Silicon carbide wafer and method for preparing the same

By controlling the ratio of vanadium to nitrogen and gaseous molecular doping technology, the problems of uneven resistivity distribution and difficulty in purity control in silicon carbide wafers are solved, and the preparation of silicon carbide wafers with high resistance uniformity and high resistivity is achieved, and the preparation of silicon carbide wafers with high resistance uniformity and high resistivity is optimized. Etching defects and microtube density.

CN113990938BActive Publication Date: 2024-12-06GLOBALWAFERS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110849347.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-01-19
Filing Date
2021-07-27
Publication Date
2024-12-06
Estimated Expiration
2041-07-27

AI Technical Summary

Technical Problem

In the preparation of high-resistance silicon carbide wafers in the prior art, there are problems such as uneven resistivity distribution and difficulty in controlling doping concentration, and it is difficult to achieve high resistance uniformity and high purity at the same time.

Method used

By controlling the ratio of vanadium to nitrogen in the range of 2:1 to 10:1 in the silicon carbide wafer, using gaseous molecules doping and preparing silicon carbide wafers at specific temperatures and gas flow conditions, ensuring uniform resistivity distribution and high purity. .

Benefits of technology

The high resistance uniformity and high resistivity of silicon carbide wafers are achieved, and the etching defect density and microtube density are excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113990938B_ABST
    Figure CN113990938B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon carbide wafer and a method for preparing the same. In the silicon carbide wafer, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 2:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 85% of the entire wafer area in the silicon carbide wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a silicon carbide wafer, in particular to a high-resistivity silicon carbide wafer and a preparation method thereof. Background Art

[0002] Currently, silicon wafers have been widely used in the semiconductor industry. Many electronic devices contain silicon chips made of silicon wafers. However, in order to improve the performance of chips, many manufacturers are trying to use silicon carbide wafers as materials to produce silicon carbide chips. Silicon carbide chips have the advantages of high temperature resistance and high stability.

[0003] In the prior art, the preparation of high-resistance silicon carbide wafers is usually accompanied by problems such as uneven resistivity distribution, difficulty in controlling doping concentration, and difficulty in controlling the purity of silicon carbide. How to prepare high-resistance silicon carbide wafers while making the resistivity uniformly distributed and controlling the purity of silicon carbide is a problem that needs to be solved at present. Summary of the invention

[0004] The present invention provides a silicon carbide wafer and a preparation method thereof, which can produce a silicon carbide wafer with high resistance uniformity and high resistivity.

[0005] Some embodiments of the present invention provide a silicon carbide wafer. In the silicon carbide wafer, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 2:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 85% of the entire wafer area in the silicon carbide wafer.

[0006] In some embodiments, the nitrogen concentration in the silicon carbide wafer is 10 16 Atom / cm 3 Up to 9.9*10 16 Atom / cm 3 The range is between 10 17 atoms / cm3 to 9*10 17 Atom / cm 3 between the range of.

[0007] In some embodiments, the nitrogen concentration in the silicon carbide wafer is 10 16 Atom / cm 3 Up to 5*10 16 Atom / cm 3 The range is between 10 17 Atom / cm 3 Up to 3.5*1017 Atom / cm 3 between the range of.

[0008] In some embodiments, the nitrogen concentration in the silicon carbide wafer is 5*10 16 Atom / cm 3 Up to 7*10 16 Atom / cm 3 The vanadium concentration is between 3.5*10 17 Atom / cm 3 Up to 5*10 17 Atom / cm 3 between the range of.

[0009] In some embodiments, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 4.5:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 90% of the entire wafer area in the silicon carbide wafer.

[0010] In some embodiments, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 7:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 95% of the entire wafer area in the silicon carbide wafer.

[0011] In some embodiments, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 8:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 100% of the entire wafer area in the silicon carbide wafer.

[0012] In some embodiments, the etch defect density of the silicon carbide wafer is less than 10,000 ea / cm 2 .

[0013] In some embodiments, the micropipe density of the silicon carbide wafer is less than 1 ea / cm 2 .

[0014] Some other embodiments of the present invention provide a method for preparing a silicon carbide wafer, which includes the following steps: providing a raw material containing carbon and silicon elements and a seed crystal located above the raw material in a reactor; introducing argon gas and vanadium gas into the reactor; heating the reactor and the raw material to form a silicon carbide material on the seed crystal; cooling the reactor and the raw material to obtain a silicon carbide ingot; and cutting the silicon carbide ingot to obtain a plurality of silicon carbide wafers.

[0015] In some embodiments, the flow rate of argon gas introduced into the reactor is in a range of 70 sccm to 85 sccm.

[0016] In some embodiments, the temperature when vanadium gas is introduced into the reactor is in the range of 2050°C to 2250°C.

[0017] Based on the above, the silicon carbide wafer formed by the preparation method of the embodiment of the present invention can have high resistance uniformity and high resistivity by introducing vanadium gaseous molecules for doping and controlling the doping concentration of vanadium and the concentration of nitrogen in a certain proportional relationship. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a schematic diagram of a crystal growth device according to an embodiment of the present invention;

[0019] FIG. 2A to FIG. 2C is a cross-sectional schematic diagram of a method for preparing a silicon carbide wafer according to some embodiments of the present invention;

[0020] Figure 3 FIG. 4 is a flow chart of a method for preparing a silicon carbide wafer according to an embodiment of the present invention.

[0021] Description of Reference Numerals

[0022] 102: Reactor

[0023] 104: Induction coil

[0024] 106: Seed Crystal

[0025] 108: Silicon carbide material

[0026] 108': Silicon carbide wafer

[0027] 108A: Dome top (first surface)

[0028] 108B: Seed end (second surface)

[0029] 110: Raw materials

[0030] D1: First direction

[0031] D2: Second direction

[0032] S10, S20, S30, S40, S50: Steps DETAILED DESCRIPTION

[0033] Reference will now be made in detail to exemplary embodiments of the present invention, examples of which are illustrated in the accompanying drawings. Whenever possible, the same reference numerals are used in the drawings and the description to refer to the same or like parts.

[0034] Figure 1 is a schematic diagram of a crystal growth device according to an embodiment of the present invention. FIG. 2A to FIG. 2Cis a cross-sectional schematic diagram of a method for preparing a silicon carbide wafer according to some embodiments of the present invention. Figure 3 1 is a flow chart of a method for preparing a silicon carbide wafer according to an embodiment of the present invention. Figure 1 Crystal growth equipment and FIG. 2A to FIG. 2C Schematic diagram, with Figure 3 The flowchart of the present invention illustrates the method for preparing a silicon carbide wafer according to some embodiments of the present invention.

[0035] like Figure 1 as well as Figure 3 As shown in step S10, in the crystal growth process, a raw material 110 containing carbon and silicon elements and a seed crystal 106 located above the raw material 110 are provided in the reactor 102. For example, the raw material 110 is, for example, silicon carbide powder, which is placed at the bottom of the reactor 102 as a solid evaporation source. The seed crystal 106 is disposed at the top of the reactor 102. In some embodiments, the seed crystal 106 can be fixed on a seed crystal carrier (not shown) by an adhesive layer. The material of the seed crystal 106 includes silicon carbide. For example, the seed crystal 106 is 6H silicon carbide or 4H silicon carbide.

[0036] like Figure 1 as well as Figure 3 As shown in step S20, in some embodiments, when the raw material 110 and the seed crystal 106 are placed in the reactor 102, the outside air will enter the reactor 102 together, so that the reactor 102 contains gases such as oxygen and nitrogen. Therefore, vanadium gas is introduced into the reactor 102, and gaseous molecules of vanadium are used for doping. This can avoid the problem of solubility limit when using solid vanadium.

[0037] In some embodiments, the flow rate of argon gas introduced into the reactor 102 is 200 sccm or less. In some embodiments, the flow rate of argon gas introduced into the reactor 102 is 150 sccm or less. In some embodiments, the flow rate of argon gas introduced into the reactor 102 is in the range of 10 sccm to 100 sccm. In some preferred embodiments, the flow rate of argon gas introduced into the reactor 102 is in the range of 70 sccm to 85 sccm. In addition, the time for introducing argon gas into the reactor 102 is between 50 hours and 300 hours. In some embodiments, the time for introducing argon gas into the reactor 102 is between 60 hours and 200 hours. In some embodiments, the time for introducing argon gas into the reactor 102 is between 60 hours and 150 hours.

[0038] In some embodiments, the temperature when the vanadium gas is introduced into the reactor 102 is in the range of 2000° C. to 2300° C. In some embodiments, the temperature when the vanadium gas is introduced into the reactor 102 is in the range of 2050° C. to 2250° C. In addition, the time for introducing the vanadium gas into the reactor 102 is in the range of 50 hours to 300 hours. In some embodiments, the time for introducing the vanadium gas into the reactor 102 is in the range of 60 hours to 200 hours. In some embodiments, the time for introducing the vanadium gas into the reactor 102 is in the range of 60 hours to 150 hours.

[0039] In some embodiments, after the argon gas and the vanadium gas are introduced into the reactor 102 , the gas pressure in the reactor 102 is set to 0.1 to 100 torr, and more preferably, the gas pressure in the reactor 102 is set to 0.1 to 20 torr.

[0040] Next, refer to Figure 1 as well as Figure 3 In step S30, the reactor 102 and the raw material 110 are heated to form a silicon carbide crystal 108 on the seed crystal 106. For example, the silicon carbide crystal 108 is formed on the seed crystal 106 by physical vapor transport (PVT). In some embodiments, the reactor 102 and the raw material 110 are heated by the induction coil 104 to form the silicon carbide crystal 108 on the seed crystal 106. During the process, the seed crystal 106 receives the raw material 110 (silicon carbide powder) solidified from the gas state, and slowly grows semiconductor material on the seed crystal 106 until a silicon carbide crystal 108 with a desired size is obtained.

[0041] refer to Figure 1 as well as Figure 3 In step S40, after the silicon carbide crystal 108 grows to the expected size, a silicon carbide ingot can be obtained. The silicon carbide ingot includes a seed crystal end 108B and a rounded end 108A opposite to the seed crystal end 108B, and the seed crystal end 108B is the end of the silicon carbide ingot close to the seed crystal 106, and the rounded end 108A is the end of the silicon carbide ingot away from the seed crystal 106. In some embodiments, the formed ingot can have different crystal structures depending on the crystal orientation of the single crystal seed crystal used. For example, silicon carbide ingots include 4H-silicon carbide, 6H-silicon carbide, etc. 4H-silicon carbide and 6H-silicon carbide belong to the hexagonal crystal system.

[0042] Next, refer to Figure 3 Step S50 and Figure 2A and Figure 2B As shown in FIG. 1 , the silicon carbide ingot (silicon carbide crystal 108) obtained through the crystal growth process is cut to form a silicon carbide wafer. Figure 2AAs shown, the silicon carbide ingot (silicon carbide material 108) can be taken out of the reactor 100. The thickness of the formed silicon carbide ingot is 5 mm to 80 mm, for example, 5 mm to 50 mm or 5 mm to 30 mm. The silicon carbide ingot (silicon carbide material 108) includes a first surface 108A and a second surface 108B opposite to the first surface 108A. The first surface 108A is, for example, a carbon surface (or a rounded end), and the second surface 108B is, for example, a silicon surface (or a seed crystal end).

[0043] Then, if Figure 2B As shown, the silicon carbide ingot (silicon carbide material 108) is cut. For example, the corners of the silicon carbide ingot are cut into equal-diameter cylinders along the first direction D1, and are ground into rounded corners to prevent the corners of the wafer from breaking due to collision. Next, the silicon carbide ingot is sliced ​​along the second direction D2 to cut and separate multiple wafers. The slicing method of the silicon carbide ingot (silicon carbide material 108) includes cutting with a tool or wire in combination with abrasive particles (abrasive particles such as diamond particles). After slicing and grinding and polishing the silicon carbide ingot, multiple wafers such as Figure 2C A silicon carbide wafer 108' is shown.

[0044] In some embodiments, in the formed silicon carbide wafer 108', the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 2:1 to 10:1, and the resistivity thereof is higher than 10 12 The portion of Ω·cm accounts for more than 85% of the entire wafer area of ​​the silicon carbide wafer 108'. In some embodiments, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 4.5:1 to 10:1, and its resistivity is higher than 10 12 The portion of Ω·cm accounts for more than 90% of the entire wafer area in the silicon carbide wafer 108'. In some preferred embodiments, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 7:1 to 10:1, and its resistivity is higher than 10 12 The portion of Ω·cm in the silicon carbide wafer 108' accounts for more than 95% of the entire wafer area. In some preferred embodiments, the ratio of vanadium concentration to nitrogen concentration (V:N) is in the range of 8:1 to 10:1, and its resistivity is higher than 10 12 The Ω·cm portion accounts for more than 100% of the entire wafer area in the silicon carbide wafer 108 ′.

[0045] In some embodiments, the nitrogen concentration in the formed silicon carbide wafer 108' is controlled to be 10 16 Atom / cm 3 Up to 9.9*10 16 Atom / cm 3 The vanadium concentration is controlled within the range of 10 17 Atom / cm3 Up to 9*10 17 Atom / cm 3 In some embodiments, the nitrogen concentration is controlled to be between 10 16 Atom / cm 3 Up to 5*10 16 Atom / cm 3 The vanadium concentration is controlled within the range of 10 17 Atom / cm 3 Up to 3.5*10 17 Atom / cm 3 In another embodiment, the nitrogen concentration is controlled within the range of 5*10 16 Atom / cm 3 Up to 7*10 16 Atom / cm 3 The vanadium concentration is controlled within the range of 3.5*10 17 Atom / cm 3 Up to 5*10 17 Atom / cm 3 between the range of.

[0046] In addition, in the embodiment of the present invention, the etch pit density (EPD) of the formed silicon carbide wafer 108 ′ is less than 10,000 ea / cm 2 In some preferred embodiments, the etching defect density of the formed silicon carbide wafer 108' is less than 9,000 ea / cm 2 In some embodiments, the micropipe density (MPD) of the formed silicon carbide wafer 108' is less than 1 ea / cm 2 In some preferred embodiments, the micropipe density (MPD) of the formed silicon carbide wafer 108' is less than 0.8 ea / cm2, and preferably equal to 0 ea / cm2.

[0047] In order to prove that the method for preparing silicon carbide wafers of the present invention can produce silicon carbide wafers with high resistance uniformity and high resistivity, the following experimental examples are used for illustration. Several experiments are listed below to verify the efficacy of the present invention, but the experimental contents are not intended to limit the scope of the present invention.

[0048] Experimental example

[0049] In the following experimental example, Figure 3The steps described above are used to prepare the silicon carbide wafer. The flow rate of the argon gas and the temperature of the vanadium gas are performed as shown in Table 1. The measurement results of the etching defect density, micropipe density, nitrogen and vanadium concentration ratio and resistivity of the obtained silicon carbide wafer are also shown in Table 1.

[0050] Table 1

[0051]

[0052] As shown in the experimental results of Table 1 above, when the temperature of the vanadium gas is controlled in the range of 2155°C to 2250°C, and the flow rate of the argon gas is controlled in the range of 70sccm to 85sccm, and the vanadium / nitrogen concentration ratio (V:N) is adjusted to meet the range of 2:1 to 10:1 by adjusting the vanadium gas introduction time, a silicon carbide wafer with high resistance uniformity and high resistivity can be obtained. As shown in Experimental Example 3, when the process meets the conditions of the present invention, and the vanadium / nitrogen concentration ratio (V:N) is controlled at 2:1, the portion with a resistivity higher than 1012Ω·cm can account for 85% of the area of ​​the entire silicon carbide wafer. As shown in Experimental Examples 1-2 and 6, when the process meets the conditions of the present invention, and the vanadium / nitrogen concentration ratio (V:N) is controlled at 4.5:1 to 6:1, the portion with a resistivity higher than 1012Ω·cm can account for 90% of the area of ​​the entire silicon carbide wafer. As shown in Experimental Example 4, when the process meets the conditions of the present invention and the vanadium / nitrogen concentration ratio (V:N) is controlled at 7:1, the portion with a resistivity higher than 1012Ω·cm can account for 95% of the area of ​​the entire silicon carbide wafer. As shown in Experimental Examples 5, 7-9, when the process meets the conditions of the present invention and the vanadium / nitrogen concentration ratio (V:N) is controlled in the range of 8:1 to 10:1, the portion with a resistivity higher than 1012Ω·cm can account for 100% of the area of ​​the entire silicon carbide wafer.

[0053] In contrast, as shown in Comparative Example 10, since the temperature of the vanadium gas and the argon gas flow rate are too high, the vanadium / nitrogen concentration ratio (V:N) exceeds the range of 10:1, and the portion with a resistivity higher than 1012Ω·cm accounts for 0% of the total wafer area of ​​the silicon carbide wafer, and the evaluation is poor. In addition, as shown in Comparative Examples 11 and 13, since the temperature of the vanadium gas and the argon gas flow rate are too low, the vanadium / nitrogen concentration ratio (V:N) is lower than the range of 2:1, and the portion with a resistivity higher than 1012Ω·cm accounts for 0% of the total wafer area of ​​the silicon carbide wafer, and the evaluation is poor. Similarly, as shown in Comparative Example 12, if the argon gas flow rate is too low and the nitrogen concentration is too high, the vanadium / nitrogen concentration ratio (V:N) is lower than the range of 2:1, and the portion with a resistivity higher than 1012Ω·cm accounts for 0% of the total wafer area of ​​the silicon carbide wafer, and the evaluation is poor.

[0054] In summary, the silicon carbide wafer formed by the preparation method of the embodiment of the present invention can have high resistance uniformity and high resistivity by introducing vanadium gaseous molecules for doping and controlling the doping concentration of vanadium and the concentration of nitrogen in a certain ratio.

Claims

1. A silicon carbide wafer, characterized in that: In the silicon carbide wafer, the ratio of vanadium concentration to nitrogen concentration is in the range of 2:1 to 10:1, and the resistivity thereof is higher than 10 12 The Ω·cm portion accounts for more than 85% of the entire wafer area in the silicon carbide wafer, and the vanadium concentration is 10 17 Atom / cm 3 Up to 9*10 17 Atom / cm 3 between the range of.

2. The silicon carbide wafer according to claim 1, characterized in that In the silicon carbide wafer, the nitrogen concentration is 10 16 Atom / cm 3 Up to 9.9*10 16 Atom / cm 3 between the ranges.

3. The silicon carbide wafer according to claim 2, characterized in that In the silicon carbide wafer, the nitrogen concentration is 10 16 Atom / cm 3 Up to 5*10 16 Atom / cm 3 and the vanadium concentration is between 10 17 Atom / cm 3 Up to 3.5*10 17 Atom / cm 3 between the range of.

4. The silicon carbide wafer according to claim 2, characterized in that In the silicon carbide wafer, the nitrogen concentration is 5*10 16 Atom / cm 3 Up to 7*10 16 Atom / cm 3 The vanadium concentration is between 3.5*10 17 Atom / cm 3 Up to 5*10 17 Atom / cm 3 between the ranges.

5. The silicon carbide wafer according to claim 1, characterized in that The ratio of the vanadium concentration to the nitrogen concentration is in the range of 4.5:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 90% of the entire wafer area in the silicon carbide wafer.

6. The silicon carbide wafer according to claim 1, characterized in that The ratio of the vanadium concentration to the nitrogen concentration is in the range of 7:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 95% of the entire wafer area in the silicon carbide wafer.

7. The silicon carbide wafer according to claim 1, characterized in that The ratio of the vanadium concentration to the nitrogen concentration is in the range of 8:1 to 10:1, and the resistivity is higher than 10 12 The Ω·cm portion accounts for more than 100% of the entire wafer area in the silicon carbide wafer.

8. The silicon carbide wafer according to claim 1, characterized in that The etching defect density of the silicon carbide wafer is less than 10,000 ea / cm 2 .

9. The silicon carbide wafer according to claim 1, characterized in that The microtube density of the silicon carbide wafer is less than 1ea / cm 2 .

10. A method for preparing a silicon carbide wafer, characterized in that: The method comprises: Providing a raw material containing carbon and silicon elements and a seed crystal located above the raw material in a reactor; Argon gas and vanadium gas are introduced into the reactor, and the flow rate of the argon gas introduced into the reactor is in the range of 70 sccm to 85 sccm, and the temperature of the vanadium gas introduced into the reactor is in the range of 2050° C. to 2250° C.; heating the reactor and the raw material to form silicon carbide material on the seed crystal; Cooling the reactor and the raw material to obtain a silicon carbide ingot; and The silicon carbide ingot is cut to obtain a plurality of silicon carbide wafers.