for example. The solution reaction can be carried out using a solution containing unreacted monomers after the polymerization reaction in the polymerization step is completed, or the copolymer contained in the solution can be separated and dissolved in a suitable solvent such as cyclohexane. In addition, since the polymerization form is a continuous type, it is preferred that the terminal modification reaction is also a continuous type.

[0142] At this time, the method of adding the terminal modifier is not particularly limited, and examples thereof include a method of adding all at once, a method of adding in batches, and a method of adding continuously.

[0143] The amount of the compound used in the terminal modification reaction can be appropriately set according to the type of compound used in the reaction, and is preferably 0.1 molar equivalent or more, more preferably 0.3 molar equivalent or more relative to the metal atom participating in the polymerization reaction possessed by the polymerization initiator. By making this amount 0.1 molar equivalent or more, the modification reaction can be fully carried out, and the dispersibility of silicon oxide can be appropriately improved.

[0144] The temperature of the terminal modification reaction is usually the same as the temperature of the polymerization reaction, preferably -20 to 150° C., more preferably 0 to 120° C., and further preferably 20 to 100° C. If the modification reaction temperature is low, the viscosity of the modified copolymer tends to increase.

[0145] On the other hand, if the temperature of the modification reaction is high, the polymerization active terminal is easily deactivated. The reaction time of the modification reaction is preferably 1 minute to 5 hours, more preferably 2 minutes to 1 hour.

[0146] (Reaction stopping step)

[0147] Anionic polymerization can be stopped by adding a known reaction terminator. Such a reaction terminator may include, but is not limited to, alcohols such as methanol, ethanol, and isopropanol, polar solvents having active protons such as acetic acid, and mixtures thereof, or mixtures of these polar solvents with non-polar solvents such as hexane and cyclohexane.

[0148] The amount of the reaction terminator added is usually sufficient in an amount equal to or twice the molar amount of the anionic polymerization initiator.

[0149] (Hydrogenation process)

[0150] When the random copolymer of the present embodiment is made into a hydrogenated copolymer, the hydrogenation method and reaction conditions are not particularly limited, and the hydrogenation may be carried out by a known method and under known conditions.

[0151] The hydrogenation is usually carried out at 20 to 150° C. and under a hydrogen pressure of 0.1 to 10 MPa in the presence of a hydrogenation catalyst.

[0152] It should be noted that the hydrogenation rate can be controlled by adjusting the amount of the hydrogenation catalyst, the hydrogen pressure during the hydrogenation reaction, the reaction time, and the like.

[0153] As a hydrogenation catalyst, a compound containing any one of the metals of Groups 4 to 11 of the periodic table can be generally used. For example, compounds containing Ti, V, Co, Ni, Zr, Ru, Rh, Pd, Hf, Re, and Pt atoms can be used, but are not limited to. More specifically, examples include: metallocene compounds of Ti, Zr, Hf, Co, Ni, Pd, Pt, Ru, Rh, and Re; supported heterogeneous catalysts in which metals such as Pd, Ni, Pt, Rh, and Ru are supported on carriers such as carbon, silicon oxide, aluminum oxide, and diatomaceous earth; homogeneous Ziegler-type catalysts in which organic salts or acetylacetonates of metal elements such as Ni and Co are combined with reducing agents such as organic aluminum; organic metal compounds or complexes of Ru, Rh, and the like; fullerenes and carbon nanotubes containing hydrogen, and the like.

[0154] Among these, metallocene compounds containing any one of Ti, Zr, Hf, Co, and Ni are preferred from the viewpoint that the hydrogenation reaction can be carried out in a homogeneous system in an inert organic solvent. Metallocene compounds containing any one of Ti, Zr, and Hf are more preferred.

[0155] The hydrogenation catalyst may be used alone or in combination of two or more.

[0156] A preferred production method for obtaining the random copolymer of the present embodiment is a method of performing solution polymerization, using the obtained polymer solution as it is, performing a modification treatment as necessary, and then subjecting the solution to a hydrogenation step as necessary.

[0157] The random copolymer of the present embodiment is obtained by removing the solvent from the polymer solution obtained above and separating the polymer. As a method for separating the random copolymer, for example, a known desolventizing method such as steam stripping, and a method for separating by drying operations such as heat treatment using a dehydrating extruder, a drying extruder, and a conveyor can be cited.

[0158] (Method for producing pellets)

[0159] The random copolymer of this embodiment can be separated in the form of pellets by removing the solvent from the polymerization solution.

[0160] Specifically, the solvent is removed by a steam stripping process to obtain pellets.

[0161] The particle size of the obtained pellets affects the drying capacity in the dehydration extrusion process, the drying extrusion process, and the conveyor process after the desolventizing process. If the average particle size of the pellets is too large, the dehydration efficiency of the drying conveyor is reduced, and the water content in the product rubber block increases. On the other hand, when the average particle size of the pellets is too fine, sufficient shear pressure cannot be applied by the dehydration extruder and the drying extruder, the dehydration efficiency is reduced, and the water content in the product rubber block increases.

[0162] From the viewpoint of preventing the particle size of the aggregates from becoming too large, the temperature of the stripping is preferably 70° C. or higher, more preferably 80° C. or higher, and even more preferably 90° C. or higher.

[0163] In addition, from the viewpoint of the amount of steam used, the stripping temperature is preferably 110° C. or lower, more preferably 100° C. or lower, and even more preferably 95° C. or lower.

[0164] <Particle size of aggregate>

[0165] The average particle size of the aggregate is preferably determined by the particle size distribution of the aggregate. In particular, the median diameter (D50), which is the central value of the aggregate particle size, is an important value in the drying process.

[0166] The particle size of the aggregates is distributed, and the ratio of large-diameter aggregates to fine-diameter aggregates significantly affects the dehydration efficiency of the aggregates as a whole. Therefore, the value of D50, which is the median value, becomes an indicator of the drying efficiency of the aggregates as a whole.

[0167] As described above, the D50 of the pellets can be controlled by adjusting the molecular weight distribution of the random copolymer to 1.30 to 1.75.

[0168] The median diameter (D50) of the pellets of the random copolymer of the present embodiment is preferably 6.0 mm or more, more preferably 8.0 mm or more, further preferably 8.5 mm or more, and even more preferably 9.0 mm or more, from the viewpoint of dehydration efficiency of the pellets by the dehydration extruder.

[0169] From the viewpoint of dehydration efficiency of the pellets by the drying conveyor, D50 of the pellets of the random copolymer of the present embodiment is preferably 12.0 mm or less, more preferably 11 mm or less, and even more preferably 10 mm or less.

[0170] D50 of the pellets can be measured by the method described in the examples below.

[0171] [Rubber composition]

[0172] The random copolymer of the present embodiment can be combined with other rubber components other than the random copolymer, a plasticizer component, a filler component, other additives as necessary, and the like to obtain a rubber composition.

[0173] <Other rubber components>

[0174] In the rubber composition, as a rubber component other than the random copolymer of the present embodiment, a known polymer blend may be included. In addition to the polymer blend, components commonly used in rubber compositions for tires may also be used, such as natural rubber (NR), isoprene rubber (IR), styrene-butadiene rubber (SBR), butadiene rubber (BR), etc.

[0175] These components may be used alone or in combination of two or more.

[0176] In the rubber composition, the content of the filler component (A) and the content of the plasticizer component (B) are not particularly limited. When the entire rubber composition is 100 mass %, the content of the filler component is preferably 20 to 50 mass %, and the content of the plasticizer component is preferably 10 to 40 mass %.

[0177] <Filling agent ingredients>

[0178] The filler component is mixed in the rubber composition for the purpose of reinforcing the rubber, and examples thereof include, but are not limited to, white fillers (inorganic fillers) such as silicon oxide, calcium carbonate, mica, aluminum hydroxide, magnesium oxide, magnesium hydroxide, clay, talc, aluminum oxide, titanium oxide, mica, and carbon black. These components may be used alone or in combination of two or more. Silicon oxide and carbon black are particularly preferred, and their combination is more preferred.

[0179] The silicon oxide is not particularly limited, and examples thereof include dry-process silicon oxide (anhydrous silicon oxide) and wet-process silicon oxide (hydrous silicon oxide). Wet-process silicon oxide is preferred because it contains a large number of silanol groups.

[0180] The nitrogen adsorption specific surface area (N2SA) of silicon oxide is preferably 60 m2 from the perspective of wear resistance. 2 / g or more, more preferably 120m 2 / g or more, preferably 300m / g from the perspective of low fuel consumption 2 / g or less, more preferably 200m 2 / g or less.

[0181] In addition, the nitrogen adsorption specific surface area of ​​silicon oxide is a value measured by the BET method in accordance with ASTM D3037-81.

[0182] Regarding the content of silicon oxide, from the perspective of low fuel consumption, it is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components, and from the perspective of Mooney viscosity, it is preferably 120 parts by mass or less, more preferably 100 parts by mass or less.

[0183] Examples of carbon black include furnace blacks such as SAF, ISAF, HAF, MAF, FEF, SRF, GPF, APF, FF, CF, SCF, and ECF; acetylene black; thermal blacks such as FT and MT; channel blacks such as EPC, MPC, and CC; graphite, etc. These materials may be used alone or in combination of two or more.

[0184] The nitrogen adsorption specific surface area (N2SA) of carbon black is usually 5 to 200 m 2 / g, preferably 50m / g from the perspective of wear resistance 2 / g or more, more preferably 80m 2 / g or more, and preferably 150m / g from the perspective of low fuel consumption 2 / g or less, more preferably 120m 2 / g or less.

[0185] The dibutyl phthalate (DBP) absorption of carbon black is generally 5 to 300 mL / 100 g, and preferably has a lower limit of 80 mL / 100 g and an upper limit of 180 mL / 100 g.

[0186] The nitrogen adsorption specific surface area can be measured according to ASTM D4820-93, and the DBP absorption value can be measured according to ASTM D2414-93.

[0187] Regarding the content of carbon black, from the perspective of wear resistance, it is preferably 1 part by mass or more, and more preferably 3 parts by mass or more, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components, and from the perspective of low fuel consumption, it is preferably 30 parts by mass or less, and more preferably 15 parts by mass or less, relative to 100 parts by mass of the rubber component.

[0188] Silicon oxide is preferably used in combination with a silane coupling agent. As the silane coupling agent, conventionally known substances can be used. Examples thereof include, but are not limited to, bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)di ...ethoxysilylethyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(3-trimethoxysilylpropyl)tri Sulfide-based compounds such as (3-trimethoxysilylpropyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropyl methacrylate monosulfide, 3-trimethoxysilylpropyl methacrylate monosulfide, 3-mercaptopropyl Trimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane and other mercapto-based, vinyltriethoxysilane, vinyltrimethoxysilane and other vinyl-based, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane and other amino-based, γ-epoxy Glycidoxy groups such as propoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and γ-glycidoxypropylmethyldimethoxysilane; nitro groups such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chlorine groups such as 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 2-chloroethyltrimethoxysilane and 2-chloroethyltriethoxysilane.

[0189] It should be noted that the above-mentioned silane coupling agents may be used alone or in combination of two or more. In particular, from the perspective of the coupling effect, processability and cost of the silane coupling agent, sulfide-based silane coupling agents are preferred, and bis(3-triethoxysilylpropyl)tetrasulfide and bis(3-triethoxysilylpropyl)disulfide are more preferred.

[0190] The content of the silane coupling agent is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, based on 100 parts by mass of silicon oxide, from the perspective of low fuel consumption and wear resistance, and is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of silicon oxide, from the perspective of Mooney viscosity.

[0191] <Plasticizer ingredients>

[0192] Examples of the plasticizer component include, but are not limited to, oils, resins, antioxidants, waxes, stearic acid, vulcanization accelerators, etc. These may be used alone or in combination of two or more.

[0193] As oil, for example, aromatic mineral oil (viscosity specific gravity constant (VGC value) 0.900-1.049), cycloparaffin mineral oil (VGC value 0.850-0.899), paraffin mineral oil (VGC value 0.790-0.849) and the like can be cited. The polycyclic aromatic content of the extender oil is preferably less than 3% by mass, more preferably less than 1% by mass. The polycyclic aromatic content is measured according to the British Petroleum Institute 346 / 92 method. In addition, the aromatic compound content (CA) of the extender oil is preferably 20% by mass or more. These extender oils can be used in combination of two or more.

[0194] Regarding the oil content, from the aspect of the Mooney viscosity of the rubber composition, it is preferably 5 parts by mass or more, and more preferably 10 parts by mass or more, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components, and from the aspect of low fuel consumption, it is preferably 50 parts by mass or less, and more preferably 40 parts by mass or less, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components.

[0195] Examples of the resin include, but are not limited to, C5 petroleum resins, C9 petroleum resins, coumarone indene resins, indene resins, phenolic resins, copolymers of α-methylstyrene and / or styrene, and the like.

[0196] These components may be used alone or in combination of two or more. In particular, coumarone indene resins, phenolic resins (particularly terpene phenol resins), α-methylstyrene and / or copolymers of styrene are preferred, and copolymers of α-methylstyrene and styrene are more preferred.

[0197] Regarding the resin content, from the perspective of wet grip performance of the rubber composition, it is preferably 1 part by mass or more, more preferably 3 parts by mass or more, relative to 100 parts by mass of the rubber component, and from the perspective of low fuel consumption, it is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components.

[0198] <Additives>

[0199] In addition to the above-mentioned components, additives such as an antioxidant, wax, stearic acid, and a vulcanization accelerator may be compounded in the rubber composition.

[0200] As the anti-aging agent, there can be mentioned, but not limited to, naphthylamine anti-aging agents such as phenyl-α-naphthylamine; diphenylamine anti-aging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; p-phenylenediamine anti-aging agents such as N-phenyl-N'-isopropyl p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl p-phenylenediamine and N,N'-di-2-naphthyl p-phenylenediamine; quinoline anti-aging agents such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol anti-aging agents such as 2,6-di-tert-butyl-4-methylphenol and styrenated phenol; bisphenol, triphenol, and polyphenol anti-aging agents such as tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate]methane, etc. These components can be used alone or in combination of two or more. In particular, p-phenylenediamine-based antioxidants are preferred, and N-phenyl-N'-isopropyl p-phenylenediamine is more preferred. The content of the antioxidant is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 4 parts by mass, based on 100 parts by mass of the rubber component including the random copolymer of this embodiment and other rubber components.

[0201] Examples of the wax include, but are not limited to, petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as plant wax and animal wax; synthetic waxes such as polymers of ethylene and propylene; and the like.

[0202] These components may be used alone or in combination of two or more. In particular, petroleum wax is preferred, and solid paraffin is more preferred. The wax content is preferably 0.1 to 5 parts by mass, and more preferably 0.2 to 4 parts by mass, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components.

[0203] As stearic acid, existing known substances can be used, for example, products of NOF Corporation, NOF Corporation, Kao Corporation, Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., etc. can be used. These substances can be used alone or in combination of two or more. With respect to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components, the content of stearic acid is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 4 parts by mass.

[0204] Examples of the vulcanization accelerator include, but are not limited to, thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, dibenzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazolyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide; sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, N-tert-butyl-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-o-tolylguanidine, and o-tolylbiguanide. These components may be used alone or in combination of two or more. In particular, for the reason of more appropriately obtaining the effect of the present invention, a sulfenamide-based vulcanization accelerator is preferred, and N-cyclohexyl-2-benzothiazolesulfenamide is more preferred. In addition, it is also preferred to further use a guanidine-based vulcanization accelerator in combination. The content of the vulcanization accelerator is preferably 0.1 to 5 parts by mass, and more preferably 0.2 to 4 parts by mass, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components.

[0205] <Vulcanizing agent, vulcanization activator, organic peroxide, processing aid, antioxidant>

[0206] In addition to the above components, the rubber composition may also contain compounding agents conventionally used in the rubber industry, such as sulfur vulcanizing agents, zinc oxide vulcanization activators, organic peroxides, lubricants and other processing aids, and antioxidants.

[0207] The vulcanizing agent is not particularly limited, and sulfur can be used appropriately. The sulfur content is preferably 0.5 to 5 parts by mass, more preferably 1 to 3 parts by mass, relative to 100 parts by mass of the rubber component including the random copolymer of the present embodiment and other rubber components. This can more appropriately obtain the effects of the present invention.

[0208] (Method for producing rubber composition)

[0209] The rubber composition is produced by a common method, that is, by kneading the above-mentioned components using a Banbury mixer, a kneader, an open roll mill, etc., and then vulcanizing the mixture.

[0210] (Application of rubber composition)

[0211] The rubber composition containing the random copolymer of the present embodiment can be used in various parts of the tire (tread, bead, tire carcass, belt layer, bead, clinch, bead packing, etc.), and can be used as a tread in particular. In the case of a tread with a two-layer structure, it is composed of a surface layer (tread crown) and an inner layer (tread base).

[0212] The tread of the multi-layer structure can be manufactured by the following methods: a method of forming the rubber composition into a sheet and bonding it into a specific shape; a method of loading the rubber composition into two or more extruders and forming two or more layers at the die outlet of the extruder.

[0213] <Pneumatic tires>

[0214] The rubber composition containing the random copolymer of the present embodiment is suitable as a raw material for a pneumatic tire. The pneumatic tire can be manufactured using the above-mentioned rubber composition by a known method. That is, the rubber component, the plasticizer component, the filler component and other various additives when necessary are mixed, extruded in accordance with the shape of each tire component such as the tread at the unvulcanized stage, and molded on a tire molding machine together with other tire components, thereby forming an unvulcanized tire, and the unvulcanized tire is heated and pressurized in a vulcanizer to obtain a pneumatic tire.

[0215] The pneumatic tire of the present embodiment can be suitably used as a tire for a passenger car, a tire for a truck or a bus, a tire for a two-wheeled vehicle, a tire for a racing car, and the like, and can be suitably used as a tire for a passenger car in particular.

[0216] Example

[0217] The present embodiment will be described in more detail below with reference to specific examples and comparative examples, but the present embodiment is not limited to the following examples and comparative examples.

[0218] Various physical properties in Examples and Comparative Examples were measured by the methods shown below.

[0219] (Weight average molecular weight (Mw) and molecular weight distribution of random copolymer)

[0220] The chromatogram was measured using a GPC measuring apparatus having three columns connected and using polystyrene-based gel as a filler, and the weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the random copolymer were determined based on a calibration curve obtained using standard polystyrene.

[0221] As the eluent, THF (tetrahydrofuran) added with 5 mmol / L triethylamine was used.

[0222] As the columns, guard columns: trade name "TSKguardcolumn SuperH-H" manufactured by Tosoh Corporation, and columns: trade names "TSKgel SuperH5000", "TSKgel SuperH6000", and "TSKgelSuperH7000" manufactured by Tosoh Corporation were used.

[0223] An RI detector (trade name "HLC8020" manufactured by Tosoh Corporation) was used under the conditions of an oven temperature of 40°C and a THF flow rate of 0.6 mL / min.

[0224] 10 mg of a sample for measurement was dissolved in 20 mL of THF to prepare a measurement solution, and 20 μL of the measurement solution was injected into a GPC measurement device for measurement.

[0225] (Confirmation of unimodal nature of molecular weight distribution of random copolymer)

[0226] The fact that the GPC curve is unimodal means that, when the random copolymer is analyzed by GPC, the slope of the tangent line of the dissolution curve shows 0° only once when the amount of change is the dissolution time.

[0227] A differential elution curve obtained by differentiating the elution curve of the random copolymer obtained in the Production Example described later was plotted to confirm the unimodal nature.

[0228] (Modification rate of random copolymer)

[0229] The random copolymer was used as a measurement sample, and the chromatogram was measured by utilizing the property that the modified basic polymer component is adsorbed by a GPC column using a silica gel as a filler.

[0230] The modification rate was determined by measuring the adsorption amount of the measurement sample solution containing the measurement sample and low molecular weight internal standard polystyrene on the silica column from the difference between the chromatogram measured by the polystyrene column and the chromatogram measured by the silica column.

[0231] Specifically, it is as follows.

[0232] Preparation of sample solution for determination:

[0233] 10 mg of the above-mentioned measurement sample and 5 mg of standard polystyrene were dissolved in 20 mL of THF (tetrahydrofuran) to prepare a measurement sample solution.

[0234] GPC measurement conditions using polystyrene columns:

[0235] The HLC-8320GPC manufactured by Tosoh Corporation was used, THF was used as the eluent, 10 μL of the sample solution for measurement was injected into the device, and the chromatogram was obtained using an RI detector under the conditions of a chromatographic column thermostat temperature of 40°C and a THF flow rate of 0.35 mL / min. As for the column, three TSKgel SuperMultiporeHZ-H manufactured by Tosoh Corporation were connected, and a TSK guard column SuperMP(HZ)-H manufactured by Tosoh Corporation was connected to the front section as a guard column for use.

[0236] GPC measurement conditions using silica column:

[0237] A product name "HLC-8320GPC" manufactured by Tosoh Corporation was used, THF was used as the eluent, 50 μL of the sample solution for measurement was injected into the device, and a chromatogram was obtained using an RI detector under the conditions of a column thermostat temperature of 40°C and a THF flow rate of 0.5 mL / min. As for the column, a product name "Zorbax PSM-1000S", "PSM-300S", and "PSM-60S" were connected for use, and a product name "DIOL 4.6×12.5mm 5micron" was connected to the front stage as a guard column for use.

[0238] Calculation method of modification rate:

[0239] Assuming that the total peak area of ​​the chromatogram obtained using a polystyrene column is 100, the peak area of ​​the sample is P1, and the peak area of ​​the standard polystyrene is P2, and the total peak area of ​​the chromatogram obtained using a silica column is 100, and the peak area of ​​the sample is P3, and the peak area of ​​the standard polystyrene is P4, the modification rate (mass %) is calculated by the following formula.

[0240] Modification rate (mass %) = [1-(P2×P3) / (P1×P4)]×100

[0241] (In the above formula, P1+P2=P3+P4=100.)

[0242] (Bound styrene content of random copolymer)

[0243] 100 mg of the sample was fixed to 100 mL with chloroform and dissolved to prepare a measurement sample. The bound styrene amount (mass %) relative to 100 mass % of the random copolymer as a sample was measured based on the absorption of the ultraviolet absorption wavelength (near 254 nm) of the phenyl group of styrene (measurement device: spectrophotometer "UV-2450" manufactured by Shimadzu Corporation).

[0244] (1,2-vinyl bond content of the butadiene portion of the random copolymer)

[0245] 50 mg of the random copolymer as a sample was dissolved in 10 mL of carbon disulfide to prepare a measurement sample. -1 The infrared spectrum was measured in a range of , and the microstructure of the butadiene part, i.e., the 1,2-vinyl bonding amount (mol %) was determined based on the absorbance at a specific wave number according to the calculation formula of the Hampton method (the method described in R.R. Hampton, Analytical Chemistry 21, 923 (1949)) (measuring device: Fourier transform infrared spectrophotometer "FT-IR230" manufactured by JASCO Corporation).

[0246] (Hydrogenation rate and ethylene structure content of random copolymer)

[0247] A large amount of methanol is added to the solution of the random copolymer after the hydrogenation reaction, so that the conjugated diene polymer before hydrogenation and the hydrogenated conjugated diene polymer are precipitated and recovered.

[0248] Next, the hydrogenated conjugated diene polymer was extracted with acetone and vacuum dried. 1 The hydrogenation rate and the amount of ethylene structure were measured for the sample subjected to H-NMR measurement.

[0249] The conditions are as follows.

[0250] (Measurement conditions)

[0251] Measuring equipment: JNM-LA400 (manufactured by JEOL)

[0252] Solvent: deuterated chloroform

[0253] Measurement samples: Extracts of polymers before and after hydrogenation

[0254] Sample concentration: 50 mg / mL

[0255] Observation frequency: 400MHz

[0256] Chemical shift standard: TMS (tetramethylsilane)

[0257] Pulse delay: 2.904 seconds

[0258] Scan times: 64 times

[0259] Pulse width: 45°

[0260] Measurement temperature: 26℃

[0261] (Iodine value of random copolymer)

[0262] The iodine value of the random copolymer was calculated according to the method described in "JIS K 0070:1992".

[0263] (Glass transition temperature of random copolymer: Tg)

[0264] The random copolymer was used as a sample and a differential scanning calorimeter "DSC3200S" manufactured by Mac Science was used in accordance with ISO 22768:2006. A DSC curve was recorded while the temperature was raised from -100°C at 20°C / min under a flow of 50 mL / min of helium. The peak top (inflection point) of the DSC differential curve was taken as the glass transition temperature.

[0265] (Particle size of random copolymer)

[0266] <Method for producing pellets>

[0267] The random copolymer polymerization solution obtained by the method described in the later-described Production Examples was stripped to remove the solvent to obtain pellets.

[0268] The operation of obtaining pellets is called agglomeration.

[0269] The conditions for agglomeration are as follows.

[0270] Water temperature: 90℃

[0271] Water volume: 8kg

[0272] Stirring tank: 30L stirring tank with stirring paddle

[0273] Stirring propeller: 2 turbine propellers

[0274] Stirring paddle rotation speed: 500rpm

[0275] Amount of polymer used in granulation: 200 g

[0276] Addition rate of polymer solution to the granulation tank: 30 g / min

[0277] <Evaluation of median diameter (D50) of pellets>

[0278] The agglomerates obtained by agglomeration were sieved using a metal mesh (JIS Z 8801-1:2000, manufactured by Okuya Metal Works, Ltd.) to separate into agglomerates corresponding to the mesh openings.

[0279] The mesh sizes of the metal mesh used are as follows.

[0280] The mass of pellets remaining on the sieves of each mesh size was measured for 22.4 mm, 19 mm, 16 mm, 13.2 mm, 9.5 mm, 8 mm, 6.7 mm, 4 mm, 3.35 mm, and 1.7 mm, and D50 was calculated.

[0281] [Preparation of hydrogenation catalyst]

[0282] In the Examples and Comparative Examples described below, the hydrogenation catalyst used in preparing the random copolymer was prepared by the following method.

[0283] Into a nitrogen-purged reaction vessel, 1 liter of dried and purified cyclohexane was added, 100 mmol of bis(η5-cyclopentadienyl)titanium dichloride was added, and an n-hexane solution containing 200 mmol of trimethylaluminum was added while stirring thoroughly. The mixture was reacted at room temperature for about 3 days to obtain a hydrogenation catalyst.

[0284] [Production Example 1 (Production of Random Copolymer 1)]

[0285] The following tank-type pressure vessel with a stirrer and a jacket for temperature control was used as a polymerization reactor and two were connected. The tank-type pressure vessel is a tank-type reactor with a stirrer, having an internal volume of 10 L, a ratio (L / D) of the internal height (L) to the diameter (D) of 4.0, an inlet at the bottom, and an outlet at the top.

[0286] 1,3-butadiene from which water had been removed in advance was mixed at 22.0 g / min, styrene at 3.9 g / min, and n-hexane at 175.0 g / min. After n-butyl lithium for deactivation of residual impurities was added at 6.0 mg / min in a static mixer provided in the middle of the pipe supplied to the reactor inlet, the mixed solution was continuously supplied to the bottom of the reactor.

[0287] Furthermore, 2,2-di(2-tetrahydrofuryl)propane as a polar substance was supplied at a rate of 0.34 mg / min and n-butyllithium as a polymerization initiator was supplied at a rate of 23.8 mg / min to the bottom of the first reactor where the mixture was vigorously mixed by a stirrer. The internal temperature of the reactor was maintained at 67°C.

[0288] The polymer solution was continuously withdrawn from the top of the first reactor and continuously supplied to the bottom of the second reactor, and the reaction was continued at 70°C, and further supplied to the static mixer from the top of the second reactor. In the static mixer, 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was added as a modifier at a rate of 24.2 mg / min to modify the growing end.

[0289] Next, 10 L of the polymerization solution was transferred to a tank-type pressure vessel having a stirrer and a temperature control jacket (the tank-type pressure vessel was a tank-type reactor with a stirrer having an internal volume of 20 L and a ratio (L / D) of the internal height (L) to the diameter (D) of 4.0), the internal temperature was set to 80°C, and hydrogen was introduced into the system.

[0290] Next, a hydrogenation catalyst was added at 60 ppm based on titanium relative to the amount of monomers fed, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and an average temperature of 85° C. After reaching a predetermined hydrogen integrated flow rate, the reaction liquid was returned to normal temperature and pressure and extracted from the reaction vessel to obtain a polymer solution.

[0291] The obtained polymer solution was pelletized under the above-mentioned pelletization conditions to obtain pellets of random copolymer 1. The pellets were separated by particle size using a metal mesh, and the mass fraction at each mesh opening was measured to calculate D50. After calculating the D50 of the pellets, the pellets were dried for 2 hours using a vacuum dryer heated to 90° C. to obtain an analysis sample of random copolymer 1.

[0292] Table 1 shows the polymerization formula, physical properties, and characteristics of the random copolymer 1.

[0293] [Production Example 2 (Production of Random Copolymer 2)]

[0294] The following tank-type pressure vessel with a stirrer and a jacket for temperature control is used as a polymerization reactor and two units are connected. The tank-type pressure vessel is a tank-type reactor with an internal volume of 10L, a ratio (L / D) of the internal height (L) to the diameter (D) of 7.0, an inlet at the bottom, an outlet at the top, and a stirrer.

[0295] 1,3-butadiene from which water had been removed in advance was mixed at 22.0 g / min, styrene at 3.9 g / min, and n-hexane at 175.0 g / min. After n-butyl lithium for deactivation of residual impurities was added at 6.0 mg / min in a static mixer provided in the middle of the pipe supplied to the reactor inlet, the mixed solution was continuously supplied to the bottom of the reactor.

[0296] Furthermore, 2,2-di(2-tetrahydrofuryl)propane as a polar substance was supplied at a rate of 0.24 mg / min and n-butyllithium as a polymerization initiator was supplied at a rate of 19.6 mg / min to the bottom of the first reactor where the mixture was vigorously mixed by a stirrer, and the internal temperature of the reactor was maintained at 67°C.

[0297] The polymer solution was continuously withdrawn from the top of the first reactor and continuously supplied to the bottom of the second reactor, and the reaction was continued at 70°C, and further supplied to the static mixer from the top of the second reactor. In the static mixer, 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was added as a modifier at a rate of 19.9 mg / min to modify the growing end.

[0298] Next, 10 L of the polymerization solution was transferred to a tank-type pressure vessel having a stirrer and a temperature control jacket (the tank-type pressure vessel was a tank-type reactor with a stirrer having an internal volume of 20 L and a ratio (L / D) of the internal height (L) to the diameter (D) of 4.0), the internal temperature was set to 80°C, and hydrogen was introduced into the system.

[0299] Next, a hydrogenation catalyst was added at 60 ppm based on titanium relative to the amount of monomers fed, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and an average temperature of 85° C. After reaching a predetermined hydrogen integrated flow rate, the reaction liquid was returned to normal temperature and pressure and extracted from the reaction vessel to obtain a polymer solution.

[0300] The obtained polymer solution was pelletized under the above-mentioned pelletization conditions to obtain pellets of random copolymer 1. The pellets were separated by particle size using a metal mesh, and the weight fraction at each mesh opening was measured to calculate D50. After calculating the D50 of the pellets, the pellets were dried for 2 hours using a vacuum dryer heated to 90° C. to obtain an analysis sample of random copolymer 2.

[0301] Table 1 shows the polymerization formula, physical properties, and characteristics of the random copolymer 2.

[0302] [Production Example 3 (Production of Random Copolymer 3)]

[0303] Polymerization was carried out in the same manner as in the random copolymer 1 of [Production Example 1] except that the addition rate of the polymerization initiator n-butyllithium was 33.5 mg / min, the addition rate of the polar substance 2,2-di(2-tetrahydrofuryl)propane was 0.75 mg / min, and the addition rate of the modifier 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was changed to 34.0 mg / min.

[0304] Table 1 shows the polymerization formula, physical properties and characteristics of the obtained random copolymer 3.

[0305] [Production Example 4 (Production of Random Copolymer 4)]

[0306] The polymerization was carried out in the same manner as in the random copolymer 2 of [Production Example 2] except that the addition rate of the polymerization initiator n-butyl lithium was 27.5 mg / min, the addition rate of the polar substance 2,2-di(2-tetrahydrofuryl)propane was 0.51 mg / min, and the addition rate of the modifier 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was changed to 28.0 mg / min.

[0307] Table 1 shows the polymerization formula, physical properties and characteristics of the obtained random copolymer 4.

[0308] [Production Example 5 (Production of Random Copolymer 5)]

[0309] Random copolymer 5 was obtained by the same polymerization conditions as in the above-mentioned [Production Example 1] except that the hydrogenation amount was changed.

[0310] Table 1 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 5.

[0311] [Production Example 6 (Production of Random Copolymer 6)]

[0312] Random copolymer 6 was obtained by the same polymerization conditions as in the above-mentioned [Production Example 2] except that the hydrogenation amount was changed.

[0313] Table 2 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 6.

[0314] [Production Example 7 (Production of Random Copolymer 7)]

[0315] Polymerization was carried out in the same manner as in the random copolymer 1 of [Production Example 1] except that the addition rate of styrene was 1.3 g / min, the addition rate of butadiene was 25 g / min, the addition rate of the polymerization initiator n-butyl lithium was 20.1 mg / min, the addition rate of the polar substance 2,2-di(2-tetrahydrofuryl)propane was 0.26 mg / min, and the addition rate of the modifier 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was changed to 20.4 mg / min.

[0316] Table 2 shows the polymerization formula, physical properties and characteristics of the obtained random copolymer 7.

[0317] [Production Example 8 (Production of Random Copolymer 8)]

[0318] The polymerization conditions other than the hydrogenation amount were the same as those in the above-mentioned [Production Example 1] to obtain a random copolymer 8.

[0319] Table 2 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 8.

[0320] [Production Example 9 (Production of Random Copolymer 9)]

[0321] The polymerization conditions other than the hydrogenation amount were the same as those in the above-mentioned [Production Example 2] to obtain a random copolymer 9.

[0322] Table 2 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 9.

[0323] [Production Example 10 (Production of Random Copolymer 10)]

[0324] Polymerization was carried out in the same manner as in the random copolymer 1 of [Production Example 1] except that the addition rate of the polymerization initiator n-butyllithium was 39.8 mg / min, the addition rate of the polar substance 2,2-di(2-tetrahydrofuryl)propane was 0.91 mg / min, and the addition rate of the modifier 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was changed to 40.3 mg / min.

[0325] Table 2 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 10.

[0326] [Production Example 11 (Production of Random Copolymer 11)]

[0327] Polymerization was carried out in the same manner as in the random copolymer 1 of [Production Example 1] except that the addition rate of the polymerization initiator n-butyllithium was 15.1 mg / min, the addition rate of the polar substance 2,2-di(2-tetrahydrofuryl)propane was 0.14 mg / min, and the addition rate of the modifier 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was changed to 15.3 mg / min.

[0328] Table 3 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 11.

[0329] [Production Example 12 (Production of Random Copolymer 12)]

[0330] The polymerization conditions other than the hydrogenation amount were the same as those in the above-mentioned [Production Example 1] to obtain a random copolymer 12.

[0331] Table 3 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 12.

[0332] [Production Example 13 (Production of Random Copolymer 13)]

[0333] The polymerization conditions other than the hydrogenation amount were the same as those in the above-mentioned [Production Example 1] to obtain a random copolymer 13.

[0334] Table 3 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 13.

[0335] [Production Example 14 (Production of Random Copolymer 14)]

[0336] The polymerization was carried out in the same manner as in the random copolymer 1 of [Production Example 1] except that the addition rate of the polymerization initiator n-butyl lithium was 13.2 mg / min, the addition rate of the polar substance 2,2-di(2-tetrahydrofuryl)propane was 0.11 mg / min, and the addition rate of the modifier 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was changed to 13.4 mg / min.

[0337] Table 3 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 14.

[0338] [Production Example 15 (Production of Random Copolymer 15)]

[0339] Polymerization was carried out in the same manner as in the random copolymer 1 of [Production Example 1] except that the addition rate of the polymerization initiator n-butyllithium was changed to 10.2 mg / min, the addition rate of the polar substance 2,2-di(2-tetrahydrofuryl)propane was changed to 0.07 mg / min, and no modifier was added.

[0340] Table 3 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 15.

[0341] [Production Example 16 (Production of Random Copolymer 16)]

[0342] The following tank-type pressure vessel with a stirrer and a jacket for temperature control was used as a polymerization reactor and two were connected. The tank-type pressure vessel is a tank-type reactor with a stirrer, having an internal volume of 10 L, a ratio (L / D) of the internal height (L) to the diameter (D) of 4.0, an inlet at the bottom, and an outlet at the top.

[0343] 1,3-butadiene from which water had been removed in advance was mixed at 22.0 g / min, styrene at 3.9 g / min, and n-hexane at 175.0 g / min. After adding n-butyl lithium for deactivation of residual impurities at 6.0 mg / min in a static mixer provided in the middle of the pipe supplied to the reactor inlet, the mixed solution was continuously supplied to the bottom of the reactor. 2,2-di(2-tetrahydrofuryl)propane as a polar substance was further supplied at a rate of 0.34 mg / min and n-butyl lithium as a polymerization initiator at a rate of 23.8 mg / min to the bottom of the first reactor which was vigorously mixed by a stirrer, and the temperature inside the reactor was maintained at 67°C.

[0344] The polymer solution was continuously withdrawn from the top of the first reactor and continuously supplied to the bottom of the second reactor, and the reaction was continued at 70°C, and further supplied to the static mixer from the top of the second reactor. In the static mixer, 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was added as a modifier at a rate of 24.2 mg / min to modify the growing end.

[0345] The obtained polymerization solution was pelletized under the above-mentioned pelletizing conditions to obtain pellets of random copolymer 16. The pellets were separated by particle size using a metal mesh, and the weight fraction at each mesh opening was measured to calculate D50. After calculating the D50 of the pellets, the pellets were dried for 2 hours using a vacuum dryer heated to 90° C. to obtain an analysis sample of random copolymer 16.

[0346] Table 4 shows the polymerization formula, physical properties, and characteristics of the random copolymer 16.

[0347] [Production Example 17 (Production of Random Copolymer 17)]

[0348] The following tank-type pressure vessel with a stirrer and a jacket for temperature control is used as a polymerization reactor and two units are connected. The tank-type pressure vessel is a tank-type reactor with an internal volume of 10L, a ratio (L / D) of the internal height (L) to the diameter (D) of 3.0, an inlet at the bottom, an outlet at the top, and a stirrer.

[0349] 1,3-butadiene from which water had been removed in advance was mixed at 22.0 g / min, styrene at 3.9 g / min, and n-hexane at 175.0 g / min. After adding n-butyl lithium for deactivation of residual impurities at 6.0 mg / min in a static mixer provided in the middle of the pipe supplied to the reactor inlet, the mixed solution was continuously supplied to the bottom of the reactor. 2,2-di(2-tetrahydrofuryl)propane as a polar substance was further supplied at a rate of 0.24 mg / min and n-butyl lithium as a polymerization initiator was supplied at a rate of 25.2 mg / min to the bottom of the first reactor which was vigorously mixed by a stirrer, and the temperature inside the reactor was maintained at 67°C.

[0350] The polymer solution was continuously withdrawn from the top of the first reactor and continuously supplied to the bottom of the second reactor, and the reaction was continued at 70°C, and further supplied to the static mixer from the top of the second reactor. In the static mixer, 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was added as a modifier at a rate of 25.6 mg / min to modify the growing end.

[0351] Next, 10 L of the polymerization solution was transferred to a tank-type pressure vessel having a stirrer and a temperature control jacket (the tank-type pressure vessel was a tank-type reactor with a stirrer having an internal volume of 20 L and a ratio (L / D) of the internal height (L) to the diameter (D) of 4.0), the internal temperature was set to 80°C, and hydrogen was introduced into the system.

[0352] Next, a hydrogenation catalyst was added at 60 ppm based on titanium relative to the amount of monomers fed, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and an average temperature of 85° C. After reaching a predetermined hydrogen integrated flow rate, the reaction liquid was returned to normal temperature and pressure and extracted from the reaction vessel to obtain a polymer solution.

[0353] The obtained polymer solution was pelletized under the above-mentioned pelletization conditions to obtain pellets of random copolymer 17. The pellets were separated by particle size using a metal mesh, and the weight fraction at each mesh was measured to calculate D50. After calculating the D50 of the pellets, the pellets were dried for 2 hours using a vacuum dryer heated to 90° C. to obtain an analysis sample of random copolymer 17.

[0354] Table 4 shows the polymerization formula, physical properties, and characteristics of the random copolymer 17.

[0355] [Production Example 18 (Production of Random Copolymer 18)]

[0356] 25800 g of n-hexane, 3.1 g of polar substance 2,2-di(2-tetrahydrofuryl)propane, 645 g of styrene, and 2814 g of 1,3-butadiene were placed in an autoclave reactor having an internal volume of 40 L and an internal height (L) to diameter (D) ratio (L / D) of 4.0. After adjusting the temperature of the contents of the reactor to 40° C., a cyclohexane solution containing 2.9 g of n-butyl lithium was added to initiate polymerization, and polymerization was carried out under adiabatic conditions.

[0357] When the polymerization conversion rate reached 99%, 840 g of butadiene was added and the polymerization was further continued for 5 minutes to obtain a reaction solution containing a polymer. Then, 2.9 g of 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilane was added as a modifier and reacted at the active sites of the above polymer for 30 minutes.

[0358] Next, the reaction liquid was kept at 80° C., and hydrogen was introduced into the system.

[0359] Next, a hydrogenation catalyst was added at 60 ppm based on titanium relative to the amount of monomers fed, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and an average temperature of 85° C. After reaching a predetermined hydrogen integrated flow rate, the reaction liquid was returned to normal temperature and pressure and extracted from the reaction vessel to obtain a polymer solution.

[0360] The obtained polymerization solution was pelletized under the above-mentioned pelletizing conditions to obtain pellets of random copolymer 18. The pellets were separated by particle size using a metal mesh, and the weight fraction at each mesh opening was measured to calculate D50. After calculating the D50 of the pellets, the pellets were dried for 2 hours using a vacuum dryer heated to 90° C. to obtain an analysis sample of random copolymer 18.

[0361] Table 5 shows the polymerization formula, physical properties, and characteristics of the random copolymer 18.

[0362] [Production Example 19 (Production of Random Copolymer 19)]

[0363] The polymerization conditions other than the hydrogenation amount were the same as those in the above-mentioned [Production Example 17] to obtain a random copolymer 19.

[0364] Table 4 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 19.

[0365] [Production Example 20 (Production of Random Copolymer 20)]

[0366] The polymerization conditions other than the hydrogenation amount were the same as those in the above-mentioned [Production Example 18] to obtain a random copolymer 20.

[0367] Table 5 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 20.

[0368] [Production Example 21 (Production of Random Copolymer 21)]

[0369] A random copolymer 21 was obtained in the same manner as in the above-mentioned [Production Example 17] except that the modifier was changed to N,N-bis(triethoxysilylpropyl)aminopropyl-1-imidazole.

[0370] Table 4 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 21.

[0371] [Production Example 22 (Production of Random Copolymer 22)]

[0372] The following tank-type pressure vessel with a stirrer and a jacket for temperature control is used as a polymerization reactor and two units are connected. The tank-type pressure vessel is a tank-type reactor with an internal volume of 10L, a ratio (L / D) of the internal height (L) to the diameter (D) of 7.0, an inlet at the bottom, an outlet at the top, and a stirrer.

[0373] 1,3-butadiene from which water had been removed in advance was mixed at 21.0 g / min, styrene at 5.2 g / min, and n-hexane at 175.0 g / min.

[0374] After adding and mixing n-butyllithium for deactivation treatment of residual impurities at 6.0 mg / min in a static mixer provided in the middle of the pipe supplied to the reactor inlet, the mixed solution was continuously supplied to the bottom of the reactor.

[0375] Furthermore, 2,2-di(2-tetrahydrofuryl)propane as a polar substance was supplied at a rate of 1.20 mg / min and n-butyllithium as a polymerization initiator was supplied at a rate of 23.8 mg / min to the bottom of the first reactor where the mixture was vigorously mixed by a stirrer. The internal temperature of the reactor was maintained at 67°C.

[0376] The polymer solution was continuously withdrawn from the top of the first reactor and continuously supplied to the bottom of the second reactor, and the reaction was continued at 70°C, and further supplied to the static mixer from the top of the second reactor. In the static mixer, 2,2-dimethoxy-1-(3-(trimethoxysilyl)propyl)-1,2-azasilacyclopentane was added as a modifier at a rate of 24.2 mg / min to modify the growing end.

[0377] Next, 10 L of the polymer solution was transferred to a tank-type pressure vessel having a stirrer and a temperature control jacket (the tank-type pressure vessel was a tank-type reactor with a stirrer having an internal volume of 20 L and a ratio (L / D) of the internal height (L) to the diameter (D) of 4.0), the internal temperature was set to 80°C, and hydrogen was introduced into the system.

[0378] Next, a hydrogenation catalyst was added at 60 ppm based on titanium relative to the amount of monomers fed, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and an average temperature of 85° C. After reaching a predetermined hydrogen integrated flow rate, the reaction liquid was returned to normal temperature and pressure and extracted from the reaction vessel to obtain a polymer solution.

[0379] The obtained polymer solution is pelletized under the above-mentioned pelletizing conditions, thereby obtaining pellets of the random copolymer 22 .

[0380] The pellets were separated by particle size using a metal mesh, and the weight fraction at each mesh opening was measured to calculate D50. After calculating D50 of the pellets, the pellets were dried in a vacuum dryer heated to 90° C. for 2 hours to obtain an analysis sample of the random copolymer 22.

[0381] Table 3 shows the polymerization formula, physical properties, and characteristics of the obtained random copolymer 22.

[0382] The random copolymers 1 to 15 and 22 of the above-mentioned Production Examples 1 to 15 and 22 were used to produce gum blocks for evaluating the product moisture content (VM) of [Examples 1 to 15 and 16].

[0383] Similarly, the random copolymers 16 to 21 of Production Examples 16 to 21 described above were used to produce the rubber blocks for evaluating the water content (VM) of the products of [Comparative Examples 1 to 6].

[0384] The method for producing the rubber block for VM evaluation is as follows.

[0385] <Production of Rubber Block for VM Evaluation>

[0386] 300 g of the agglomerates in the water-containing state obtained in Production Examples 1 to 22 were respectively used for the production of the rubber block for VM evaluation.

[0387] The agglomerates of the random copolymer were passed through a 6-inch roll with a gap set at 2 mm and heated to 80 °C 10 times for dehydration. Then, the dehydrated agglomerates were passed through a 6-inch roll heated to 110 °C 15 times for drying.

[0388] After heating 35 g of the agglomerates prepared by the above method to 60 °C, they were filled into a rectangular parallelepiped container with a long side of 42 mm, a short side of 21 mm, and a depth of 40 mm, and compressed by applying a pressure of 3.5 MPa for 10 seconds in a cylinder to obtain the rubber block for VM evaluation.

[0389] <Evaluation>

[0390] Next, as the evaluation of Examples 1 to 16 and Comparative Examples 1 to 6, the dehydration efficiency was evaluated using the water content (VM) of the product.

[0391] The evaluation method of VM is as follows.

[0392] 10 g of the rubber block for VM evaluation was put into a halogen heater heated to 110 °C and heated for 20 minutes.

[0393] The water content (VM) in the sample was calculated from the mass change after heating.

[0394] The calculation formula of VM is as follows.

[0395] VM (wt%) = (mass of the sample before heating - mass of the sample after heating) / mass of the sample before heating × 100

[0396] From the aspect of preventing the pressure of the mixer from rising due to the gasification of water when the rubber composition obtained using the random copolymer is processed into a tire product, when VM is 0.75 wt% or less, it is judged to be practically good.

[0397] The VM values in Examples 1 to 16 and Comparative Examples 1 to 6 are shown in Tables 6 to 9.

[0398]

[0399]

[0400]

[0401]

[0402]

[0403]

[0404] As can be seen from Tables 6 to 9, VM was improved in the gel blocks using the random copolymers of Examples.

[0405] Industrial Applicability

[0406] The random copolymer of the present embodiment has industrial applicability in the fields of tire parts, automobile interior and exterior products, anti-vibration rubber, belts, shoes, foams, various industrial products, and the like.

Claims

1. A random copolymer comprising an aromatic vinyl monomer unit, a conjugated diene monomer unit and an ethylene structure, The molecular weight distribution based on GPC is unimodal. The molecular weight distribution is 1.30~1.75, The hydrogenation rate is 72 mol% to 97 mol%, The iodine value of the random copolymer is 14 or more and 200 or less.

2. The random copolymer according to claim 1, which has a weight average molecular weight of 300,000 to 800,000.

3. The random copolymer according to claim 1 or 2, which has a glass transition temperature of -70°C to -50°C.

4. The random copolymer according to claim 1 or 2, wherein The molecular weight distribution is 1.40~1.

75.

5. The random copolymer according to claim 1 or 2, wherein The coupling rate was above 60%.

6. The random copolymer according to claim 1 or 2, wherein The content of the aromatic vinyl monomer unit is 10% by mass or more and 50% by mass or less.

7. The random copolymer according to claim 1 or 2, which is in the form of pellets having a median diameter of 6.0 mm to 12.0 mm.

8. A method for producing pellets, which is a method for producing pellets of the random copolymer according to any one of claims 1 to 7, comprising the following steps: a step of polymerizing an aromatic vinyl compound and a conjugated diene compound in a solution, and A step of obtaining pellets by removing the solvent from a solution containing a polymer, This production method can obtain pellets having a median diameter (D50) of 6.0 mm or more and 12.0 mm or less.

9. The method for producing pellets according to claim 8, wherein: The polymerization is continuous.

10. The method for producing pellets according to claim 8 or 9, wherein: The desolventizing is performed by steam stripping at a temperature of 70°C to 110°C.

11. The method for producing pellets according to claim 8 or 9, further comprising: In the modification step, a terminal modification agent containing a nitrogen atom is reacted with the active terminal of the polymer obtained in the polymerization step.

12. The method for producing pellets according to claim 8 or 9, further comprising a step of hydrogenating the polymer obtained in the polymerization step.

13. The method for producing pellets according to claim 8 or 9, wherein: In the polymerization step, a randomizer is added in an amount of 0.01 molar equivalent to 1000 molar equivalent per 1 mole of the polymerization initiator.

14. The method for producing pellets according to claim 8 or 9, wherein: In the polymerization step, a polymerization reactor having an aspect ratio of 4.0 or more is used.

15. A pneumatic tire comprising: The random copolymer according to any one of claims 1 to 7; Rubber components other than the random copolymer; Plasticizer ingredients; and Filler ingredients.